Wheat straw cellulose full-biodegradable composite material

By using fully biodegradable raw materials such as wheat straw cellulose, PBS, and PLA, as well as pH-responsive fungal spore microcapsules, combined with a staged extrusion process, the contradiction between the mechanical properties and degradability of wheat straw cellulose-based composite materials during service was resolved, achieving efficient and complete degradation of the material after disposal.

CN120988437APending Publication Date: 2025-11-21DATONG ZHONGZHI BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511492210.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-20
Publication Date
2025-11-21

AI Technical Summary

Technical Problem

Existing technologies struggle to ensure that wheat straw cellulose-based composite materials possess excellent mechanical properties during service while simultaneously enabling them to be precisely triggered and initiate an efficient and complete biodegradation process under specific environmental conditions after disposal. This results in a contradiction between service stability and end-of-life degradation throughout the material's life cycle.

Method used

Using fully biodegradable raw materials such as wheat straw cellulose, PBS, and PLA, the mechanical properties are improved by using hydrophobically modified micronized cellulose as a reinforcing phase. The degradation timing is precisely controlled by pH-responsive fungal spore microcapsules, and the staged extrusion process ensures the synergistic optimization of material stability during use and degradation after disposal.

Benefits of technology

This technology enables materials to maintain their performance while also possessing environmentally triggered degradation capabilities, ensuring structural stability during service and efficient and complete degradation after disposal. It resolves the contradiction between mechanical properties and degradability throughout the material's life cycle.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of composite materials, and particularly relates to a wheat straw cellulose full-biodegradable composite material which is prepared by the following steps: (1) preparing hydrophobically modified MFC; (2) pre-degrading PLA (polylactic acid); (3) preparing fungal spore microcapsules; and (4) extruding and granulating to obtain the wheat straw cellulose full-biodegradable composite material. According to the scheme, full-biodegradable raw materials such as wheat straw cellulose, PBS and PLA are selected as main bodies, high-value utilization of agricultural waste is achieved, the degradable property of the material is guaranteed from the source, meanwhile, the mechanical property is improved by introducing a hydrophobic modified micron cellulose reinforced phase, the degradation time is precisely regulated and controlled in cooperation with a pH response type fungal spore microcapsule, and the degradation efficiency is improved. And the material has environment-triggered degradation capability while maintaining the use performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite materials, and more specifically, relates to a fully biodegradable composite material made from wheat straw cellulose. Background Technology

[0003] Developing environmentally friendly materials derived from renewable resources and possessing full biodegradability has become a core development direction in the field of materials science and engineering. Among these, utilizing abundant and inexpensive agricultural waste, such as wheat straw, and transforming it into high-performance composite materials through high-value-added technologies not only provides an effective way to solve the problem of agricultural waste disposal but also aligns with the strategic need to build a green and low-carbon industrial system. The main chemical components of wheat straw are cellulose, hemicellulose, and lignin. Its cellulose fraction, due to its excellent mechanical properties, low density, and biodegradability, is considered an ideal natural filler for preparing reinforcing composite materials.

[0004] Wheat straw cellulose, as a natural polymer material, has a surface rich in hydrophilic hydroxyl groups, while the biodegradable polymer matrix (such as polylactic acid PLA, polybutylene succinate PBS, etc.) is significantly hydrophobic. This inherent polarity difference leads to extremely poor interfacial compatibility between the two, making the interfacial layer a weak point in the entire composite material system. To ensure sufficient strength and durability of the material during its service life (such as as packaging material, disposable tableware, or agricultural mulch film), cellulose must be hydrophobically modified or compatibilizers must be introduced to strengthen the interfacial bonding between the fiber and the matrix. Although this strengthened interface improves the macroscopic mechanical properties of the material, after the material is discarded, the tight interfacial structure forms a physical barrier, tightly encapsulating the cellulose within the hydrophobic polymer matrix. This greatly hinders the erosion of cellulose by moisture and microorganisms, thus significantly slowing down the overall degradation rate of the material. Conversely, if a weak interface is retained or designed to accelerate degradation, the material is highly susceptible to premature dissociation and performance degradation during service due to moisture intrusion at the interface, rendering it unable to meet basic application requirements. Therefore, existing technologies face a dilemma: strengthened interfaces designed to improve service life inevitably inhibit end-of-life degradation efficiency; while weak interfaces designed to promote end-of-life degradation sacrifice service life reliability. This fundamental conflict in interface performance requirements across different stages of the material's lifecycle is the core bottleneck currently facing the development of wheat straw cellulose-based composite materials technology, and cannot be fundamentally resolved simply by adjusting component ratios or using conventional interface modification methods.

[0005] Therefore, how to break through the limitations of the existing technical framework, and through systematic innovative design of composite material systems, to ensure that the materials have excellent mechanical properties and structural stability during service, while enabling them to be precisely triggered and start an efficient and complete biodegradation process under specific environmental conditions after disposal, thereby fundamentally solving the inherent contradiction between service stability and end-of-life degradability, has become a key technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention

[0006] To address the aforementioned issues, this invention provides a fully biodegradable wheat straw cellulose composite material. It selects fully biodegradable raw materials such as wheat straw cellulose, PBS, and PLA as the main components, achieving high-value utilization of agricultural waste while ensuring the material's biodegradability from the source. Furthermore, the mechanical properties are enhanced by introducing a hydrophobically modified micronized cellulose reinforcing phase, and pH-responsive fungal spore microcapsules are used to precisely control the degradation timing, enabling the material to maintain its performance while possessing environmentally triggered degradation capabilities.

[0007] To achieve the above objectives, the technical solution of the present invention is as follows: A fully biodegradable composite material made from wheat straw cellulose is prepared through the following steps: Step (1) Preparation of hydrophobically modified MFC: Chop wheat straw into 1-3 cm lengths and put it into a 5 wt% sodium hydroxide solution. Use 3-8 parts of sodium hydroxide per 100 parts of wheat straw. Stir at 70-90℃ for 1-3 h. After draining the alkaline solution, wash with water until neutral. Immerse in a 3 wt% hydrogen peroxide solution. Use 2-5 parts of hydrogen peroxide per 100 parts of wheat straw. Bleach at 70-90℃ for 0.5-2 h. Wash and dry. Dissociate the fibers using a disc mill. Adjust the disc gap to 0.1-0.3 mm and circulate the mill 3-5 times to obtain micron-sized cellulose MFC with an aspect ratio of 15-25. Subsequently, 100 parts of micronized cellulose MFC were immersed in a mixed solution containing 2-5 parts of citric acid and 20-40 parts of glycerol, and reacted at 75±5℃ for 2-4 h; the reaction system was then transferred to an ice-water bath at 0-5℃ and cooled to 25±5℃ within 10 min; 0.5-2 parts of molten beeswax or an equal mass of rice bran wax or candelilla wax and 0.1-0.5 parts of nano-silica with a particle size of 10-30 nm were added, and the mixture was dispersed at a high speed of 2000 rpm for 20 min; after filtration, the mixture was vacuum dried at 60℃ for 12 h to obtain hydrophobically modified MFC; Step (2) PLA pre-degradation: Place polylactic acid PLA in a constant temperature and humidity chamber at 75±5℃ and 85±5% for 24-72 h; Step (3) Preparation of fungal spore microcapsules: Adjust the concentration of Aspergillus niger spore suspension to 10.8 CFU / mL, add 1-10 wt% sodium alginate solution to form a core material solution; dissolve 85 parts PLA in dichloromethane to prepare a 14-16 wt% solution, add 12-18 parts nano-kaolin with a particle size of 10-30 nm, and ultrasonically disperse at 300 W for 20 min; mix the core material solution and oil phase at a volume ratio of 1:2.8-3.2, and homogenize and emulsify at 12000 rpm for 10 min to form a W / O emulsion; inject the emulsion into 0.1-0.2 mol / L calcium chloride solution, stir at 500 rpm for 30 min to prepare microcapsules, filter and collect the microcapsules, spray-coat with 0.4-0.6 wt% stearic acid ethanol solution, dry and sieve to obtain 50-150 μm particles; coat the surface of the microcapsules with a pH-responsive layer of 1.8-2.2 wt% chitosan acetate solution, drain and cure at 60℃ for 1 h; Step (4) Composite granulation: Prepare materials by weight: 100 parts PBS resin, 5-15 parts pre-degraded PLA obtained in step (3), 5-15 parts standard PLA with a weight average molecular weight of 150,000 Da, 30-50 parts hydrophobically modified MFC, 0.5-2 parts PBS-g-MAH with a maleic anhydride grafting rate of 1.8±0.2%, 0.2-1 parts antioxidant 306, 1-6 parts glycerol, and 1-3 parts fungal spore microcapsules; First-stage extrusion: Hydrophobic modified MFC and 50 parts of PBS were fed into a co-rotating twin-screw extruder with an aspect ratio of 45:1. The temperatures in zone 1 were 110℃, zone 2 was 115℃, zone 3 was 120℃, zone 4 was 120℃, and zone 5 was 125℃. The screw speed was 200±50 rpm. Extrusion granulation was carried out. Second-stage extrusion: The masterbatch obtained from the first-stage extrusion, the remaining 50 parts of PBS, pre-degradable PLA, standard PLA, PBS-g-MAH, antioxidant 306, and glycerol are fed into the extruder; fungal spore microcapsules are injected through the side feed port in the Z6 zone of the melt plasticizing section, the melt temperature is controlled at 140±5℃, the residence time is ≤60 s, and the mass ratio of the side feed port feeding speed to the main screw speed is 1:10; the temperatures of each zone are set as follows: Zone 1 130℃, Zone 2 135℃, Zone 3 140℃, Zone 4 145℃, Zone 5 140℃, melt pressure ≤8MPa, screw speed 150 rpm, and the wheat straw cellulose fully biodegradable composite material is obtained by extrusion granulation.

[0008] This solution aims to achieve full biodegradability, with its technical approach closely centered on the efficient utilization and functional synergy of natural biodegradable raw materials. Its key technical features are reflected in the targeted design of multiple stages: micron-sized fibers are prepared by alkali treatment, bleaching, and grinding of wheat straw cellulose; these fibers are then citric acid esterified, wax-coated, and reinforced with nanoparticles to achieve hydrophobic modification, preserving the reinforcing potential of natural fibers while improving their compatibility with the hydrophobic matrix; pre-degradation of PLA is performed to regulate its molecular weight and optimize processing flowability, while standard PLA is introduced to maintain the matrix's mechanical properties; the preparation of fungal spore microcapsules incorporates a pH-responsive release mechanism to ensure material stability during use and precise triggering of degradation activity after disposal; the staged extrusion process reduces fiber agglomeration through masterbatch premixing, and the side-feeding method avoids the destruction of spore activity caused by long-term high-temperature treatment, achieving uniform dispersion and functional retention of each component. In terms of parameter design, from the temperature and time of raw material processing to the temperature and speed control of the processing process, all are centered around balancing the mechanical properties, processing performance and degradation efficiency of the material. It not only adapts to the chemical characteristics of natural fibers and the processing requirements of polymer matrix, but also ensures that the material can achieve complete biodegradation in the natural environment after completing its function through the slow-release design of microcapsules and the selection of biodegradable raw materials, ultimately achieving the goal of preparing a fully biodegradable material that has both practical performance and environmental protection attributes.

[0009] The key parameters of this scheme are designed around the preservation of fungal activity, the balance of material properties, and the controllability of degradation, forming a mutually reinforcing technical logic. Regarding the protection of fungal spore activity, a side-feeding method is used during the second-stage extrusion to inject microcapsules during the melt plasticizing stage, while simultaneously controlling the melt temperature at 140±5℃ and the residence time at ≤60s. This design avoids damage to the spores during the initial high-temperature plasticizing stage and reduces thermal stress damage to the spore structure through shorter heating time and suitable temperature, ensuring that the spores retain their biological activity after processing. In microcapsule preparation, the 50-150μm sieve particle size is matched with the coating parameters of the chitosan pH-responsive layer. The particle size ensures the structural integrity of the microcapsules under extrusion shear force, while the chitosan layer remains stable under neutral conditions in normal service environments, preventing premature spore release and providing a physical barrier for activity preservation. The PLA pre-degradation parameters are set at 75±5℃, humidity 85±5%, and time 24-72h. These conditions can moderately reduce the molecular weight of PLA to improve processing fluidity, while avoiding excessive degradation that would lead to loss of matrix strength. This, combined with standard PLA, creates a balance between mechanical and processing properties, laying the foundation for the structural stability of the composite material during service. The achievement of non-degradation during service and degradation in the natural environment depends on the pH-responsive release mechanism of the microcapsules and the material's inherent degradability: During service, the chitosan layer remains stable in a neutral environment, preventing fungal spores from functioning. PBS and the PLA matrix degrade slowly under normal operating conditions, ensuring material functional stability. Upon entering the natural environment, pH changes in soil and other environments trigger the decomposition of the chitosan layer. Released Aspergillus niger spores multiply under suitable conditions, secreting enzymes that accelerate the decomposition of cellulose and the matrix material. Simultaneously, the biodegradability of PBS and PLA is activated, ultimately achieving complete degradation of the material in the natural environment.

[0010] Preferably, the beeswax mentioned in step (1) can be replaced with an equal amount of rice bran wax or candelilla wax.

[0011] Preferably, the pH-responsive layer of the microcapsule in step (3) is coated with a 2 wt% chitosan acetate solution, drained, and then cured at 60°C for 1 h.

[0012] By coating the surface of microcapsules with a 2 wt% chitosan-acetic acid solution to form a pH-responsive layer, the theoretical advantage lies in utilizing the natural pH sensitivity of chitosan to achieve intelligent response regulation of the microcapsules to the acidity or alkalinity of the environment. Chitosan molecules are rich in amino groups, which readily protonate under acidic conditions to form positively charged ammonium ions. This leads to enhanced electrostatic repulsion between molecular chains, a looser structure, and increased hydrophilicity and swelling. Conversely, in neutral or alkaline environments, the degree of amino protonation decreases, the molecular chains become more compact, hydrophilicity weakens, and the structure becomes more stable. This characteristic allows the microcapsules to dynamically adjust their surface properties according to changes in the pH of their environment—for example, in acidic environments, the degree of chitosan protonation increases, and the microcapsule surface becomes more porous, promoting the release of fungal spores; in neutral or weakly alkaline environments, chitosan maintains a lower protonation level, resulting in a denser surface structure and delayed spore release.

[0013] Preferably, in step (4), the melt temperature of the second-stage extrusion is 140±5℃, and the mass ratio of the side feed port feeding speed to the main screw speed is 1:10.

[0014] Preferably, the sodium alginate solution in step (3) has a mass concentration of 1-5 wt%.

[0015] Preferably, the nano-silica in step (1) has a particle size of 10-30 nm, a high-speed dispersion speed of 2000 rpm, and a dispersion time of 20 min.

[0016] Preferably, the concentration of the fungal spore suspension in step (3) is 10⁸ CFU / mL, and the microcapsule sieve particle size range is 50-150 μm.

[0017] Compared to existing technologies, the advantages of this solution are: 1. From the perspective of composition, this solution selects fully biodegradable raw materials such as wheat straw cellulose, PBS, and PLA as the main components, which not only realizes the high-value utilization of agricultural waste, but also ensures the biodegradability of the material from the source. At the same time, the mechanical properties are improved by introducing hydrophobically modified micronized cellulose reinforcement phase, and the degradation timing is precisely controlled by pH-responsive fungal spore microcapsules, so that the material can have environmentally triggered degradation capability while maintaining its performance. 2. From a process perspective, the staged extrusion process solves the problem of natural fiber agglomeration by first preparing masterbatches of MFC and PBS, and then injecting microcapsules at specific stages using a side-feeding method, which avoids the destruction of spore activity caused by high-temperature and long-term processing. The combination of PLA pre-degradation treatment and standard PLA balances processing flowability and matrix strength. The overall process design not only ensures the effective preservation of the functions of each component, but also achieves synergistic optimization of material properties and degradation characteristics.

[0018] Compared to existing technologies, the advantages of this solution are: 1. From the perspective of composition, this solution selects fully biodegradable raw materials such as wheat straw cellulose, PBS, and PLA as the main components, which not only realizes the high-value utilization of agricultural waste, but also ensures the biodegradability of the material from the source. At the same time, the mechanical properties are improved by introducing hydrophobically modified micronized cellulose reinforcement phase, and the degradation timing is precisely controlled by pH-responsive fungal spore microcapsules, so that the material can have environmentally triggered degradation capability while maintaining its performance. 2. From a process perspective, the staged extrusion process solves the problem of natural fiber agglomeration by first preparing masterbatches of MFC and PBS, and then injecting microcapsules at specific stages using a side-feeding method, which avoids the destruction of spore activity caused by high-temperature and long-term processing. The combination of PLA pre-degradation treatment and standard PLA balances processing flowability and matrix strength. The overall process design not only ensures the effective preservation of the functions of each component, but also achieves synergistic optimization of material properties and degradation characteristics.

[0019] Example 2 A fully biodegradable composite material made from wheat straw cellulose is prepared through the following steps: Step (1) Preparation of hydrophobically modified MFC: Chop wheat straw into 1cm lengths and add it to a 5wt% sodium hydroxide solution (3 parts sodium hydroxide per 100 parts wheat straw). Stir at 70℃ for 1 hour. After draining the alkaline solution, wash with water until neutral. Immerse in a 3wt% hydrogen peroxide solution (2 parts hydrogen peroxide per 100 parts wheat straw) and bleach at 70℃ for 0.5 hours. Wash and dry. Dissociate the fibers using a disc mill, adjust the disc gap to 0.1mm, and circulate for 3 hours. First, micron-sized cellulose MFC with an aspect ratio of 15 was obtained. Then, 100 parts of micron-sized cellulose MFC were immersed in a mixed solution containing 2 parts of citric acid and 20 parts of glycerol and reacted at 70°C for 2 hours. The reaction system was then transferred to an ice-water bath at 0°C and cooled to 20°C within 10 minutes. 0.5 parts of molten rice bran wax and 0.1 parts of nano-silica with a particle size of 10 nm were added and dispersed at a high speed of 2000 rpm for 20 minutes. After filtration, the mixture was vacuum dried at 60°C for 12 hours to obtain hydrophobically modified MFC. Step (2) PLA pre-degradation: Place polylactic acid PLA in a constant temperature and humidity chamber at 70℃ and 80% for 24 hours; Step (3) Preparation of fungal spore microcapsules: Adjust the concentration of Aspergillus niger spore suspension to 10. 8CFU / mL was added to a 1wt% sodium alginate solution to form a core material solution; 85 parts of PLA were dissolved in dichloromethane to prepare a 14wt% solution, and 12 parts of 10nm nano-kaolin were added. The solution was ultrasonically dispersed at 300W for 20min; the core material solution and oil phase were mixed at a volume ratio of 1:2.8 and homogenized at 12000rpm for 10min to form a W / O emulsion; the emulsion was injected into a 0.1mol / L calcium chloride solution and stirred at 500rpm for 30min; the microcapsules were collected by filtration, spray-coated with a 0.4wt% stearic acid ethanol solution, dried, and sieved to obtain 50μm particles; the surface of the microcapsules was coated with a pH-responsive layer of a 1.8wt% chitosan acetate solution, drained, and cured at 60℃ for 1h; Step (4) Composite Granulation: Prepare materials by weight: 100 parts PBS resin, 5 parts pre-degraded PLA obtained in step (3), 5 parts standard PLA with a weight average molecular weight of 150,000 Da, 30 parts hydrophobically modified MFC, 0.5 parts PBS-g-MAH with a maleic anhydride grafting rate of 1.6%, 0.2 parts antioxidant 306, 1 part glycerol, and 1 part fungal spore microcapsules; First-stage extrusion: Put the hydrophobically modified MFC and 50 parts PBS into a co-rotating twin-screw extruder with a length-to-diameter ratio of 45:1. The temperature of zone 1 is 110℃, zone 2 is 115℃, zone 3 is 120℃, zone 4 is 120℃, and zone 5 is 125℃. The screw speed is 150 rpm. Granulation; Second-stage extrusion: The masterbatch obtained from the first-stage extrusion, the remaining 50 parts of PBS, pre-degradable PLA, standard PLA, PBS-g-MAH, antioxidant 306, and glycerol were fed into the extruder; fungal spore microcapsules were injected through the side feed port in the Z6 zone of the melt plasticizing section, the melt temperature was controlled at 135℃, the residence time was 50s, and the mass ratio of the side feed port feeding speed to the main screw speed was 1:10; the temperatures of each zone were set as follows: Zone 1 130℃, Zone 2 135℃, Zone 3 140℃, Zone 4 145℃, Zone 5 140℃, melt pressure 6MPa, screw speed 150rpm, and extrusion granulation was used to obtain a fully biodegradable wheat straw cellulose composite material.

[0020] Example 3 A fully biodegradable composite material made from wheat straw cellulose is prepared through the following steps: Step (1) Preparation of hydrophobically modified MFC: Chop wheat straw into 3cm lengths and put it into a 5wt% sodium hydroxide solution (8 parts sodium hydroxide per 100 parts wheat straw). Stir at 90℃ for 3h. After draining the alkaline solution, wash with water until neutral. Immerse in a 3wt% hydrogen peroxide solution (5 parts hydrogen peroxide per 100 parts wheat straw) and bleach at 90℃ for 2h. Wash and dry. Dissociate the fibers using a disc mill, adjust the disc gap to 0.3mm, and circulate and grind 5 times. Micronized cellulose MFC with an aspect ratio of 25 was obtained. Subsequently, 100 parts of micronized cellulose MFC were immersed in a mixed solution containing 5 parts of citric acid and 40 parts of glycerol and reacted at 80°C for 4 hours. The reaction system was then transferred to an ice-water bath at 5°C and cooled to 30°C within 10 minutes. 2 parts of molten candelilla wax and 0.5 parts of nano-silica with a particle size of 30 nm were added and dispersed at a high speed of 2000 rpm for 20 minutes. After filtration, the mixture was vacuum dried at 60°C for 12 hours to obtain hydrophobically modified MFC. Step (2) PLA pre-degradation: Place polylactic acid PLA in a constant temperature and humidity chamber at 80℃ and 90% for 72h; Step (3) Preparation of fungal spore microcapsules: Adjust the concentration of Aspergillus niger spore suspension to 10. 8 CFU / mL was added to a 10wt% sodium alginate solution to form a core material solution; 85 parts of PLA were dissolved in dichloromethane to prepare a 16wt% solution, and 18 parts of 30nm nano-kaolin were added. The solution was ultrasonically dispersed at 300W for 20min; the core material solution and oil phase were mixed at a volume ratio of 1:3.2 and homogenized at 12000rpm for 10min to form a W / O emulsion; the emulsion was injected into a 0.2mol / L calcium chloride solution and stirred at 500rpm for 30min; the microcapsules were collected by filtration, spray-coated with a 0.6wt% stearic acid ethanol solution, dried, and sieved to obtain 150μm particles; the surface of the microcapsules was coated with a pH-responsive layer of a 2.2wt% chitosan acetate solution, drained, and cured at 60℃ for 1h; Step (4) Composite Granulation: Prepare materials by weight: 100 parts PBS resin, 15 parts pre-degraded PLA obtained in step (3), 15 parts standard PLA with a weight average molecular weight of 150,000 Da, 50 parts hydrophobically modified MFC, 2 parts PBS-g-MAH with a maleic anhydride grafting rate of 2.0%, 1 part antioxidant 306, 6 parts glycerol, and 3 parts fungal spore microcapsules; First-stage extrusion: Put the hydrophobically modified MFC and 50 parts PBS into a co-rotating twin-screw extruder with a length-to-diameter ratio of 45:1. The temperature of zone 1 is 110℃, zone 2 is 115℃, zone 3 is 120℃, zone 4 is 120℃, and zone 5 is 125℃. The screw speed is 250 rpm. Extrusion is carried out. Granulation; Second-stage extrusion: The masterbatch obtained from the first-stage extrusion, the remaining 50 parts of PBS, pre-degradable PLA, standard PLA, PBS-g-MAH, antioxidant 306, and glycerol are fed into the extruder; Fungal spore microcapsules are injected through the side feed port in the Z6 zone of the melt plasticizing section, the melt temperature is controlled at 145℃, the residence time is 60s, and the mass ratio of the side feed port feeding speed to the main screw speed is 1:10; the temperatures of each zone are set as follows: Zone 1 130℃, Zone 2 135℃, Zone 3 140℃, Zone 4 145℃, Zone 5 140℃, melt pressure 8MPa, screw speed 150rpm, and extrusion granulation is used to obtain a fully biodegradable wheat straw cellulose composite material.

[0021] Example 4 A fully biodegradable composite material made from wheat straw cellulose is prepared through the following steps: Step (1) Preparation of hydrophobically modified MFC: Chop wheat straw into 1.5 cm lengths and add it to a 5 wt% sodium hydroxide solution (4 parts sodium hydroxide per 100 parts wheat straw). Stir at 75°C for 1.5 h. After draining the alkaline solution, wash with water until neutral. Immerse in a 3 wt% hydrogen peroxide solution (2.5 parts hydrogen peroxide per 100 parts wheat straw) and bleach at 75°C for 1 h. Wash and dry. Dissociate the fibers using a disc mill, adjust the disc gap to 0.15 mm, and circulate the mill. The mixture was milled three times to obtain micronized cellulose MFC with an aspect ratio of 18. Then, 100 parts of the micronized cellulose MFC were immersed in a mixed solution containing 3 parts citric acid and 25 parts glycerol, and reacted at 73°C for 2.5 h. The reaction system was then transferred to an ice-water bath at 2°C and cooled to 22°C within 10 min. 0.8 parts of molten beeswax and 0.2 parts of 15 nm nano-silica were added, and the mixture was dispersed at a high speed of 2000 rpm for 20 min. After filtration, the mixture was vacuum dried at 60°C for 12 h to obtain hydrophobically modified MFC. Step (2) PLA pre-degradation: Place polylactic acid PLA in a constant temperature and humidity chamber at 73℃ and 82% for 36 hours; Step (3) Preparation of fungal spore microcapsules: Adjust the concentration of Aspergillus niger spore suspension to 10. 8CFU / mL, add 3wt% sodium alginate solution to form core material solution; dissolve 85 parts PLA in dichloromethane to prepare 14.5wt% solution, add 14 parts 15nm nano-kaolin, and ultrasonically disperse at 300W power for 20min; mix core material solution and oil phase at a volume ratio of 1:2.9, and homogenize emulsify at 12000rpm for 10min to form W / O emulsion; inject the emulsion into 0.12mol / L calcium chloride solution, stir at 500rpm for 30min; filter and collect microcapsules, spray-coat with 0.45wt% stearic acid ethanol solution, dry and sieve 80μm particles; coat the surface of microcapsules with 1.9wt% chitosan acetate solution to form a pH-responsive layer, drain and cure at 60℃ for 1h; Step (4) Composite Granulation: Prepare materials by weight: 100 parts PBS resin, 8 parts pre-degraded PLA obtained in step (3), 8 parts standard PLA with a weight average molecular weight of 150,000 Da, 35 parts hydrophobically modified MFC, 0.8 parts PBS-g-MAH with a maleic anhydride grafting rate of 1.7%, 0.4 parts antioxidant 306, 2 parts glycerol, and 1.5 parts fungal spore microcapsules; First-stage extrusion: Put the hydrophobically modified MFC and 50 parts PBS into a co-rotating twin-screw extruder with a length-to-diameter ratio of 45:1. The temperature of zone 1 is 110℃, zone 2 is 115℃, zone 3 is 120℃, zone 4 is 120℃, and zone 5 is 125℃. The screw speed is 180 rpm. Granulation; Second-stage extrusion: The masterbatch obtained from the first-stage extrusion, the remaining 50 parts of PBS, pre-degradable PLA, standard PLA, PBS-g-MAH, antioxidant 306, and glycerol were fed into the extruder; fungal spore microcapsules were injected through the side feed port in the Z6 zone of the melt plasticizing section, the melt temperature was controlled at 138℃, the residence time was 52s, and the mass ratio of the side feed port feeding speed to the main screw speed was 1:10; the temperatures of each zone were set as follows: Zone 1 130℃, Zone 2 135℃, Zone 3 140℃, Zone 4 145℃, Zone 5 140℃, melt pressure 6.5MPa, screw speed 150rpm, and extrusion granulation was used to obtain a fully biodegradable wheat straw cellulose composite material.

[0022] Example 5 A fully biodegradable composite material made from wheat straw cellulose is prepared through the following steps: Step (1) Preparation of hydrophobically modified MFC: Chop wheat straw into 2.5 cm lengths and add it to a 5 wt% sodium hydroxide solution (7 parts sodium hydroxide per 100 parts wheat straw). Stir at 85°C for 2.5 h. After draining the alkaline solution, wash with water until neutral. Immerse in a 3 wt% hydrogen peroxide solution (4.5 parts hydrogen peroxide per 100 parts wheat straw) and bleach at 85°C for 1.8 h. Wash and dry. Dissociate the fibers using a disc mill, adjust the disc gap to 0.25 mm, and circulate the mill. The mixture was milled four times to obtain micronized cellulose MFC with an aspect ratio of 22. Then, 100 parts of the micronized cellulose MFC were immersed in a mixed solution containing 4 parts citric acid and 35 parts glycerol, and reacted at 77°C for 3.5 h. The reaction system was then transferred to an ice-water bath at 4°C and cooled to 28°C within 10 min. 1.8 parts of molten candelilla wax and 0.4 parts of 25 nm nano-silica were added, and the mixture was dispersed at a high speed of 2000 rpm for 20 min. After filtration, the mixture was vacuum dried at 60°C for 12 h to obtain hydrophobically modified MFC. Step (2) PLA pre-degradation: Place polylactic acid PLA in a constant temperature and humidity chamber at 77℃ and 88% for 60h; Step (3) Preparation of fungal spore microcapsules: Adjust the concentration of Aspergillus niger spore suspension to 10. 8 CFU / mL was added to an 8wt% sodium alginate solution to form a core material solution; 85 parts of PLA were dissolved in dichloromethane to prepare a 15.5wt% solution, and 16 parts of 25nm nano-kaolin were added. The solution was ultrasonically dispersed at 300W for 20min; the core material solution and oil phase were mixed at a volume ratio of 1:3.1 and homogenized at 12000rpm for 10min to form a W / O emulsion; the emulsion was injected into a 0.18mol / L calcium chloride solution and stirred at 500rpm for 30min; the microcapsules were collected by filtration, spray-coated with a 0.55wt% stearic acid ethanol solution, dried, and sieved to obtain 120μm particles; the surface of the microcapsules was coated with a pH-responsive layer of a 2.1wt% chitosan acetate solution, drained, and cured at 60℃ for 1h; Step (4) Composite Granulation: Prepare materials by weight: 100 parts PBS resin, 12 parts pre-degraded PLA obtained in step (3), 12 parts standard PLA with a weight average molecular weight of 150,000 Da, 45 parts hydrophobically modified MFC, 1.6 parts PBS-g-MAH with a maleic anhydride grafting rate of 1.9%, 0.8 parts antioxidant 306, 5 parts glycerol, and 2.5 parts fungal spore microcapsules; First-stage extrusion: Add hydrophobically modified MFC and 50 parts PBS to a co-rotating twin-screw extruder with a length-to-diameter ratio of 45:1. The temperatures in zones 1, 2, 3, 4, and 5 are 110℃, 115℃, 120℃, 120℃, and 125℃, and the screw speed is 230 rpm. Granulation; Second-stage extrusion: The masterbatch obtained from the first-stage extrusion, the remaining 50 parts of PBS, pre-degradable PLA, standard PLA, PBS-g-MAH, antioxidant 306, and glycerol are fed into the extruder; fungal spore microcapsules are injected through the side feed port in the Z6 zone of the melt plasticizing section, the melt temperature is controlled at 142℃, the residence time is 58s, and the mass ratio of the side feed port feeding speed to the main screw speed is 1:10; the temperatures of each zone are set as follows: Zone 1 130℃, Zone 2 135℃, Zone 3 140℃, Zone 4 145℃, Zone 5 140℃, melt pressure 7.5MPa, screw speed 150rpm, and extrusion granulation is used to obtain a fully biodegradable wheat straw cellulose composite material.

[0023] Comparative Example 1 The difference from Example 1 is that micronized cellulose MFC was added directly without any subsequent modification or other operations.

[0024] Comparative Example 2 The difference from Example 1 is that no molten beeswax or an equal amount of rice bran wax or candelilla wax was added.

[0025] Comparative Example 3 The difference from Example 1 is that 100 parts of micronized cellulose MFC were immersed in a mixed solution containing 10 parts of citric acid and 40 parts of glycerol.

[0026] Comparative Example 4 The difference from Example 1 is that no fungal spore microcapsules were added.

[0027] Comparative Example 5 The difference from Example 1 is that the microcapsules were not spray-coated with stearic acid ethanol solution.

[0028] Comparative Example 6 The difference from Example 1 is that the component ratio in step (4) is as follows: Step (4) Composite granulation: Prepare materials by mass: 100 parts PBS resin, 20 parts pre-degraded PLA obtained in step (3), 40 parts hydrophobic modified MFC, 1.5 parts PBS-g-MAH with maleic anhydride grafting rate of 1.8%, 0.8 parts antioxidant 306, 4 parts glycerol, and 2 parts fungal spore microcapsules.

[0029] Comparative Example 7 The difference from Example 1 is that the component ratio in step (4) is as follows: Step (4) Composite granulation: Prepare materials by mass: 100 parts PBS resin, 10 parts pre-degraded PLA obtained in step (3), 20 parts standard PLA with a weight average molecular weight of 150,000 Da, 40 parts hydrophobically modified MFC, 1.5 parts PBS-g-MAH with a maleic anhydride grafting rate of 1.8%, 0.8 parts antioxidant 306, 4 parts glycerol, and 2 parts fungal spore microcapsules.

[0030] Comparative Example 8 The difference from Example 1 is that 60 parts of hydrophobic modified MFC are added to the component ratio in step (4).

[0031] Comparative Example 9 The difference from Example 1 is that the Aspergillus niger spores were not coated and were added directly.

[0032] Comparative Example 10 The difference from Example 1 is that fungal spore microcapsules are injected through the side feed port, and the melt temperature is controlled at 155°C.

[0033] Comparative Example 11 The difference from Example 1 is that in step (4) composite granulation: by mass parts, 100 parts of PBS resin, 5-15 parts of pre-degraded PLA obtained in step (3), 5-15 parts of standard PLA with a weight average molecular weight of 150,000 Da, 30-50 parts of hydrophobic modified MFC, 0.5-2 parts of PBS-g-MAH with a maleic anhydride grafting rate of 1.8±0.2%, 0.2-1 parts of antioxidant 306, 1-6 parts of glycerol, and 1-3 parts of fungal spore microcapsules are put into a co-rotating twin-screw extruder with a length-to-diameter ratio of 45:1. The temperature of zone 1 is 110℃, zone 2 is 115℃, zone 3 is 120℃, zone 4 is 120℃, and zone 5 is 125℃. The screw speed is 200±50 rpm. The extrusion granulation is carried out to obtain a fully biodegradable wheat straw cellulose composite material.

[0034] Performance testing: 1. According to the national standard GB / T1040.3-2006 Determination of tensile properties of plastics - Part 3: Test conditions for films and sheets; 2. According to GB / T1843-2008 "Determination of Impact Properties of Simply Supported Beams in Plastics"; 3. According to GB / T9341-2008 "Determination of Flexural Properties of Plastics"; 4. According to GB / T19277.1-2011 Determination of final aerobic biodegradability of materials under controlled composting conditions - Method for determining carbon dioxide released - Part 1: General method; 5. Refer to GB / T39086-2020 "Determination of final aerobic biodegradation capacity in plastic soil by measuring oxygen consumption or carbon dioxide production in a closed respiration meter"; 6. Enzyme activity detection: Take 5g of material and place it in a buffer system with pH 5.8±0.2 (such as citrate-disodium hydrogen phosphate), keep it at constant humidity (soil moisture content 30-40%), add 0.1% yeast extract to provide basic nutrition, and avoid fungal inactivation due to insufficient nutrition. Regularly detect the cellulase and lipase activities secreted by Aspergillus niger in the surrounding environment (such as cellulase activity measured by 3,5-dinitrosalicylic acid method) to assess whether the spores can effectively initiate degradation after release.

[0035] The test results are shown in Table 1.

[0036] Table 1. Test results of the examples and comparative examples. Serial Number Tensile strength (MPa) Elongation at break (%) Impact strength of a simply supported beam (kJ / m²) Bending strength (MPa) 60-day compost degradation rate (%) 90-day soil degradation rate (%) Cellulase activity (U / g) after 60 days Lipase activity (U / g) after 60 days Example 1 32.5 185 7.2 38.2 75.3 62.5 22.8 16.5 Example 2 29.8 170 6.8 35.5 72.1 59.8 20.5 15.2 Example 3 31.2 190 7.5 37.8 76.5 63.2 23.5 17 Example 4 30.5 178 7 36.8 73.6 60.5 21.2 15.8 Example 5 33 195 7.8 39 77.2 64 24 17.5 Comparative Example 1 18.2 95 4 22.5 58.6 45.2 12.5 9 Comparative Example 2 20.5 110 4.5 25 60.2 47.8 13.2 9.5 Comparative Example 3 22 120 5 26.8 62.5 50.1 14 10.2 Comparative Example 4 31.8 180 7 37.5 35.2 28.6 3.5 2 Comparative Example 5 25 140 5.5 30.2 55.8 48 16.5 12 Comparative Example 6 23.2 130 5.2 27.5 68 55.5 18 13.5 Comparative Example 7 28.5 160 6.5 34 65.2 52.8 17.2 12.8 Comparative Example 8 21 115 4.8 25.5 61 49.2 13.8 10 Comparative Example 9 32 182 7.1 38 40.5 32 5 3.5 Comparative Example 10 19.5 105 4.2 24 38.8 30.5 4.2 2.8 Comparative Example 11 17 90 3.8 21 56.5 46 12 8.5 The performance characteristics of the embodiments are reflected in the synergistic effect of each core component and process parameter within the optimized range, which jointly contributes to the excellent balance between the mechanical properties and biodegradability of the material. The preparation of hydrophobically modified MFC is the key foundation: wheat straw is treated with alkali to remove impurities, bleached and purified, and then milled in a disc mill to obtain micron-sized cellulose with an aspect ratio of 15-25. Then, ester groups are introduced by citric acid esterification, a hydrophobic layer is formed by wax coating, and nano-SiO2 is filled and reinforced. This not only improves the compatibility of cellulose with the hydrophobic matrix of PBS / PLA, but also retains the rigidity reinforcement of the fiber, resulting in a tensile strength of 29.8-33 MPa and a flexural strength of 35.5-39 MPa, which are significantly higher than the unmodified system. The pre-degradation of PLA regulates the molecular weight to optimize the processing flowability. In synergy with standard PLA, it avoids the strength loss caused by excessive degradation and improves the toughness of the matrix through compatibility with PBS, so that the elongation at break is maintained at 170-195% and the simply supported beam impact strength is 6.8-7.8 kJ / m². The pH-responsive design of the fungal spore microcapsules ensures stability during use. In composting or soil environments, the chitosan layer decomposes to release Aspergillus niger spores, whose secreted cellulase and lipase accelerate the degradation of cellulose and the matrix. The degradation rate in composting is 72.1-77.2% after 60 days, and the degradation rate in soil is 59.8-64% after 90 days, demonstrating the controllability of waste degradation under natural conditions. The staged extrusion process further ensures performance: the first stage, low-temperature preparation of MFC-PBS masterbatch reduces fiber aggregation; the second stage, side-feeding injection of microcapsules avoids high-temperature damage to spore activity. Combined with the interfacial compatibilization of PBS-g-MAH and the plasticizing effect of glycerol, the various embodiments ultimately achieve a highly efficient synergy between mechanical enhancement and biodegradation, exhibiting a pattern of stable and excellent performance as the core parameters are synergistically optimized within the preferred range.

[0037] Comparative Example 1, lacking hydrophobic modification of the micronized cellulose MFC, resulted in a significant decrease in mechanical properties such as tensile strength and elongation at break due to the strong hydrophilicity and poor compatibility with the hydrophobic matrix. The activities of cellulase and lipase, related to degradation, were also significantly reduced, leading to overall performance far inferior to Example 1. Comparative Example 2, lacking wax coating and with insufficient hydrophobic modification, still exhibited inadequate compatibility between the MFC and the matrix. While its mechanical properties and degradation efficiency were better than Comparative Example 1, they were still lower than Example 1, indicating that wax is crucial for improving hydrophobicity and compatibility. Comparative Example 3, due to excessive citric acid content and over-esterification that damaged the structural integrity of the MFC, had limited improvement in compatibility, resulting in mechanical and degradation performance inferior to Example 1. Comparative Example 4, without fungal spore microcapsules, showed mechanical properties close to Example 1, but lacked a degradation triggering mechanism, achieving a 60-day compost degradation rate of only 35.2% and almost zero enzyme activity, confirming the decisive role of microcapsules in biodegradation. Comparative Example 5, with microcapsules not coated with stearic acid ethanol, suffered from insufficient microcapsule stability, potentially leading to premature spore release. The structure was damaged, resulting in decreased mechanical properties and a lower degradation rate than in Example 1. In Comparative Example 6, excessive pre-degraded PLA and no standard PLA resulted in a decrease in matrix strength due to excessive low molecular weight components. Although the degradation rate was slightly higher, the mechanical properties were significantly damaged. In Comparative Example 7, excessive standard PLA resulted in better mechanical properties than Comparative Example 6, but the degradation rate was lower than in Example 1 because standard PLA degrades more slowly. In Comparative Example 8, excessive hydrophobic modified MFC caused fiber agglomeration and uneven dispersion, resulting in decreased mechanical properties and reduced degradation efficiency. In Comparative Example 9, Aspergillus niger spores were added directly without coating. The spores were inactivated or released prematurely during processing, making it impossible to effectively initiate degradation after disposal. The degradation rate and enzyme activity were far lower than in Example 1. In Comparative Example 10, the melt temperature was too high during microcapsule injection. The high temperature destroyed spore activity and affected the matrix structure, resulting in a significant decrease in both mechanical properties and degradation performance. In Comparative Example 11, no staged extrusion was used. The fiber agglomeration was severe and the microcapsules were inactivated by long-term high-temperature treatment. The mechanical properties and degradation performance were the worst, highlighting the importance of staged extrusion for component dispersion and spore protection.

Claims

1. A fully biodegradable composite material made from wheat straw cellulose, characterized in that, It is prepared through the following steps: Step (1) Preparation of hydrophobically modified MFC: Chop wheat straw into 1-3 cm lengths and put it into a 5 wt% sodium hydroxide solution. Use 3-8 parts of sodium hydroxide per 100 parts of wheat straw. Stir at 70-90℃ for 1-3 h. After draining the alkaline solution, wash with water until neutral. Immerse in a 3 wt% hydrogen peroxide solution. Use 2-5 parts of hydrogen peroxide per 100 parts of wheat straw. Bleach at 70-90℃ for 0.5-2 h. Wash and dry. Dissociate the fibers using a disc mill to obtain micronized cellulose MFC. Subsequently, 100 parts of micronized cellulose MFC were immersed in a mixed solution containing 2-5 parts of citric acid and 20-40 parts of glycerol, and reacted at 75±5℃ for 2-4 h; the reaction system was transferred to an ice-water bath at 0-5℃ and cooled to 25±5℃ within 10 min; 0.5-2 parts of biowax and 0.1-0.5 parts of nano silica were added, dispersed at high speed, filtered, and dried to obtain hydrophobically modified MFC; Step (2) PLA pre-degradation: Place PLA in a constant temperature and humidity chamber at 75±5℃ and 85±5% for 24-72 hours; Step (3) Preparation of fungal spore microcapsules: Adjust the concentration of Aspergillus niger spore suspension to 10. 8 CFU / mL, add 1-10wt% sodium alginate solution to form core material solution; dissolve 85 parts PLA in dichloromethane to prepare 14-16 wt% solution, add 12-18 parts nano-kaolin with a particle size of 10-30 nm, and disperse by ultrasonication; The core material solution and oil phase were mixed at a volume ratio of 1:2.8-3.2 and homogenized to form a W / O emulsion. The emulsion was injected into a 0.1-0.2 mol / L calcium chloride solution to form microcapsules. The microcapsules were collected by filtration and spray-coated with a 0.4-0.6 wt% stearic acid ethanol solution. After drying, the microcapsules were sieved and then coated with a pH-responsive layer with a 1.8-2.2 wt% chitosan acetate solution. The mixture was then solidified to obtain fungal spore microcapsules. Step (4) Composite granulation: Prepare materials by weight: 100 parts PBS resin, 5-15 parts pre-degraded PLA obtained in step (3), 5-15 parts standard PLA, 30-50 parts hydrophobically modified MFC, 0.5-2 parts PBS-g-MAH, 0.2-1 parts antioxidant 306, 1-6 parts glycerol, and 1-3 parts fungal spore microcapsules; First-stage extrusion: Hydrophobically modified MFC and 50 parts of PBS were extruded and granulated; Second-stage extrusion: The masterbatch obtained from the first-stage extrusion, the remaining 50 parts of PBS, pre-degradable PLA, standard PLA, PBS-g-MAH, antioxidant 306, and glycerol are fed into the extruder; fungal spore microcapsules are injected through the side feed port in the Z6 zone of the melt plasticizing section, and extrusion granulation is performed to obtain a fully biodegradable wheat straw cellulose composite material.

2. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, The biowax mentioned in step (1) is one of beeswax, rice bran wax or candelilla wax.

3. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, The nano-silica has a particle size of 10-30 nm; the high-speed dispersion speed is 2000 rpm, the dispersion time is 20 min; the drying temperature is 60℃, under vacuum conditions, and the drying time is 12 h.

4. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, The ultrasonic dispersion process described in step (3) is as follows: ultrasonic dispersion at 300 W power for 20 min.

5. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, The sodium alginate solution in step (3) has a mass concentration of 1-5 wt%.

6. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, The particle size range obtained by sieving after drying in step (3) is 50-150 μm.

7. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, The standard PLA in step (4) has a weight-average molecular weight of 150,000 Da; the maleic anhydride grafting rate of the PBS-g-MAH is 1.8 ± 0.2%.

8. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, First-stage extrusion: Hydrophobic modified MFC and 50 parts of PBS were fed into a co-rotating twin-screw extruder with an aspect ratio of 45:

1. The temperatures in zones 1, 2, 3, 4 and 5 were 110℃, 115℃, 120℃, and 125℃, and the screw speed was 200±50 rpm.

9. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, In step (4), the second stage of extrusion is as follows: the mass ratio of the side feed port feeding speed to the main screw speed is 1:10; the temperature of each zone is set as follows: zone 1 130℃, zone 2 135℃, zone 3 140℃, zone 4 145℃, zone 5 140℃, melt pressure ≤8 MPa, and screw speed 150 rpm.

10. The fully biodegradable wheat straw cellulose composite material according to claim 1, characterized in that, When injecting fungal spore microcapsules through the side feed port in the Z6 zone of the melting and plasticizing section, the melt temperature is controlled at 140±5℃ and the residence time is ≤60s.