Wear-resistant self-curing insulating coating material and preparation method thereof
By using lightweight hollow glass microspheres and polydopamine-coated wear-resistant agents, combined with an epoxy-organic silicone composite curing system, the problems of wear resistance and self-curing properties in the process of lightweighting insulating coating materials were solved. This enabled the preparation of self-curing insulating coating materials at room temperature, which possess excellent insulation and wear resistance.
Patent Information
- Application Number
- CN202511368693.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-24
- Publication Date
- 2025-11-28
AI Technical Summary
Existing insulating coating materials struggle to maintain excellent wear resistance and self-curing properties during the process of achieving lightweighting, and traditional methods often lead to a decline in mechanical strength and electrical insulation performance.
Lightweight hollow glass microspheres are used as fillers, and their interfacial bonding with resin is improved by treatment with 2-hydroxyethyl methacrylate phosphate. At the same time, polydopamine-coated abrasion-resistant agent is used to enhance the bonding with the matrix. Combined with an epoxy-silicone composite curing system, room temperature self-curing is achieved.
A coating material with ultra-lightweight properties, excellent insulation and wear resistance was prepared. It can self-cur at room temperature and maintain good mechanical strength and electrical insulation properties.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating technology and relates to a wear-resistant self-curing insulating coating material and its preparation method. Background Technology
[0002] As electronic and electrical equipment develops towards miniaturization, lightweighting, and high power density, unprecedented challenges are posed to the insulation and protection of its internal components. Traditional insulating coating materials (such as epoxy resin and silicone resin) possess good insulation properties, but their high density and inherent weight severely limit their application in electrical equipment.
[0003] Currently, the main technical routes for achieving lightweight insulation materials include: 1. Introducing chemical foaming agents or physical hollow microspheres, but this often leads to a decrease in mechanical strength and wear resistance; 2. Using polymers with low density, but these materials usually have a slow curing speed and require high temperature or ultraviolet assistance; 3. Using aerogel composite materials, but they are brittle and have poor toughness, making it difficult to form a dense and continuous coating layer.
[0004] Therefore, how to make insulating coating materials have ultra-lightweight properties while maintaining excellent wear resistance and self-curing properties is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] The purpose of this invention is to provide a wear-resistant self-curing insulating coating material and its preparation method. The method of this invention maintains the excellent insulation and wear resistance of the coating material while using lightweight hollow glass microsphere fillers, and can self-cur at room temperature.
[0006] The objective of this invention can be achieved through the following technical solutions: On one hand, the present invention provides a wear-resistant self-curing insulating coating material, comprising the following components by weight: 50-80 parts epoxy resin, 5-10 parts polydimethylsiloxane, 5-15 parts curing agent, 15-30 parts filler, 2-5 parts dispersant, 3-5 parts leveling agent, 5-15 parts wear-resistant agent, 5-8 parts flame retardant, 3-5 parts coupling agent, and 1-3 parts pigment.
[0007] This invention uses epoxy resin as the base resin, which provides excellent adhesion and superior electrical insulation: high volume resistivity and dielectric strength, making it an ideal insulating material. Simultaneously, the invention incorporates polydimethylsiloxane, an organosilicon compound. The polydimethylsiloxane used in this invention is hydroxyl-terminated, which can undergo condensation crosslinking by absorbing moisture from the air. Furthermore, it can act as a flexible chain segment, improving the brittleness of pure epoxy resin. Therefore, through the epoxy-organosilicon composite curing system, room temperature self-curing is achieved without additional heating, simplifying the construction process.
[0008] In this invention, the wear resistance and insulation properties of the coating material are ensured through the interaction between the high-strength epoxy resin matrix, wear-resistant agent, filler, and other additives.
[0009] The preparation process of the filler is as follows: Hollow glass microspheres were dispersed in a sodium hydroxide solution with a mass fraction of 3-4% and a solid-liquid mass ratio of 1:10. The mixture was stirred at 300 r / min at 50℃ for 1-1.5 h. After stirring, the mixture was filtered, washed with ethanol, and vacuum dried at 60℃ for 8-12 h to obtain pretreated hollow glass microspheres. Pretreated hollow glass microspheres were dispersed in a solution of 2-hydroxyethyl methacrylate phosphate with a mass fraction of 8-12%, and p-toluenesulfonic acid with a mass fraction of 1% of the hollow glass microspheres was added and mixed. The mass ratio of the pretreated hollow glass microspheres to the 2-hydroxyethyl methacrylate phosphate solution was 1:5. The mixture was heated to 50-70°C and stirred for 2-4 hours. After filtration and washing, the filler was obtained.
[0010] This invention first activates hollow glass microspheres with alkali. This pretreatment condition maximizes the preservation of the spherical structure and mechanical strength of the microspheres, making them less prone to breakage during subsequent processing and stirring, and fully leveraging their inherent advantages of being lightweight and heat-insulating. Then, treatment with 2-hydroxyethyl methacrylate phosphate enhances the interfacial bonding between the microsphere filler and the resin. The introduction of 2-hydroxyethyl methacrylate phosphate helps reduce the surface energy of the microspheres. The phosphate groups on it can form hydrogen bonds with the hydroxyl groups on the microsphere surface, and can also exist stably on the surface of the microspheres through covalent bonding. This solves the problem of interfacial compatibility between inorganic glass and organic resin, effectively preventing the microspheres from agglomerating and settling in the resin system, achieving uniform and stable dispersion. Simultaneously, it forms a more compact integral structure with the resin matrix. Because the filler prepared by this invention can not only physically fill but also better participate in curing, becoming part of the cross-linking network, it improves the overall performance of the coating material, giving it better thermal stability and mechanical strength.
[0011] Therefore, the filler has good dispersibility and strong interfacial bonding, and can significantly reduce the overall density of the coating by adding a sufficient amount of hollow glass microspheres without sacrificing mechanical properties.
[0012] Furthermore, the preparation process of the wear-resistant agent is as follows: Alumina and zirconium carbide in a mass ratio of 1:1 were ball-milled at 300 r / min to obtain a powder mixture. Dopamine hydrochloride was added to a Tris-HCl buffer solution with a pH of 8.5-9, and the mixture was stirred. The powder mixture was then added, and the mixture was stirred at 40-45℃ for 10-12 h. After filtration, washing, and drying, the wear-resistant agent was prepared.
[0013] Alumina and zirconium carbide were ball-milled in a 1:1 ratio. Al₂O₃ provided good matrix hardness and insulation, while zirconium carbide, as a reinforcing phase, significantly improved the top-level wear resistance of the mixed powder. Then, dopamine was self-polymerized under alkaline conditions to form polydopamine, thereby forming a coating on the wear-resistant agent surface and enhancing its bonding with the matrix.
[0014] Furthermore, because the wear-resistant agent is encapsulated by the polydopamine insulating layer, the electrical insulation properties of the coating material are not reduced by the addition of zirconium carbide. The active functional groups of polydopamine can also interact with polydimethylsiloxane, thereby helping to promote the curing of the system.
[0015] Furthermore, the curing agent is a mixture of N,N-dimethylaminopropylamine and diethyltoluenediamine in a mass ratio of 3:1.
[0016] An amine-based curing agent is used to react with the epoxy resin, ensuring that the reaction occurs at room temperature to form a three-dimensional network.
[0017] Furthermore, the dispersant is one or more of sodium polyacrylate and polycarboxylate.
[0018] The dispersant used in this invention can prevent the agglomeration of solid particles such as fillers and wear-resistant agents, ensuring that they are uniformly dispersed in the resin, avoiding sedimentation, and ensuring that the resulting coating has uniform composition and stable performance.
[0019] Furthermore, the flame retardant is one or more of aluminum hydroxide, antimony oxide, ammonium hydrogen phosphate, and hexaphenyloxytriphosphazene.
[0020] By adding phosphorus-based, nitrogen-based, or halogen-free flame retardants to the system, a dense carbon layer can be formed in the flame, isolating oxygen and achieving flame retardancy or self-extinguishing upon removal of the flame, thus meeting the safety standards for electronic and electrical products.
[0021] Furthermore, the coupling agent is one or more of the silane coupling agents KH550, KH560 and KH570.
[0022] Furthermore, the pigment is one or more of phthalocyanine green, phthalocyanine blue, titanium dioxide, vermilion red, malachite green, and Hansa yellow.
[0023] Furthermore, the leveling agent is one or more of BYK341, BYK345, and BYK337.
[0024] By adding a leveling agent to the system to reduce the surface tension of the coating material, brush marks, orange peel and other phenomena caused during construction are eliminated, making the coating surface smooth and flat. This is not only aesthetically pleasing, but also more conducive to wear resistance and insulation.
[0025] Furthermore, the mass-to-volume ratio of the mixture powder, dopamine hydrochloride, and Tris-HCl buffer solution is 1 g : (0.5~1) g : 700 mL.
[0026] On the other hand, the present invention also provides a preparation process for a wear-resistant self-curing insulating coating material, comprising the following steps: S1. According to the weight proportions, at 50~60℃, after uniformly mixing the filler and wear-resistant agent, continue to add the coupling agent and stir at a speed of 500 r / min for 0.5~1h; under nitrogen protection, continue to add epoxy resin, polydimethylsiloxane, dispersant, curing agent, leveling agent, flame retardant and pigment, and stir at a speed of 800~1200 r / min for 60~120min to obtain mixture A; S2. Transfer the mixture A obtained in step S1 to a vacuum degassing machine and remove bubbles for 10 to 30 minutes under a vacuum of -0.095 to -0.098 MPa to obtain the wear-resistant self-curing insulating coating material.
[0027] The beneficial effects of this invention are: This invention provides a wear-resistant, self-curing insulating coating material and its preparation process. Using epoxy resin as a base material, a composite curing system of epoxy resin and polydimethylsiloxane is utilized to achieve self-curing at room temperature. The density of the coating material is reduced by using lightweight filler hollow glass microspheres treated with 2-hydroxyethyl methacrylate phosphate, thereby improving mechanical strength and interfacial adhesion while maintaining mechanical properties. Polydopamine surface coating prevents agglomeration of the wear-resistant agent when added to the resin and avoids subsequent detachment, thus improving wear resistance. Furthermore, the active functional groups of polydopamine form strong chemical bonds with the epoxy resin, making the wear-resistant agent more than just a simple physical filler. The coating material prepared by this invention uses lightweight fillers, exhibits ultra-lightweight properties, excellent insulation and wear resistance, and can self-cur at room temperature. Detailed Implementation
[0028] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with embodiments, is provided below.
[0029] It should be noted that, unless otherwise specified, the raw materials used in the following embodiments can be obtained by commercial purchase or conventional methods, and the experimental methods without specific conditions are all conventional methods and conditions well known in the art.
[0030] The curing agent is a mixture of N,N-dimethylaminopropylamine and diethyltoluenediamine in a mass ratio of 3:1.
[0031] In the following examples and comparative examples, the epoxy resin was purchased from Hubei Wande Chemical Co., Ltd., item number: WD6200; and the polydimethylsiloxane was purchased from Wuhan Shuer Biotechnology Co., Ltd., item number: 08778.
[0032] Example 1 It includes the following components by weight: 50 parts epoxy resin, 5 parts polydimethylsiloxane, 5 parts curing agent, 15 parts filler, 2 parts sodium polyacrylate, 3 parts BYK341, 5 parts wear-resistant agent, 5 parts aluminum hydroxide, 3 parts KH550, and 1 part titanium dioxide.
[0033] Preparation of filler: Hollow glass microspheres were dispersed in a 3% sodium hydroxide solution with a solid-liquid mass ratio of 1:10. The mixture was stirred at 300 r / min for 1 h at 50 °C. After stirring, the mixture was filtered, washed with ethanol, and vacuum dried at 60 °C for 8 h to obtain pretreated hollow glass microspheres. Pretreated hollow glass microspheres were dispersed in an 8% (w / w) solution of 2-hydroxyethyl methacrylate phosphate, and 1% (w / w) of p-toluenesulfonic acid was added to mix. The mass ratio of the pretreated hollow glass microspheres to the 2-hydroxyethyl methacrylate phosphate solution was 1:5. The mixture was heated to 50°C and stirred for 2 hours. After filtration and washing, the filler was obtained.
[0034] Preparation of wear-resistant agents: Alumina and zirconium carbide in a mass ratio of 1:1 were ball-milled at 300 r / min to obtain a powder mixture. Dopamine hydrochloride was added to a Tris-HCl buffer solution with a pH of 8.5-9, and the mixture was stirred. Then, the powder mixture was added, and the mixture was stirred at 40℃ for 10 h. After filtration, washing, and drying, the wear-resistant agent was prepared. The concentration of the Tris-HCl buffer solution was 0.03 mol / L, and the mass-volume ratio of the powder mixture, dopamine hydrochloride, and Tris-HCl buffer solution was 1 g: 0.5 g: 700 mL.
[0035] Preparation of wear-resistant self-curing insulating coating material: S1. According to the weight proportions, at 50℃, after uniformly mixing the filler and wear-resistant agent, continue to add the coupling agent and stir at a speed of 500 r / min for 0.5 h; under nitrogen protection, continue to add epoxy resin, polydimethylsiloxane, dispersant, curing agent, leveling agent, flame retardant and pigment, and stir at a speed of 800 r / min for 60 min to obtain mixture A; S2. Transfer the mixture A obtained in step S1 to a vacuum degassing machine and remove bubbles for 10 minutes under a vacuum of -0.095 MPa to obtain a wear-resistant self-curing insulating coating material.
[0036] Example 2 It includes the following components by weight: 60 parts epoxy resin, 7 parts polydimethylsiloxane, 10 parts curing agent, 22 parts filler, 3 parts sodium polyacrylate, 4 parts BYK345, 10 parts wear-resistant agent, 6 parts aluminum hydroxide, 4 parts KH560, and 2 parts titanium dioxide.
[0037] Preparation of filler: Hollow glass microspheres were dispersed in a 3.5% sodium hydroxide solution with a solid-liquid mass ratio of 1:10. The mixture was stirred at 300 r / min for 1.2 h at 50 °C. After stirring, the mixture was filtered, washed with ethanol, and vacuum dried at 60 °C for 10 h to obtain pretreated hollow glass microspheres. Pretreated hollow glass microspheres were dispersed in a 10% (w / w) solution of 2-hydroxyethyl methacrylate phosphate, and 1% (w / w) of p-toluenesulfonic acid was added to mix. The mass ratio of the pretreated hollow glass microspheres to the 2-hydroxyethyl methacrylate phosphate solution was 1:5. The mixture was heated to 60°C and stirred for 3 hours. After filtration and washing, the filler was obtained.
[0038] Preparation of wear-resistant agents: Alumina and zirconium carbide in a mass ratio of 1:1 were ball-milled at 300 r / min to obtain a powder mixture. Dopamine hydrochloride was added to a Tris-HCl buffer solution with a pH of 8.5-9, and the mixture was stirred. Then, the powder mixture was added, and the mixture was stirred at 42℃ for 11 h. After filtration, washing, and drying, the wear-resistant agent was prepared. The concentration of the Tris-HCl buffer solution was 0.04 mol / L, and the mass-volume ratio of the powder mixture, dopamine hydrochloride, and Tris-HCl buffer solution was 1 g: 0.7 g: 700 mL.
[0039] Preparation of wear-resistant self-curing insulating coating material: S1. According to the weight proportions, at 55℃, after uniformly mixing the filler and wear-resistant agent, continue to add the coupling agent and stir at a speed of 500 r / min for 0.7 h; under nitrogen protection, continue to add epoxy resin, polydimethylsiloxane, dispersant, curing agent, leveling agent, flame retardant and pigment, and stir at a speed of 1000 r / min for 90 min to obtain mixture A; S2. Transfer the mixture A obtained in step S1 to a vacuum degassing machine and remove bubbles for 20 minutes under a vacuum of -0.097 MPa to obtain a wear-resistant self-curing insulating coating material.
[0040] Example 3 It includes the following components by weight: 80 parts epoxy resin, 10 parts polydimethylsiloxane, 15 parts curing agent, 30 parts filler, 5 parts sodium polyacrylate, 5 parts BYK341, 15 parts wear-resistant agent, 8 parts aluminum hydroxide, 5 parts KH550, and 3 parts titanium dioxide.
[0041] Preparation of filler: Hollow glass microspheres were dispersed in a 4% sodium hydroxide solution with a solid-liquid mass ratio of 1:10. The mixture was stirred at 300 r / min for 1.5 h at 50 °C. After stirring, the mixture was filtered, washed with ethanol, and vacuum dried at 60 °C for 12 h to obtain pretreated hollow glass microspheres. Pretreated hollow glass microspheres were dispersed in a 12% (w / w) solution of 2-hydroxyethyl methacrylate phosphate, and 1% (w / w) of p-toluenesulfonic acid was added to mix. The mass ratio of the pretreated hollow glass microspheres to the 2-hydroxyethyl methacrylate phosphate solution was 1:5. The mixture was heated to 70°C and stirred for 4 hours. After filtration and washing, the filler was obtained.
[0042] Preparation of wear-resistant agents: Alumina and zirconium carbide in a mass ratio of 1:1 were ball-milled at 300 r / min to obtain a powder mixture. Dopamine hydrochloride was added to a Tris-HCl buffer solution with a pH of 8.5-9, and the mixture was stirred. Then, the powder mixture was added, and the mixture was stirred at 45℃ for 12 h. After filtration, washing, and drying, the wear-resistant agent was prepared. The concentration of the Tris-HCl buffer solution was 0.03-0.06 mol / L, and the mass-volume ratio of the powder mixture, dopamine hydrochloride, and Tris-HCl buffer solution was 1 g: 1 g: 700 mL.
[0043] Preparation of wear-resistant self-curing insulating coating material: S1. According to the weight proportions, at 60℃, the filler and wear-resistant agent are mixed evenly, and then the coupling agent is added. The mixture is stirred at a speed of 500 r / min for 1 hour. Under nitrogen protection, epoxy resin, polydimethylsiloxane, dispersant, curing agent, leveling agent, flame retardant and pigment are added. The mixture is stirred at a speed of 1200 r / min for 120 minutes to obtain mixture A. S2. Transfer the mixture A obtained in step S1 to a vacuum degassing machine and remove bubbles for 30 minutes under a vacuum of -0.098 MPa to obtain a wear-resistant self-curing insulating coating material.
[0044] Comparative Example 1 This comparative example is basically the same as Example 1, except that the hollow glass microspheres in this comparative example have not been pretreated.
[0045] Comparative Example 2 This comparative example is basically the same as Example 1, except that the filler used in this comparative example is hollow glass microspheres without any treatment.
[0046] Comparative Example 3 This comparative example is basically the same as Example 1, except that the wear-resistant agent in this comparative example is alumina and zirconium carbide in a mass ratio of 1:1, and has not been treated with polydopamine.
[0047] Comparative Example 4 This comparative example is basically the same as Example 1, except that polydimethylsiloxane was not added in this comparative example.
[0048] Performance testing The specific technical parameters and properties after curing of the wear-resistant self-curing insulating coating material prepared in Example 1 are summarized in Table 1 below: Table 1 project Measured values <![CDATA[Density (g / cm 3 )]]> 1.14 Curing time / min 27 Curing and drying time / h 18 Hardness after curing / Shore A 57 Tensile strength after curing / MPa 18.4 Breakdown voltage / kV 46.7 Surface resistivity / Ω <![CDATA[2.8◊10 13 ]]> Cable immersion withstand voltage test (in water, 65.0kV, 240) No breakdown, no flashover Simulated metal-to-metal contact zero-distance long-term withstand voltage test (in air, 45.0 kV, 240 min) No breakdown, no flashover The coating materials of Examples 1-3 and Comparative Examples 1-4 were applied by scraping according to GB / T 1727, with the coating thickness controlled at 0.5 mm. The coating thickness was measured according to GB / T 13452.2. After preparation, the test panels were placed under conditions conforming to GB / T 9278 for 7 days before testing.
[0049] 1. Adhesion rating conforms to GB / T 9286-2021; 2. Insulation performance: The breakdown voltage was tested according to GB / T 1408.1-2016 "Test methods for electrical strength of insulating materials - Part 1: Test under power frequency". The test conditions were: electric heating at 100℃ for 2 hours, cooling for 3 hours, repeated 3 times, in normal water, rapid voltage increase method, voltage increase rate 2000V / s. 3. Abrasion resistance: (1) Testing standard: GB / T 1768; (2) Test conditions: Instrument: Taber Abraser 5135; Grinding wheel: CS-10 rubber wheel; Load: 1000g / wheel; Rotation speed: 60rpm; Number of revolutions: 1000 revolutions; (3) Operation procedure: Fix the sample on the turntable, with the grinding wheel in contact with the surface, start the instrument, pause every 250 revolutions, remove the grinding debris with a soft brush, and weigh the sample mass loss with an electronic balance (accuracy 0.1mg) after the test is completed. (4) Calculation: Taber abrasion index = [mass loss (mg)] × 1000 / revolutions.
[0050] The test results are shown in Table 2 below: Table 2 Group Adhesion rating / level Breakdown voltage / kV Taber abrasion resistance index / mg Example 1 1 46.7 45 Example 2 1 44.3 40 Example 3 1 45.4 43 Comparative Example 1 2 45.2 49 Comparative Example 2 3 42.1 57 Comparative Example 3 2 43.7 50 Comparative Example 4 1 42.7 47 Based on the above data, it can be seen that the self-curing coating material prepared by the present invention has excellent wear resistance and insulation properties.
[0051] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A wear-resistant, self-curing, insulating coating material, characterized in that, It includes the following components by weight: 50-80 parts epoxy resin, 5-10 parts polydimethylsiloxane, 5-15 parts curing agent, 15-30 parts filler, 2-5 parts dispersant, 3-5 parts leveling agent, 5-15 parts abrasion resistant agent, 5-8 parts flame retardant, 3-5 parts coupling agent, and 1-3 parts pigment. The preparation process of the filler is as follows: Hollow glass microspheres were dispersed in a sodium hydroxide solution with a mass fraction of 3-4% and a solid-liquid mass ratio of 1:
10. The mixture was stirred at 300 r / min at 50℃ for 1-1.5 h. After stirring, the mixture was filtered, washed with ethanol, and vacuum dried at 60℃ for 8-12 h to obtain pretreated hollow glass microspheres. Pretreated hollow glass microspheres were dispersed in a solution of 2-hydroxyethyl methacrylate phosphate with a mass fraction of 8-12%, and p-toluenesulfonic acid with a mass fraction of 1% of the hollow glass microspheres was added and mixed. The mass ratio of the pretreated hollow glass microspheres to the 2-hydroxyethyl methacrylate phosphate solution was 1:
5. The mixture was heated to 50-70°C and stirred for 2-4 hours. After filtration and washing, the filler was obtained.
2. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The preparation process of the wear-resistant agent is as follows: Alumina and zirconium carbide in a mass ratio of 1:1 were ball-milled at 300 r / min to obtain a powder mixture. Dopamine hydrochloride was added to a Tris-HCl buffer solution with a pH of 8.5-9, and the mixture was stirred. The powder mixture was then added, and the mixture was stirred at 40-45℃ for 10-12 h. After filtration, washing, and drying, the wear-resistant agent was prepared.
3. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The curing agent is a mixture of N,N-dimethylaminopropylamine and diethyltoluenediamine in a mass ratio of 3:
1.
4. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The dispersant is one or more of sodium polyacrylate and polycarboxylate.
5. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The flame retardant is one or more of aluminum hydroxide, antimony oxide, ammonium hydrogen phosphate, and hexaphenyloxytriphosphazene.
6. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The coupling agent is one or more of the silane coupling agents KH550, KH560 and KH570.
7. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The pigment is one or more of phthalocyanine green, phthalocyanine blue, titanium dioxide, vermilion red, malachite green, and Hansa yellow.
8. The wear-resistant self-curing insulating coating material according to claim 1, characterized in that, The leveling agent is one or more of BYK341, BYK345, and BYK337.
9. The wear-resistant self-curing insulating coating material according to claim 2, characterized in that, The mass-to-volume ratio of the mixture powder, dopamine hydrochloride, and Tris-HCl buffer solution is 1 g : (0.5~1) g : 700 mL.
10. A preparation process for a wear-resistant self-curing insulating coating material as described in any one of claims 1-9, characterized in that, Includes the following steps: S1. According to the weight proportions, at 50~60℃, after uniformly mixing the filler and wear-resistant agent, continue to add the coupling agent and stir at a speed of 500 r / min for 0.5~1h; under nitrogen protection, continue to add epoxy resin, polydimethylsiloxane, dispersant, curing agent, leveling agent, flame retardant and pigment, and stir at a speed of 800~1200 r / min for 60~120min to obtain mixture A; S2. Transfer the mixture A obtained in step S1 to a vacuum degassing machine and remove bubbles for 10 to 30 minutes under a vacuum of -0.095 to -0.098 MPa to obtain the wear-resistant self-curing insulating coating material.
Citation Information
Cited By
Flame-retardant brazing paste as well as preparation method and brazing process thereof
CN121820949A