Modified degradable polyester-based potash fertilizer anti-blocking agent and preparation method thereof
By modifying and degrading polyester-based anti-caking agents for potassium fertilizers, and utilizing amidation reactions and nanomaterials, the problem of potassium fertilizer caking has been solved, achieving efficient anti-caking and resource utilization, and enhancing the commercial value and ease of use of potassium fertilizers.
Patent Information
- Application Number
- CN202511223300.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-29
- Publication Date
- 2025-12-16
AI Technical Summary
Existing potash fertilizers are prone to caking during storage and transportation, and existing anti-caking agents have problems such as environmental impact, high cost, and poor anti-caking effect.
A modified degradable polyester-based potassium fertilizer anti-caking agent is adopted. Through amidation reaction, monoamino cage-type silsesquioxane and amino silicone oil are grafted onto the low viscosity degradable polyester molecular chain, combined with fly ash, graphite phase carbon nitride nanosheets and silicon dioxide, to form an anti-caking agent with steric hindrance and lubrication functions.
It achieves a loose and fluid state for potash fertilizer, with an anti-caking rate of over 90%, reducing costs and improving the convenience of fertilization and market competitiveness.
Smart Images

Figure 4QC5LQTMYPCEBKIFP7MB6DGNRBIP0DWZHXL1LAWY
Abstract
Description
Technical Field
[0001] This invention belongs to the field of anti-caking agent technology, specifically relating to a modified degradable polyester-based potassium fertilizer anti-caking agent and its preparation method. Background Technology
[0002] Potash fertilizer is one of the three essential fertilizers in agricultural production. However, it is highly susceptible to moisture absorption and caking during storage and transportation, causing significant inconvenience and severely impacting its commercial value and application effectiveness. The main causes of caking include capillary hygroscopic absorption between particles, crystal bridging, and particle deformation and adhesion caused by external pressure. Currently, most commercially available anti-caking agents for potash fertilizer use surfactants (such as amines), inorganic inert powders (such as talc and diatomaceous earth), or film-forming substances (such as paraffin wax and polymer emulsions). These methods have several drawbacks: surfactants have limited effectiveness and may affect the soil environment; inert powders require large amounts, resulting in uneven coating, easy detachment, and poor anti-caking durability; while film-forming substances such as synthetic polymers are expensive and mostly derived from non-renewable petroleum resources.
[0003] While polyethylene terephthalate (PET) is widely used in packaging materials such as plastic bottles and films, it also generates a large amount of waste polyester. Current technologies typically involve alcoholysis or hydrolysis of waste polyester to produce low-molecular-weight monomers, which are then repolymerized to generate recycled polyester for reuse. This purification process is complex and costly, posing significant challenges to practical applications. However, there are no reports on a method of directly degrading waste polyester into low-polymerization-degree polyesters and further modifying them into chemical products with specific functions.
[0004] Therefore, developing a potassium fertilizer anti-caking agent with excellent anti-caking effect and the ability to utilize waste polyester resources is of great practical significance and market value. Summary of the Invention
[0005] The purpose of this invention is to provide a modified degradable polyester-based potassium fertilizer anti-caking agent and its preparation method, so as to solve the problems in the background art.
[0006] The objective of this invention can be achieved through the following technical solutions: A modified degradable polyester-based potassium fertilizer anti-caking agent comprises the following raw materials in parts by weight: The mixture comprises 40-50 parts of modified degradable polyester, 25-35 parts of fly ash, 15-25 parts of silica, and 8-12 parts of graphite-phase carbon nitride nanosheets; wherein the modified degradable polyester is prepared by an amidation reaction of a low-viscosity degradable polyester with a degree of polymerization of 10-20 and a mono-amino cage-type silsesquioxane and an amino silicone oil.
[0007] Furthermore, the modified degradable polyester is prepared through the following steps: Step S1: After pretreating the waste polyester sheets, first replace the air with nitrogen and preheat to 180℃ for 10-15 minutes to relax the amorphous regions in the waste polyester and reduce local over-degradation caused by internal stress. Then, under nitrogen protection, heat to 275-285℃ and stir for 20-30 minutes to degrade. Then, cool to 250℃ and vacuum for 10-15 minutes to stabilize the product distribution and remove small molecule compounds. Finally, rapidly cool to room temperature to obtain low-viscosity degraded polyester with a degree of polymerization of 10-20. Step S2: The low-viscosity degradable polyester, mono-amino cage-type silsesquioxane, and amino silicone oil are dissolved in N,N-dimethylformamide and stirred until homogeneous. Then, N,N'-dicyclohexylcarbodiimide is added as a dehydrating agent. The mixture is stirred and reacted at 70-90°C under nitrogen protection for 4-8 hours. After the reaction is completed and cooled to room temperature, the product is poured into methanol to precipitate. The precipitate is collected by filtration, washed three times with methanol, and dried under vacuum to obtain the modified degradable polyester. The reaction process of the low-viscosity degradable polyester with the mono-amino cage-type silsesquioxane is as follows: .
[0008] Furthermore, the pretreatment involves crushing the waste polyester sheets to a particle size ≤1mm and vacuum drying them to a moisture content ≤30ppm, in order to improve heat transfer efficiency and eliminate hydrolysis side reactions.
[0009] Furthermore, the rapid cooling rate is 40-50℃ / min.
[0010] Furthermore, the ratio of the low-viscosity degradable polyester, monoamino cage-type silsesquioxane, amino silicone oil, N,N-dimethylformamide, and N,N'-dicyclohexylcarbodiimide is 20g:4-6g:6-12g:500mL:4.5g. By reacting the amino silicone oil containing two amino groups with the low-viscosity degradable polyester containing terminal carboxyl groups, the molecular weight of the modified degradable polyester can be adjusted to obtain a modified degradable polyester with a molecular weight in the range of 1000-4000.
[0011] Furthermore, the fly ash has a particle size of 20-50μm, which provides the main skeletal support and prevents large-area direct contact between particles, forming physical gaps; the silica has a particle size of 1-5μm, which can fill the gaps between potassium fertilizer particles, providing fine physical isolation and effectively destroying crystal bridges.
[0012] A method for preparing a modified degradable polyester-based potassium fertilizer anti-caking agent includes the following steps: Modified degradable polyester was added to fly ash, silica, and graphitic carbon nitride nanosheets in a high-speed mixer and mixed at 2000-4000 rpm for 30 minutes to obtain a modified degradable polyester-based potassium fertilizer anti-caking agent.
[0013] Beneficial effects: This invention uses waste polyester sheets as raw materials and, through precise temperature gradient control, degrades the waste polyester into a highly reactive, low-viscosity biodegradable polyester, achieving resource recycling of waste polyester. Then, it synergistically modifies the low-viscosity biodegradable polyester using monoamino cage-like silsesquioxanes and amino silicone oils. Through an amidation reaction, the monoamino cage-like silsesquioxanes and amino silicone oils are grafted onto the molecular chain of the low-viscosity biodegradable polyester to obtain a modified biodegradable polyester. When used in potash fertilizer, the rigid nanocage-like structure POSS in the modified biodegradable polyester has significant steric hindrance, increasing the spacing between potash fertilizer particles and preventing close contact and the formation of crystal bridges. Meanwhile, the amino silicone oil provides a lubricating layer between potash fertilizer particles, making the particles easier to slide under pressure and preventing the formation of hard lumps. In addition to the modified degradable polyester that has both steric hindrance and lubrication functions, the anti-caking agent of this invention also makes full use of the supporting skeleton effect of fly ash, the void-filling effect of silica, and the interpenetrating isolation effect of graphite phase carbon nitride nanosheets. This makes the resulting anti-caking agent inexpensive and effectively prevents potassium fertilizer from caking during storage and transportation, maintaining its loose and fluid state. The anti-caking rate is greater than 90%, which greatly facilitates farmers' use and mechanized fertilization, and enhances the market competitiveness of the end product. Detailed Implementation
[0014] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0015] Example 1 This embodiment provides a modified degradable polyester, which is prepared through the following steps: Step S1: Crush 100g of waste polyester flakes to a particle size ≤1mm and vacuum dry to a moisture content ≤30ppm. Then, replace the air with nitrogen and preheat to 180℃ for 10min. Then, under nitrogen protection, heat to 275℃ and stir to degrade for 20min. Then, cool to 250℃ and vacuum for 10min. Finally, rapidly cool to room temperature at a cooling rate of 40℃ / min to obtain a low viscosity degraded polyester with a degree of polymerization of 20. Step S2: 20g of low-viscosity degradable polyester, 4g of monoamino cage-type silsesquioxane and 6g of amino silicone oil were dissolved in 500mL of N,N-dimethylformamide and stirred until homogeneous. Then, 4.5g of N,N'-dicyclohexylcarbodiimide was added. The mixture was stirred and reacted at 70℃ under nitrogen protection for 8h. After the reaction was completed and cooled to room temperature, the product was poured into a large amount of methanol to precipitate. The precipitate was collected by filtration, washed three times with methanol, and dried under vacuum at 60℃ for 24h to obtain a light yellow waxy solid of modified degradable polyester.
[0016] Example 2 This embodiment provides a modified degradable polyester, which is prepared through the following steps: Step S1: Crush 100g of waste polyester flakes to a particle size ≤1mm and vacuum dry to a moisture content ≤30ppm. Then, replace the air with nitrogen and preheat to 180℃ for 12min. Then, under nitrogen protection, heat to 280℃ and stir to degrade for 25min. Then, cool to 250℃ and vacuum for 13min. Finally, rapidly cool to room temperature at a cooling rate of 45℃ / min to obtain a low viscosity degraded polyester with a degree of polymerization of 15. Step S2: 20g of low-viscosity degradable polyester, 5g of monoamino cage-type silsesquioxane and 9g of amino silicone oil were dissolved in 500mL of N,N-dimethylformamide and stirred until homogeneous. Then, 4.5g of N,N'-dicyclohexylcarbodiimide was added. The mixture was stirred and reacted at 80℃ under nitrogen protection for 6h. After the reaction was completed and cooled to room temperature, the product was poured into a large amount of methanol to precipitate. The precipitate was collected by filtration, washed three times with methanol, and dried under vacuum at 60℃ for 24h to obtain a light yellow waxy solid of modified degradable polyester.
[0017] Example 3 This embodiment provides a modified degradable polyester, which is prepared through the following steps: Step S1: Crush 100g of waste polyester flakes to a particle size ≤1mm and vacuum dry to a moisture content ≤30ppm. Then, replace the air with nitrogen and preheat to 180℃ for 15min. Then, under nitrogen protection, heat to 285℃ and stir to degrade for 30min. Then, cool to 250℃ and vacuum for 15min. Finally, rapidly cool to room temperature at a cooling rate of 50℃ / min to obtain a low viscosity degraded polyester with a degree of polymerization of 10. Step S2: 20g of low-viscosity degradable polyester, 6g of monoamino cage-type silsesquioxane and 12g of amino silicone oil were dissolved in 500mL of N,N-dimethylformamide and stirred until homogeneous. Then, 4.5g of N,N'-dicyclohexylcarbodiimide was added. The mixture was stirred and reacted at 90℃ under nitrogen protection for 4h. After the reaction was completed and cooled to room temperature, the product was poured into a large amount of methanol to precipitate. The precipitate was collected by filtration, washed three times with methanol, and dried under vacuum at 60℃ for 24h to obtain a light yellow waxy solid of modified degradable polyester.
[0018] Comparative Example 1 The difference between this comparative example and Example 3 is that in step S2, 6g of monoamino cage-type silsesquioxane was replaced with an equal amount of amino silicone oil, while the other raw materials and steps are the same.
[0019] Comparative Example 2 The difference between this comparative example and Example 3 is that in step S2, 12g of amino silicone oil is replaced with an equal amount of monoamino cage-type silsesquioxane, while the other raw materials and steps are the same.
[0020] Example 4 This embodiment provides a modified degradable polyester-based potassium fertilizer anti-caking agent, comprising the following raw materials in parts by weight: Example 1 prepared 40 parts of modified degradable polyester, 25 parts of fly ash with a particle size of 50 μm, 15 parts of silica with a particle size of 5 μm, and 8 parts of graphite phase carbon nitride nanosheets; the preparation included the following steps: the above-mentioned parts by weight of modified degradable polyester, fly ash, silica, and graphite phase carbon nitride nanosheets were added to a high-speed mixer and mixed at 2000 rpm for 30 min to obtain a modified degradable polyester-based potassium fertilizer anti-caking agent.
[0021] Example 5 This embodiment provides a modified degradable polyester-based potassium fertilizer anti-caking agent, comprising the following raw materials in parts by weight: Example 2 prepared 45 parts of modified degradable polyester, 30 parts of fly ash with a particle size of 35 μm, 20 parts of silica with a particle size of 3 μm, and 10 parts of graphite phase carbon nitride nanosheets; the preparation included the following steps: the above-mentioned parts by weight of modified degradable polyester, fly ash, silica, and graphite phase carbon nitride nanosheets were added to a high-speed mixer and mixed at 3000 rpm for 30 min to obtain a modified degradable polyester-based potassium fertilizer anti-caking agent.
[0022] Example 6 This embodiment provides a modified degradable polyester-based potassium fertilizer anti-caking agent, comprising the following raw materials in parts by weight: Example 3 prepared 50 parts of modified degradable polyester, 35 parts of fly ash with a particle size of 20 μm, 25 parts of silica with a particle size of 1 μm, and 12 parts of graphite phase carbon nitride nanosheets; the preparation included the following steps: the above-mentioned parts by weight of modified degradable polyester, fly ash, silica, and graphite phase carbon nitride nanosheets were added to a high-speed mixer and mixed at 4000 rpm for 30 min to obtain a modified degradable polyester-based potassium fertilizer anti-caking agent.
[0023] Comparative Example 3 The difference between this comparative example and Example 6 is that a commercially available fatty amine anti-caking agent is used to replace the modified degradable polyester prepared in Example 3 in an equal amount, while the other raw materials and steps are the same.
[0024] Comparative Example 4 The difference between this comparative example and Example 6 is that the modified degradable polyester prepared in Comparative Example 1 is used to replace the modified degradable polyester prepared in Example 3 in an equal amount, while the other raw materials and steps are the same.
[0025] Comparative Example 5 The difference between this comparative example and Example 6 is that the modified degradable polyester prepared in Comparative Example 2 is used to replace the modified degradable polyester prepared in Example 3 in an equal amount, while the other raw materials and steps are the same.
[0026] Anti-caking performance tests were conducted on Examples 4-6 and Comparative Examples 3-5. The test method was as follows: potassium chloride fertilizer was added to a coating machine and heated to 60°C. Then, 1 wt% of potassium fertilizer anti-caking agent was added to the potassium chloride fertilizer, and the coating was carried out for 10 minutes. After discharge, potassium chloride fertilizer samples containing anti-caking agent were obtained. 100g of the sample was packaged in a plastic self-sealing bag and laid flat on the test platform. A 10kg steel plate was placed horizontally on top of the packaging bag, and then a 50kg weight was added on top of the steel plate. After 7 days, the weight and steel plate were removed, and the potassium sulfate fertilizer sample was poured out of the packaging bag onto a 4-mesh sieve. After sieving, the weight of the sieve residue was weighed. The anti-caking rate was calculated by dividing the weight of the sieve residue by 100. The higher the anti-caking rate, the better. The results are shown in Table 1. Table 1 As can be seen from the data in Table 1, compared with commercially available fatty amine anti-caking agents, the anti-caking agents prepared in Examples 4-6 of this invention have a higher anti-caking rate when used in potassium chloride fertilizer, showing a more superior anti-caking effect. As can be seen from the data in Comparative Examples 4 and 5, the synergistic modification of monoamino cage-type silsesquioxane and amino silicone oil can enable the modified degradable polyester to achieve better performance in anti-caking agents.
[0027] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0028] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A modified degradable polyester-based potassium fertilizer anti-caking agent, characterized in that, Including the following parts by weight of raw materials: The mixture comprises 40-50 parts of modified degradable polyester, 25-35 parts of fly ash, 15-25 parts of silica, and 8-12 parts of graphite-phase carbon nitride nanosheets; wherein the modified degradable polyester is prepared by an amidation reaction of a low-viscosity degradable polyester with a degree of polymerization of 10-20 and a mono-amino cage-type silsesquioxane and an amino silicone oil.
2. The modified degradable polyester-based potassium fertilizer anti-caking agent according to claim 1, characterized in that, The modified degradable polyester is prepared by the following steps: Step S1: After pretreating the waste polyester sheets, first replace the air with nitrogen and preheat to 180℃ for 10-15 minutes, then heat to 275-285℃ under nitrogen protection and stir to degrade for 20-30 minutes, then cool to 250℃ and vacuum for 10-15 minutes, and finally rapidly cool to room temperature to obtain a low-viscosity degraded polyester with a degree of polymerization of 10-20. Step S2: The low-viscosity degradable polyester, monoamino cage-type silsesquioxane and amino silicone oil are dissolved in N,N-dimethylformamide and stirred until uniform. Then N,N'-dicyclohexylcarbodiimide is added and stirred at 70-90℃ for 4-8 hours under nitrogen protection. After cooling to room temperature, the product is poured into methanol to precipitate. After filtration, washing and vacuum drying, the modified degradable polyester is obtained.
3. The modified degradable polyester-based potassium fertilizer anti-caking agent according to claim 2, characterized in that, The pretreatment involves crushing waste polyester sheets to a particle size ≤1mm and vacuum drying them to a moisture content ≤30ppm.
4. The modified degradable polyester-based potassium fertilizer anti-caking agent according to claim 2, characterized in that, The rapid cooling rate is 40-50℃ / min.
5. The modified degradable polyester-based potassium fertilizer anti-caking agent according to claim 2, characterized in that, The ratio of the low-viscosity degradable polyester, monoamino cage-type silsesquioxane, amino silicone oil, N,N-dimethylformamide and N,N'-dicyclohexylcarbodiimide is 20g:4-6g:6-12g:500mL:4.5g.
6. The modified degradable polyester-based potassium fertilizer anti-caking agent according to claim 1, characterized in that, The fly ash has a particle size of 20-50 μm; the silica has a particle size of 1-5 μm.
7. The preparation method of the modified degradable polyester-based potassium fertilizer anti-caking agent according to claim 1, characterized in that, Includes the following steps: Modified degradable polyester was added to fly ash, silica, and graphitic carbon nitride nanosheets in a high-speed mixer and mixed at 2000-4000 rpm for 30 minutes to obtain a modified degradable polyester-based potassium fertilizer anti-caking agent.