A hot rolling leveling process for high-strength steel
By controlling the tapping temperature, electromagnetic induction heating, segmented cooling, and high-frequency ultrasonic oscillation, the problem of insufficient steel strength caused by the internal and external temperature difference during hot rolling was solved, achieving high strength, high toughness, and high elongation steel properties, and ensuring the quality stability of the steel plate.
Patent Information
- Application Number
- CN202511350765.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-22
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-09-22
AI Technical Summary
During hot rolling, the temperature difference between the surface and the interior causes a "hard core steel", which leads to inconsistent stretching speeds during rolling cracking and leveling. In particular, titanium alloys are prone to cracking and insufficient steel strength.
By controlling the tapping temperature, electromagnetic induction heating, intermediate billet dwell time, finishing rolling temperature, segmented cooling, and high-frequency ultrasonic oscillation, combined with specific chemical composition and heating power, uniform cooling and phase transformation control of steel are achieved, avoiding the generation of brittle phases and forming fine bainite lath bundles.
It achieves comprehensive performance of high strength, high toughness and high elongation, reduces performance fluctuations caused by traditional cooling, ensures the quality stability of steel plates, and avoids the generation of cracks and brittle phases.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal rolling technology, and more particularly to a hot rolling leveling process for high-strength steel. Background Technology
[0002] High-strength hot-rolled steel is a type of high-strength steel produced through a hot-rolling process. Hot rolling involves rolling a steel billet at high temperatures to impart high strength. This type of steel can withstand greater pressure and tension while maintaining good plasticity and weldability.
[0003] The development history of high-strength hot-rolled steel can be traced back to the ever-increasing demand for improved steel strength and performance. With industrial development, traditional steel can no longer meet the material performance requirements of some high-end fields. Therefore, the research and development of high-strength hot-rolled steel with higher strength and better overall performance has become an inevitable trend.
[0004] However, during the hot rolling process, due to the difference between surface and internal temperatures, the surface temperature quickly reaches the target value, but the center forms a "hard core steel" (high surface temperature, low center temperature) due to the lag in heat conduction. The temperature difference between the inside and outside can reach up to 50°C. This eventually leads to cracks caused by uneven stretching speed during rolling and leveling, resulting in insufficient steel strength. This is especially true for titanium alloys, which are more prone to cracking due to the poor thermal conductivity of titanium. Summary of the Invention
[0005] This application provides a hot rolling and leveling process for high-strength steel, which solves the problem of inconsistent internal and external temperatures in the prior art, thereby reducing cracks and increasing rigidity and strength.
[0006] This application provides a hot rolling leveling process for high-strength steel, including the following steps: S1. Control the tapping temperature to 1260-1300℃; S2. Control the dwell time of the intermediate billet in the hot rolling box to be 12-25 seconds, and perform edge electromagnetic induction heating; S3. Control the temperature entering the finishing mill to be 1060-1100℃ and the temperature exiting the finishing mill to be 870-890℃; S4. The hot-rolled strip is cooled in stages, including: first, the strip is rapidly cooled from the finishing rolling temperature to 550-560°C at a cooling rate of 60°C per second; then, the surface temperature of the strip is warmed back to 580°C by radiant heating tubes at a heating rate of 15°C per second; relax on the roller table for 8 seconds; and finally, the strip is cooled to -550°C at a cooling rate of 30°C per second before being coiled.
[0007] Furthermore, the finishing rolling step also includes applying high-frequency ultrasonic oscillation to the strip at a frequency of 20 kHz, an amplitude of 10 μm, an action time of 6 seconds, and an energy density of 50 joules per cubic centimeter.
[0008] Furthermore, the chemical composition of high-strength steel, by mass percentage, includes: C: 0.18-0.24%, Mn: 1.9-2.4%, S: ≤0.004%, P: ≤0.02%, Si: 1.4-2.0%, Als: 0.04-0.06%, N: <0.006%, Nb: 0.02-0.05%, Ti: 0.045-0.06%, B: 0.001-0.002%; the remainder is Fe or impurities.
[0009] Furthermore, the electromagnetic induction heating power in the hot roll box is 300-350KW / m.
[0010] Furthermore, the warming process includes holding the temperature at 580°C for 2 seconds before allowing it to cool naturally.
[0011] Furthermore, the process includes dry leveling of the obtained hot-rolled steel coils, with elongation controlled at 0.8%-1.2%, inlet tension at 250 MPa, outlet tension at 280 MPa, rolling speed at 300-500 m / min, and surface roughness controlled at 2.0-2.5 μm.
[0012] One or more technical solutions provided in the embodiments of this application have at least the following technical effects or advantages: This process avoids the formation of brittle phases (excessive martensite) and soft phases (ferrite), ultimately achieving a combination of high strength, high toughness, and high elongation. Rapid cooling and precise phase transformation control suppress grain growth, resulting in fine bainite lath bundles, further enhancing strength and toughness. The entire process is precisely controllable, reducing performance fluctuations caused by water temperature and speed variations in traditional cooling methods, thus ensuring the stability of steel plate performance and quality. Detailed Implementation
[0013] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to limit the invention; the term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0014] Example 1: A high-strength steel product with a thickness of 2.5 mm and a width of 1550 mm has the following chemical composition: C: 0.18-0.24%, Mn: 1.9-2.4%, S: ≤0.004%, P: ≤0.02%, Si: 1.4-2.0%, Als: 0.04-0.06%, N: <0.006%, Nb: 0.02-0.05%, Ti: 0.045-0.06%, B: 0.001-0.002%; the remainder is Fe or impurities.
[0015] B is added using an Fe-B alloy scheme, with a B content of 20% and a particle size of 13mm. Before the end of LF refining of molten steel, aluminum wire is added for pre-deoxidation (aluminum addition amount 0.015-0.025%) to make [O] ≤20ppm. Then, after heating to 1620℃, Fe-B is fed in at a wire feeding speed of 100m / min. Argon gas is soft-blown for 15min at a flow rate of 100NL / min. The superheat of continuous casting is controlled at 15℃, and the cooling rate is ≤10℃ / min.
[0016] Its hot rolling leveling process includes: tapping temperature control, hot coil box relaxation, finishing rolling temperature control, and segmented cooling relaxation. The specific steps are as follows: S1. Steel tapping temperature control: The target steel tapping temperature is controlled at 1280-1300℃; S2. Hot roll box relaxation: Control the dwell time of the intermediate billet in the hot roll box to 12-25s, and use electromagnetic induction heating at the edge (300kW / m). S3. Finishing mill temperature control: Control the temperature entering the finishing mill to be 1060-1080℃ and the temperature exiting the finishing mill to be 870℃; S5. Segmented Cooling and Relaxation: After the hot-rolled strip exits the finishing mill, a segmented cooling mode is adopted. First, it is put into an ultra-fast cooling device with a cooling rate of 60℃ / s to rapidly reduce the strip temperature from 870℃ to 550℃. Then, the surface is heated back to 580℃ through a gas radiant tube (heating rate of 15℃ / s). After relaxing on the roller table for 8 seconds, it is put into traditional laminar flow cooling with a cooling rate of 30℃ / s to reduce the strip temperature to 550℃ before coiling.
[0017] The technical solutions described in the embodiments of this application above have at least the following technical effects or advantages: The most crucial and primary role of boron in steel is to significantly improve its hardenability. Due to the small atomic size of boron, it preferentially segregates on austenite grain boundaries during the cooling process of austenite. Grain boundaries are the most preferred sites for ferrite nucleation, and the segregation of boron effectively "occupies" these nucleation sites, reducing the grain boundary energy. This greatly delays the transformation of austenite into proeutectoid ferrite and pearlite. By suppressing high-temperature transformation, supercooled austenite can remain at a lower temperature (around 550℃) before undergoing phase transformation, thereby promoting the formation of intermediate-temperature transformation products (bainite) and even low-temperature transformation products (martensite), resulting in a steel with a high-strength and high-toughness microstructure. The high Ti content results in a much stronger affinity between Ti and N than between B and N. Ti preferentially combines with N to form stable TiN particles, thus fixing the free nitrogen in the steel and preventing it from reacting with B. Al is added at the end of LF refining for pre-deoxidation, aiming to reduce [O] in the molten steel to below 20 ppm. Al has a very strong affinity for O, forming Al2O3, which fixes the free oxygen in the steel and prevents it from reacting with B. Al is added after sufficient deoxidation ([O] ≤ 20 ppm) and heating, ensuring that oxygen and nitrogen are fixed to the maximum extent, and the molten pool environment is stable for B.
[0018] The extremely high cooling rate bypasses the temperature range of austenite-ferrite and pearlite transformation (typically around 700-500℃); due to the significantly improved hardenability of boron, this cooling rate is sufficient to maintain the supercooled austenite up to 550℃ with almost no phase transformation; the high cooling rate is only effective on the surface, while ferrite will still form in the core due to insufficient cooling rate, the presence of boron ensures that this goal is achieved throughout the entire cross-section; highly supercooled, metastable, homogeneous austenite is obtained, preparing for subsequent phase transformation and avoiding the formation of any soft phase structures such as proeutectoid ferrite and pearlite; after rapid cooling to 550℃, the steel plate temperature is relatively low, and if isothermally cooled directly at this temperature, a large amount of martensitic oxidation will begin to form. Martensite, while possessing extremely high strength, exhibits relatively poor toughness. Rapidly reheating to 580℃ introduces the microstructure into the bainitic transformation region, ensuring the phase transformation occurs at the optimal temperature (around 580℃) within the bainitic zone. This reheating process acts as a "relaxation," homogenizing the temperature and providing sufficient chemical driving force for the bainitic shear transformation. A brief isothermal treatment at 580℃ is crucial for bainite nucleation and the initiation of growth. Allowing a certain amount of bainite to form at this temperature results in a more uniform bainitic microstructure. After relaxation, the phase transformation has begun, and subsequent laminar cooling (30℃ / s) continues to cool the steel plate to the coiling temperature of 550℃, further completing the bainitic phase transformation. During and after the phase transformation, the carbonitrides of Nb and Ti exhibit fine and dispersed precipitation, resulting in precipitation strengthening. B, on the other hand, ensures that the phase transformation can continue to the end, generating high-strength bainite, ultimately yielding a multiphase microstructure dominated by fine lath bainite, containing a small amount of martensite and fine carbide precipitation. The interaction between B and Ti was also investigated to verify their impact on the properties of titanium alloys. The titanium alloy (6% Al, 4% V, the remainder Ti or impurities) was doped with 0.005% B, with O ≤ 0.15%, N ≤ 0.03%, and H ≤ 0.005%. The tapping temperature was 1020℃, the finishing mill inlet temperature was 960℃, the holding time was 15s, and after finishing milling, it was cooled to 750℃ at 45℃ / s, then reheated to 820℃, held for 8s, and then cooled to 580℃ at 25℃. Compared to the titanium alloy without 0.005% B, YS increased by 3.4%, UTS increased by 2.8%, E1 decreased by 6.7%, and KV2 increased by 12.7%.
[0019] Bainitic microstructure inherently possesses high strength and high toughness. This process avoids the formation of brittle phases (excessive martensite) and soft phases (ferrite), ultimately resulting in a comprehensive performance of high strength, high toughness, and high elongation. Rapid cooling and precise phase transformation control suppress grain growth, resulting in fine bainitic lath bundles, further enhancing strength and toughness. The entire process is precisely controllable, reducing performance fluctuations caused by traditional cooling and ensuring the stability of steel plate performance and quality.
[0020] Experimental verification was conducted, and the experimental groups are shown in Table 1. Table 1 Experimental Grouping in Example 1
[0021] The tensile strength (UTS), yield strength (YS), and elongation (EI) of high-strength steel were tested according to GB / T228-2002. The impact energy (KV2) was tested according to GB / T 229-2020. The test results are shown in Table 2. Table 2 Detection Results of Example 1
[0022] Example 2: The above example skips the temperature range of austenite to ferrite and pearlite transformation by segmented cooling relaxation, and finally obtains a multiphase structure with fine lath bainite as the main component and a small amount of martensite and fine carbide precipitation. However, the temperature control requirements are high. If the ambient temperature is low, the radiant tube has a low reheating efficiency and a short holding time at 580°C. This can easily cause undiffuse boron to accumulate at the grain boundaries and form FeB flakes, resulting in the steel coil breaking into ceramic-like pieces when uncoiling. Therefore, further improvements are made based on Example 1.
[0023] S1. Steel tapping temperature control: The target steel tapping temperature is controlled at 1260-1280℃; S2. Hot roll box relaxation: Control the dwell time of the intermediate billet in the hot roll box to 15-20s, and use electromagnetic induction heating at the edges (350kW / m). S3. Finishing Rolling Temperature Control: The temperature entering the finishing rolling mill is controlled at 1080-1100℃, and the temperature exiting the finishing rolling mill is controlled at 890℃. High-frequency ultrasonic vibration is performed at a frequency of 20kHz, an amplitude of 10μm, a duration of 6s, and an energy density of 50J / cm³. 3 ; S4. Segmented Cooling and Relaxation: After the hot-rolled strip exits the finishing mill, a segmented cooling mode is adopted. First, it is put into an ultra-fast cooling device with a cooling rate of 60℃ / s to rapidly reduce the strip temperature from 870℃ to 560℃. Then, the surface is heated back to 580℃ through a gas radiant tube (heating rate of 15℃ / s). After holding for 2 seconds, it is naturally cooled to 580℃. Then, it relaxes on the roller table for 8 seconds and is then put into traditional laminar flow cooling with a cooling rate of 30℃ / s to reduce the strip temperature to 550℃ before coiling.
[0024] The technical solutions described in the embodiments of this application above have at least the following technical effects or advantages: At 550℃, although boron atoms possess mobility, their kinetic energy remains low. Especially when they agglomerate at grain boundaries to form clusters, they need to overcome a higher energy barrier to redissolve back into the lattice. This instantaneously raises the temperature to 590℃, greatly increasing the thermal vibrational energy of all atoms. This makes it easier for boron atoms to overcome the "friction" caused by surrounding iron (Fe) atoms and the "adsorption" effect at grain boundaries. This allows them to detach from the low-energy state at the grain boundaries and re-dissolve into the austenite grains, breaking the initial agglomeration of boron atoms (the rudimentary form of Fe-B clusters) and making their distribution more uniform. After the "redistribution" of boron atoms is completed, the phase transformation stage begins. Bainitic phase transformation requires a certain degree of supercooling to occur, and 580℃ is the optimal temperature window for bainitic transformation in this steel grade. Slowly cooling from 590℃ to 580℃ increases the system's chemical driving force (free energy difference ΔG). Lowering the temperature means increased supercooling, leading to a larger free energy difference between austenite and bainite, providing a stronger impetus for bainite nucleation. Simultaneously, the slow cooling avoids thermal stress caused by sudden temperature drops, making the phase transformation process more stable. At the high temperature of 590℃, the phase transformation driving force is actually reduced (due to the small supercooling), resulting in a very low bainite nucleation rate. Within these 2 seconds, thermal energy is almost entirely used to increase atomic kinetic energy and promote boron diffusion, rather than undergoing a violent phase transformation simultaneously. This prevents the phase transformation from starting while boron is still highly segregated, thus fundamentally preventing the formation of the brittle FeB phase at grain boundaries. When the temperature drops to 580℃, the distribution of boron (B) is significantly improved. At this point, the strong chemical driving force (ΔG) mainly acts to promote the shear growth of bainite. Since B is homogenized, it can more effectively play its positive role of "occupying grain boundaries and suppressing ferrite" without having a negative effect due to excessive local concentration. At low temperatures, the segregated B atoms are not isolated; they have begun to form short-range ordered clusters with Fe atoms. These are precursors of brittle intermetallic compounds such as FeB or Fe2B. They are small in size but stable. The high temperature of 590℃ and the additional energy input are sufficient to break the bonds of these weakly stable clusters. The bonds between Fe and B become unstable under higher thermal perturbations, causing these precursor clusters to disintegrate. The B atoms are "released" and reintegrated into the austenite matrix, reducing the brittle phase.
[0025] Bainitic transformation is a diffusion-shear hybrid transformation. Its nucleation preferentially occurs at defects such as grain boundaries. After the "purification" of high temperature step, harmful B clusters at the grain boundaries are removed, but the presence of B atoms still lowers the grain boundary energy. At this point, the grain boundary is no longer a nucleation site for brittle phases, but transforms into a clean and effective site suitable for bainite nucleation. The uniformly distributed B atoms continue to play a role in inhibiting the nucleation of polygonal ferrite at the grain boundaries, thereby driving the phase transformation to a path more conducive to bainite formation. During the isothermal process at 580℃, bainite lath bundles can uniformly nucleate and grow from the pure grain boundaries. Fine carbides (such as carbonitrides of Nb and Ti) will also precipitate during or after the phase transformation, playing a precipitation strengthening role. High-temperature step-gradient purification cleans the austenite grain boundaries and removes the precursors of brittle phases. The subsequent phase transformation at the optimal temperature allows bainite to nucleate healthily on the pure grain boundaries, while microalloyed carbonitrides can also precipitate uniformly and dispersedly within the grains. The synergistic effect of these two factors results in a toughened microstructure with a fine, uniform lath bainite matrix, clean grain boundaries, and fine dispersed strengthening phases, avoiding the weak grain boundary phase (FeB) and thus solving the problem of uncoiling and breakage. At the finishing rolling temperature of 1080-1100℃, the carbonitrides of Nb and Ti are not completely dissolved, and they pin the grain boundaries with fine particles, strongly inhibiting austenite recrystallization. Rolling with a reduction rate of >65% introduces high-density deformation bands, dislocation entanglements, and shear bands into the non-recrystallized austenite. These defects greatly increase the total grain boundary area, providing a large number of nucleation sites for subsequent phase transformations, which is a prerequisite for achieving ultrafine grains. Acousto-plastic effect (dislocation modulation): High-frequency vibration stress of 20kHz is transmitted into the strip in the form of waves, interacting with the dense dislocation network. This alternating stress effectively promotes dislocation slip, multiplication, and annihilation, reducing the friction of dislocation movement. Its effect is equivalent to an "in-situ energy introduction" to the rolled microstructure, providing additional driving force for dynamic recovery and subsequent phase deformation nucleation; the cavitation effect of ultrasound in the molten metal is transformed into a local energy burst at the solid metal defect. The instantaneous high pressure, high temperature, and shock wave generated by the collapse of cavitation bubbles provide huge energy fluctuations at the nucleation points (dislocations, vacancies) of Nb / Ti carbonitride precipitation, significantly reducing the precipitation nucleation barrier, accelerating precipitation kinetics, and thus achieving a 30% increase in precipitated phase density; The equilibrium segregation of boron atoms towards the grain boundary is a diffusion process driven by concentration gradient and energy difference. The high-frequency stress field and numerous instantaneous point defects generated by ultrasonic vibration disrupt the directional diffusion path of boron atoms. Boron atoms are forced to engage in non-equilibrium exchange with vacancies, or their diffusion paths are continuously interrupted by mechanical vibration, effectively delaying the dynamic process of their arrival and stable residence at the grain boundary; this buys time for subsequent rapid cooling, "freezing" the boron atoms within the austenite grain before segregation. The energy and disturbance provided by the ultrasonic field, together with the energy stored in deformation, greatly improve the nucleation rate of bainite. Bainite laths not only nucleate at the original austenite grain boundaries, but also on countless deformation bands and dislocation cells, ultimately refining the lath bundle size to 0.2 μm. High-density nanoscale Nb / Ti carbonitride precipitates are dispersed on a uniform and fine bainitic matrix; the ultrasonic field suppresses the segregation of B and avoids the brittle FeB phase, allowing the high toughness of lath bainite to be fully utilized; fine grain strengthening and precipitation strengthening greatly improve yield strength; ultrafine grain structure and high-cleanliness grain boundaries together ensure high impact energy.
[0026] The same test was conducted as in Example 1, with the following composition: C: 0.2%, Mn: 2.2%, Si: 1.6%, Als: 0.05%, Nb: 0.03%, Ti: 0.05%, B: 0.001%; the remainder being Fe or impurities. The experimental groups are shown in Table 3; the test results are shown in Table 4. Table 3 Experimental Grouping in Example 2
[0027] Table 4 Experimental Results of Example 2
[0028] Example 3: This example provides a leveling process to complement the above-mentioned hot rolling process for high-strength steel; The leveling process is dry leveling, using a six-roll leveling machine, with an elongation of 0.8%-1.2%, an inlet tension of 250 MPa, and an outlet tension of 280 MPa; the surface roughness is controlled to be Ra2.0 - 2.5μm; the rolling speed is 300-500 m / min.
[0029] The technical solutions described in the embodiments of this application above have at least the following technical effects or advantages: Ultra-high strength bainitic steel exhibits a significant physical yield phenomenon. Its stress-strain curve initially contains an upper and lower yield point, followed by a yield elongation zone. The leveling mill applies a small plastic elongation of 0.8%-1.2%, causing the strip to undergo a "pre-deformation" between the rolls. This deformation exceeds the material's yield elongation. This process causes a large number of dislocations in the grains to multiply and break free from the pinning of the Cottrell atmosphere, becoming movable dislocations. When the strip is subsequently subjected to stress again, these pre-existing movable dislocations can immediately initiate slip, thus eliminating the upper and lower yield points and transforming the stress-strain curve into a smooth, continuous curve. This fundamentally prevents the formation of Lüders bands. The high tension (250-280 MPa) combined with the rolling force produces continuous tensile and bending deformation on the strip. Under tension, the strip is straightened, and simultaneously, the bending of the rolls corrects shape defects (such as wavy edges and center wavy areas). By applying different reduction amounts (larger reduction at wavy areas and smaller reduction at flat areas), corresponding plastic deformation is generated, thereby correcting microscopic plate shape defects and obtaining excellent flatness. The purpose of a small elongation is to generate only enough movable dislocations to eliminate the yield plateau, but to avoid introducing excessive work hardening. An excessively large elongation will significantly increase the yield strength and tensile strength, but will sacrifice elongation and toughness. It can perfectly preserve the mechanical properties of the hot-rolled base material: strength loss <10MPa, and almost no decay in elongation and impact toughness.
[0030] Using high tension can reduce the required rolling force, thereby reducing roll flattening and mill bounce, which is beneficial for achieving precise control of small elongation, while reducing severe damage to the microstructure.
[0031] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. For those skilled in the art, the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A hot-rolling leveling process for high-strength steel, characterized in that, Includes the following steps: S1. Control the tapping temperature to 1260-1300℃; S2. Control the dwell time of the intermediate billet in the hot rolling box to be 12-25 seconds, and perform edge electromagnetic induction heating; S3. Control the temperature entering the finishing mill to be 1060-1100℃ and the temperature exiting the finishing mill to be 870-890℃. Apply high-frequency ultrasonic oscillation to the strip steel with a frequency of 20kHz, an amplitude of 10μm, an action time of 6 seconds, and an energy density of 50 joules per cubic centimeter. S4. The hot-rolled strip is cooled in stages, including: first, the strip is rapidly cooled from the finishing rolling temperature to 550-560°C at a cooling rate of 60°C per second; then, the surface temperature of the strip is warmed back to 580°C by radiant heating tubes at a heating rate of 15°C per second; relax on the roller table for 8 seconds; and finally, the strip is cooled to 550°C at a cooling rate of 30°C per second before being coiled. The chemical composition of high-strength steel, by mass percentage, includes: C: 0.18-0.24%, Mn: 1.9-2.4%, S: ≤0.004%, P: ≤0.02%, Si: 1.4-2.0%, Als: 0.04-0.06%, N: <0.006%, Nb: 0.02-0.05%, Ti: 0.045-0.06%, B: 0.001-0.002%; the remainder is Fe or impurities.
2. The high-strength steel hot rolling leveling process as described in claim 1, characterized in that, The electromagnetic induction heating power in the hot roll box is 300-350KW / m.
3. The high-strength steel hot rolling leveling process as described in claim 1, characterized in that, It also includes dry leveling of the obtained hot-rolled steel coil, with elongation controlled at 0.8%-1.2%, inlet tension at 250MPa, outlet tension at 280MPa, rolling speed at 300-500m / min, and surface roughness controlled at Ra2.0-2.5μm.
Citation Information
Patent Citations
Tempering-free ultrahigh-strength steel Q890D for engineering machinery and production method of tempering-free ultrahigh-strength steel Q890D
CN112853223A
Production method for thinning hot-rolled high-strength strip steel above 980 MPa
CN114101339A