Low-temperature lithium iron phosphate material, preparation method thereof and lithium ion battery

By preparing micron-sized flat lithium iron phosphate particles, the problem of balancing high compaction density and low-temperature performance of lithium iron phosphate materials under low-temperature conditions has been solved, achieving high efficiency in low-temperature performance and low-cost industrial production.

CN121044555AActive Publication Date: 2025-12-02安徽得壹能源科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511214753.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-28
Publication Date
2025-12-02
Estimated Expiration
2045-08-28

AI Technical Summary

Technical Problem

Existing technologies struggle to balance the high density and low-temperature performance of lithium iron phosphate materials in low-temperature environments, and production costs are high and processes are complex.

Method used

A method for preparing micron-sized flat lithium iron phosphate particles was adopted. By controlling the reaction pH value, using the synergistic effect of α-hydroxy polycarboxylic acid complexing agent and ferrous salt, and combining sand milling and spray drying sintering processes, precursor particles with specific crystal orientations were formed, and a phosphoric acid adsorption electrostatic barrier was introduced to optimize the crystal structure.

Benefits of technology

It achieves good low-temperature performance under high actual density (≥2.5g/cm3), and the discharge capacity retention rate at -20℃ is over 75%. It simplifies the process, reduces production costs, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121044555A_ABST
    Figure CN121044555A_ABST
Patent Text Reader

Abstract

The invention discloses a low-temperature lithium iron phosphate material, a preparation method thereof and a lithium ion battery, and belongs to the technical field of lithium ion batteries. The preparation method comprises the following steps: mixing and dissolving ferrite and a polycarboxylic acid complexing agent containing alpha-hydroxyl in water, then introducing a phosphoric acid solution and a lithium source solution, and controlling the pH value in the system to be less than or equal to 3; reacting at 20-55 DEG C for 4-8 hours, and washing and drying a solid product to obtain a precursor; sanding the precursor, a carbon source, phosphoric acid and a doping agent to obtain slurry; and carrying out spray drying, sintering and crushing on the slurry to obtain the low-temperature lithium iron phosphate material. According to the invention, oriented growth of lithium iron phosphate crystal grains can be realized, and the lithium iron phosphate with a micron-sized flat structure is obtained, so that the material keeps good low-temperature performance while maintaining high compaction density (greater than or equal to 2.5 g / cm < 3 >).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and in particular to a low-temperature lithium iron phosphate material, its preparation method, and a lithium-ion battery. Background Technology

[0002] The information disclosed in the background section of this invention is intended only to enhance the understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] In the field of lithium-ion batteries, lithium iron phosphate cathode materials have become the core choice for power batteries due to their excellent safety and economy. However, the degradation of their electrochemical performance at low temperatures has always been a key bottleneck restricting the industry's development. The essence of this problem stems from the intrinsic properties of the material: low temperatures significantly increase the diffusion resistance of lithium ions in the olivine structure, while also causing a surge in solid-liquid interface impedance, leading to a sharp deterioration in ion transport kinetics and severely limiting the reliability of applications in cold regions.

[0004] To improve low-temperature performance, existing technologies mainly focus on nano-sizing, surface coating, and elemental doping, but all have significant limitations. While nano-sizing can shorten the ion diffusion path, the excessively fine particles severely sacrifice compaction density, and the high specific surface area exacerbates interfacial side reactions. Although surface coating technology can improve conductivity, the process is complex and the coating uniformity is difficult to control, leading to a significant increase in mass production costs. Although elemental doping can optimize lattice channels, in traditional processes, dopants tend to agglomerate, forming ineffective regions. This requires a lengthy precursor preparation process, which not only consumes a lot of energy but also results in insufficient performance stability.

[0005] More importantly, the existing technology system has never been able to effectively resolve the technical contradiction between high compaction density and low-temperature performance. Although micron-scale materials can achieve high compaction density through particle gradation, the random stacking of spherical particles leads to insufficient exposure of highly active crystal faces, which limits the performance of low-temperature kinetic properties. On the other hand, although nanomaterials have excellent low-temperature kinetic potential, the insufficient compaction density causes a decrease in the volumetric energy density of the battery, and the harsh production conditions and high-energy-consuming processes further increase production costs.

[0006] Therefore, how to provide a method for preparing lithium iron phosphate cathode materials that can take into account both the high density and low temperature performance of lithium iron phosphate, and has low production cost and simple process is an urgent problem to be solved. Summary of the Invention

[0007] In view of this, the present invention provides a low-temperature lithium iron phosphate material and its preparation method, as well as a lithium-ion battery. The preparation method provided by the present invention can prepare micron-sized flat lithium iron phosphate particles, synergistically improve the high-pressure density and low-temperature performance of lithium iron phosphate material, and simplify the process and reduce production costs.

[0008] In a first aspect, the present invention provides a method for preparing a low-temperature lithium iron phosphate material, comprising the following steps: Ferrous salt and a polycarboxylic acid complexing agent containing α-hydroxyl groups were mixed and dissolved in water, and then phosphoric acid solution and lithium source solution were introduced to control the pH of the system to ≤3. The reaction was carried out at 20~55℃ for 4~8h under inert gas protection, and the solid product was washed and dried to obtain the precursor. The precursor, carbon source, phosphoric acid and dopant are milled to obtain a slurry; The slurry is spray-dried, sintered, and pulverized to obtain a low-temperature lithium iron phosphate material.

[0009] Preferably, the mass ratio of the ferrous salt to the α-hydroxyl-containing polycarboxylic acid complexing agent is (0.3~0.5):1; in the step of introducing the phosphoric acid solution and the lithium source solution, the molar ratio of Li, Fe and P is controlled to be (1.00~1.05):1:(1.00~1.05).

[0010] Preferably, the ferrous salt is selected from one or more of ferrous sulfate, ferrous nitrate, or ferrous chloride; and the α-hydroxyl-containing polycarboxylic acid complexing agent is selected from one or more of citric acid, tartaric acid, or gluconic acid.

[0011] Preferably, the lithium source is selected from one or more of lithium hydroxide, lithium carbonate, or lithium dihydrogen phosphate; and the carbon source is selected from one or more of glucose, sucrose, starch, or phenolic resin.

[0012] Preferably, the dopant is selected from one or more of titanium source, vanadium source, magnesium source, aluminum source or manganese source.

[0013] Furthermore, the dopant is TiO2 and V2O5, and the mass ratio of TiO2 to V2O5 is (2~8):1.

[0014] Preferably, the mass ratio of the precursor, carbon source, phosphoric acid and dopant is 100 : (6~10) : (0.4~1.5) : (0.2~0.4); the solvent in the sand milling process is water.

[0015] Preferably, the spray drying temperature is 180~260℃; the sintering temperature is 600~800℃, and the sintering time is 4~16h.

[0016] Secondly, the present invention provides a low-temperature lithium iron phosphate material prepared by the above preparation method.

[0017] Thirdly, the present invention provides a lithium-ion battery comprising the aforementioned low-temperature lithium iron phosphate material.

[0018] Compared with the prior art, the present invention has achieved the following beneficial effects: (1) This invention achieves the directional growth of lithium iron phosphate grains by precisely controlling the pH value of the reaction system within the range of 1 to 3, combined with the synergistic effect of α-hydroxy polycarboxylic acid complexing agent and ferrous salt. This results in the formation of a micron-scale flattened lithium iron phosphate structure with an average long axis length of approximately 1 to 3 μm and an average short axis length of approximately 0.5 to 1 μm. This unique morphology shortens the lithium-ion diffusion path, improves ion transport efficiency at low temperatures, and allows the material to maintain a high compaction density (≥2.5 g / cm³). 3 While maintaining good low-temperature performance, the discharge capacity retention rate at -20℃ is as high as 75% or more, solving the problem of severe capacity decay of traditional lithium iron phosphate in low-temperature environments.

[0019] (2) In the sand milling stage, phosphoric acid is introduced to adsorb onto the surface of the dopant to form an electrostatic barrier, which effectively inhibits the aggregation of nanoscale dopant and is beneficial to improving the low-temperature ionic conductivity.

[0020] (3) The precursor synthesis of the present invention adopts atmospheric pressure liquid phase reaction, which avoids the high temperature and high pressure of high pressure hydrothermal or solvothermal reaction, which is safer and has lower energy consumption. At the same time, the preparation process is simple and easy to operate, and the material structure and performance can be precisely controlled without complicated post-processing steps. The process has high repeatability and low production cost, which is suitable for large-scale industrial production and provides a feasible path for the commercial application of low temperature lithium iron phosphate materials. Attached Figure Description

[0021] The accompanying drawings, which form part of this specification, are used to provide a further understanding of the invention. The illustrative embodiments and descriptions of the invention are used to explain the invention and do not constitute an undue limitation thereof. Obviously, those skilled in the art can obtain other drawings based on these drawings without any inventive effort.

[0022] Figure 1 These are scanning electron microscope images of the precursor prepared in Example 1 of this invention; Figure 2 These are scanning electron microscope images of the low-temperature lithium iron phosphate material prepared in Example 1 of this invention; Figure 3 These are scanning electron microscope images of the lithium iron phosphate material prepared in Comparative Example 1 of this invention; Figure 4These are the discharge curves of the lithium iron phosphate materials of Example 1 and Comparative Example 1 of the present invention at -10°C. Detailed Implementation

[0023] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0024] This invention provides a method for preparing a low-temperature lithium iron phosphate material, comprising the following steps: Ferrous salt and a polycarboxylic acid complexing agent containing α-hydroxyl groups were mixed and dissolved in water, and then phosphoric acid solution and lithium source solution were introduced to control the pH of the system to ≤3. The reaction was carried out at 20~55℃ for 4~8h under inert gas protection, and the solid product was washed and dried to obtain the precursor. The precursor, carbon source, phosphoric acid and dopant are milled to obtain a slurry; The slurry is spray-dried, sintered, and pulverized to obtain a low-temperature lithium iron phosphate material.

[0025] In the precursor preparation stage of this invention, the polycarboxylic acid complexing agent containing α-hydroxyl groups can react with Fe... 2+ The formation of iron ion complexes with rigid chelate structures forces iron ions to align along specific crystal orientations, while simultaneously controlling the Fe content by regulating the complexation equilibrium. 2+ The slow release of PO4 prevents particle aggregation caused by rapid precipitation. Furthermore, the strongly acidic environment of the reaction system (pH ≤ 3) inhibits the release of PO4. 3- Hydrolysis of PO4 3- It mainly exists in the form of H2PO4⁻, avoiding localized high concentrations of PO4. 3- This process triggers explosive nucleation; simultaneously, the steric hindrance effect of the iron-ion complex with its rigid chelate structure drives the crystal to preferentially grow along the highly ion-diffusion-active surface, forming precursor particles with specific crystal orientations. The precursor preparation process of this invention does not require high-temperature and high-pressure environments; it can be carried out at room temperature or under micro-heating conditions, significantly reducing equipment and energy costs.

[0026] The grinding process disperses the precursor, carbon source, phosphoric acid, and dopants into a nanoscale slurry using mechanical force. On one hand, the collision and shearing action of the grinding media breaks down hard agglomerates of the precursor, reducing particle size and increasing specific surface area, providing a sufficient interface for atomic diffusion during subsequent sintering. On the other hand, it ensures uniform mixing of the carbon source and precursor particles, guaranteeing a uniform carbon layer coating on the lithium iron phosphate surface after sintering, constructing a continuous electronically conductive network. The addition of phosphoric acid is not as a phosphorus source; phosphate ions (PO4) are used. 3-The oxygen atoms adsorb onto the dopant surface through lone pair electrons, forming a negatively charged adsorption layer. This adsorption layer generates a strong electrostatic repulsion force, which effectively inhibits the aggregation of nanoscale dopants. At the same time, phosphate molecules interpenetrate between precursor particles, reducing the viscosity of the slurry and ensuring that a uniform slurry with atomically dispersed dopant elements is obtained after sand milling.

[0027] Spray drying removes the solvent through atomization, while the sintering process promotes the dehydration, decomposition, and crystal phase transformation of the precursor through high temperature. At the same time, the carbon source is pyrolyzed to form an amorphous carbon layer, and the dopant enters the crystal lattice to replace some Fe or Li sites, optimizing the lattice parameters and ion diffusion channels. Finally, a micron-sized flat low-temperature lithium iron phosphate material with high crystallinity, excellent conductivity, and a specific flat morphology with high uniformity of particle size is obtained. It provides a fast channel for lithium ions to penetrate vertically, while ensuring high compaction density.

[0028] In an optional embodiment of the present invention, the mass ratio of the ferrous salt to the α-hydroxyl-containing polycarboxylic acid complexing agent is (0.3~0.5):1; a higher addition amount of the α-hydroxyl-containing polycarboxylic acid complexing agent ensures interaction with Fe. 2+ Fully complexed, its hydroxyl and carboxyl groups can coordinate with Fe through polydentate coordination. 2+ Stable chelates are formed; excess complexing agent can inhibit Fe 2+ To ensure the free concentration of the system, avoid non-uniform precipitation caused by excessively high local concentrations; and at the same time ensure that the pH value of the system is stable below 3.

[0029] In this invention, during the step of introducing the phosphoric acid solution and lithium source solution, the molar ratio of Li, Fe, and P is controlled to be (1.00~1.05): 1: (1.00~1.05); in the subsequent sintering process, Li... + Potassium (P) may be lost due to volatilization or reaction with impurities, and it may also precipitate as lithium phosphate. The micro-excess design ensures accurate stoichiometry of LiFePO4 in the final product, avoiding Fe... 2+ Or Li defects may affect electrochemical performance.

[0030] In optional embodiments of the present invention, the ferrous salt is selected from one or more of ferrous sulfate, ferrous oxalate, or ferrous chloride; in one or more embodiments of the present invention, the ferrous salt is selected from ferrous sulfate. The α-hydroxyl-containing polycarboxylic acid complexing agent is selected from one or more of citric acid, tartaric acid, or gluconic acid.

[0031] This invention does not impose special restrictions on the inert gas used; nitrogen, argon, or other rare gases can be used. This invention also does not impose special restrictions on the washing and drying steps for obtaining the precursor; for example, multiple centrifugal washing or vacuum filtration washing can be performed using water, ethanol, or an ethanol-water solution, and drying can be done using conventional drying or vacuum drying.

[0032] In optional embodiments of the present invention, the lithium source is selected from one or more of lithium hydroxide, lithium carbonate, or lithium dihydrogen phosphate; the carbon source is selected from one or more of glucose, sucrose, starch, or phenolic resin. In one or more embodiments of the present invention, the lithium source is preferably lithium hydroxide, which is a strong base that can quickly neutralize phosphoric acid to adjust pH and has high solubility; the carbon source is preferably glucose, because its molecular structure contains a large number of hydroxyl groups, which can combine with precursor particles through hydrogen bonds during sand milling, and after spray granulation and high-temperature sintering, it pyrolyzes into amorphous carbon, which uniformly coats the surface of lithium iron phosphate to construct an electronically conductive network.

[0033] In an optional embodiment of the present invention, the dopant is selected from one or more of titanium, vanadium, magnesium, aluminum, or manganese sources. 4+ with Fe 2+ With radii close to each other, it can partially replace Fe sites to form a solid solution, introducing lattice defects to improve electronic conductivity; V 5+ Li sites can be easily replaced, and Li can be suppressed through electricity price compensation mechanisms. + Vacancy formation; Al 3+ Doping can enhance the oxygen bond energy of the lattice and improve the cycling stability of the material. Dopants optimize lithium-ion diffusion channels by changing lattice parameters, thereby improving ion transport kinetics at low temperatures. Furthermore, the dopants are TiO2 and V2O5, with a mass ratio of TiO2 to V2O5 of (2~8):1.

[0034] In an optional embodiment of the present invention, the mass ratio of the precursor, carbon source, phosphoric acid, and dopant is 100 : (6~10) : (0.4~1.5) : (0.2~0.4); more preferably, it is 100 : (8~9) : (0.5~1) : (0.3~0.4). A suitable ratio ensures that the lithium iron phosphate material has excellent overall performance. The solvent in the sand milling process is water. The present invention does not impose special limitations on the specific parameters of the sand milling process; commonly used sand milling methods in the art can be used.

[0035] In an optional embodiment of the present invention, the spray drying temperature is 180~260℃; smooth-surfaced particles are formed through rapid evaporation of moisture. The sintering temperature is 600~800℃, and the sintering time is 4~16h, more preferably 8~15h; this ensures sufficient atomic diffusion, forming a highly crystalline olivine structure, while ensuring complete pyrolysis of the carbon source and avoiding residual organic matter from affecting conductivity. The sintering of the present invention is carried out under an inert atmosphere, such as nitrogen or argon.

[0036] This invention provides a low-temperature lithium iron phosphate material prepared by the above-described preparation method. The low-temperature lithium iron phosphate material obtained by the preparation method of this invention has the morphology of flattened particles with a long axis of approximately 1-3 μm and a short axis of approximately 0.5-2 μm.

[0037] This invention provides a lithium-ion battery comprising the aforementioned low-temperature lithium iron phosphate material.

[0038] A lithium-ion battery may include a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode uses a positive electrode active material including the aforementioned low-temperature lithium iron phosphate material. This invention does not impose any special restrictions on the selection of the negative electrode, separator, and electrolyte; commonly used negative electrodes, separators, and electrolytes in the art can be used.

[0039] The technical solution of the present invention will be further described below with reference to specific embodiments. The present invention does not impose any special restrictions on the source of reagents used in the following embodiments; commercially available products well known to those skilled in the art can be used.

[0040] Example 1 This embodiment provides a low-temperature lithium iron phosphate material and its preparation method.

[0041] (1) Ferrous sulfate and citric acid were dissolved in water at a mass ratio of 0.4:1. Then, 85wt% phosphoric acid aqueous solution and 5wt% lithium hydroxide aqueous solution were added to control the pH of the system to about 2. The molar ratio of Li, Fe and P was 1.03:1:1.03. The reaction was carried out at 30℃ for 6 hours under N2 protection. After filtration, the solid product was washed with deionized water and then dried to obtain the precursor. The scanning electron microscope image of the precursor is shown below. Figure 1 As shown, the precursor is composed of micron-sized flat single particles, indicating that oriented growth occurred during the reaction process.

[0042] (2) The precursor, glucose, phosphoric acid, TiO2 and V2O5 are mixed and sand-milled in water at a mass ratio of 100:8:1:0.3:0.05 to obtain a slurry.

[0043] (3) The slurry was spray-dried at 180°C, then heated to 700°C under N2 atmosphere and sintered for 10 hours. After cooling to room temperature, it was pulverized by airflow to obtain low-temperature lithium iron phosphate material.

[0044] The scanning electron microscope image of the low-temperature lithium iron phosphate material prepared in this embodiment is as follows: Figure 2 As shown, the low-temperature lithium iron phosphate material after sintering and pulverization still maintains the orientation structure of the precursor. Its surface is smoother than that of the precursor, and the surface is covered with a carbon layer with a long axis of about 1~3μm and a short axis of about 0.5~2μm.

[0045] Example 2 This embodiment provides a low-temperature lithium iron phosphate material and its preparation method.

[0046] (1) Ferrous sulfate and tartaric acid were dissolved in water at a mass ratio of 0.4:1. Then, 85wt% phosphoric acid aqueous solution and 5wt% lithium hydroxide aqueous solution were added to control the pH of the system to about 2.8 and the molar ratio of Li, Fe and P to be 1.03:1:1.03. The reaction was carried out at 35℃ for 8 hours under N2 protection. After filtration, the solid product was washed with deionized water and then dried to obtain the precursor.

[0047] (2) The precursor, glucose, phosphoric acid, TiO2 and V2O5 are mixed and sand-milled in water at a mass ratio of 100:8.5:0.5:0.2:0.1 to obtain a slurry.

[0048] (3) The slurry was spray-dried at 180°C, then heated to 720°C and sintered for 12 hours under N2 atmosphere. After cooling to room temperature, it was pulverized by airflow to obtain low-temperature lithium iron phosphate material.

[0049] The low-temperature lithium iron phosphate material prepared in this embodiment consists of micron-sized flat particles.

[0050] Example 3 The difference between this embodiment and Example 1 is that in this embodiment, the molar ratio of Li, Fe, and P is 1.02:1:1.02, and the precursor, glucose, phosphoric acid, TiO2, and V2O5 are mixed and milled in water at a mass ratio of 100:9:1.2:0.2:0.1. All other steps and conditions are the same.

[0051] Example 4 The difference between this embodiment and Example 1 is that in this embodiment, the precursor, glucose, phosphoric acid, TiO2, and V2O5 are mixed and milled in water at a mass ratio of 100:8.5:1.2:0.3:0.1. All other steps and conditions are the same.

[0052] Example 5 The difference between this embodiment and Example 1 is that in this embodiment, the molar ratio of Li, Fe, and P is 1.01:1:1.01, and the precursor, glucose, phosphoric acid, TiO2, and V2O5 are mixed and milled in water at a mass ratio of 100:8:1.2:0.2:0.1. All other steps and conditions are the same.

[0053] Comparative Example 1 This comparative example provides a method for preparing lithium iron phosphate.

[0054] Iron phosphate and lithium carbonate were mixed in water at a Li:Fe molar ratio of 1.03:1. Glucose, phosphoric acid, TiO2, and V2O5 were added to the solution, and the mass ratio of the total mass of iron phosphate and lithium carbonate to that of glucose, phosphoric acid, TiO2, and V2O5 was controlled at 100:8:1:0.3:0.05. The mixture was then milled to obtain a homogeneous slurry. The slurry was spray-dried at 200°C, then sintered at 750°C for 15 hours under a N2 atmosphere. After cooling to room temperature, it was subjected to air jet milling to obtain lithium iron phosphate material.

[0055] The scanning electron microscope image of the lithium iron phosphate material obtained in this comparative example is as follows: Figure 3 As shown in the figure, the lithium iron phosphate material obtained by this method is in the form of spherical particles with a particle size distribution between 0.5 and 5 μm.

[0056] Comparative Example 2 The difference between this comparative example and Example 1 is that in step (1) of this comparative example, the pH of the system is controlled to be around 5.

[0057] Comparative Example 3 The difference between this comparative example and Example 1 is that acetic acid is used instead of citric acid in this comparative example.

[0058] Comparative Example 4 The difference between this comparative example and Example 1 is that oxalic acid is used instead of citric acid in this comparative example.

[0059] Test case 1. Powder performance testing The specific surface area, compaction density, and residual carbon content of the lithium iron phosphate material powders in the examples and comparative examples were tested. The specific surface area was tested using the static adsorption method, the compaction density was tested using a powder compaction density tester, and the residual carbon content was tested using the carbon-sulfur analysis method.

[0060] The test results are summarized in Table 1.

[0061] Table 1. Test results of lithium iron phosphate material powder properties in the examples and comparative examples.

[0062] As can be seen from Table 1, the lithium iron phosphate material in the examples has a high compaction density, reaching 2.5 g / cm³. 3 The above, up to 2.6 g / cm³ 3 This is beneficial for improving the volumetric energy density of batteries.

[0063] 2. Battery performance testing A positive electrode slurry was prepared by mixing lithium iron phosphate material, conductive agent SP, and binder PVDF in N-methylpyrrolidone at a mass ratio of 97:1:2, coating it onto aluminum foil, drying it, and then rolling it to obtain a positive electrode sheet. A negative electrode slurry was prepared by mixing artificial graphite, conductive agent SP, binder SBR, and binder CMC in deionized water at a mass ratio of 96:1:1.5:1.5, coating it onto copper foil, drying it, and then rolling it to obtain a negative electrode sheet. The electrolyte was an equal-volume mixture of ethylene carbonate (EC) and dimethyl carbonate (DMC) containing 1 mol / L LiPF6. The cells were assembled into 2025-type coin cells in an argon-filled glove box. The discharge capacities of Examples 1-5 and Comparative Examples 1-4 at 25°C and 0.5C rate, and at -20°C and 0.33C rate, were tested, and the discharge capacity retention rate at -20°C was calculated. The results are shown in Table 2.

[0064] The formula for calculating the discharge capacity retention rate at -20℃ is as follows: -20℃ discharge capacity retention rate = (0.33C discharge capacity at -20℃ / 0.5C discharge capacity at 25℃) × 100%.

[0065] Table 2 Battery performance data for examples and comparative examples

[0066] In the preparation process of Examples 1 to 3 of the present invention, the crystal preferentially grows along the highly ion-diffusion-active surface to form precursor particles with specific crystal orientation. Ti and V elements are used for doping modification, and the final lithium iron phosphate material is a micron-sized flat particle. As can be seen from Tables 1 and 2, the lithium iron phosphate material prepared in the examples of the present invention has both high compaction characteristics and good low-temperature performance.

[0067] The batteries of Example 1 and Comparative Example 1 were discharged at -10°C and 1C, and discharge curves were plotted. Figure 4 As shown, the normalized low-temperature discharge capacity curve of Example 1 shows that the overall voltage plateau is better than that of Comparative Example 1, which is beneficial to the capacity performance under low temperature conditions and improves the capacity loss of the cathode material under low temperature conditions.

[0068] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a low-temperature lithium iron phosphate material, characterized in that, Includes the following steps: Ferrous salt and a polycarboxylic acid complexing agent containing α-hydroxyl groups were mixed and dissolved in water, and then phosphoric acid solution and lithium source solution were introduced to control the pH of the system to ≤3. The reaction was carried out at 20~55℃ for 4~8h under inert gas protection, and the solid product was washed and dried to obtain the precursor. The precursor, carbon source, phosphoric acid and dopant are milled to obtain a slurry; The slurry is spray-dried, sintered, and pulverized to obtain a low-temperature lithium iron phosphate material.

2. The preparation method according to claim 1, characterized in that, The mass ratio of the ferrous salt to the α-hydroxyl-containing polycarboxylic acid complexing agent is (0.3~0.5):1; in the step of introducing phosphoric acid solution and lithium source solution, the molar ratio of Li, Fe and P is controlled to be (1.00~1.05):1:(1.00~1.05).

3. The preparation method according to claim 1, characterized in that, The ferrous salt is selected from one or more of ferrous sulfate, ferrous oxalate, or ferrous chloride; the α-hydroxy polycarboxylic acid complexing agent is selected from one or more of citric acid, tartaric acid, or gluconic acid.

4. The preparation method according to claim 1, characterized in that, The lithium source is selected from one or more of lithium hydroxide, lithium carbonate, or lithium dihydrogen phosphate; the carbon source is selected from one or more of glucose, sucrose, starch, or phenolic resin.

5. The preparation method according to claim 1, characterized in that, The dopant is selected from one or more of titanium, vanadium, magnesium, aluminum or manganese sources.

6. The preparation method according to claim 5, characterized in that, The dopants are TiO2 and V2O5, and the mass ratio of TiO2 to V2O5 is (2~8):

1.

7. The preparation method according to claim 1, characterized in that, The mass ratio of the precursor, carbon source, phosphoric acid, and dopant is 100 : (6~10) : (0.4~1.5) : (0.2~0.4); the solvent used in the sand milling process is water.

8. The preparation method according to claim 1, characterized in that, The spray drying temperature is 180~260℃; the sintering temperature is 600~800℃, and the sintering time is 4~16h.

9. The low-temperature lithium iron phosphate material prepared by the preparation method according to any one of claims 1 to 8.

10. A lithium-ion battery, characterized in that, Including the low-temperature lithium iron phosphate material as described in claim 9.

Citation Information

Patent Citations

  • Preparation method of lithium iron phosphate

    CN112938927A

  • Lithium iron phosphate material, preparation method therefor and use thereof

    WO2025138541A1