Solvent-free epoxy coating and preparation method thereof

By combining modified and reinforced composite fillers and diluents, a multi-level core-shell structure is formed, which solves the problem of poor adhesion of solvent-free epoxy coatings and improves the coating's high adhesion, wear resistance and corrosion resistance.

CN120966344APending Publication Date: 2025-11-18GANSU JINHONGQIAO GRP CO LTD

Patent Information

Application Number
CN202511493621.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-20
Publication Date
2025-11-18

AI Technical Summary

Technical Problem

Solvent-free epoxy coatings have poor adhesion to the substrate, and the cured coating is prone to peeling off, affecting the coating's wear resistance and corrosion resistance.

Method used

High-performance modified and reinforced composite fillers are used, including a combination of nano-silica, dopamine hydrochloride, hexadecylamine and polyetheramine D-230. Through polydopamine coating and covalent bonding, a multi-level core-shell structure is formed, which enhances the interfacial bonding and dispersibility between the filler and epoxy resin. A composite reactive diluent and curing agent polyetheramine D-230 are used to form an interpenetrating network structure.

Benefits of technology

It significantly improves the adhesion, abrasion resistance and corrosion resistance of the coating, reduces the risk of the coating peeling off the substrate after curing, and enhances the mechanical interlocking strength of the coating and the barrier effect against corrosive media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120966344A_ABST
    Figure CN120966344A_ABST
Patent Text Reader

Abstract

The invention discloses a solvent-free epoxy coating and a preparation method thereof, and relates to the technical field of coatings. The solvent-free epoxy coating is composed of a component A and a component B, the component A is composed of a high-performance modified reinforced composite filler, epoxy resin, a composite reactive diluent, a defoaming agent and a leveling agent; the component B is a curing agent polyether amine D-230; the high-performance modified reinforced composite filler is uniformly dispersed and stably embedded into an epoxy resin base material, and internal stress caused by filler agglomeration and poor interface can be reduced due to excellent compatibility and dispersibility, so that the coating is not easy to fall off from the base material after being cured; and the excellent adhesion and dispersibility also avoid abrasion, shedding and cracks caused by insufficient adhesion or interface defects, so that the toughness and wear resistance of the coating are enhanced, the permeation of a corrosive medium is fully isolated, and the adhesion, wear resistance and corrosion resistance of the coating are further enhanced under the assistance of auxiliaries such as the composite reactive diluent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating technology, specifically referring to a solvent-free epoxy coating and its preparation method. Background Technology

[0002] Solvent-based coatings contain a large amount of solvents, and these volatile organic compounds evaporate during film formation. This not only wastes resources but also damages the environment. Furthermore, solvent evaporation can cause defects such as pinholes and craters in the coating. Water, oxygen, and corrosive media can penetrate into the substrate, causing corrosion. The expansion of corrosion products can cause the coating to crack, resulting in coating peeling, blistering, and other phenomena, leading to the loss of the coating's anti-corrosion function. Solvent-free coatings, on the other hand, do not contain volatile solvent components, thus saving resources and being very environmentally friendly. Among them, solvent-free epoxy coatings, as a high-performance protective coating, are widely used in modern industry. Due to their 100% solid content, almost no solvent evaporates after coating; all components are converted into a paint film, resulting in a thick paint film. At the same time, the emission of volatile organic compounds is extremely low.

[0003] The existing technology currently suffers from the following main problems:

[0004] Solvent-free epoxy coatings have poor adhesion to the substrate, and the cured coating is prone to peeling off, which adversely affects the coating's wear resistance and corrosion resistance, thus limiting the coating's performance. Summary of the Invention

[0005] In view of the above situation and to overcome the defects of the prior art, the present invention proposes a solvent-free epoxy coating, comprising the following components in parts by weight: 80-90 parts of component A and 22-30 parts of component B.

[0006] Component A comprises the following components in parts by weight: 20-30 parts of high-performance modified and reinforced composite filler, 60-80 parts of epoxy resin, 8-15 parts of composite reactive diluent, 0.4-0.8 parts of defoamer, and 0.4-0.8 parts of leveling agent.

[0007] Component B is the curing agent polyetheramine D-230.

[0008] The high-performance modified and reinforced composite filler comprises the following components in parts by weight: 10-30 parts of nano silica, 5-15 parts of dopamine hydrochloride, 30-50 parts of hexadecylamine, 20-40 parts of diethylenetriamine, and 10-20 parts of polyetheramine D-230.

[0009] The preparation method of the high-performance modified and reinforced composite filler specifically includes the following steps:

[0010] (1) Dissolve 0.04-0.06 g of tris(hydroxymethyl)aminomethane hydrochloride in 50 mL of deionized water, adjust the pH to 8.5 with 0.4% sodium hydroxide solution to obtain a buffer solution for later use, disperse 0.1-0.3 g of nano-silica in 10 mL of deionized water to obtain a silica sol for later use, then dissolve dopamine hydrochloride in the buffer solution, sonicate for 50-60 min, and then slowly add it dropwise into the silica sol. React at room temperature for 12-24 h, wash with deionized water and centrifuge 2-3 times, collect the solid product, and vacuum dry at 50-60 °C for 6-8 h to obtain polydopamine-coated silica. Silicon, through polydopamine coating, improves the filler properties of nano-silica. The polydopamine coating not only adheres strongly to nano-silica but also forms chemical bonds or strong hydrogen bonds with the epoxy resin base, enhancing the interfacial bonding force between the filler and the base, reducing the wear and damage of the epoxy resin itself. It can also form a strong adhesion to the substrate surface after the coating is cured, increasing the contact area and mechanical interlocking effect between the coating and the substrate. The polydopamine coating also enables the nano-silica to be evenly dispersed, forming a denser and more tortuous physical barrier, increasing the diffusion path of corrosive media such as water, oxygen, and chloride ions.

[0011] (2) Add the polydopamine-coated silica from step (1) to 50 mL of anhydrous ethanol and sonicate for 40-60 min to obtain a polydopamine-coated silica dispersion. Add hexadecylamine to 50 mL of anhydrous ethanol and stir until completely dissolved. Then slowly add it to the polydopamine-coated silica dispersion while stirring and adding 0.2-0.4 mL of diethylenetriamine dropwise. After the addition is complete, raise the temperature to 50-60 °C and react for 12-18 h. Wash the product with anhydrous ethanol and centrifuge 2-3 times. Finally, vacuum dry at 70-80 °C for 8-10 h to obtain the hydrophobic modified silica. Polydopamine-coated silica, under the cross-linking and catalytic action of diethylenetriamine, has its long chains of hexadecylamine covalently anchored to the polydopamine coating layer and extending outward to form a low surface energy hydrophobic layer. This effectively blocks the penetration of water molecules, thereby improving corrosion resistance. The strong covalent bonds ensure that stress can be transferred from the soft resin base to the hard silica particles, reducing the wear of the resin base and enhancing wear resistance. Furthermore, the dispersed rigid silica nanoparticles also form microscopic anchor points in the coating, increasing the mechanical interlocking strength and thus improving the adhesion of the coating.

[0012] (3) Add the hydrophobic modified polydopamine-coated silica from step (2) to 50 mL of anhydrous ethanol, and ultrasonically disperse for 20-30 min to obtain a hydrophobic modified polydopamine-coated silica dispersion for later use. Dissolve polyetheramine D-230 in 10 mL of anhydrous ethanol and stir for 20-30 min to obtain a polyetheramine D-230 ethanol solution for later use. Then slowly add the polyetheramine D-230 ethanol solution dropwise to the hydrophobic modified polydopamine-coated silica dispersion. In the dispersion, the temperature is raised to 50-60℃, and the reaction is stirred for 12-18 hours. The product is washed with anhydrous ethanol and centrifuged 3-4 times. It is then vacuum-dried at 60-80℃ for 8-10 hours to obtain a high-performance modified and reinforced composite filler. By coating the exterior of the hydrophobically modified polydopamine-coated silica with a layer of hydrophilic and flexible polyetheramine chains, a multi-level, amphiphilic core-shell structure is formed, which can be perfectly embedded in epoxy resin matrix, effectively improving the filler's compatibility with epoxy resin matrix. The coating exhibits excellent compatibility and dispersibility. Covalent bonds and the entanglement of polyether chains with epoxy resin ensure efficient transfer of external forces from the resin matrix to the rigid core. The flexible polyether chains on the outer layer effectively absorb and dissipate impact energy, preventing crack formation and propagation, thus making the coating more robust and wear-resistant. Polyetheramine D-230 enables high-performance modified reinforced composite fillers and epoxy resin to interpenetrate and entangle, forming an interpenetrating network structure that blurs the interface between the filler and resin. Simultaneously, the flexible segments help alleviate internal stress caused by curing shrinkage and thermal expansion and contraction, preventing stress concentration that leads to decreased adhesion. Excellent compatibility and dispersibility also reduce internal stress caused by filler agglomeration and poor interface, making the coating less prone to detachment from the substrate after curing, thus significantly improving coating adhesion. Furthermore, excellent adhesion and dispersibility prevent microcracks caused by insufficient adhesion or interface defects, effectively isolating corrosive media penetration, improving corrosion resistance, and providing long-term protection for the substrate.

[0013] Preferably, in step (1), the amount of dopamine hydrochloride added is 0.05-0.15g. The addition of dopamine hydrochloride can form a polydopamine coating on the surface of nano silica. The catechol groups in polydopamine can consume oxygen, inhibit the cathode reaction, and delay the corrosion process from an electrochemical perspective.

[0014] Preferably, in step (2), the amount of hexadecylamine added is 0.3-0.5g. The long-chain alkyl group introduced by hexadecylamine imparts hydrophobic modification effect, which improves the hydrophobicity and corrosion resistance of the material.

[0015] Preferably, in step (3), the amount of polyetheramine D-230 added is 0.1-0.2g. The long flexible chain of polyetheramine D-230 can better penetrate and wrap into the epoxy resin molecular chain, which greatly improves the compatibility and dispersibility in the epoxy resin base. Furthermore, polyetheramine D-230 can also participate in the subsequent curing of epoxy resin, so that the filler-resin form an integral and robust network.

[0016] This invention also provides a method for preparing a solvent-free epoxy coating, specifically including the following steps:

[0017] S1. The high-performance modified and reinforced composite filler and epoxy resin are premixed at 200-300 rpm for 3-5 minutes, wherein the epoxy resin is bisphenol A type epoxy resin. Then, the mixture is dispersed at 1000-2000 rpm for 10-15 minutes using a high-speed disperser. The mixture is then ground 2-4 times using a three-roll mill. The ground base material is transferred to a mixing tank. The composite active diluent, defoamer, and leveling agent are gradually added at a stirring speed of 300-600 rpm and stirred for 15-20 minutes to obtain component A. By uniformly and stably dispersing the high-performance modified and reinforced composite filler into the epoxy resin, and with the assistance of other additives, the wear resistance, adhesion, and corrosion resistance of the epoxy resin are improved.

[0018] S2. Mix component B with component A described in step S1 evenly, and stir at 200-300 rpm for 2-3 minutes to obtain a solvent-free epoxy coating. The ether bonds in the molecular chain of polyetheramine D-230 curing agent in component B have good flexibility and wettability, which helps the coating to better wet the substrate, penetrate into the micropores, form a strong mechanical interlocking effect, improve adhesion, and further enhance wear resistance and corrosion resistance, thereby improving the coating's performance.

[0019] Preferably, in step S1, the composite reactive diluent is obtained by mixing neopentyl glycol diglycidyl ether and allyl glycidyl ether in a mass ratio of 7:3. Neopentyl glycol diglycidyl ether serves as the performance skeleton, forming rigid crosslinking points in the polymer network, thereby enhancing the material's resistance to deformation under external forces. Allyl glycidyl ether serves as a regulating agent, reducing viscosity and allowing for better leveling, wetting, and penetration into the micropores of the substrate, thus generating a strong mechanical interlocking effect.

[0020] The beneficial effects achieved by this invention are as follows:

[0021] This invention achieves this by uniformly dispersing and stably embedding a high-performance modified and reinforced composite filler into an epoxy resin matrix. Its excellent compatibility and dispersibility reduce internal stress caused by filler agglomeration and poor interfacial properties, making the coating less prone to detachment from the substrate after curing. Furthermore, its excellent adhesion and dispersibility prevent wear, detachment, and cracking caused by insufficient adhesion or interfacial defects. This enhances the coating's toughness and wear resistance while effectively isolating it from corrosive media. Simultaneously, with the assistance of additives such as composite reactive diluents, the coating's adhesion, wear resistance, and corrosion resistance are further enhanced, significantly improving its performance. The high-performance modified and reinforced composite filler uses nano-silica as its core, sequentially passing through a polydopamine coating layer and a hexadecylamine hydrophobic layer. The filler is modified by layers of polyetheramine and a hydrophilic flexible layer, forming a multi-level, amphiphilic core-shell structure. The adhesion of polydopamine, covalent bonding, and the entanglement of polyether chains with epoxy resin effectively improve the compatibility and dispersibility of the high-performance modified reinforced composite filler in the epoxy resin matrix, enhancing the interfacial bonding between the high-performance modified reinforced composite filler and the epoxy resin matrix. This also ensures that external forces are efficiently transferred from the resin matrix to the internal rigid core. The flexible polyether chains of the outer layer effectively absorb and dissipate impact energy, preventing the generation and propagation of cracks, thus making the coating more tough and wear-resistant. Furthermore, the excellent compatibility and dispersibility reduce internal stress caused by filler agglomeration and poor interfacial properties, further enhanced by the strong adhesion. This further enhances the adhesion of the coating, making it less likely to peel off the substrate after curing. Simultaneously, excellent adhesion and dispersibility prevent microcracks caused by insufficient adhesion or interface defects, effectively isolating the penetration of corrosive media and improving corrosion resistance. In the composite reactive diluent, neopentyl glycol diglycidyl ether serves as the performance framework, forming rigid cross-linking points in the polymer network. This not only enhances the material's resistance to external deformation but also effectively blocks the penetration of corrosive media such as water, oxygen, and chloride ions through the constructed highly cross-linked and dense network. Allyl glycidyl ether acts as a regulating agent, reducing viscosity and allowing for better leveling, wetting, and penetration into the micropores of the substrate, thereby generating a strong mechanical interlocking effect. The long-chain allyl groups of propyl glycidyl ether have an internal plasticizing effect, improving flexibility. This effectively absorbs and releases internal stress caused by curing shrinkage or thermal expansion and contraction, avoiding coating peeling due to stress concentration. Furthermore, good leveling properties reduce defects such as pinholes and microbubbles in the coating, eliminating shortcuts for corrosive media penetration. The combination of these two factors not only improves the processability and workability of the coating but also enhances its adhesion, abrasion resistance, and corrosion resistance. This invention uses high-performance modified reinforced composite fillers, epoxy resin, composite reactive diluent, defoamer, leveling agent, and curing agent polyetheramine D-230 to prepare a solvent-free epoxy coating, which significantly enhances the coating's adhesion, abrasion resistance, and corrosion resistance, improving the coating's performance. Attached Figure Description

[0022] Figure 1 These are adhesion results diagrams for Examples 1-4 and Comparative Examples 1-3 of the present invention;

[0023] Figure 2 The figures show the volume wear rate results for Examples 1-4 and Comparative Examples 1-3 of the present invention.

[0024] Figure 3 The images show the maximum corrosion length results for Examples 1-4 and Comparative Examples 1-3 of this invention. Detailed Implementation

[0025] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this application.

[0027] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods; unless otherwise specified, the experimental materials used in the following embodiments are all purchased from commercial channels.

[0028] Example 1

[0029] This embodiment proposes a solvent-free epoxy coating comprising the following components in parts by weight: 90 parts of component A and 30 parts of component B.

[0030] Component A comprises the following components in parts by weight: 30 parts of high-performance modified and reinforced composite filler, 80 parts of epoxy resin, 15 parts of composite reactive diluent, 0.8 parts of defoamer, and 0.8 parts of leveling agent.

[0031] Component B is the curing agent polyetheramine D-230.

[0032] The high-performance modified and reinforced composite filler comprises the following components in parts by weight: 30 parts nano silica, 15 parts dopamine hydrochloride, 50 parts hexadecylamine, 40 parts diethylenetriamine, and 20 parts polyetheramine D-230.

[0033] The preparation method of high-performance modified and reinforced composite fillers specifically includes the following steps:

[0034] (1) Dissolve 0.06g of tris(hydroxymethyl)aminomethane hydrochloride in 50mL of deionized water, adjust the pH to 8.5 with 0.4% sodium hydroxide solution to obtain a buffer solution for later use, disperse 0.3g of nano-silica in 10mL of deionized water to obtain a silica sol for later use, then dissolve dopamine hydrochloride in the buffer solution, sonicate for 60min, and then slowly add it dropwise into the silica sol. The amount of dopamine hydrochloride added is 0.15g. The addition of dopamine hydrochloride can form a polydopamine coating on the surface of nano-silica. The catechol groups in polydopamine can consume oxygen and inhibit the cathodic reaction, thus delaying the corrosion process from an electrochemical perspective. React at room temperature for 24h, wash with deionized water and centrifuge 3 times. The solid product was collected and vacuum dried at 60℃ for 8 hours to obtain polydopamine-coated silica. The polydopamine coating improved the filler properties of the nano silica. The polydopamine coating not only adhered to the nano silica with strong adhesion, but also formed chemical bonds or strong hydrogen bonds with the epoxy resin base, which enhanced the interfacial bonding force between the filler and the base, reduced the wear and damage of the epoxy resin itself, and formed a strong adhesion to the substrate surface after the coating was cured, which increased the contact area and mechanical interlocking effect between the coating and the substrate. The polydopamine coating also enabled the nano silica to be evenly dispersed, forming a denser and more tortuous physical barrier, increasing the diffusion path of corrosive media such as water, oxygen, and chloride ions.

[0035] (2) The polydopamine-coated silica from step (1) was added to 50 mL of anhydrous ethanol and ultrasonically treated for 60 min to obtain a polydopamine-coated silica dispersion for later use. Hexadecylamine was added to 50 mL of anhydrous ethanol at a dosage of 0.5 g. The long-chain alkyl group introduced by hexadecylamine imparts hydrophobic modification, improving the hydrophobicity and corrosion resistance of the material. After stirring until completely dissolved, it was slowly added to the polydopamine-coated silica dispersion while stirring and adding 0.4 mL of diethylenetriamine dropwise. After the addition was completed, the temperature was raised to 60 °C and the reaction was carried out for 18 h. The product was washed with anhydrous ethanol and centrifuged 3 times. Finally, it was discharged at 80 °C. Vacuum drying at ℃ for 10 h yielded hydrophobic modified polydopamine-coated silica. Under the cross-linking and catalytic action of diethylenetriamine, the long chains of hexadecylamine were covalently anchored on the polydopamine coating and extended outward to form a low surface energy hydrophobic layer, which effectively blocked the penetration of water molecules and thus improved corrosion resistance. The strong covalent bond ensured that stress could be transferred from the soft resin base to the hard silica particles, reducing the wear of the resin base and enhancing wear resistance. Furthermore, the dispersed rigid silica nanoparticles also formed microscopic anchor points in the coating, increasing the mechanical interlocking strength and thus improving the adhesion of the coating.

[0036] (3) Add the hydrophobically modified polydopamine-coated silica from step (2) to 50 mL of anhydrous ethanol and ultrasonically disperse for 30 min to obtain a hydrophobically modified polydopamine-coated silica dispersion for later use. Dissolve polyetheramine D-230 in 10 mL of anhydrous ethanol. The amount of polyetheramine D-230 added is 0.2 g. The long flexible chain of polyetheramine D-230 can better penetrate and wrap around the epoxy resin molecular chain, which greatly improves the compatibility and dispersibility in the epoxy resin matrix. Furthermore, polyetheramine D-230 can also participate in subsequent processes. The curing of epoxy resin forms a robust, integrated network of filler and resin. After stirring for 30 minutes, a polyetheramine D-230 ethanol solution is obtained and set aside. This solution is then slowly added dropwise to a dispersion of hydrophobically modified polydopamine-coated silica. The mixture is heated to 60°C and stirred for 18 hours. The product is washed four times with anhydrous ethanol and centrifuged. It is then vacuum-dried at 80°C for 10 hours to obtain a high-performance modified and reinforced composite filler. This process, by coating the hydrophobically modified polydopamine-coated silica with a layer of hydrophilic, flexible polyetheramine chains, forms… A multi-level, amphiphilic core-shell structured material can be perfectly embedded in epoxy resin matrix, effectively improving the compatibility and dispersibility of fillers in epoxy resin matrix. Covalent bonding and the entanglement of polyether chains with epoxy resin ensure that external forces are efficiently transferred from the resin matrix to the internal rigid core. The outer flexible polyether chains effectively absorb and dissipate impact energy, preventing crack initiation and propagation, thus making the coating more robust and wear-resistant. Polyetheramine D-230 enables high-performance modified reinforced composite fillers and epoxy resin to interpenetrate and entangle, forming an interpenetrating network. The structure blurs the interface between the filler and the resin. At the same time, the flexible segments help alleviate the internal stress caused by curing shrinkage and thermal expansion and contraction, avoiding stress concentration that leads to decreased adhesion. Excellent compatibility and dispersibility can also reduce internal stress caused by filler agglomeration and poor interface, making the coating less likely to fall off the substrate after curing. This significantly improves the adhesion of the coating. Furthermore, excellent adhesion and dispersibility also avoid microcracks caused by insufficient adhesion or interface defects, effectively isolating the penetration of corrosive media, improving corrosion resistance, and providing long-term protection for the substrate.

[0037] This embodiment provides a method for preparing a solvent-free epoxy coating, specifically including the following steps:

[0038] S1. The high-performance modified and reinforced composite filler and epoxy resin are premixed at 300 rpm for 5 minutes, wherein the epoxy resin is bisphenol A type epoxy resin. Then, the mixture is dispersed at 2000 rpm for 15 minutes using a high-speed disperser. The mixture is then ground four times using a three-roll mill. The ground base material is transferred to a mixing tank, and a composite reactive diluent, defoamer, and leveling agent are gradually added at a stirring speed of 600 rpm. The mixture is stirred and mixed for 20 minutes. The composite reactive diluent consists of neopentyl glycol diglycidyl ether and allyl glycidyl ether. The mixture was prepared by mixing in a mass ratio of 7:3. Neopentyl glycol diglycidyl ether served as the performance backbone, forming rigid crosslinking points in the polymer network, which enhanced the material's resistance to deformation under external forces. Allyl glycidyl ether served as a regulating agent, which reduced viscosity, allowing for better leveling, wetting, and penetration into the micropores of the substrate, thereby generating a strong mechanical interlocking effect, resulting in component A. By uniformly and stably dispersing the high-performance modified and reinforced composite filler into the epoxy resin, and with the assistance of other additives, the wear resistance, adhesion, and corrosion resistance of the epoxy resin were improved.

[0039] S2. Mix component B with component A described in step S1 until homogeneous, and stir at 300 rpm for 3 minutes to obtain a solvent-free epoxy coating. The ether bonds in the molecular chain of the curing agent polyetheramine D-230 in component B have good flexibility and wettability, which helps the coating to better wet the substrate, penetrate into the micropores, form a strong mechanical interlocking effect, improve adhesion, and further enhance wear resistance and corrosion resistance, thereby improving the coating's performance.

[0040] Example 2

[0041] This embodiment proposes a solvent-free epoxy coating comprising the following components in parts by weight: 80 parts of component A and 22 parts of component B.

[0042] Component A comprises the following components in parts by weight: 20 parts of high-performance modified and reinforced composite filler, 60 parts of epoxy resin, 8 parts of composite reactive diluent, 0.4 parts of defoamer, and 0.4 parts of leveling agent.

[0043] Component B is the curing agent polyetheramine D-230.

[0044] The high-performance modified and reinforced composite filler comprises the following components in parts by weight: 10 parts nano silica, 5 parts dopamine hydrochloride, 30 parts hexadecylamine, 20 parts diethylenetriamine, and 10 parts polyetheramine D-230.

[0045] The preparation method of high-performance modified and reinforced composite fillers specifically includes the following steps:

[0046] (1) Dissolve 0.04 g of tris(hydroxymethyl)aminomethane hydrochloride in 50 mL of deionized water, adjust the pH to 8.5 with 0.4% sodium hydroxide solution to obtain a buffer solution for later use, disperse 0.1 g of nano-silica in 10 mL of deionized water to obtain a silica sol for later use, then dissolve dopamine hydrochloride in the buffer solution, the amount of dopamine hydrochloride added is 0.05 g. The addition of dopamine hydrochloride can form a polydopamine coating on the surface of nano-silica. The catechol groups in polydopamine can consume oxygen and inhibit the cathodic reaction, thus delaying the corrosion process from an electrochemical perspective. After ultrasonic dispersion for 50 min, slowly drop it into the silica sol and react at room temperature for 12 h. Wash with deionized water and centrifuge twice. The solid product was collected and vacuum dried at 50℃ for 6 hours to obtain polydopamine-coated silica. The polydopamine coating improved the filler properties of the nano silica. The polydopamine coating not only adhered to the nano silica with strong adhesion, but also formed chemical bonds or strong hydrogen bonds with the epoxy resin base, which enhanced the interfacial bonding force between the filler and the base, reduced the wear and damage of the epoxy resin itself, and formed a strong adhesion to the substrate surface after the coating was cured, which increased the contact area and mechanical interlocking effect between the coating and the substrate. The polydopamine coating also enabled the nano silica to be evenly dispersed, forming a denser and more tortuous physical barrier, which increased the diffusion path of corrosive media such as water, oxygen, and chloride ions.

[0047] (2) The polydopamine-coated silica from step (1) was added to 50 mL of anhydrous ethanol and ultrasonically treated for 40 min to obtain a polydopamine-coated silica dispersion for later use. Hexadecylamine was added to 50 mL of anhydrous ethanol at a dosage of 0.3 g. The long-chain alkyl group introduced by hexadecylamine imparts hydrophobic modification, improving the hydrophobicity and corrosion resistance of the material. After stirring until completely dissolved, it was slowly added to the polydopamine-coated silica dispersion while stirring and adding 0.2 mL of diethylenetriamine dropwise. After the addition was completed, the temperature was raised to 50 °C and the reaction was carried out for 12 h. The product was washed with anhydrous ethanol and centrifuged twice. Finally, it was measured at 7 °C. Vacuum drying at 0℃ for 8 hours yielded hydrophobic modified polydopamine-coated silica. Under the cross-linking and catalytic action of diethylenetriamine, the long chains of hexadecylamine were covalently anchored on the polydopamine coating and extended outward to form a low surface energy hydrophobic layer, which effectively blocked the penetration of water molecules and thus improved corrosion resistance. The strong covalent bond ensured that stress could be transferred from the soft resin base to the hard silica particles, reducing the wear of the resin base and enhancing wear resistance. Furthermore, the dispersed rigid silica nanoparticles also formed microscopic anchor points in the coating, increasing the mechanical interlocking strength and thus improving the adhesion of the coating.

[0048] (3) Add the hydrophobically modified polydopamine-coated silica from step (2) to 50 mL of anhydrous ethanol and ultrasonically disperse for 20 min to obtain a hydrophobically modified polydopamine-coated silica dispersion for later use. Dissolve polyetheramine D-230 in 10 mL of anhydrous ethanol. The amount of polyetheramine D-230 added is 0.1 g. The long flexible chain of polyetheramine D-230 can better penetrate and wrap around the epoxy resin molecular chain, which greatly improves the compatibility and dispersibility in the epoxy resin matrix. Furthermore, polyetheramine D-230 can also participate in subsequent processes. The curing of epoxy resin forms a robust, integrated network of filler and resin. After stirring for 20 minutes, a polyetheramine D-230 ethanol solution is obtained and set aside. This solution is then slowly added dropwise to a dispersion of hydrophobically modified polydopamine-coated silica. The mixture is heated to 50°C and stirred for 12 hours. The product is washed three times with anhydrous ethanol and centrifuged. It is then vacuum-dried at 60°C for 8 hours to obtain a high-performance modified and reinforced composite filler. This process, by coating the hydrophobically modified polydopamine-coated silica with a layer of hydrophilic, flexible polyetheramine chains, forms... A multi-level, amphiphilic core-shell structured material can be perfectly embedded in epoxy resin matrix, effectively improving the compatibility and dispersibility of fillers in epoxy resin matrix. Covalent bonding and the entanglement of polyether chains with epoxy resin ensure that external forces are efficiently transferred from the resin matrix to the internal rigid core. The outer flexible polyether chains effectively absorb and dissipate impact energy, preventing crack initiation and propagation, thus making the coating more robust and wear-resistant. Polyetheramine D-230 enables high-performance modified reinforced composite fillers and epoxy resin to interpenetrate and entangle, forming an interpenetrating network. The structure blurs the interface between the filler and the resin. At the same time, the flexible segments help alleviate the internal stress caused by curing shrinkage and thermal expansion and contraction, avoiding stress concentration that leads to decreased adhesion. Excellent compatibility and dispersibility can also reduce internal stress caused by filler agglomeration and poor interface, making the coating less likely to fall off the substrate after curing. This significantly improves the adhesion of the coating. Furthermore, excellent adhesion and dispersibility also avoid microcracks caused by insufficient adhesion or interface defects, effectively isolating the penetration of corrosive media, improving corrosion resistance, and providing long-term protection for the substrate.

[0049] This embodiment provides a method for preparing a solvent-free epoxy coating, specifically including the following steps:

[0050] S1. Premix the high-performance modified reinforced composite filler and epoxy resin at 200 rpm for 3 minutes. The epoxy resin is bisphenol A type epoxy resin. Then disperse it at 1000 rpm for 10 minutes using a high-speed disperser. Grind the mixture twice using a three-roll mill. Transfer the ground base material to a mixing tank. Gradually add the composite reactive diluent, defoamer, and leveling agent at 300 rpm and mix for 15 minutes. The composite reactive diluent consists of neopentyl glycol diglycidyl ether and allyl glycidyl ether. The mixture was prepared by mixing in a mass ratio of 7:3. Neopentyl glycol diglycidyl ether served as the performance backbone, forming rigid crosslinking points in the polymer network, which enhanced the material's resistance to deformation under external forces. Allyl glycidyl ether served as a regulating agent, which reduced viscosity, allowing for better leveling, wetting, and penetration into the micropores of the substrate, thereby generating a strong mechanical interlocking effect, resulting in component A. By uniformly and stably dispersing the high-performance modified and reinforced composite filler into the epoxy resin, and with the assistance of other additives, the wear resistance, adhesion, and corrosion resistance of the epoxy resin were improved.

[0051] S2. Mix component B with component A described in step S1 until homogeneous, and stir at 200 rpm for 2 minutes to obtain a solvent-free epoxy coating. The ether bonds in the molecular chain of the curing agent polyetheramine D-230 in component B have good flexibility and wettability, which helps the coating to better wet the substrate, penetrate into the micropores, form a strong mechanical interlocking effect, improve adhesion, and further enhance wear resistance and corrosion resistance, thereby improving the coating's performance.

[0052] Example 3

[0053] This embodiment proposes a solvent-free epoxy coating comprising the following components in parts by weight: 85 parts of component A and 26 parts of component B.

[0054] Component A comprises the following components in parts by weight: 25 parts of high-performance modified and reinforced composite filler, 70 parts of epoxy resin, 11.5 parts of composite reactive diluent, 0.6 parts of defoamer, and 0.6 parts of leveling agent.

[0055] Component B is the curing agent polyetheramine D-230.

[0056] High-performance modified and reinforced composite filler, comprising the following components in parts by weight: 20 parts nano silica, 10 parts dopamine hydrochloride, 40 parts hexadecylamine, 30 parts diethylenetriamine, and 15 parts polyetheramine D-230.

[0057] The preparation method of high-performance modified and reinforced composite fillers specifically includes the following steps:

[0058] (1) Dissolve 0.05g of tris(hydroxymethyl)aminomethane hydrochloride in 50mL of deionized water, adjust the pH to 8.5 with 0.4% sodium hydroxide solution to obtain a buffer solution for later use, disperse 0.2g of nano-silica in 10mL of deionized water to obtain a silica sol for later use, then dissolve dopamine hydrochloride in the buffer solution, the amount of dopamine hydrochloride added is 0.10g. The addition of dopamine hydrochloride can form a polydopamine coating on the surface of nano-silica. The catechol groups in polydopamine can consume oxygen and inhibit the cathodic reaction, thus delaying the corrosion process from an electrochemical perspective. After ultrasonic dispersion for 55min, slowly drop it into the silica sol and react at room temperature for 18h. Wash with deionized water and centrifuge twice. The solid product was collected and vacuum dried at 55℃ for 7 hours to obtain polydopamine-coated silica. The polydopamine coating improved the filler properties of the nano silica. The polydopamine coating not only adhered to the nano silica with strong adhesion, but also formed chemical bonds or strong hydrogen bonds with the epoxy resin base material, which enhanced the interfacial bonding force between the filler and the base material, reduced the wear and damage of the epoxy resin itself, and formed a strong adhesion to the substrate surface after the coating was cured, which increased the contact area and mechanical interlocking effect between the coating and the substrate. The polydopamine coating also enabled the nano silica to be evenly dispersed, forming a denser and more tortuous physical barrier, which increased the diffusion path of corrosive media such as water, oxygen, and chloride ions.

[0059] (2) The polydopamine-coated silica from step (1) was added to 50 mL of anhydrous ethanol and ultrasonically treated for 50 min to obtain a polydopamine-coated silica dispersion for later use. Hexadecylamine was added to 50 mL of anhydrous ethanol at a dosage of 0.4 g. The long-chain alkyl group introduced by hexadecylamine imparts hydrophobic modification, improving the hydrophobicity and corrosion resistance of the material. After stirring until completely dissolved, it was slowly added to the polydopamine-coated silica dispersion while stirring and adding 0.3 mL of diethylenetriamine dropwise. After the addition was completed, the temperature was raised to 55 °C and the reaction was carried out for 15 h. The product was washed with anhydrous ethanol and centrifuged twice. Finally, it was measured at 7 °C. Vacuum drying at 5℃ for 9 hours yielded hydrophobic modified polydopamine-coated silica. Under the cross-linking and catalytic action of diethylenetriamine, the long chains of hexadecylamine were covalently anchored on the polydopamine coating and extended outward to form a low surface energy hydrophobic layer, which effectively blocked the penetration of water molecules and thus improved corrosion resistance. The strong covalent bond ensured that stress could be transferred from the soft resin base to the hard silica particles, reducing the wear of the resin base and enhancing wear resistance. Furthermore, the dispersed rigid silica nanoparticles also formed microscopic anchor points in the coating, increasing the mechanical interlocking strength and thus improving the adhesion of the coating.

[0060] (3) Add the hydrophobically modified polydopamine-coated silica from step (2) to 50 mL of anhydrous ethanol and ultrasonically disperse for 25 min to obtain a hydrophobically modified polydopamine-coated silica dispersion for later use. Dissolve polyetheramine D-230 in 10 mL of anhydrous ethanol. The amount of polyetheramine D-230 added is 0.15 g. The long flexible chain of polyetheramine D-230 can better penetrate and wrap around the epoxy resin molecular chain, which greatly improves the compatibility and dispersibility in the epoxy resin matrix. Furthermore, polyetheramine D-230 can also participate in the subsequent... The epoxy resin was cured to form a robust, integrated network of filler and resin. After stirring for 25 minutes, a polyetheramine D-230 ethanol solution was obtained and set aside. This solution was then slowly added dropwise to a dispersion of hydrophobically modified polydopamine-coated silica. The mixture was heated to 55°C and stirred for 15 hours. The product was washed three times with anhydrous ethanol and centrifuged. It was then vacuum-dried at 70°C for 9 hours to obtain a high-performance modified and reinforced composite filler. This process, by coating the hydrophobically modified polydopamine-coated silica with a layer of hydrophilic and flexible polyetheramine chains, formed… A multi-level, amphiphilic core-shell structured material can be perfectly embedded in epoxy resin matrix, effectively improving the compatibility and dispersibility of fillers in epoxy resin matrix. Covalent bonding and the entanglement of polyether chains with epoxy resin ensure that external forces are efficiently transferred from the resin matrix to the internal rigid core. The outer flexible polyether chains effectively absorb and dissipate impact energy, preventing crack initiation and propagation, thus making the coating more robust and wear-resistant. Polyetheramine D-230 enables high-performance modified reinforced composite fillers and epoxy resin to interpenetrate and entangle, forming an interpenetrating network. The structure blurs the interface between the filler and the resin. At the same time, the flexible segments help alleviate the internal stress caused by curing shrinkage and thermal expansion and contraction, avoiding stress concentration that leads to decreased adhesion. Excellent compatibility and dispersibility can also reduce internal stress caused by filler agglomeration and poor interface, making the coating less likely to fall off the substrate after curing. This significantly improves the adhesion of the coating. Furthermore, excellent adhesion and dispersibility also avoid microcracks caused by insufficient adhesion or interface defects, effectively isolating the penetration of corrosive media, improving corrosion resistance, and providing long-term protection for the substrate.

[0061] This embodiment provides a method for preparing a solvent-free epoxy coating, specifically including the following steps:

[0062] S1. The high-performance modified reinforced composite filler and epoxy resin are premixed at 250 rpm for 4 min, wherein the epoxy resin is bisphenol A type epoxy resin. Then, the mixture is dispersed at 1500 rpm for 12.5 min using a high-speed disperser. The mixture is then ground three times using a three-roll mill. The ground base material is transferred to a mixing tank, and a composite reactive diluent, defoamer, and leveling agent are gradually added at a stirring speed of 450 rpm. The mixture is stirred and mixed for 17.5 min. The composite reactive diluent consists of neopentyl glycol diglycidyl ether and allyl glycidyl ether. The oil and ether were mixed at a mass ratio of 7:3. Neopentyl glycol diglycidyl ether served as the performance backbone, forming rigid crosslinking points in the polymer network and enhancing the material's resistance to deformation under external forces. Allyl glycidyl ether served as a regulating agent, reducing viscosity and allowing for better leveling, wetting, and penetration into the micropores of the substrate, thereby generating a strong mechanical interlocking effect, resulting in component A. By uniformly and stably dispersing the high-performance modified and reinforced composite filler into the epoxy resin, and with the assistance of other additives, the wear resistance, adhesion, and corrosion resistance of the epoxy resin were improved.

[0063] S2. Mix component B with component A described in step S1 until homogeneous, and stir at 250 rpm for 2.5 min to obtain a solvent-free epoxy coating. The ether bonds in the molecular chain of the curing agent polyetheramine D-230 in component B have good flexibility and wettability, which helps the coating to better wet the substrate, penetrate into the micropores, form a strong mechanical interlocking effect, improve adhesion, and further enhance wear resistance and corrosion resistance, thereby improving the coating's performance.

[0064] Example 4

[0065] This embodiment proposes a solvent-free epoxy coating comprising the following components in parts by weight: 90 parts of component A and 22 parts of component B.

[0066] Component A comprises the following components in parts by weight: 20 parts of high-performance modified and reinforced composite filler, 80 parts of epoxy resin, 15 parts of composite reactive diluent, 0.8 parts of defoamer, and 0.8 parts of leveling agent.

[0067] Component B is the curing agent polyetheramine D-230.

[0068] High-performance modified and reinforced composite filler, comprising the following components in parts by weight: 30 parts nano silica, 15 parts dopamine hydrochloride, 30 parts hexadecylamine, 20 parts diethylenetriamine, and 10 parts polyetheramine D-230.

[0069] The preparation method of high-performance modified and reinforced composite fillers specifically includes the following steps:

[0070] (1) Dissolve 0.06g of tris(hydroxymethyl)aminomethane hydrochloride in 50mL of deionized water, adjust the pH to 8.5 with 0.4% sodium hydroxide solution to obtain a buffer solution for later use, disperse 0.3g of nano-silica in 10mL of deionized water to obtain silica sol for later use, then dissolve dopamine hydrochloride in the buffer solution, the amount of dopamine hydrochloride added is 0.15g. The addition of dopamine hydrochloride can form a polydopamine coating on the surface of nano-silica. The catechol groups in polydopamine can consume oxygen and inhibit the cathodic reaction, thus delaying the corrosion process from an electrochemical perspective. After ultrasonic dispersion for 50min, slowly drop it into the silica sol and react at room temperature for 12h. Wash with deionized water and centrifuge 3 times. The solid product was collected and vacuum dried at 60℃ for 6 hours to obtain polydopamine-coated silica. The polydopamine coating improved the filler properties of the nano silica. The polydopamine coating not only adhered to the nano silica with strong adhesion, but also formed chemical bonds or strong hydrogen bonds with the epoxy resin base, which enhanced the interfacial bonding force between the filler and the base, reduced the wear and damage of the epoxy resin itself, and formed a strong adhesion to the substrate surface after the coating was cured, which increased the contact area and mechanical interlocking effect between the coating and the substrate. The polydopamine coating also enabled the nano silica to be evenly dispersed, forming a denser and more tortuous physical barrier, increasing the diffusion path of corrosive media such as water, oxygen, and chloride ions.

[0071] (2) The polydopamine-coated silica from step (1) was added to 50 mL of anhydrous ethanol and ultrasonically treated for 40 min to obtain a polydopamine-coated silica dispersion for later use. Hexadecylamine was added to 50 mL of anhydrous ethanol at a dosage of 0.3 g. The long-chain alkyl group introduced by hexadecylamine imparts hydrophobic modification, improving the hydrophobicity and corrosion resistance of the material. After stirring until completely dissolved, it was slowly added to the polydopamine-coated silica dispersion while stirring and adding 0.2 mL of diethylenetriamine dropwise. After the addition was completed, the temperature was raised to 60 °C and the reaction was carried out for 12 h. The product was washed with anhydrous ethanol and centrifuged 3 times. Finally, it was measured at 8 °C. Vacuum drying at 0℃ for 8 hours yielded hydrophobic modified polydopamine-coated silica. Under the cross-linking and catalytic action of diethylenetriamine, the long chains of hexadecylamine were covalently anchored on the polydopamine coating and extended outward to form a low surface energy hydrophobic layer, which effectively blocked the penetration of water molecules and thus improved corrosion resistance. The strong covalent bond ensured that stress could be transferred from the soft resin base to the hard silica particles, reducing the wear of the resin base and enhancing wear resistance. Furthermore, the dispersed rigid silica nanoparticles also formed microscopic anchor points in the coating, increasing the mechanical interlocking strength and thus improving the adhesion of the coating.

[0072] (3) Add the hydrophobically modified polydopamine-coated silica from step (2) to 50 mL of anhydrous ethanol and ultrasonically disperse for 20 min to obtain a hydrophobically modified polydopamine-coated silica dispersion for later use. Dissolve polyetheramine D-230 in 10 mL of anhydrous ethanol. The amount of polyetheramine D-230 added is 0.1 g. The long flexible chain of polyetheramine D-230 can better penetrate and wrap around the epoxy resin molecular chain, which greatly improves the compatibility and dispersibility in the epoxy resin matrix. Furthermore, polyetheramine D-230 can also participate in subsequent processes. The curing of epoxy resin forms a robust, integrated network of filler and resin. After stirring for 20 minutes, a polyetheramine D-230 ethanol solution is obtained and set aside. This solution is then slowly added dropwise to a dispersion of hydrophobically modified polydopamine-coated silica. The mixture is heated to 60°C and stirred for 12 hours. The product is washed four times with anhydrous ethanol and centrifuged. It is then vacuum-dried at 80°C for 8 hours to obtain a high-performance modified and reinforced composite filler. This process, by coating the hydrophobically modified polydopamine-coated silica with a layer of hydrophilic, flexible polyetheramine chains, forms… A multi-level, amphiphilic core-shell structured material can be perfectly embedded in epoxy resin matrix, effectively improving the compatibility and dispersibility of fillers in epoxy resin matrix. Covalent bonding and the entanglement of polyether chains with epoxy resin ensure that external forces are efficiently transferred from the resin matrix to the internal rigid core. The outer flexible polyether chains effectively absorb and dissipate impact energy, preventing crack initiation and propagation, thus making the coating more robust and wear-resistant. Polyetheramine D-230 enables high-performance modified reinforced composite fillers and epoxy resin to interpenetrate and entangle, forming an interpenetrating network. The structure blurs the interface between the filler and the resin. At the same time, the flexible segments help alleviate the internal stress caused by curing shrinkage and thermal expansion and contraction, avoiding stress concentration that leads to decreased adhesion. Excellent compatibility and dispersibility can also reduce internal stress caused by filler agglomeration and poor interface, making the coating less likely to fall off the substrate after curing. This significantly improves the adhesion of the coating. Furthermore, excellent adhesion and dispersibility also avoid microcracks caused by insufficient adhesion or interface defects, effectively isolating the penetration of corrosive media, improving corrosion resistance, and providing long-term protection for the substrate.

[0073] This embodiment provides a method for preparing a solvent-free epoxy coating, specifically including the following steps:

[0074] S1. The high-performance modified reinforced composite filler and epoxy resin are premixed at 300 rpm for 3 minutes, wherein the epoxy resin is bisphenol A type epoxy resin. Then, the mixture is dispersed at 2000 rpm for 10 minutes using a high-speed disperser. The mixture is then ground four times using a three-roll mill. The ground base material is transferred to a mixing tank, and a composite reactive diluent, defoamer, and leveling agent are gradually added at a stirring speed of 600 rpm. The mixture is stirred and mixed for 15 minutes. The composite reactive diluent consists of neopentyl glycol diglycidyl ether and allyl glycidyl ether. The mixture was prepared by mixing in a mass ratio of 7:3. Neopentyl glycol diglycidyl ether served as the performance backbone, forming rigid crosslinking points in the polymer network, which enhanced the material's resistance to deformation under external forces. Allyl glycidyl ether served as a regulating agent, which reduced viscosity, allowing for better leveling, wetting, and penetration into the micropores of the substrate, thereby generating a strong mechanical interlocking effect, resulting in component A. By uniformly and stably dispersing the high-performance modified and reinforced composite filler into the epoxy resin, and with the assistance of other additives, the wear resistance, adhesion, and corrosion resistance of the epoxy resin were improved.

[0075] S2. Mix component B with component A described in step S1 until homogeneous, and stir at 300 rpm for 2 minutes to obtain a solvent-free epoxy coating. The ether bonds in the molecular chain of the curing agent polyetheramine D-230 in component B have good flexibility and wettability, which helps the coating to better wet the substrate, penetrate into the micropores, form a strong mechanical interlocking effect, improve adhesion, and further enhance wear resistance and corrosion resistance, thereby improving the coating's performance.

[0076] Comparative Example 1

[0077] This comparative example provides a solvent-free epoxy coating, which differs from Example 1 in that the high-performance modified and reinforced composite filler does not contain dopamine hydrochloride, hexadecylamine, or diethylenetriamine; the preparation method of the high-performance modified and reinforced composite filler does not include step (2), and dopamine hydrochloride is not added in step (1); the preparation method of the solvent-free epoxy coating is the same as that of Example 1.

[0078] Comparative Example 2

[0079] This comparative example provides a solvent-free epoxy coating, which differs from Example 1 in that the high-performance modified and reinforced composite filler does not contain polyetheramine D-230; the preparation method of the high-performance modified and reinforced composite filler does not include step (3); and the preparation method of the solvent-free epoxy coating is the same as that of Example 1.

[0080] Comparative Example 3

[0081] This comparative example provides a solvent-free epoxy coating, which differs from Example 1 in that the composite reactive diluent does not contain allyl glycidyl ether; the preparation method of the high-performance modified reinforced composite filler is the same as that of Example 1; and allyl glycidyl ether is not added in step S1 of the preparation method of the solvent-free epoxy coating.

[0082] Experimental Example 1

[0083] Adhesion test

[0084] Test samples: Solvent-free epoxy coatings prepared in Examples 1-4 and Comparative Examples 1-3.

[0085] Test method: The test samples were tested using a pull-out adhesion tester and measured according to ASTM D4541 standard. The pressure system was calibrated by NIST with an accuracy of ±1% (full scale) and the value was accurate to 0.01.

[0086] Figure 1 The figures show the adhesion results for Examples 1-4 and Comparative Examples 1-3. As shown, the adhesion of Examples 1-4 is 14.7-16.2 MPa, indicating good adhesion; the adhesion of Comparative Examples 1-3 is 10.0-12.5 MPa, indicating moderate adhesion. The high-performance modified reinforced composite filler in Comparative Example 1 does not contain dopamine hydrochloride, hexadecylamine, or diethylenetriamine. Therefore, the introduction of a polydopamine coating layer and a hexadecylamine hydrophobic layer cannot improve the compatibility and dispersibility of the filler in the epoxy resin. The uneven dispersion of the filler prevents it from forming microscopic anchor points in the coating, which is detrimental to increasing mechanical interlocking strength. Furthermore, it cannot utilize the super-strong adhesion. The use of fillers to enhance coating adhesion results in only average adhesion. The high-performance modified reinforced composite filler in Comparative Example 2 does not contain polyetheramine D-230, making it unable to penetrate or entangle with epoxy resin, which is detrimental to improving the interfacial bonding between the filler and resin. Furthermore, the lack of flexible chain segments is also detrimental to alleviating internal stress caused by curing shrinkage and thermal expansion and contraction, affecting adhesion and resulting in only average adhesion. The composite reactive diluent in Comparative Example 3 does not contain allyl glycidyl ether, making it unable to exert a plasticizing effect through the long-chain olefins of allyl glycidyl ether. This is detrimental to absorbing and releasing internal stress caused by curing shrinkage or thermal expansion and contraction, increasing the risk of coating peeling and resulting in only average adhesion.

[0087] Experiment Example 2

[0088] Abrasion resistance test

[0089] Test samples: Solvent-free epoxy coatings prepared in Examples 1-4 and Comparative Examples 1-3.

[0090] Test Method: The test sample was uniformly coated onto a ceramic fiber board (330×300×3mm) to form a sample with a coating thickness of 2±0.1mm. After complete curing, the wear performance of the sample was tested using a UMT-Tribolbab ball-and-disc friction testing machine. A Si3N4 ball with a diameter of 6.35mm was used as the friction pair material. The sliding test load (F) was 10N, the rotation speed (R) was 364r / min, the rotation radius (d) was 3.5mm, and the test time (T) was 60min. The total wear volume (Vm) of the coating was measured using an Alphastep P-7 probe contact profilometer, and the volumetric wear rate (mm) of the coating was calculated using the following formula. 3 / N·m):

[0091] Volumetric wear rate (mm) 3 / N·m)=Vm / (3.14×F×d×R×T).

[0092] Figure 2 The figures show the volumetric wear rate results for Examples 1-4 and Comparative Examples 1-3; as shown, the volumetric wear rate for Examples 1-4 is 0.5-1.2 × 10⁻⁶. -5 mm 3 / N·m indicates strong wear resistance; the volumetric wear rate of comparative examples 1-3 is 2.8-5.6×10 - 5 mm 3 / N·m indicates that the wear resistance is average. The high-performance modified and reinforced composite filler in Comparative Example 1 does not contain dopamine hydrochloride, hexadecylamine, or diethylenetriamine. Therefore, it cannot stabilize the uniform dispersion of the filler in the epoxy resin through polydopamine adhesion and hexadecylamine covalent bonding. This hinders the transfer of external force from the resin matrix to the internal rigid core, increasing epoxy resin wear and resulting in average wear resistance. The high-performance modified and reinforced composite filler in Comparative Example 2 does not contain polyetheramine D-230. Therefore, it cannot stably embed the filler into the epoxy resin matrix through the entanglement of polyetheramine chains. This also hinders the efficient transfer of external force from the resin matrix to the internal rigid core, resulting in average wear resistance. The composite reactive diluent in Comparative Example 3 does not contain allyl glycidyl ether, which is detrimental to adjusting the viscosity and leveling properties of the coating and cannot balance the crosslinking density of neopentyl glycol diglycidyl ether. This increases the risk of brittleness in the coating, making it prone to cracking and resulting in average wear resistance.

[0093] Experimental Example 3

[0094] Corrosion resistance test

[0095] Test samples: Solvent-free epoxy coatings prepared in Examples 1-4 and Comparative Examples 1-3.

[0096] Test method: According to the national standard GB / T1771-2007, the test sample is marked with an "X" on the substrate and then placed in a salt spray chamber at a temperature of 35±2℃. The salt spray solution deposition rate is 1.5±0.5mL / h. A 5% NaCl solution (pH 6.5-7.2) is used to conduct a salt spray resistance test for 500h. After the test, the rust is peeled off along the "X" mark, and the length of the maximum corrosion on the substrate is measured and recorded as the maximum corrosion length (mm). The smaller the maximum corrosion length, the stronger the corrosion resistance.

[0097] Figure 3 The figures show the maximum corrosion length results for Examples 1-4 and Comparative Examples 1-3. As shown, the maximum corrosion length for Examples 1-4 is 0.3-0.9 mm, indicating good corrosion resistance. The maximum corrosion length for Comparative Examples 1-3 is 1.8-3.6 mm, indicating moderate corrosion resistance. The high-performance modified reinforced composite filler in Comparative Example 1 does not contain dopamine hydrochloride, hexadecylamine, or diethylenetriamine. Therefore, it cannot covalently anchor the long chain of hexadecylamine to the polydopamine coating layer, thus failing to form a low surface energy hydrophobic layer on the silica surface. This is detrimental to blocking water molecule penetration and reducing microcracks caused by insufficient adhesion or interface defects, and thus cannot effectively isolate corrosive media. The infiltration of corrosive media results in only moderate corrosion resistance. In Comparative Example 2, the high-performance modified reinforced composite filler lacks polyetheramine D-230, making it unable to form a multi-layered, amphiphilic core-shell structure. This hinders the uniform dispersion and stable embedding of the filler into the epoxy resin matrix. Consequently, the excellent interfacial bonding between the high-performance modified reinforced composite filler and the epoxy resin matrix fails to block the infiltration of corrosive media, leading to only moderate corrosion resistance. Similarly, in Comparative Example 3, the composite reactive diluent lacks allyl glycidyl ether, preventing it from wetting and penetrating the micropores of the substrate by improving coating viscosity. This hinders the reduction of pinholes and microbubbles after coating curing, increasing the penetration pathways of corrosive media and resulting in only moderate corrosion resistance.

[0098] The above experimental results show that the adhesion, wear resistance, and corrosion resistance of Examples 1-4 of the present invention are significantly better than those of Comparative Examples 1-3. Among them, Example 1, which uses high-performance modified reinforced composite filler and composite reactive diluent, has better adhesion, stronger wear resistance, and better corrosion resistance. The high-performance modified reinforced composite filler is uniformly dispersed and stably embedded in the epoxy resin matrix. The excellent compatibility and dispersibility can reduce the internal stress caused by filler agglomeration and poor interface, making it less likely for the coating to fall off the substrate after curing. In addition, the excellent adhesion and dispersibility also avoid wear, peeling, and cracking caused by insufficient adhesion or interface defects. This not only enhances the toughness and wear resistance of the coating, but also effectively isolates the penetration of corrosive media. At the same time, with the assistance of additives such as composite reactive diluent, the adhesion, wear resistance, and corrosion resistance of the coating are further enhanced.

[0099] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.

[0100] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention. The actual application is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar methods and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.

Claims

1. A solvent-free epoxy coating, characterized in that: The solvent-free epoxy coating comprises the following components in parts by weight: 80-90 parts of component A and 22-30 parts of component B; component A comprises the following components in parts by weight: 20-30 parts of high-performance modified and reinforced composite filler, 60-80 parts of epoxy resin, 8-15 parts of composite reactive diluent, 0.4-0.8 parts of defoamer, and 0.4-0.8 parts of leveling agent; component B is curing agent polyetheramine D-230; the high-performance modified and reinforced composite filler comprises the following components in parts by weight: 10-30 parts of nano silica, 5-15 parts of dopamine hydrochloride, 30-50 parts of hexadecylamine, 20-40 parts of diethylenetriamine, and 10-20 parts of polyetheramine D-230.

2. A method for preparing a solvent-free epoxy coating according to claim 1, characterized in that: Specifically, the following steps are included: S1. Premix the high-performance modified and reinforced composite filler and epoxy resin at 200-300 rpm for 3-5 minutes, wherein the epoxy resin is bisphenol A type epoxy resin. Then disperse it at 1000-2000 rpm for 10-15 minutes using a high-speed disperser. Grind the mixture 2-4 times using a three-roll mill. Transfer the ground base material to a mixing tank. Gradually add the composite reactive diluent, defoamer, and leveling agent at 300-600 rpm and mix for 15-20 minutes to obtain component A. S2. Mix component B with component A from step S1 until homogeneous, and stir at 200-300 rpm for 2-3 minutes to obtain a solvent-free epoxy coating.

3. The method for preparing solvent-free epoxy coating according to claim 2, characterized in that: In step S1, the composite reactive diluent is obtained by mixing neopentyl glycol diglycidyl ether and allyl glycidyl ether in a mass ratio of 7:

3.

4. The method for preparing solvent-free epoxy coating according to claim 3, characterized in that: The preparation method of the high-performance modified and reinforced composite filler specifically includes the following steps: (1) Dissolve 0.04-0.06g of tris(hydroxymethyl)aminomethane hydrochloride in 50mL of deionized water, adjust the pH to 8.5 with 0.4% sodium hydroxide solution to obtain a buffer solution for later use, disperse 0.1-0.3g of nano-silica in 10mL of deionized water to obtain silica sol for later use, then dissolve dopamine hydrochloride in the buffer solution, sonicate for 50-60min, and then slowly drop it into the silica sol. React at room temperature for 12-24h, wash with deionized water and centrifuge 2-3 times, collect the solid product, and vacuum dry at 50-60℃ for 6-8h to obtain polydopamine-coated silica; (2) Add the polydopamine-coated silica from step (1) to 50 mL of anhydrous ethanol and treat it with ultrasound for 40-60 min to obtain a polydopamine-coated silica dispersion for later use. Add hexadecylamine to 50 mL of anhydrous ethanol and stir until completely dissolved. Then slowly add it to the polydopamine-coated silica dispersion while stirring and adding 0.2-0.4 mL of diethylenetriamine dropwise. After the addition is complete, raise the temperature to 50-60 °C and react for 12-18 h. Wash the product with anhydrous ethanol and centrifuge 2-3 times. Finally, vacuum dry it at 70-80 °C for 8-10 h to obtain hydrophobic modified polydopamine-coated silica. (3) Add the hydrophobic modified polydopamine-coated silica from step (2) to 50 mL of anhydrous ethanol and ultrasonically disperse for 20-30 min to obtain a hydrophobic modified polydopamine-coated silica dispersion for later use. Dissolve polyetheramine D-230 in 10 mL of anhydrous ethanol and stir for 20-30 min to obtain a polyetheramine D-230 ethanol solution for later use. Then slowly add the polyetheramine D-230 ethanol solution to the hydrophobic modified polydopamine-coated silica dispersion, heat to 50-60℃, stir and react for 12-18 h, wash and centrifuge with anhydrous ethanol 3-4 times, and vacuum dry the product at 60-80℃ for 8-10 h to obtain a high-performance modified and reinforced composite filler.

5. The method for preparing solvent-free epoxy coating according to claim 4, characterized in that: In step (1), the amount of dopamine hydrochloride added is 0.05-0.15g.

6. The method for preparing solvent-free epoxy coating according to claim 5, characterized in that: In step (2), the amount of hexadecylamine added is 0.3-0.5g.

7. The method for preparing solvent-free epoxy coating according to claim 6, characterized in that: In step (3), the amount of polyetheramine D-230 added is 0.1-0.2g.

Citation Information

Patent Citations

  • Solvent-free flexible anticorrosion epoxy coating material, preparation method thereof and using method thereof

    CN103788735A

  • Wire drawing process for preparing high-toughness antioxidant PP plastic wire

    CN112625351A

  • Wet-coating solvent-free heavy anti-corrosion coating composition as well as preparation method and application thereof

    CN112760006A

  • Graphene type low-viscosity thin-coating high-hardness super-wear-resistant solvent-free epoxy coating and preparation thereof

    CN114381182A

  • Solvent-free wave-absorbing coating and preparation method thereof

    CN116410645A

Cited By

  • Thermal insulation coating and preparation method thereof

    CN121022207A