A hollow fiber ultrafiltration membrane and its preparation method
By constructing a loose functional layer during the molding process of hollow fiber ultrafiltration membrane using a one-step interfacial polymerization technique, the problems of wide pore size distribution and low separation accuracy of hollow fiber ultrafiltration membrane in the field of high-precision separation are solved, achieving high throughput and effective desalination, simplifying the production process and improving operability.
Patent Information
- Application Number
- CN202511645522.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-11-11
AI Technical Summary
Existing hollow fiber ultrafiltration membranes suffer from problems such as wide pore size distribution, low separation accuracy, and no salt rejection rate in the field of high-precision separation. Furthermore, the existing composite membrane preparation process is complex and costly, making it difficult to simultaneously improve the desalination rate and maintain the flux.
A one-step interfacial polymerization technique is used to construct a loose functional layer in situ during the hollow fiber ultrafiltration membrane molding process, simplifying the production process. Through small-pore functional design, it can effectively retain divalent and high-valent salts and heavy metal salts while maintaining a high flux.
It achieves effective desalination of hollow fiber ultrafiltration membranes while maintaining high flux, solving the problem of improving desalination rate and maintaining flux, simplifying the production process and improving operability.
Smart Images

Figure CN121177985B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water treatment technology, and in particular to a hollow fiber ultrafiltration membrane and its preparation method. Background Technology
[0002] With the increasing severity of water scarcity and pollution, human survival and health are seriously threatened. Therefore, the protection of the water environment has received growing attention from human society, and various water treatment technologies have gradually developed. Among them, membrane separation technology, as a highly efficient, energy-saving, and environmentally friendly water treatment technology, has been increasingly widely applied.
[0003] Ultrafiltration membranes, as an important membrane separation material, possess advantages such as high separation efficiency, low operating pressure, and high flux, and have been widely used in drinking water purification, wastewater treatment, food and pharmaceutical, and chemical industries. Currently, common membrane types include flat sheet membranes, spiral wound membranes, tubular membranes, and hollow fiber membranes. Compared to flat sheet, spiral wound, and tubular membranes, hollow fiber membranes have become one of the main forms of ultrafiltration membranes due to their large specific surface area, high packing density, high flux, and simple and versatile membrane module maintenance and cleaning.
[0004] However, traditional hollow fiber ultrafiltration membranes suffer from problems such as wide pore size distribution, low separation accuracy, and virtually no salt rejection rate, limiting their application in specialized separation fields such as high-precision separation of salt-containing or heavy metal-containing saline solutions. To address this issue, researchers have developed various composite membranes with desalination capabilities, such as combining nanofiltration or reverse osmosis membranes with ultrafiltration membranes, or introducing functional groups onto the surface of ultrafiltration membranes through chemical grafting. However, the fabrication processes for these composite membranes are complex and costly, the modified layers are prone to detachment, and flux attenuation is significant.
[0005] In recent years, functionalized ultrafiltration membranes have gradually become a research hotspot. By introducing specific functional groups or functional layers on or inside the membrane surface, membrane materials can be endowed with special properties, such as hydrophilicity, antibacterial properties, antifouling properties, and desalination properties, thereby improving the separation performance and stability of the membrane. However, existing technologies generally suffer from the problem of "difficulty in simultaneously improving desalination rate and maintaining flux," and their processes are complex and lack operability. Summary of the Invention
[0006] To address the technical challenge of simultaneously improving desalination efficiency and maintaining flux in existing ultrafiltration membranes, this invention provides a method for preparing a hollow fiber ultrafiltration membrane. This invention also provides the hollow fiber ultrafiltration membrane prepared by the above method. This invention simplifies the production process through a one-step interfacial polymerization technique; the resulting hollow fiber ultrafiltration membrane, as a small-pore functionalized hollow fiber ultrafiltration membrane, not only has high flux but also effectively desalinates.
[0007] A method for preparing a hollow fiber ultrafiltration membrane includes the following steps: S1. Preparation of spinning solution: Mix polymer resin, pore-forming agent, spinning solution auxiliary agent, functional modifier A, and first solvent to obtain spinning solution; the spinning solution ratio is 14-24wt% polymer resin, 2-16wt% pore-forming agent, 0.1-5wt% spinning solution auxiliary agent, 0.05-0.8wt% functional modifier A, and the balance is the first solvent; S2. Preparation of core solution: Mix functional modifier B, core solution additive, acid binder, second solvent and deionized water to obtain core solution; the core solution ratio is functional modifier B 0.5-10wt%, core solution additive 0.1-2wt%, acid binder 0.1-3wt%, second solvent 0-30wt%, and the balance is deionized water; S3. Filter the spinning solution, defoam it, and keep it at a constant temperature of 35-65℃; Keep the core fluid at a constant temperature of 30-60℃; S4. Take the spinning solution and core solution from step S3 and prepare the nascent membrane by wet spinning. S5. The primary membrane is post-processed to obtain a hollow fiber ultrafiltration membrane; There is no requirement for the order of steps S1 and S2.
[0008] Preferably, in step S1, the polymer resin, pore-forming agent, spinning solution aid, functional modifier A, and the first solvent are stirred at 70-90°C for 6-18 hours to obtain a uniformly mixed spinning solution. In step S2, the functional modifier B, core fluid additive, acid binder, second solvent, and deionized water are stirred at 30-60℃ for 0.5-3h to obtain a uniformly mixed core fluid.
[0009] Preferably, in step S3, the spinning solution is filtered using a 300-800 mesh filter and then vacuum degassed for 2-12 hours.
[0010] Preferably, in step S4, wet spinning specifically involves: extruding the spinning solution through an annular spinneret, with the core solution at the center; after extrusion, the resulting membrane fibers are subjected to an air bath, and then fall into a coagulation bath at 40-65°C to form a nascent membrane, which is then collected to obtain the primary membrane.
[0011] Preferably, in step S5, the post-treatment specifically involves rinsing the nascent membrane with clean water for 6-18 hours, followed by a shaping treatment and drying at 20-60°C to obtain the final product.
[0012] Preferably, the polymer resin is at least one selected from polysulfone, polyethersulfone, sulfonated polysulfone, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, and polylactic acid; The pore-forming agent is at least one of polyvinylpyrrolidone, polyethylene glycol, and polyvinyl alcohol; The spinning solution auxiliaries are at least one of inorganic salts and C1-C3 alcohols; Functional modifier A is at least one of pyromellitic phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, phthaloyl chloride, and adipyl chloride; The first solvent is at least one of N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and tetrahydrofuran.
[0013] Preferably, polyvinylpyrrolidone is at least one of K30, K60, K70, K80, and K90; The molecular weight of polyethylene glycol is 200-20000; more preferably, the molecular weight of polyethylene glycol is 200-2000. The molecular weight of polyvinyl alcohol is 10,000-100,000; The inorganic salt is at least one of LiCl, ZnCl2, CaCl2, MgCl2, and FeCl3; The C1-C3 alcohols are at least one of methanol, ethanol, ethylene glycol, propanol, and isopropanol.
[0014] Preferably, the functional modifier B is a combination of small molecule polyamines and large molecule polyamines; the small molecule polyamine is at least one of piperazine, 2,2'-dimethylpiperazine, m-phenylenediamine, p-phenylenediamine, mesentyltriamine, diethylenetriamine, polypeptide, and amino acid; the large molecule polyamine is at least one of polyethyleneimine, polyamide-amine (PAMAM), polyacrylamide, and polyamine. The core fluid additive is at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium camphor sulfonate, Tween, and hydrogenated castor oil polyoxyethylene ether; The acid-binding agent is at least one of sodium phosphate, disodium hydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium hydroxide, potassium phosphate, dipotassium hydrogen phosphate, potassium carbonate, and potassium bicarbonate. The second solvent is at least one of N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and dimethyl sulfoxide.
[0015] Hollow fiber ultrafiltration membranes prepared by any of the above methods.
[0016] Commercially available ultrafiltration membranes are ineffective at retaining ions and have virtually no effect on inorganic salts, thus offering little to no desalination performance. Currently, most composite membranes require multiple steps in their preparation, including base membrane fabrication, interfacial polymerization, and post-treatment, making the process complex. Furthermore, enhancing the desalination performance of the membrane can drastically reduce its water flux. Some existing hollow fiber ultrafiltration membranes improve fiber strength through material blending modification. However, due to differences in glass transition temperatures, the delayed phase separation times of different materials during phase transition vary, resulting in poor blending modification effects. Furthermore, some blending modifications introduce polymers with rigid segments, significantly shortening their lifespan in practical applications.
[0017] Compared with existing technologies, this invention utilizes a one-step interfacial polymerization technique to construct a loose functional layer in situ during the hollow fiber ultrafiltration membrane forming process. This integrates interfacial polymerization into the spinning process, simplifying the production flow, improving membrane fabrication efficiency, and enhancing the operability and controllability of continuous production. Furthermore, the established loose functional layer enables the ultrafiltration membrane to effectively retain divalent and high-valent salts, as well as heavy metal salts, while maintaining a high flux. The hollow fiber ultrafiltration membrane prepared in this application, as a small-pore functionalized hollow fiber ultrafiltration membrane, not only possesses high flux but also effectively desalinates.
[0018] The preferred functional modifier B is a combination of small-molecule and large-molecule polyamines. Due to the difference in reaction rates between large-molecule and small-molecule polyamines and acyl chlorides, there is also competition for reaction priority. By controlling the ratio and concentration in the core liquid, a synergistic reaction effect can be achieved, making the interfacial polymerization reaction more moderate; forming a "loose-dense" gradient structure, with a gradient distribution of crosslinking density on the functional layer surface, balancing the rejection rate and flux. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 A cross-sectional scanning electron microscope image of the hollow fiber ultrafiltration membrane prepared in Example 1 of the present invention. Detailed Implementation
[0021] To enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0022] Example 1 The selected reagents and their preparation methods are as follows:
[0023] The preparation steps are as follows: S1. Preparation of spinning solution: Polysulfone, polyvinylpyrrolidone K30, polyvinyl alcohol 1788, LiCl, methanol, pyromellitic methyl chloride and dimethylacetamide are added to the reaction vessel and mixed and stirred until completely dissolved. Stirred at 70°C for 15 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Add piperazine, polyethyleneimine, sodium dodecyl sulfonate, Tween-80, sodium phosphate, sodium bicarbonate, dimethylacetamide and deionized water to the core solution tank and stir at 35°C for 1.5 hours to obtain a uniformly mixed core solution. S3. Filter the spinning solution with a 300-mesh filter to remove impurities, then perform vacuum degassing for 4 hours, while keeping the spinning solution temperature constant at 35°C. Keep the core fluid at a constant temperature of 30°C; S4. The spinning solution pretreated in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 40°C coagulation bath to form a nascent membrane, which is then collected by a take-up wheel. S5. Rinse the nascent membrane with clean water for 7 hours, then perform a shaping treatment and air dry at 20°C to obtain a hollow fiber ultrafiltration membrane.
[0024] Cross-sectional scanning electron microscope image of the hollow fiber ultrafiltration membrane prepared in Example 1 is shown below. Figure 1 As shown.
[0025] Example 2 The selected reagents and their preparation methods are as follows:
[0026] The preparation steps are as follows: S1. Preparation of spinning solution: Add polyethersulfone, polyvinylpyrrolidone K60, polyethylene glycol 200, ZnCl2, ethylene glycol, adipic acid chloride and dimethylformamide into the reaction vessel and mix and stir until completely dissolved. Stir at 90°C for 7 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Add 2,2'-dimethylpiperazine, m-phenylenediamine, polyamidoamine, sodium dodecylbenzenesulfonate, sodium carbonate, dimethylformamide and deionized water to the core solution tank and stir at 45°C for 2.5 hours to obtain a uniformly mixed core solution. S3. Filter the spinning solution with a 400-mesh filter to remove impurities, and then perform vacuum degassing for 11 hours while keeping the spinning solution temperature constant at 60°C. The core fluid was kept at a constant temperature of 55°C. S4. The spinning solution pretreated in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 60°C coagulation bath to form a nascent membrane, which is then collected by a take-up wheel. S5. Rinse the nascent membrane with clean water for 17 hours, then perform a shaping treatment and dry at 50°C to obtain a hollow fiber ultrafiltration membrane.
[0027] Example 3 The selected reagents and their preparation methods are as follows:
[0028] The preparation steps are as follows: S1. Preparation of spinning solution: Polyvinylidene fluoride, polyvinylpyrrolidone K30, polyvinylpyrrolidone K90, LiCl, FeCl3, pyromellitic methyl chloride and dimethylacetamide are added to the reaction vessel and mixed and stirred until completely dissolved. Stirred at 80°C for 12 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Add piperazine, m-phenylenediamine, polyethyleneimine, polyacrylamide, sodium camphor sulfonate, hydrogenated castor oil polyoxyethylene ether, disodium hydrogen phosphate, sodium hydroxide, and deionized water to the core solution tank and stir at 60°C for 0.5 h to obtain a uniformly mixed core solution. S3. Filter the spinning solution with an 800-mesh filter to remove impurities, and then perform vacuum degassing for 8 hours while keeping the spinning solution temperature constant at 45°C. Keep the core fluid at a constant temperature of 45℃; S4. The spinning solution after the pretreatment in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 45°C coagulation bath to form a membrane. The membrane is collected by a take-up wheel to obtain the nascent membrane. S5. Rinse the nascent membrane with clean water for 12 hours, then perform a shaping treatment and dry at 45°C to obtain a hollow fiber ultrafiltration membrane.
[0029] Example 4 The selected reagents and their preparation methods are as follows:
[0030] The preparation steps are as follows: S1. Preparation of spinning solution: Polysulfone, polyvinylpyrrolidone K30, polyethylene glycol 800, polyvinyl alcohol 1788, ethanol, pyromellitic methyl methacrylate chloride, adipyl chloride and dimethylacetamide are added to the reaction vessel and mixed and stirred until completely dissolved. Stirred at 75°C for 13 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Diethylenetriamine, polyamine, polyethyleneimine, sodium camphor sulfonate, sodium dodecyl sulfonate, hydrogenated castor oil polyoxyethylene ether, sodium phosphate, sodium hydroxide, potassium phosphate, dimethylacetamide and deionized water are added to the core solution tank and stirred at 50°C for 1.5 hours to obtain a uniformly mixed core solution. S3. Filter the spinning solution with a 600-mesh filter to remove impurities, and then perform vacuum degassing for 10 hours while keeping the spinning solution temperature constant at 50°C. Keep the core fluid at a constant temperature of 40℃; S4. The spinning solution pretreated in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 55°C coagulation bath to form a nascent membrane, which is then collected by a take-up wheel. S5. Rinse the nascent membrane with clean water for 11 hours, then perform a shaping treatment and dry at 35°C to obtain a hollow fiber ultrafiltration membrane.
[0031] Example 5 The selected reagents and their preparation methods are as follows:
[0032] The preparation steps are as follows: S1. Preparation of spinning solution: Polysulfone, polyvinylpyrrolidone K70, polyethylene glycol 1000, MgCl2, isopropanol, trimesoyl chloride, isophthaloyl chloride and N-methylpyrrolidone are added to the reaction vessel and mixed and stirred until completely dissolved. Stirred at 85°C for 6 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Add piperazine, arginine, polyethyleneimine, sodium dodecylbenzenesulfonate, sodium camphor sulfonate, potassium hydroxide, potassium bicarbonate, N-methylpyrrolidone and deionized water to the core solution tank and stir at 55°C for 1 hour to obtain a uniformly mixed core solution. S3. Filter the spinning solution with a 600-mesh filter to remove impurities, and then perform vacuum degassing for 11 hours while keeping the spinning solution temperature constant at 55°C. Keep the core fluid at a constant temperature of 50°C; S4. The spinning solution pretreated in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 65°C coagulation bath to form a membrane. The membrane is collected by a take-up wheel to obtain the nascent membrane. S5. Rinse the nascent membrane with clean water for 14 hours, then perform a shaping treatment and dry at 40°C to obtain a hollow fiber ultrafiltration membrane.
[0033] Comparative Example 1 The selected reagents and their preparation methods are as follows:
[0034] The preparation steps are as follows: S1. Preparation of spinning solution: Polysulfone, polyvinylpyrrolidone K30, LiCl, methanol, and dimethylacetamide are added to the reaction vessel and mixed and stirred until completely dissolved. Stirred at 70°C for 15 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Sodium dodecyl sulfonate, Tween-80, dimethylacetamide and deionized water are added to the core solution tank and stirred at 35°C for 1.5 hours to obtain a uniformly mixed core solution. S3. Filter the spinning solution with an 800-mesh filter to remove impurities, and then perform vacuum degassing for 7 hours while keeping the spinning solution temperature constant at 40°C. Keep the core fluid at a constant temperature of 40℃; S4. The spinning solution pretreated in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 45°C coagulation bath to form a nascent membrane, which is then collected by a take-up wheel.
[0035] S5. Rinse the nascent membrane with clean water for 10 hours, then perform a shaping treatment and dry at 45°C to obtain a conventional hollow fiber ultrafiltration membrane.
[0036] Comparative Example 2 The selected reagents and their preparation methods are as follows:
[0037] The preparation steps are as follows: S1. Preparation of spinning solution: Add polyethersulfone, polyvinylpyrrolidone K60, polyethylene glycol 200, ZnCl2, ethylene glycol, and dimethylformamide into the reaction vessel and mix and stir until completely dissolved. Stir at 90°C for 7 hours to obtain a uniformly mixed spinning solution. S2. Preparation of core solution: Sodium dodecylbenzenesulfonate, dimethylformamide and deionized water are added to the core solution tank and stirred at 45°C for 2.5 hours to obtain a uniformly mixed core solution. S3. Filter the spinning solution with a 400-mesh filter to remove impurities, and then perform vacuum degassing for 11 hours while keeping the spinning solution temperature constant at 60°C. The core fluid was kept at a constant temperature of 55°C. S4. The spinning solution pretreated in step S3 is extruded through an annular spinneret, with the core liquid at the center. After extrusion, the membrane filaments pass through an air bath and then fall into a 60°C coagulation bath to form a nascent membrane, which is then collected by a take-up wheel.
[0038] S5. Rinse the nascent membrane with clean water for 17 hours, then perform a shaping treatment and dry at 50°C to obtain a conventional hollow fiber ultrafiltration membrane.
[0039] Test case In this experiment, a self-made hollow fiber filtration performance evaluation device was used to test the flux and separation performance of the hollow fiber ultrafiltration membranes prepared in Examples 1-5, the conventional hollow fiber ultrafiltration membranes prepared in Comparative Examples 1-2, and a commercially available polysulfone hollow fiber ultrafiltration membrane.
[0040] The test methods for flux and the rejection rate of inorganic salts (divalent salts, high-valent salts, and heavy metal salts) include: setting the operating pressure to 2 bar, running stably at 25°C for 10 minutes, taking a certain volume of filtrate, and recording the sampling time. The membrane flux Q is calculated using Formula 1; the rejection rate of inorganic salts (divalent salts, high-valent salts, and heavy metal salts) is calculated using Formula 2.
[0041] The flux test used deionized water as the spiking solution, while the simulated spiking solutions for the inorganic salt (divalent salt, high-valent salt, heavy metal salt) rejection rate test were 500 mg / L MgSO4, 500 mg / L FeCl3, and 50 mg / L Pb(NO3)2 solutions. Formulas 1 and 2 are shown below: Formula 1: Q=V / (A*t) In Formula 1, Q is the flux (L·m -2 ·h -1 V is the volume of permeate collected within time t (L), and A is the effective filtration area of the membrane (m²). 2 ), where t is the permeate collection time (h).
[0042] R = (1 - C1 / C2) * 100% (Formula 2) In Formula 2, R is the desalination rate (%), C1 is the solute concentration on the product water side (mg / L), and C2 is the solute concentration on the feed water side (mg / L).
[0043] The results of flux and rejection tests are shown in the table below:
[0044] The test results show that although the flux of Comparative Example 1, Comparative Example 2, and a commercially available polysulfone hollow fiber ultrafiltration membrane can reach over 200, their rejection rates for MgSO4, FeCl3, and Pb(NO3)2 are very low, less than 10.0%. In contrast, the hollow fiber ultrafiltration membranes of Examples 1-5 of this application can maintain a flux of around 100, while also exhibiting high rejection rates for various salts. This balance between flux and rejection rate solves the problem in existing technologies where it is difficult to simultaneously improve desalination rate and maintain flux.
[0045] The above description is merely an embodiment of the present invention. It should be noted that those skilled in the art can make improvements without departing from the inventive concept of the present invention, but these improvements all fall within the protection scope of the present invention.
Claims
1. A method for preparing a hollow fiber ultrafiltration membrane, characterized in that, Includes the following steps: S1. Preparation of spinning solution: Mix polymer resin, pore-forming agent, spinning solution auxiliary agent, functional modifier A, and first solvent to obtain spinning solution; the spinning solution ratio is 14-24wt% polymer resin, 2-16wt% pore-forming agent, 0.1-5wt% spinning solution auxiliary agent, 0.05-0.8wt% functional modifier A, and the balance is the first solvent; S2. Preparation of the core solution: Mix functional modifier B, core solution additive, acid-binding agent, second solvent, and deionized water to obtain the core solution; the core solution ratio is: functional modifier B 0.5-10wt%, core solution additive 0.1-2wt%, acid-binding agent 0.1-3wt%, second solvent 0-30wt%, and the balance is deionized water; wherein, Functional modifier B is a combination of small-molecule polyamines and large-molecule polyamines; the small-molecule polyamine is at least one of piperazine, 2,2'-dimethylpiperazine, m-phenylenediamine, p-phenylenediamine, mesentyltriamine, diethylenetriamine, polypeptide, and amino acid; the large-molecule polyamine is at least one of polyethyleneimine, polyamide-amine, polyacrylamide, and polyamine. The core fluid additive is at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium camphor sulfonate, Tween, and hydrogenated castor oil polyoxyethylene ether; The acid-binding agent is at least one of sodium phosphate, disodium hydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium hydroxide, potassium phosphate, dipotassium hydrogen phosphate, potassium carbonate, and potassium bicarbonate. S3. Filter the spinning solution, defoam it, and keep it at a constant temperature of 35-65℃; Keep the core fluid at a constant temperature of 30-60℃; S4. Take the spinning solution and core solution from step S3 and prepare the nascent membrane by wet spinning. S5. The primary membrane is post-processed to obtain a hollow fiber ultrafiltration membrane; There is no requirement for the order of steps S1 and S2.
2. The preparation method according to claim 1, characterized in that, In step S1, the polymer resin, pore-forming agent, spinning solution auxiliaries, functional modifier A, and the first solvent are stirred at 70-90°C for 6-18 hours to obtain a uniformly mixed spinning solution. In step S2, the functional modifier B, core fluid additive, acid binder, second solvent, and deionized water are stirred at 30-60℃ for 0.5-3h to obtain a uniformly mixed core fluid.
3. The preparation method according to claim 1, characterized in that, In step S3, the spinning solution is filtered using a 300-800 mesh filter and then vacuum degassed for 2-12 hours.
4. The preparation method according to claim 1, characterized in that, In step S4, wet spinning specifically involves: extruding the spinning solution through an annular spinneret, with the core solution at the center; after extrusion, the resulting membrane fibers are subjected to an air bath, and then fall into a coagulation bath at 40-65℃ to form a nascent membrane, which is then collected to obtain the primary membrane.
5. The preparation method according to claim 1, characterized in that, In step S5, the post-processing is as follows: the nascent membrane is rinsed with clean water for 6-18 hours, then shaped and dried at 20-60℃ to obtain the final product.
6. The preparation method according to any one of claims 1-5, characterized in that, The polymer resin is at least one of polysulfone, polyethersulfone, sulfonated polysulfone, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, and polylactic acid; The pore-forming agent is at least one of polyvinylpyrrolidone, polyethylene glycol, and polyvinyl alcohol; The spinning solution auxiliaries are at least one of inorganic salts and C1-C3 alcohols; Functional modifier A is at least one of pyromellitic phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, phthaloyl chloride, and adipyl chloride; The first solvent is at least one of N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and tetrahydrofuran.
7. The preparation method according to claim 6, characterized in that, Polyvinylpyrrolidone is at least one of K30, K60, K70, K80, and K90; The molecular weight of polyethylene glycol is 200-20000; The molecular weight of polyvinyl alcohol is 10,000-100,000; The inorganic salt is at least one of LiCl, ZnCl2, CaCl2, MgCl2, and FeCl3; The C1-C3 alcohols are at least one of methanol, ethanol, ethylene glycol, propanol, and isopropanol.
8. The preparation method according to any one of claims 1-5, characterized in that, The second solvent is at least one of N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and dimethyl sulfoxide.
9. The hollow fiber ultrafiltration membrane prepared by any one of claims 1-8.
Citation Information
Patent Citations
Method for preparing polyamide hollow-fiber nano-osmosis membrane
CN110523281A
Preparation method of composite membrane
CN118384719A