Production process of functional fiber woven non-woven fabric body
By employing functional fiber woven nonwoven fabric production technology and using modified fibers and nano-agents, the problems of insufficient abrasion resistance, stain resistance, heat insulation and tensile strength of fiber woven nonwoven fabrics have been solved, resulting in a significant improvement in the overall performance of the product.
Patent Information
- Application Number
- CN202511378815.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-25
- Publication Date
- 2025-10-31
- Estimated Expiration
- 2045-09-25
AI Technical Summary
Existing fiber-woven nonwoven fabric products have poor abrasion resistance, poor stain resistance, poor heat insulation, insufficient tensile strength, and unsatisfactory water resistance and UV stability.
The production process of nonwoven fabric using functional fiber weaving involves a composite structure of nonwoven fabric matrix, intermediate layer and outer layer. Modified spandex fiber, polyester fiber, polyester fiber and hemp fiber are interwoven and formed by spraying an outer layer agent. Combined with modified nano-agent and modified liquid treatment, the wear resistance, stain resistance, heat insulation and tensile strength of the fibers are improved.
It significantly improves the abrasion resistance, stain resistance, heat insulation and tensile strength of nonwoven fabrics, and the overall coordination and stability of the product under normal and special conditions are significantly superior.
Smart Images

Figure CN120867114A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nonwoven fabric technology, specifically to a production process for a functional fiber woven nonwoven fabric body. Background Technology
[0002] Nonwoven fabric, also known as non-woven cloth, is composed of oriented or randomly arranged fibers. It is a new generation of environmentally friendly material, named for its resemblance to cloth and some of its properties. Nonwoven fabrics are mainly classified according to their production methods into spunlace nonwoven fabric, thermally bonded nonwoven fabric, wet-laid nonwoven fabric, spunbond nonwoven fabric, meltblown nonwoven fabric, and needle-punched nonwoven fabric. Existing fiber-woven nonwoven fabrics suffer from poor abrasion resistance, poor stain resistance and heat insulation, and low tensile strength, resulting in unsatisfactory overall performance. Furthermore, their poor washability and UV stability limit their usability. Summary of the Invention
[0003] In view of the deficiencies of the prior art, the purpose of this invention is to provide a production process for functional fiber woven nonwoven fabric bodies to solve the problems mentioned in the background art.
[0004] The present invention solves the technical problem by adopting the following technical solution: This invention provides a production process for a functional fiber woven nonwoven fabric body. The nonwoven fabric body includes a nonwoven fabric substrate, an intermediate layer is provided on the upper and lower parts of the nonwoven fabric substrate, and an outer layer is provided on the outside of the intermediate layer. The intermediate layer is bonded to the upper and lower parts of the nonwoven fabric substrate with polyurethane adhesive, and the amount of polyurethane adhesive used is 20g / m². 2 ; The nonwoven fabric matrix is woven from functional fibers, including first modified spandex fibers and polyester fibers. The first modified spandex fibers are used as warp threads and polyester fibers are used as weft threads. The warp and weft threads are woven together to form the nonwoven fabric matrix. The middle layer is formed by interweaving second modified polyester fibers and hemp fibers. The outer layer is coated with an outer layer agent onto the surface of the intermediate layer, with a coating thickness of 0.1-0.15 mm.
[0005] Preferably, the preparation method of the outer layer agent is as follows: Mix 30-35 parts by weight of polyurethane resin with a solid content of 45%, 15-25 parts by weight of bisphenol A type epoxy resin, 4-7 parts by weight of m-phenylenediamine curing agent, and 40-45 parts by weight of acetone solvent evenly, and then add 5-8 parts by weight of modified nano-agent and continue to mix thoroughly to obtain the outer layer agent. The preparation method of the modified nanoparticles is as follows: S1a: Mix 3-5 parts of β-cyclodextrin, 1-2 parts of silane coupling agent KH560 and 15-20 parts of aqueous ethanol solution thoroughly to obtain β-cyclodextrin solution; S1b: Nano-calcium carbonate, nano-bentonite, and β-cyclodextrin were mixed and compounded in a weight ratio of (2-3):(4-6):11. After mixing, the mixture was filtered and dried to obtain the modified nano-agent.
[0006] Preferably, the mass fraction of the ethanol-water solution is 75-80%; the stirring speed is 750-850 r / min, and the stirring time is 2 h.
[0007] Preferably, the method for preparing the first modified spandex fiber is as follows: The spandex fiber was immersed in a sufficient amount of the first modification solution for immersion treatment. After immersion, it was dried at room temperature to obtain the first modified spandex fiber. The immersion power of the immersion treatment was 450-500W, the immersion time was 1h, and the immersion pressure was 10-15MPa. The preparation method of the first modified liquid is as follows: S21: Mix 5-8 parts of flake boron nitride, 3-5 parts of glass fiber, 5-8 parts of sodium carboxymethyl cellulose, 7-11 parts of sodium alginate solution, and 1-2 parts of nano silica sol thoroughly, then filter and dry to obtain flake boron nitride modifier. S22: 4-7 parts of flake boron nitride modifier, 5-8 parts of 8% (w / w) dopamine hydrochloride solution and 1-2 parts of nano zinc oxide are mixed evenly to obtain flake boron nitride solution; S23: Mix 2-4 parts of attapulgite, 3-5 parts of sodium lignosulfonate solution and 1-2 parts of mullite whiskers thoroughly to obtain a compound solution; mix the compound solution and flake boron nitride solution at a weight ratio of 5:(9-11) and ultrasonically treat to obtain the first modified solution.
[0008] Preferably, the sodium lignosulfonate solution has a mass fraction of 10-15%; the sodium alginate solution has a mass fraction of 6-10%.
[0009] Preferably, the ultrasonic power of the blending ultrasonic treatment is 350-400W, and the ultrasonic treatment lasts for 1 hour.
[0010] Preferably, the method for preparing the second modified polyester fiber is as follows: The polyester fiber was impregnated in a sufficient amount of the second modification solution. The impregnation power was 400-500W, the impregnation time was 1 hour, the impregnation pressure was 15MPa, and after the impregnation was completed, it was dried at room temperature to obtain the second modified polyester fiber.
[0011] Preferably, the second modified liquid comprises the following raw materials in parts by weight: 3-5 parts glass microspheres, 2-5 parts lanthanum oxide, 4-6 parts chitosan solution, 1-2 parts magnesium aluminum spinel, and 2-4 parts zirconium silicate.
[0012] Preferably, the chitosan solution has a mass fraction of 2-5%.
[0013] Compared with the prior art, the present invention has the following beneficial effects: The nonwoven fabric body of this invention is made of a nonwoven fabric matrix, an intermediate layer and an outer layer in combination. The nonwoven fabric matrix is woven from a first modified spandex fiber and polyester fiber, the intermediate layer is woven from a second modified polyester fiber and hemp fiber, and the outer layer is formed by spraying an outer layer agent. Through the coordination between the layers, the product has excellent wear resistance, stain resistance, heat insulation and tensile strength, and the overall coordination effect of the product is significant. At the same time, the product has excellent water resistance and UV stability. The first modified spandex fiber is treated by immersing the spandex fiber in a sufficient amount of the first modification solution. The first modification solution contains a compounding solution and a flake-shaped boron nitride solution, which are ultrasonically modified together. The flake-shaped boron nitride has a flake structure and excellent mechanical strength; its flake morphology can form a physical barrier on the fiber surface, improving the abrasion resistance and tear resistance of the spandex fiber. Simultaneously, the good chemical stability of boron nitride enhances the fiber's wash resistance and UV resistance. Glass fiber, as a rigid reinforcing phase, further enhances the fiber's breaking strength due to its high strength properties. Furthermore, the process involves re-blending sodium carboxymethyl cellulose, sodium alginate solution, and nano-silica sol raw materials. Through the synergistic coordination of these raw materials, the fiber's properties are further improved. The product's performance is further enhanced by the following steps: Ratosite, a layered clay mineral, has a lamellar structure that forms a barrier layer on the fiber surface, further enhancing the product's barrier properties and optimizing its insulation functions. Meanwhile, mullite whiskers, with their high-strength, high-modulus needle-like structure, form a "point-line-surface" multi-dimensional reinforcement system with lamellar boron nitride and glass fibers, further improving the product's performance. The intermediate layer of polyester fiber is impregnated in a second modification solution. The glass microspheres in the second modification solution harmonize with lanthanum oxide, magnesium aluminum spinel, and zirconium silicate raw materials. Through the synergistic effect of these raw materials, they work together to enhance the product's performance. The curing agents, including polyurethane resin, bisphenol A epoxy resin, and m-phenylenediamine, as well as the blending and modifying nano-agents in the outer layer, optimize the product's performance through the co-coordination of raw materials. The modified nano-agents are composed of nano-calcium carbonate, nano-bentonite, and β-cyclodextrin solution. The β-cyclodextrin solution contains β-cyclodextrin, silane coupling agent KH560, and ethanol aqueous solution, which are mutually blended and optimized. Through the co-coordination and synergy of raw materials, β-cyclodextrin, with its amphiphilic structure, is compatible with both organic and inorganic materials. Combined with the silane coupling agent KH560, it acts as a bridge, connecting with nano-calcium carbonate and nano-bentonite on one hand, and with organic groups on the other, enhancing the connectivity of the raw materials. At the same time, nano-bentonite, with its layered silicate structure, acts as a barrier, while also coordinating with nano-calcium carbonate, optimizing the product's performance coordination, and improving the system's water resistance and UV stability. Attached Figure Description
[0014] Figure 1 This is a schematic diagram of the nonwoven fabric body structure of the present invention. Detailed Implementation
[0015] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to specific examples. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0016] The production process of a functional fiber woven nonwoven fabric body according to this embodiment includes the following steps: The nonwoven fabric matrix 1 is woven from functional fibers, including first modified spandex fibers and polyester fibers. The first modified spandex fibers are used as warp and polyester fibers are used as weft. The warp and weft are woven to form the nonwoven fabric matrix 1. The intermediate layer 2 is formed by interlacing and weaving second modified polyester fibers and hemp fibers. The intermediate layer 2 is bonded to the upper and lower parts of the nonwoven fabric matrix 1 with polyurethane adhesive, and the amount of polyurethane adhesive used is 20g / m². 2 ; The outer layer 3 is formed by spraying an outer layer agent onto the surface of the intermediate layer 2. The spraying thickness is 0.1-0.15mm. The outer layer 3, the intermediate layer 2, and the non-woven fabric substrate 1 are arranged sequentially from top to bottom.
[0017] The preparation method of the outer layer agent in this embodiment is as follows: Mix 30-35 parts by weight of polyurethane resin with a solid content of 45%, 15-25 parts by weight of bisphenol A type epoxy resin, 4-7 parts by weight of m-phenylenediamine curing agent, and 40-45 parts by weight of acetone solvent evenly, and then add 5-8 parts by weight of modified nano-agent and continue to mix thoroughly to obtain the outer layer agent. The preparation method of the modified nanoparticles is as follows: S1a: Mix 3-5 parts of β-cyclodextrin, 1-2 parts of silane coupling agent KH560 and 15-20 parts of aqueous ethanol solution thoroughly to obtain β-cyclodextrin solution; S1b: Nano-calcium carbonate, nano-bentonite, and β-cyclodextrin were mixed and compounded in a weight ratio of (2-3):(4-6):11. After mixing, the mixture was filtered and dried to obtain the modified nano-agent.
[0018] In this embodiment, the ethanol-water solution has a mass fraction of 75-80%; the stirring speed is 750-850 r / min, and the stirring time is 2 h.
[0019] The preparation method of the first modified spandex fiber in this embodiment is as follows: The spandex fiber was immersed in a sufficient amount of the first modification solution for immersion treatment. After immersion, it was dried at room temperature to obtain the first modified spandex fiber. The immersion power of the immersion treatment was 450-500W, the immersion time was 1h, and the immersion pressure was 10-15MPa. The preparation method of the first modified liquid is as follows: S21: Mix 5-8 parts of flake boron nitride, 3-5 parts of glass fiber, 5-8 parts of sodium carboxymethyl cellulose, 7-11 parts of sodium alginate solution, and 1-2 parts of nano silica sol thoroughly, then filter and dry to obtain flake boron nitride modifier. S22: 4-7 parts of flake boron nitride modifier, 5-8 parts of 8% (w / w) dopamine hydrochloride solution and 1-2 parts of nano zinc oxide are mixed evenly to obtain flake boron nitride solution; S23: Mix 2-4 parts of attapulgite, 3-5 parts of sodium lignosulfonate solution and 1-2 parts of mullite whiskers thoroughly to obtain a compound solution; mix the compound solution and flake boron nitride solution at a weight ratio of 5:(9-11) and ultrasonically treat to obtain the first modified solution.
[0020] In this embodiment, the sodium lignosulfonate solution has a mass fraction of 10-15%; the sodium alginate solution has a mass fraction of 6-10%.
[0021] In this embodiment, the ultrasonic power for the blending ultrasonic treatment is 350-400W, and the ultrasonic treatment lasts for 1 hour.
[0022] The preparation method of the second modified polyester fiber in this embodiment is as follows: The polyester fiber was impregnated in a sufficient amount of the second modification solution. The impregnation power was 400-500W, the impregnation time was 1 hour, the impregnation pressure was 15MPa, and after the impregnation was completed, it was dried at room temperature to obtain the second modified polyester fiber.
[0023] The second modified liquid in this embodiment comprises the following raw materials in parts by weight: 3-5 parts glass microspheres, 2-5 parts lanthanum oxide, 4-6 parts chitosan solution, 1-2 parts magnesium aluminum spinel, and 2-4 parts zirconium silicate.
[0024] The chitosan solution in this embodiment has a mass fraction of 2-5%. Example 1
[0025] The production process of a functional fiber woven nonwoven fabric body according to this embodiment includes the following steps: The nonwoven fabric matrix 1 is woven from functional fibers, including first modified spandex fibers and polyester fibers. The first modified spandex fibers are used as warp and polyester fibers are used as weft. The warp and weft are woven to form the nonwoven fabric matrix 1. The intermediate layer 2 is formed by interlacing and weaving second modified polyester fibers and hemp fibers. The intermediate layer 2 is bonded to the upper and lower parts of the nonwoven fabric matrix 1 with polyurethane adhesive, and the amount of polyurethane adhesive used is 20g / m². 2 ; The outer layer 3 is formed by spraying an outer layer agent onto the surface of the intermediate layer 2, with a spraying thickness of 0.1 mm. The outer layer 3, the intermediate layer 2, and the non-woven fabric substrate 1 are arranged sequentially from top to bottom.
[0026] The preparation method of the outer layer agent in this embodiment is as follows: 30 parts by weight of polyurethane resin with a solid content of 45%, 15 parts by weight of bisphenol A type epoxy resin, 4 parts of m-phenylenediamine curing agent, and 40 parts of acetone solvent are mixed evenly, and then 5 parts of modified nano-agent are added and mixed evenly to obtain the outer layer agent. The preparation method of the modified nanoparticles is as follows: S1a: Mix 3 parts of β-cyclodextrin, 1 part of silane coupling agent KH560 and 15 parts of ethanol aqueous solution thoroughly to obtain β-cyclodextrin solution; S1b: Nano-calcium carbonate, nano-bentonite, and β-cyclodextrin were mixed and compounded in a weight ratio of 2:4:11. After mixing, the mixture was filtered and dried to obtain the modified nano-agent.
[0027] In this embodiment, the ethanol-water solution has a mass fraction of 75%; the stirring speed for the mixing process is 750 r / min, and the stirring time is 2 h.
[0028] The preparation method of the first modified spandex fiber in this embodiment is as follows: The spandex fiber was immersed in a sufficient amount of the first modification solution for immersion treatment. After immersion, it was dried at room temperature to obtain the first modified spandex fiber. The immersion power of the immersion treatment was 450W, the immersion time was 1h, and the immersion pressure was 10MPa. The preparation method of the first modified liquid is as follows: S21: Mix 5 parts of flake boron nitride, 3 parts of glass fiber, 5 parts of sodium carboxymethyl cellulose, 7 parts of sodium alginate solution and 1 part of nano silica sol thoroughly, then filter and dry to obtain flake boron nitride modifier. S22: 4 parts of flake boron nitride modifier, 5 parts of 8% (w / w) dopamine hydrochloride solution and 1 part of nano zinc oxide are mixed evenly to obtain flake boron nitride solution; S23: Mix 2 parts of attapulgite, 3 parts of sodium lignosulfonate solution and 1 part of mullite whiskers thoroughly to obtain a mixed solution; mix the mixed solution and flake boron nitride solution at a weight ratio of 5:9 and sonicate to obtain the first modified solution.
[0029] In this embodiment, the sodium lignosulfonate solution has a mass fraction of 10%; the sodium alginate solution has a mass fraction of 6%.
[0030] In this embodiment, the ultrasonic power for the blending ultrasonic treatment is 350W, and the ultrasonic treatment lasts for 1 hour.
[0031] The preparation method of the second modified polyester fiber in this embodiment is as follows: The polyester fiber was impregnated in a sufficient amount of the second modification solution. The impregnation power was 400W, the impregnation time was 1 hour, and the impregnation pressure was 15MPa. After the impregnation was completed, the fiber was dried at room temperature to obtain the second modified polyester fiber.
[0032] The second modified liquid in this embodiment comprises the following raw materials in parts by weight: 3 parts glass microspheres, 2 parts lanthanum oxide, 4 parts chitosan solution, 1 part magnesium aluminum spinel, and 2 parts zirconium silicate.
[0033] The chitosan solution in this embodiment has a mass fraction of 2%. Example 2
[0034] The production process of a functional fiber woven nonwoven fabric body according to this embodiment includes the following steps: The nonwoven fabric matrix 1 is woven from functional fibers, including first modified spandex fibers and polyester fibers. The first modified spandex fibers are used as warp and polyester fibers are used as weft. The warp and weft are woven to form the nonwoven fabric matrix 1. The intermediate layer 2 is formed by interlacing and weaving second modified polyester fibers and hemp fibers. The intermediate layer 2 is bonded to the upper and lower parts of the nonwoven fabric matrix 1 with polyurethane adhesive, and the amount of polyurethane adhesive used is 20g / m². 2 ; The outer layer 3 is formed by spraying an outer layer agent onto the surface of the intermediate layer 2, with a spraying thickness of 0.15 mm. The outer layer 3, the intermediate layer 2, and the non-woven fabric substrate 1 are arranged sequentially from top to bottom.
[0035] The preparation method of the outer layer agent in this embodiment is as follows: 35 parts by weight of polyurethane resin with a solid content of 45%, 25 parts by weight of bisphenol A type epoxy resin, 7 parts of m-phenylenediamine curing agent, and 45 parts of acetone solvent were mixed evenly, and then 8 parts of modified nano-agent were added and mixed evenly to obtain the outer layer agent. The preparation method of the modified nanoparticles is as follows: S1a: Mix 5 parts of β-cyclodextrin, 2 parts of silane coupling agent KH560 and 20 parts of ethanol aqueous solution thoroughly to obtain β-cyclodextrin solution; S1b: Nano-calcium carbonate, nano-bentonite, and β-cyclodextrin were mixed and compounded in a weight ratio of 3:6:11. After mixing, the mixture was filtered and dried to obtain the modified nano-agent.
[0036] In this embodiment, the ethanol-water solution has a mass fraction of 80%; the stirring speed for the mixing process is 850 r / min, and the stirring time is 2 h.
[0037] The preparation method of the first modified spandex fiber in this embodiment is as follows: The spandex fiber was immersed in a sufficient amount of the first modification solution for immersion treatment. After immersion, it was dried at room temperature to obtain the first modified spandex fiber. The immersion power of the immersion treatment was 500W, the immersion time was 1h, and the immersion pressure was 15MPa. The preparation method of the first modified liquid is as follows: S21: Mix 8 parts of flake boron nitride, 5 parts of glass fiber, 8 parts of sodium carboxymethyl cellulose, 11 parts of sodium alginate solution and 2 parts of nano silica sol thoroughly, then filter and dry to obtain flake boron nitride modifier. S22: 7 parts of flake boron nitride modifier, 8 parts of 8% (w / w) dopamine hydrochloride solution and 2 parts of nano zinc oxide are mixed evenly to obtain flake boron nitride solution; S23: Mix 4 parts of attapulgite, 5 parts of sodium lignosulfonate solution and 2 parts of mullite whiskers thoroughly to obtain a compound solution; mix the compound solution and flake boron nitride solution at a weight ratio of 5:11 and sonicate to obtain the first modified solution.
[0038] In this embodiment, the sodium lignosulfonate solution has a mass fraction of 15%; the sodium alginate solution has a mass fraction of 10%.
[0039] In this embodiment, the ultrasonic power for the blending ultrasonic treatment is 400W, and the ultrasonic treatment lasts for 1 hour.
[0040] The preparation method of the second modified polyester fiber in this embodiment is as follows: The polyester fiber was impregnated in a sufficient amount of the second modification solution. The impregnation power was 500W, the impregnation time was 1 hour, and the impregnation pressure was 15MPa. After the impregnation was completed, the fiber was dried at room temperature to obtain the second modified polyester fiber.
[0041] The second modified liquid in this embodiment comprises the following raw materials in parts by weight: 5 parts glass microspheres, 5 parts lanthanum oxide, 6 parts chitosan solution, 2 parts magnesium aluminum spinel, and 4 parts zirconium silicate.
[0042] The chitosan solution in this embodiment has a mass fraction of 5%. Example 3
[0043] The production process of a functional fiber woven nonwoven fabric body according to this embodiment includes the following steps: The nonwoven fabric matrix 1 is woven from functional fibers, including first modified spandex fibers and polyester fibers. The first modified spandex fibers are used as warp and polyester fibers are used as weft. The warp and weft are woven to form the nonwoven fabric matrix 1. The intermediate layer 2 is formed by interlacing and weaving second modified polyester fibers and hemp fibers. The intermediate layer 2 is bonded to the upper and lower parts of the nonwoven fabric matrix 1 with polyurethane adhesive, and the amount of polyurethane adhesive used is 20g / m². 2 ; The outer layer 3 is formed by spraying an outer layer agent onto the surface of the intermediate layer 2, with a spraying thickness of 0.12 mm. The outer layer 3, the intermediate layer 2, and the non-woven fabric substrate 1 are arranged sequentially from top to bottom.
[0044] The preparation method of the outer layer agent in this embodiment is as follows: 32.5 parts by weight of polyurethane resin with a solid content of 45%, 20 parts by weight of bisphenol A epoxy resin, 5.5 parts by weight of m-phenylenediamine curing agent, and 42.5 parts by weight of acetone solvent were mixed evenly, and then 6.5 parts by weight of modified nano-agent were added and mixed evenly to obtain the outer layer agent. The preparation method of the modified nanoparticles is as follows: S1a: Mix 4 parts of β-cyclodextrin, 1.5 parts of silane coupling agent KH560 and 17.5 parts of ethanol aqueous solution thoroughly to obtain β-cyclodextrin solution; S1b: Nano-calcium carbonate, nano-bentonite, and β-cyclodextrin were mixed and compounded in a weight ratio of 2.5:5:11. After mixing, the mixture was filtered and dried to obtain the modified nano-agent.
[0045] In this embodiment, the ethanol-water solution has a mass fraction of 78.5%; the stirring speed is 800 r / min, and the stirring time is 2 h.
[0046] The preparation method of the first modified spandex fiber in this embodiment is as follows: The spandex fiber was immersed in a sufficient amount of the first modification solution for immersion treatment. After immersion, it was dried at room temperature to obtain the first modified spandex fiber. The immersion power of the immersion treatment was 475W, the immersion time was 1h, and the immersion pressure was 12.5MPa. The preparation method of the first modified liquid is as follows: S21: 6.5 parts of flake boron nitride, 4 parts of glass fiber, 6.5 parts of sodium carboxymethyl cellulose, 9 parts of sodium alginate solution, and 1.5 parts of nano silica sol are mixed and stirred thoroughly, then filtered and dried to obtain flake boron nitride modifier; S22: 5.5 parts of flake boron nitride modifier, 6.5 parts of 8% (w / w) dopamine hydrochloride solution and 1.5 parts of nano zinc oxide are mixed evenly to obtain flake boron nitride solution; S23: Mix 3 parts of attapulgite, 4 parts of sodium lignosulfonate solution and 1.5 parts of mullite whiskers thoroughly to obtain a compound solution; mix the compound solution and flake boron nitride solution at a weight ratio of 5:10 and sonicate to obtain the first modified solution.
[0047] In this embodiment, the sodium lignosulfonate solution has a mass fraction of 12.5%; the sodium alginate solution has a mass fraction of 8%.
[0048] In this embodiment, the ultrasonic power for the blending ultrasonic treatment is 375W, and the ultrasonic treatment lasts for 1 hour.
[0049] The preparation method of the second modified polyester fiber in this embodiment is as follows: The polyester fiber was impregnated in a sufficient amount of the second modification solution. The impregnation power was 450W, the impregnation time was 1 hour, the impregnation pressure was 15MPa, and after the impregnation was completed, it was dried at room temperature to obtain the second modified polyester fiber.
[0050] The second modified liquid in this embodiment comprises the following raw materials in parts by weight: 4 parts glass microspheres, 3.5 parts lanthanum oxide, 5 parts chitosan solution, 1.5 parts magnesium aluminum spinel, and 3 parts zirconium silicate.
[0051] The chitosan solution in this embodiment has a mass fraction of 3.5%.
[0052] Comparative Example 1. Unlike Example 3, no nano-calcium carbonate or nano-bentonite was added during the preparation of the modified nano-agent.
[0053] Comparative Example 2. Unlike Example 3, β-cyclodextrin was not added in the preparation of the modified nanoparticles.
[0054] Comparative Example 3. Unlike Example 3, the first modification liquid was not added in the preparation of the first modified spandex fiber.
[0055] Comparative Example 4. Unlike Example 3, no flake boron nitride solution was added to the first modified solution.
[0056] Comparative Example 5. Unlike Example 3, no sheet boron nitride or glass fiber was added to the sheet boron nitride solution.
[0057] Comparative Example 6. Unlike Example 3, no compounding solution was added to the first modified solution.
[0058] Comparative Example 7. Unlike Example 3, no attapulgite and mullite whiskers were added to the reconstitution solution.
[0059] Comparative Example 8. Unlike Example 3, no second modifying liquid was added during the preparation of the second modified polyester fiber.
[0060] Comparative Example 9. Unlike Example 3, the second modified liquid did not contain glass microspheres or lanthanum oxide.
[0061] Comparative Example 10. Unlike Example 3, magnesium aluminum spinel and zirconium silicate were not added to the second modified liquid.
[0062] Examples 1-3 and Comparative Examples 1-10 were subjected to abrasion resistance (according to GB / T21196.3-2007 "Textiles - Martindale Method - Determination of Abrasion Resistance of Fabrics - Part 3 - Determination of Mass Loss", with a sample size of 38 mm in diameter, a load of 9 kPa, and 600 rpm of friction, and the mass loss rate was recorded), stain resistance, thermal insulation (the warmth retention rate of the UV-resistant thermal insulation fabric was tested according to GB / T11048-2008 standard), and tensile strength tests. The performance test results are as follows:
[0063] From Examples 1-3 and Comparative Examples 1-10, it can be seen that Example 3 of the present invention has excellent wear resistance, stain resistance, heat insulation and fracture strength, and the overall coordination effect of the product is significant.
[0064] This invention further tests the product's resistance to washing and UV radiation (the product is tested at a UV intensity of 300 W / m). 2 The product was irradiated for 24 hours under the specified conditions, then washed with water 5 times (this constitutes one cycle of 10 cycles). The performance test results are as follows:
[0065] As can be seen from Comparative Examples 1-10 and Examples 1-3; The product of Example 3 not only exhibits excellent wear resistance, stain resistance, heat insulation, and tensile strength under normal conditions, but also maintains excellent performance under conditions of water resistance and UV resistance, demonstrating significant stability in water resistance and UV resistance. As can be seen from Comparative Examples 1-10 and Example 3, the performance of the products tends to deteriorate when nano-calcium carbonate and nano-bentonite are not added in the preparation of the modified nano-agent, and β-cyclodextrin solution is not added in the preparation of the modified nano-agent. The performance of the product is most obvious when the modified nano-agent of the present invention is used. The first modified spandex fiber was not prepared without the first modifying liquid, and the second modified polyester fiber was not prepared without the second modifying liquid. The performance of the products tended to deteriorate, especially under conditions of water washing resistance and UV resistance. The first modified solution did not contain flake boron nitride solution, nor did it contain flake boron nitride or glass fiber. The first modified solution also did not contain a compounding solution, nor did it contain attapulgite or mullite whiskers. All of these resulted in varying degrees of performance degradation in the products. The first modified spandex fiber modified with the first modified solution obtained using the specific method of this invention exhibited the most significant performance improvement. Meanwhile, the second modified solution did not contain glass microspheres, lanthanum oxide, magnesium aluminum spinel, or zirconium silicate. All of these results in a deterioration in the product performance. Only the second modified solution prepared using the method of this invention showed the most significant performance improvement; other methods were not as effective as those of this invention.
[0066] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
[0067] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A production process for a functional fiber woven nonwoven fabric body, characterized in that, The nonwoven fabric body includes a nonwoven fabric substrate (1), with an intermediate layer (2) provided on the upper and lower parts of the nonwoven fabric substrate (1), and an outer layer (3) provided on the outside of the intermediate layer (2). The intermediate layer (2) is bonded to the upper and lower parts of the nonwoven fabric matrix (1) by polyurethane adhesive, with the amount of polyurethane adhesive being 20 g / m. 2 ; The nonwoven fabric matrix (1) is woven from functional fibers, including first modified spandex fibers and polyester fibers. The first modified spandex fibers are used as warp and polyester fibers are used as weft. The warp and weft are woven to form the nonwoven fabric matrix (1); the intermediate layer (2) is formed by interlacing and weaving second modified polyester fibers and hemp fibers. The outer layer (3) is coated with an outer layer agent on the surface of the intermediate layer (2), with a coating thickness of 0.1-0.15 mm.
2. The production process of a functional fiber woven nonwoven fabric body according to claim 1, characterized in that, The preparation method of the outer layer agent is as follows: Mix 30-35 parts by weight of polyurethane resin with a solid content of 45%, 15-25 parts by weight of bisphenol A type epoxy resin, 4-7 parts by weight of m-phenylenediamine curing agent, and 40-45 parts by weight of acetone solvent evenly, and then add 5-8 parts by weight of modified nano-agent and continue to mix thoroughly to obtain the outer layer agent. The preparation method of the modified nanoparticles is as follows: S1a: Mix 3-5 parts of β-cyclodextrin, 1-2 parts of silane coupling agent KH560 and 15-20 parts of aqueous ethanol solution thoroughly to obtain β-cyclodextrin solution; S1b: Nano-calcium carbonate, nano-bentonite, and β-cyclodextrin were mixed and compounded in a weight ratio of (2-3):(4-6):
11. After mixing, the mixture was filtered and dried to obtain the modified nano-agent.
3. The production process of a functional fiber woven nonwoven fabric body according to claim 2, characterized in that, The ethanol-water solution has a mass fraction of 75-80%; the stirring speed for the mixing process is 750-850 r / min, and the stirring time is 2 h.
4. The production process of a functional fiber woven nonwoven fabric body according to claim 2, characterized in that, The preparation method of the first modified spandex fiber is as follows: The spandex fiber was immersed in a sufficient amount of the first modification solution for immersion treatment. After immersion, it was dried at room temperature to obtain the first modified spandex fiber. The immersion power of the immersion treatment was 450-500W, the immersion time was 1h, and the immersion pressure was 10-15MPa. The preparation method of the first modified liquid is as follows: S21: Mix 5-8 parts of flake boron nitride, 3-5 parts of glass fiber, 5-8 parts of sodium carboxymethyl cellulose, 7-11 parts of sodium alginate solution, and 1-2 parts of nano silica sol thoroughly, then filter and dry to obtain flake boron nitride modifier. S22: 4-7 parts of flake boron nitride modifier, 5-8 parts of 8% (w / w) dopamine hydrochloride solution and 1-2 parts of nano zinc oxide are mixed evenly to obtain flake boron nitride solution; S23: Mix 2-4 parts of attapulgite, 3-5 parts of sodium lignosulfonate solution and 1-2 parts of mullite whiskers thoroughly to obtain a compound solution; mix the compound solution and flake boron nitride solution at a weight ratio of 5:(9-11) and ultrasonically treat to obtain the first modified solution.
5. The production process of a functional fiber woven nonwoven fabric body according to claim 4, characterized in that, The sodium lignosulfonate solution has a mass fraction of 10-15%; the sodium alginate solution has a mass fraction of 6-10%.
6. The production process of a functional fiber woven nonwoven fabric body according to claim 4, characterized in that, The ultrasonic power of the blending ultrasonic treatment is 350-400W, and the ultrasonic treatment lasts for 1 hour.
7. The production process of a functional fiber woven nonwoven fabric body according to claim 1, characterized in that, The preparation method of the second modified polyester fiber is as follows: The polyester fiber was impregnated in a sufficient amount of the second modification solution. The impregnation power was 400-500W, the impregnation time was 1 hour, the impregnation pressure was 15MPa, and after the impregnation was completed, it was dried at room temperature to obtain the second modified polyester fiber.
8. The production process of a functional fiber woven nonwoven fabric body according to claim 7, characterized in that, The second modified liquid comprises the following raw materials in parts by weight: 3-5 parts glass microspheres, 2-5 parts lanthanum oxide, 4-6 parts chitosan solution, 1-2 parts magnesium aluminum spinel, and 2-4 parts zirconium silicate.
9. The production process of a functional fiber woven nonwoven fabric body according to claim 8, characterized in that, The chitosan solution has a mass fraction of 2-5%.
Citation Information
Patent Citations
Synthetic leather for luggage and production method of synthetic leather
CN104264500A
Articles comprising melt-processable cellulose acetate composition comprising alkaline filler
CN118382371A
Flame-retardant fiber fireproof thermal-insulation knitted composite cotton and preparation process thereof
CN119840263A
Composite washable polyester warp knitted fabric and production method thereof
CN119956554A
High-temperature-resistant polypropylene capacitor film and preparation method thereof
CN120059351A
Cited By
Moisture absorption and sweat releasing fabric and preparation process thereof
CN121087682A
Integrated ultralight running fabric and preparation method thereof
CN121381264A
A production process of a high-strength vamp mesh fabric
CN122382762A
Graphene-modified super-soft knitted lyocell fiber product and preparation method thereof
CN122382763A