Forging method for reducing bar concave center

By using upper and lower circular arc anvils and controlling forging parameters during bar forging, the problem of uneven deformation on the surface and in the core of the bar was solved, achieving uniform fine grains and reducing concave cores, thus improving the bar yield.

CN120940555APending Publication Date: 2025-11-14AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202511129877.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-13
Publication Date
2025-11-14

AI Technical Summary

Technical Problem

During the forging process, large-diameter bars are prone to uneven deformation due to the uneven pressure on the surface and core, resulting in problems such as concave cores and poor surface quality.

Method used

The design and control of forging parameters, including upsetting and drawing steps, are adopted by using upper and lower arc anvils. The design of the bar upsetting process is to form an arc-shaped end with a central bulge, and the drawing process starts from a specific position to press down. Combined with appropriate temperature and pressing amount control, the indentation caused by insufficient core deformation is prevented.

Benefits of technology

This method achieves uniform fine-grained deformation of the bar stock, reduces concave defects, and improves the yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120940555A_ABST
    Figure CN120940555A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of titanium alloy material preparation, and particularly relates to a forging method for reducing bar caves. By designing the special tool for the bar arc, when the bar is upset, the end of the bar can form an arc-shaped end with the center protruding, the concave center caused by small deformation of the center during drawing can be prevented, the bar is pressed downwards from the position away from the end by a certain distance in the drawing process, the temperature of the outer circumference of the bar is lower than that of the center at the moment, and therefore the bar is not prone to deformation. The deformation resistance of the center part is lower, materials on the end face of the part, not subjected to drawing-out, of the bar can be extruded towards the center part to avoid sinking, meanwhile, in the second round of deformation, the arc anvil is adopted for upsetting so as to flatten uneven deformation of the end in the first round of deformation, and in the third round of deformation, the bar is long and not prone to deformation. Upsetting is not carried out, so that bending deformation of the bar is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy material preparation technology, specifically a forging method for reducing the concavity of bar stock. Background Technology During the forging process of large-diameter bars, the uneven pressure on the surface and core of the bar leads to uneven deformation of the surface and core. The surface deformation is large while the core deformation is small, which easily causes core depression. The surface of the bar has good metal fluidity and the edges are not constrained, which easily leads to defects such as irregular edge shape, which seriously affects the surface quality and yield of the bar. Summary of the Invention

[0002] The purpose of this invention is to provide a forging method that reduces the concave center of the bar stock, thereby obtaining uniform fine-grained bars, reducing the concave center, and improving the yield.

[0003] The technical solution of this invention: A process for reducing the concave center of a bar stock, wherein the original diameter of the bar stock is Φ550-620mm, the length is 1000mm-1500mm, and the diameter of the drawn bar stock is Φ200-250mm; comprising the following steps: Step 1: Design and manufacture upper and lower circular arc anvils for upsetting bar stock. The chord length L of the circular arc anvil is equal to the diameter R+ of the bar stock, and the arc height H is 100-200mm. Step 2: Heat the bar to the forging temperature and hold it at that temperature. Preheat the upper and lower circular anvils. Use the upper and lower circular anvils for upsetting. Place the lower circular anvil on the lower anvil surface. Place the bar to be upset vertically on the circular surface of the lower circular anvil. Place the circular surface of the upper circular anvil on the top of the bar and start upsetting. Upset the bar to 70% of its original height. After upsetting, rotate the bar 90° along the axial direction to start drawing. When drawing, start pressing down from a distance of 100-150mm from either end to draw the bar. Control the amount of pressure applied with each hammer blow. Lengthen the bar diameter to 450-480mm. Hot material can be returned to the furnace during the drawing process. Step 3: Perform a second round of drawing on the bar obtained in Step 2. Use upper and lower circular arc anvils for upsetting. Place the lower circular arc anvil on the lower anvil surface. Place the bar obtained in Step 2 vertically on the circular arc surface of the lower circular arc anvil. Place the circular arc surface of the upper circular arc anvil on the top of the bar obtained in Step 2 and start upsetting. Upset downwards by 100-150mm. After upsetting, rotate the bar 90° along the axial direction. When drawing, start pressing down from a distance of 150-200mm from any end to draw. Control the amount of pressing down with each hammer. Lengthen the diameter of the bar to 300-320mm. Hot material can be returned to the furnace during the drawing process. Step 4: Directly perform the third round of drawing on the bar obtained in Step 3. When drawing, start pressing down from a distance of 100-150mm from the end and draw the bar diameter to Φ200-250mm. Hot material can be returned to the furnace during the drawing process.

[0004] In step two, the upsetting speed is 5-15 mm / s.

[0005] In step two, the forging temperature is 10-70℃ below the phase transformation point.

[0006] The preheating temperature of the upper and lower circular anvils in step two is 200-300℃.

[0007] In step two, the amount of pressure applied with each hammer blow is controlled to be 100-150mm.

[0008] In step three, the amount of pressure applied with each hammer blow is controlled to be 80-100mm.

[0009] In step four, the amount of pressure applied with each hammer blow is controlled to be 30-50mm.

[0010] Steps two, three, and four can be completed within 1-3 hours.

[0011] The pressing speed during the stretching process in steps two, three, and four is 10-20 mm / s.

[0012] Technical effects of this invention: By designing a special tooling for the arc of bar stock, this invention can form a centrally convex arc-shaped end of the bar stock during upsetting. This prevents the concave center caused by small deformation of the core during drawing. During the bar stock drawing process, the pressure is applied from a certain distance from the end. At this time, the temperature of the outer circumference of the bar stock is lower than that of the core, and the deformation resistance of the core is lower. This allows the material on the end face of the bar stock that has not been drawn to be squeezed towards the core, avoiding concavity. At the same time, the use of an arc anvil for upsetting during the second round of deformation is to smooth out the uneven deformation of the end during the first round of deformation. During the third round of deformation, since the bar stock is longer at this time, upsetting is not performed to prevent the bar stock from bending and deforming. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of an arc-shaped anvil used for upsetting. Detailed Implementation

[0014] To better understand the purpose, technical solution, and advantages of this invention, the following detailed description is provided in conjunction with embodiments.

[0015] A process for reducing concave cores in bar stock, wherein the original diameter of the bar stock is Φ550-620mm, the length is 1000mm-1500mm, and the diameter of the drawn bar stock is Φ200-250mm; the process includes the following steps: Step 1: Design and manufacture upper and lower circular arc anvils for upsetting bar stock. The chord length L of the circular arc anvil is equal to the diameter R+ of the bar stock, and the arc height H is 100-200mm. Step Two: Heat the bar stock to the forging temperature and hold it at that temperature. Preheat the upper and lower circular arc anvils. Use both anvils for upsetting. Place the lower circular arc anvil on its lower anvil face, and place the bar stock to be upset vertically on the arc face of the lower circular arc anvil. Place the arc face of the upper circular arc anvil on the top of the bar stock and begin upsetting at a speed of 5-15 mm / s. Upset the bar stock to 70% of its original height. After upsetting, rotate the bar stock 90° along its axis to begin drawing. When drawing, start pressing down from a distance of 100-150 mm from either end, controlling the amount of reduction per hammer blow. Lengthen the bar stock to a diameter of 450-480 mm. Hot material can be recycled during the drawing process. The forging temperature is 10-70℃ below the phase transformation point, and the preheating temperature of the upper and lower circular arc anvils is 200-300℃. The reduction per hammer blow is controlled at 100-150 mm.

[0016] Step 3: Perform a second round of drawing on the bar obtained in Step 2. Use upper and lower circular arc anvils for upsetting. Place the lower circular arc anvil on the lower anvil surface. Place the bar obtained in Step 2 vertically on the circular arc surface of the lower circular arc anvil. Place the circular arc surface of the upper circular arc anvil on the top of the bar obtained in Step 2 and begin upsetting. Upset downwards by 100-150mm. After upsetting, rotate the bar 90° along the axial direction. When drawing, start pressing down from a distance of 150-200mm from any end to draw the bar. Control the amount of pressure applied with each hammer blow to draw the diameter of the bar to 300-320mm. Hot material can be returned to the furnace during the drawing process. The amount of pressure applied with each hammer blow should be controlled at 80-100mm.

[0017] Step 4: Directly perform the third round of drawing on the bar obtained in Step 3. When drawing, start pressing down from a distance of 100-150mm from the end, and draw the bar diameter to Φ200-250mm. Hot material can be returned to the furnace during the drawing process. The amount of pressing down per hammer is controlled at 30-50mm.

[0018] Steps two, three, and four can be completed within 1-3 fires, with a pressing speed of 10-20 mm / s during the drawing process.

[0019] Example 1: Drawing a bar with an original diameter of Φ580mm and a length of 1200mm to a diameter of Φ250mm involves the following steps: Step 1: Design and manufacture upper and lower arc-shaped anvils for bar upsetting. The chord length of the arc-shaped anvil is 750mm and the height is 150mm.

[0020] Step 2: Heat the bar stock. Preheat the upper and lower circular anvils to 200℃. After heating the bar stock to 830℃ and removing it from the furnace, place one end on the lower circular anvil and place the upper circular anvil on the other end of the bar stock for upsetting. Upset to 840mm at a speed of 8mm / s. After upsetting, place the bar stock on a flat anvil and rotate it 90° along the axis to begin drawing. When drawing, start pressing down from a distance of 120mm from the end, controlling the deformation per hammer blow to 120mm at a pressing speed of 15mm / s. Lengthen the bar stock to a diameter of 450mm.

[0021] Step 3: The bar obtained in Step 2 is upset using an upper and lower circular anvil. The upset height is 150mm. After upset, the bar is rotated 90° along the axis and drawn. When drawing, the bar is pressed down from a distance of 150mm from the end. Each hammer press is 100mm, and the pressing speed is 15mm / s. The diameter of the drawn bar is 300mm.

[0022] Step 4: Directly perform the third drawing of the bar obtained in Step 3. When drawing, start pressing down from a distance of 100mm from the end, with each hammer press down 50mm at a speed of 15mm / s, and draw the bar diameter by 250mm.

[0023] Example 2: Drawing a bar with an original diameter of 600mm and a length of 1000mm to a diameter of 200mm involves the following steps: Step 1: Design and manufacture upper and lower arc-shaped anvils for bar upsetting. The chord length of the arc-shaped anvil is 800mm and the height is 150mm.

[0024] Step 2: Heat the bar stock. Preheat the upper and lower circular anvils to 200℃. After heating the bar stock to 780℃ and removing it from the furnace, place one end on the lower circular anvil and place the upper circular anvil on the other end of the bar stock for upsetting. Upset to 700mm at a speed of 6mm / s. After upsetting, place the bar stock on a flat anvil and rotate it 90° along the axial direction to begin drawing. When drawing, start pressing down from a distance of 150mm from the end, controlling the deformation per hammer blow to 150mm at a pressing speed of 12mm / s. Lengthen the bar stock to a diameter of 450mm.

[0025] Step 3: The bar obtained in Step 2 is upset using an upper and lower circular anvil. The upset height is 140mm. After upset, the bar is rotated 90° along the axis and drawn. When drawing, the bar is pressed down from a distance of 150mm from the end. Each hammer blow is 100mm, and the pressing speed is 12mm / s. The diameter of the drawn bar is 320mm.

[0026] Step 4: The bar obtained in Step 3 is hot-returned to the furnace. After exiting the furnace, it is drawn for the third time. When drawing, the bar is pressed down from a distance of 110mm from the end. Each hammer press is 50mm, and the pressing speed is 12mm / s, which lengthens the diameter of the bar by 200mm.

Claims

1. A process for reducing the concavity of bar stock, characterized in that, The original diameter of the bar is Φ550-620mm, and the length is 1000mm-1500mm. After drawing, the diameter of the bar is Φ200-250mm. The process includes the following steps: Step 1: Design and manufacture upper and lower circular arc anvils for upsetting bar stock. The chord length L of the circular arc anvil is equal to the diameter R+ of the bar stock, and the arc height H is 100-200mm. Step 2: Heat the bar to the forging temperature and hold it at that temperature. Preheat the upper and lower circular anvils. Use the upper and lower circular anvils for upsetting. Place the lower circular anvil on the lower anvil surface. Place the bar to be upset vertically on the circular surface of the lower circular anvil. Place the circular surface of the upper circular anvil on the top of the bar and start upsetting. Upset the bar to 70% of its original height. After upsetting, rotate the bar 90° along the axial direction to start drawing. When drawing, start pressing down from a distance of 100-150mm from either end to draw the bar. Control the amount of pressure applied with each hammer blow. Lengthen the bar diameter to 450-480mm. Hot material can be returned to the furnace during the drawing process. Step 3: Perform a second round of drawing on the bar obtained in Step 2. Use upper and lower circular arc anvils for upsetting. Place the lower circular arc anvil on the lower anvil surface. Place the bar obtained in Step 2 vertically on the circular arc surface of the lower circular arc anvil. Place the circular arc surface of the upper circular arc anvil on the top of the bar obtained in Step 2 and start upsetting. Upset downwards by 100-150mm. After upsetting, rotate the bar 90° along the axial direction. When drawing, start pressing down from a distance of 150-200mm from any end to draw. Control the amount of pressing down with each hammer. Lengthen the diameter of the bar to 300-320mm. Hot material can be returned to the furnace during the drawing process. Step 4: Directly perform the third round of drawing on the bar obtained in Step 3. When drawing, start pressing down from a distance of 100-150mm from the end and draw the bar diameter to Φ200-250mm. Hot material can be returned to the furnace during the drawing process.

2. In the process of reducing the concave core of the bar stock according to claim 1, in step two, the upsetting speed is 5-15 mm / s.

3. In the process of reducing the concave core of the bar stock according to claim 1, in step two, the forging temperature is 10-70°C below the phase transformation point.

4. The process method for reducing the concave center of the bar stock according to claim 1, characterized in that, The preheating temperature of the upper and lower arc anvils in step two is 200-300℃.

5. In the process of reducing the concave core of the bar according to claim 1, in step two, the amount of pressing down per hammer is controlled at 100-150mm.

6. In the process of reducing the concave core of the bar according to claim 1, in step three, the amount of pressing down per hammer is controlled at 80-100mm.

7. In the process of reducing the concave core of the bar according to claim 1, in step four, the amount of pressing down per hammer is controlled to be 30-50mm.

8. The process method for reducing the concave center of a bar according to claim 1, characterized in that, Steps two, three, and four can be completed within 1-3 heat cycles.

9. The process method for reducing the concave center of a bar according to claim 1, characterized in that, The pressing speed during the stretching process described in steps two, three, and four is 10-20 mm / s.

Citation Information

Patent Citations

  • Upper and lower arc anvil tool for shaft forging forming of large hydraulic press and forging and drawing method

    CN103920841A

  • Metal bar arc anvil upsetting method

    CN112077248A

  • Forging Method for Improving the Transverse Impact Energy of H13Mo2ESR Die Flat Steel

    CN114932182A

  • Forging method for forging center defect of continuous casting billet

    CN118385429A

  • Forging method of hollow shaft forge piece with flanges at two ends

    CN119839211A