Low-moisture ceramic slurry and low-moisture ceramic diaphragm

By combining hydrophobic modified ceramic materials and high-temperature resistant binders, the problem of easy moisture absorption in alumina ceramic separators is solved, achieving high heat resistance and high ionic conductivity in low-moisture ceramic slurry and separators, thereby improving the safety and performance of lithium batteries.

CN121182291APending Publication Date: 2025-12-23CHONGQING HOUSHENG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511353445.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-22
Publication Date
2025-12-23

AI Technical Summary

Technical Problem

Existing alumina ceramic separators are prone to absorbing moisture in lithium batteries, leading to increased moisture content, which affects the stability of the slurry and the performance of the separator, and in turn causes safety problems.

Method used

Hydrophobic modified ceramic materials and high-temperature resistant binders are used. Alumina is modified by hydrophobic silane coupling agent and high-temperature resistant binder is introduced to form a hydrophobic barrier and chemical bridging, which reduces water adsorption and enhances the bonding strength and high-temperature stability of the ceramic layer.

Benefits of technology

It significantly reduces the moisture content of ceramic slurry and separator, improves high-temperature resistance and ionic conductivity, enhances slurry uniformity and coating performance, prevents agglomeration, and strengthens battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses low-moisture ceramic slurry and a low-moisture ceramic diaphragm, and belongs to the technical field of battery diaphragms. The low-moisture ceramic slurry is prepared from the following components in parts by mass: 25 to 55 parts of a hydrophobic modified ceramic material, 1 to 10 parts of a thickening agent, 8 to 20 parts of a high-temperature-resistant binder, 0.05 to 0.1 part of a wetting agent, 1 to 5 parts of a dispersing agent and 25 to 50 parts of a solvent, the solvent is ultrapure water; the hydrophobic modified ceramic material is obtained by modifying aluminum oxide with a hydrophobic silane coupling agent, and the hydrophobic silane coupling agent is obtained by reacting 4-allyl-N, N-dimethylaniline with 3-mercaptopropyltrimethoxysilane, and the hydrophobic silane coupling agent is obtained by reacting 4-allyl-N, N-dimethylaniline with 3-mercaptopropyltrimethoxysilane. The high-temperature-resistant adhesive is obtained by polymerizing butyl acrylate, acryloyloxybenzophenone and hydroxypropyl acrylate; the prepared low-moisture ceramic slurry is good in high temperature resistance, and a low-moisture ceramic diaphragm prepared from the low-moisture ceramic slurry is high in ionic conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery separator technology, specifically to a low-moisture ceramic slurry and a low-moisture ceramic separator. Background Technology

[0002] With the rapid development of the new energy industry, lithium batteries have been widely used in consumer electronics, energy storage systems, and electric vehicles due to their advantages such as high energy density, long cycle life, and environmental friendliness. Among the four key materials of lithium batteries (positive electrode, negative electrode, electrolyte, and separator), the separator, as the internal physical isolation layer of the battery, not only prevents direct contact between the positive and negative electrodes from causing short circuits, but also has a significant impact on the battery's safety, cycle performance, and rate performance. Especially in power battery applications, batteries generate a large amount of heat during charging and discharging. If the separator's thermal stability is insufficient, it is prone to thermal shrinkage or even melting, leading to internal short circuits and potentially causing serious safety accidents such as thermal runaway. Therefore, improving the high-temperature resistance of the separator has become one of the important directions for the development of power battery technology.

[0003] To meet the high safety requirements of power batteries, ceramic-coated separator technology has emerged and developed rapidly. Among them, alumina ceramics, due to their excellent thermal stability, chemical inertness, and mechanical strength, are widely used as coating materials for separators. By coating a polyolefin-based membrane with an alumina ceramic layer, the heat resistance of the separator can be significantly improved, and thermal shrinkage at high temperatures can be suppressed, thereby enhancing the overall safety of the battery. Currently, alumina ceramic separators are widely used in high-end power batteries.

[0004] However, in practical applications, the high hygroscopicity of alumina materials is becoming increasingly prominent. In particular, conventionally used alumina typically contains 5%–10% γ-alumina phase, which possesses high surface activity and a large specific surface area, and its particle size is usually difficult to reduce to below 100 nanometers. While this nanoscale fine particle structure is beneficial for forming a dense ceramic coating, it also significantly increases the surface energy of the material, making it highly susceptible to adsorbing moisture from the environment. During slurry preparation and membrane coating, if the alumina powder is highly hygroscopic, it will lead to an increase in the moisture content of the ceramic slurry, thereby affecting the slurry's stability, rheological properties, and coating uniformity. More seriously, residual moisture is difficult to completely remove during subsequent drying, ultimately remaining in the ceramic membrane, resulting in excessive moisture content in the finished membrane.

[0005] Moisture content in the separator is one of the key control indicators in the lithium battery production process. Excessive moisture content can react with lithium salts in the electrolyte to generate corrosive substances such as HF. This not only corrodes electrode materials and current collectors but also damages the stability of the solid electrolyte interface film, leading to increased internal resistance, accelerated capacity decay, and even safety issues such as gas expansion and leakage.

[0006] Therefore, how to effectively reduce the moisture content of ceramic diaphragms while ensuring their high heat resistance, especially controlling the moisture absorption risk caused by γ-alumina, has become a key technical bottleneck restricting the development of high-performance ceramic diaphragms. Summary of the Invention

[0007] The purpose of this invention is to provide a low-moisture ceramic slurry and a low-moisture ceramic diaphragm to solve the technical problems mentioned in the background section.

[0008] The technical solution to achieve the objective of this invention is: In a first aspect, the present invention discloses a low-moisture ceramic slurry, wherein, by mass parts, the raw material components include 25-55 parts by mass of hydrophobic modified ceramic material, 1-10 parts by mass of thickener, 8-20 parts by mass of high-temperature resistant binder, 0.05-0.1 parts by mass of wetting agent, 1-5 parts by mass of dispersant, and 25-50 parts by mass of solvent.

[0009] Furthermore, the hydrophobic modified ceramic material is obtained by modifying alumina with a hydrophobic silane coupling agent.

[0010] Furthermore, the hydrophobic silane coupling agent is obtained by reacting 4-allyl-N,N-dimethylaniline with 3-mercaptopropyltrimethoxysilane, and the specific reaction process is as follows: .

[0011] Furthermore, the high-temperature resistant adhesive is obtained by polymerizing butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate.

[0012] The high-temperature resistant adhesive of the present invention is obtained by polymerizing butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate. The benzophenone structure is stably introduced into the polymer backbone of the high-temperature resistant adhesive to form repeating units with rigid aromatic ring structures, which effectively improves the high-temperature resistance of the high-temperature resistant adhesive.

[0013] Further, the dispersant is one or more mixed solvents selected from methanol, propanol, n-butanol, isopropanol, ethylene glycol, dimethyl ether, diethyl ether, propylene glycol, glycerol, propanol, and butanone.

[0014] Secondly, the present invention discloses a method for preparing a low-moisture ceramic slurry as described in the first aspect, the preparation steps of which are as follows: (1) Under nitrogen protection, hydrophobic modified ceramic material and 80-160 parts by mass of n-butyllithium solution are mixed, water is removed by vacuum distillation, and the mixture is stirred at 80-90℃ for 11-13h. Then 100-120 parts by mass of dry diethyl ether is added and mixed, and then frozen with liquid nitrogen to obtain mixture A. High-temperature resistant binder is mixed with 50-70 parts by mass of diethyl ether and stirred for 55-65min. Then it is added dropwise to mixture A under nitrogen protection. After the addition is completed within 1h, the mixture is reacted at room temperature for 11-13h. Then the diethyl ether is removed by vacuum distillation to obtain premixed ceramic slurry. (2) Stir the solvent, dispersant and premixed ceramic slurry at 1000~1800r / min for 5~15min, then add the thickener and stir at 800~1500r / min for 1~2h, then grind with a grinder and add wetting agent, stirring at 30~80r / min for 5~10min to obtain low moisture ceramic slurry.

[0015] Further, the preparation steps of the hydrophobic modified ceramic material are as follows: 180-200 parts by mass of anhydrous ethanol and water in a volume ratio of 19:1 are mixed with 0.5-0.7 parts by mass of hydrophobic silane coupling agent, stirred at 55-65°C for 25-35 minutes, and then 18-22 parts by mass of alumina are added. Stirring is continued for 8 hours, and the mixture is filtered and dried to obtain the hydrophobic modified ceramic material.

[0016] Further, the preparation steps of the high-temperature resistant adhesive are as follows: 100 parts by weight of mixed acrylic monomers are added to 200-500 parts by weight of anhydrous ethanol; 1-3 parts by weight of ammonium persulfate are added, the temperature is set to 65-70℃, and the reaction is carried out for 10-12 hours under a nitrogen atmosphere to obtain the high-temperature resistant adhesive.

[0017] Furthermore, the mass ratio of butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate in the mixed acrylic monomers is 1:(0.8~1.2):(0.3~0.6).

[0018] Thirdly, the present invention provides a low-moisture ceramic membrane, which is prepared by coating the low-moisture ceramic slurry described in the first aspect onto the surface of a base membrane and then drying it.

[0019] By adopting the above technical solution, the present invention has the following beneficial effects: (1) This invention effectively solves the problem of alumina easily absorbing water in traditional slurries by using hydrophobic modified ceramic materials and introducing high-temperature resistant binders in low-moisture ceramic slurries. Among them, hydrophobic modified ceramic materials can significantly reduce the material's ability to adsorb water, thereby reducing the water content in the slurry. At the same time, the addition of high-temperature resistant binders not only enhances the bonding strength of the ceramic layer, but also maintains structural stability in high-temperature environments, significantly improving the high-temperature resistance of the prepared ceramic diaphragm.

[0020] (2) The hydrophobic modified ceramic material of the present invention is obtained by surface modification of alumina by a hydrophobic silane coupling agent; the alkoxy group of the silane coupling agent can undergo a condensation reaction with the hydroxyl group on the surface of alumina to form a stable chemical bond, while the hydrophobic structure in its molecule is arranged outward to build a dense hydrophobic barrier on the surface of alumina particles; this hydrophobic structure significantly reduces the surface energy of the material, effectively preventing the adsorption and penetration of water molecules, thereby greatly reducing the affinity of alumina for environmental moisture. The modified alumina not only maintains the original high thermal stability and mechanical strength, but also has excellent hydrophobic properties, fundamentally alleviating the moisture absorption problem caused by the high specific surface area and surface activity of γ-alumina.

[0021] (3) The hydrophobic silane coupling agent used in this invention is synthesized by a mercapto-olefin click chemical reaction of 4-allyl-N,N-dimethylaniline and 3-mercaptopropyltrimethoxysilane. Under the action of an initiator, the thiol group (-SH) and the carbon-carbon double bond (C=C) undergo an efficient and selective addition reaction to generate a novel silane coupling agent containing a siloxane anchoring group and an aromatic tertiary amine organic functional group. Among them, 3-mercaptopropyltrimethoxysilane provides a hydrolyzable methoxy group, which can be firmly bonded to the hydroxyl groups on the surface of alumina particles. The aromatic tertiary amine structure in 4-allyl-N,N-dimethylaniline has strong hydrophobicity and steric hindrance effect, and forms a dense nonpolar organic layer on the surface of alumina after grafting with the coupling agent. This hydrophobic layer effectively shields the active sites on the surface of alumina, significantly reduces its surface energy and hydrophilicity, thereby endowing the modified alumina with excellent hydrophobic properties.

[0022] (4) The high-temperature resistant adhesive of the present invention is obtained by polymerizing butyl acrylate, acryloyloxybenzophenone and hydroxypropyl acrylate. The benzophenone structure is stably introduced into the polymer backbone of the high-temperature resistant adhesive to form a repeating unit with a rigid aromatic ring structure, which effectively improves the high-temperature resistance of the high-temperature resistant adhesive.

[0023] (5) In the preparation process of the low-moisture ceramic slurry of the present invention, the hydrophobic modified ceramic material is first mixed with the high-temperature resistant binder, and n-butyllithium is introduced to react, and then mixed with other raw materials to obtain the final product; the N,N-dimethylaniline group on the surface of the hydrophobic modified ceramic material undergoes a nucleophilic reaction with n-butyllithium to generate a nitrogen-lithium active species with strong electron-donating ability; the benzene ring in this active species undergoes a nucleophilic addition reaction with the carbonyl group in the high-temperature resistant binder molecular chain, and the connection between the two phases is achieved by forming a carbon-carbon chemical bond; at the same time, the lithium ion forms a coordination bond with the oxygen atom in the carbonyl group and undergoes a cyclization reaction in the molecule, and finally A binary ring structure centered on lithium ions and containing nitrogen and oxygen atoms was constructed. This lithium complex not only establishes a strong chemical bridge between ceramic particles and polymer binder, significantly enhancing the dispersion stability of hydrophobically modified ceramic materials in the slurry system, preventing agglomeration and sedimentation, thereby improving the uniformity and coating performance of the slurry; simultaneously, lithium ions, as mobile charge carriers, are moderately anchored in the coordination structure at the polymer-ceramic interface, enabling ion conduction through a hopping mechanism under an electric field, effectively constructing ion transport channels and significantly improving the ion transport capability of the ceramic membrane; the specific reaction process is as follows: .

[0024] (6) The low-moisture ceramic diaphragm of the present invention is made from low-moisture ceramic slurry, which has good high temperature resistance and high ionic conductivity. Detailed Implementation

[0025] To better understand the above technical solution, the following will provide a detailed explanation of the technical solution in conjunction with specific implementation methods.

[0026] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] The following embodiments are only used to illustrate the technical solutions of the present invention more clearly, and should not be used to limit the scope of protection of the present invention. The solvent is water; The dispersant is diethyl ether; The thickener is sodium carboxymethyl cellulose; The wetting agent is 3-(methacryloyloxy)propyltrimethoxysilane.

[0028] Example 1 A method for preparing a low-moisture ceramic slurry, comprising the following steps: (1) Weigh and mix the raw materials as follows: 25 parts by mass of hydrophobic modified ceramic material, 1 part by mass of thickener, 8 parts by mass of high temperature resistant binder, 0.05 parts by mass of wetting agent, 1 part by mass of dispersant, and 25 parts by mass of solvent; (2) Under nitrogen protection, the hydrophobic modified ceramic material and 80 parts by mass of 1.6M n-butyllithium solution were mixed, and water was removed by vacuum distillation. The mixture was stirred at 80°C for 11 h. Then, 100 parts by mass of dry diethyl ether was added and mixed. The mixture was then frozen with liquid nitrogen to obtain mixture A. The high-temperature resistant binder was mixed with 50 parts by mass of diethyl ether and stirred for 55 min. Then, it was added dropwise to mixture A under nitrogen protection. After the addition was completed within 1 h, the mixture was reacted at room temperature for 11 h. Then, the diethyl ether was removed by vacuum distillation to obtain the premixed ceramic slurry. (3) Stir the solvent, dispersant and premixed ceramic slurry at 1000 r / min for 5 min, then add the thickener and stir at 800 r / min for 1 h, then grind with a grinder and add wetting agent, stirring at 30 r / min for 5 min to obtain low moisture ceramic slurry.

[0029] The preparation steps of the hydrophobic modified ceramic material are as follows: 180 parts by mass of anhydrous ethanol and water in a volume ratio of 19:1 are mixed with 0.5 parts by mass of hydrophobic silane coupling agent, stirred at 55°C for 25 min, and then 18 parts by mass of alumina are added. Stirring is continued for 8 h, filtered and dried to obtain the hydrophobic modified ceramic material.

[0030] The preparation steps of the high-temperature resistant adhesive are as follows: 100 parts by mass of mixed acrylic monomers are added to 200 parts by mass of anhydrous ethanol; 1 part by mass of ammonium persulfate is added, the temperature is set to 65°C, and the reaction is carried out for 10 hours under a nitrogen atmosphere to obtain the high-temperature resistant adhesive; wherein, the mass ratio of butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate in the mixed acrylic monomers is 1:0.8:0.3.

[0031] Example 2 A method for preparing a low-moisture ceramic slurry, comprising the following steps: (1) Weigh and mix the raw materials: 40 parts by mass of hydrophobic modified ceramic material, 5 parts by mass of thickener, 14 parts by mass of high temperature resistant binder, 0.07 parts by mass of wetting agent, 3 parts by mass of dispersant, and 40 parts by mass of solvent; (2) Under nitrogen protection, the hydrophobic modified ceramic material and 120 parts by mass of 1.6M n-butyllithium solution were mixed, and water was removed by vacuum distillation. The mixture was stirred at 85°C for 12 hours. Then, 110 parts by mass of dry diethyl ether was added and mixed. The mixture was then frozen with liquid nitrogen to obtain mixture A. The high-temperature resistant binder was mixed with 60 parts by mass of diethyl ether and stirred for 60 minutes. Then, it was added dropwise to mixture A under nitrogen protection. After the addition was completed within 1 hour, the mixture was reacted at room temperature for 12 hours. Then, the diethyl ether was removed by vacuum distillation to obtain the premixed ceramic slurry. (3) Stir the solvent, dispersant and premixed ceramic slurry at 1400 r / min for 10 min, then add the thickener and stir at 1300 r / min for 1.5 h, then grind with a grinder and add wetting agent, stirring at 50 r / min for 8 min to obtain low moisture ceramic slurry.

[0032] The preparation steps of the hydrophobic modified ceramic material are as follows: 190 parts by mass of anhydrous ethanol and water in a volume ratio of 19:1 are mixed with 0.6 parts by mass of hydrophobic silane coupling agent, stirred at 60°C for 30 min, and then 20 parts by mass of alumina are added. Stirring is continued for 8 h, filtered and dried to obtain the hydrophobic modified ceramic material.

[0033] The preparation steps of the high-temperature resistant adhesive are as follows: 100 parts by mass of mixed acrylic monomers are added to 300 parts by mass of anhydrous ethanol; 2 parts by mass of ammonium persulfate are added, the temperature is set to 70°C, and the reaction is carried out for 11 hours under a nitrogen atmosphere to obtain the high-temperature resistant adhesive; wherein, the mass ratio of butyl acrylate, acryloyloxybenzophenone and hydroxypropyl acrylate in the mixed acrylic monomers is 1:1:0.5.

[0034] Example 3 A method for preparing a low-moisture ceramic slurry, comprising the following steps: (1) Weigh and mix the raw materials as follows: 55 parts by mass of hydrophobic modified ceramic material, 10 parts by mass of thickener, 20 parts by mass of high temperature resistant binder, 0.1 parts by mass of wetting agent, 5 parts by mass of dispersant, and 50 parts by mass of solvent; (2) Under nitrogen protection, the hydrophobic modified ceramic material and 160 parts by mass of 1.6M n-butyllithium solution were mixed, and water was removed by vacuum distillation. The mixture was stirred at 90°C for 13 hours. Then, 120 parts by mass of dry diethyl ether was added and mixed. The mixture was then frozen with liquid nitrogen to obtain mixture A. The high-temperature resistant binder was mixed with 70 parts by mass of diethyl ether and stirred for 65 minutes. Then, it was added dropwise to mixture A under nitrogen protection. After the addition was completed within 1 hour, the mixture was reacted at room temperature for 13 hours. Then, the diethyl ether was removed by vacuum distillation to obtain the premixed ceramic slurry. (3) Stir the solvent, dispersant and premixed ceramic slurry at 1800 r / min for 15 min, then add the thickener and stir at 1500 r / min for 2 h, then grind with a grinder and add wetting agent, stirring at 80 r / min for 10 min to obtain low moisture ceramic slurry.

[0035] The preparation steps of the hydrophobic modified ceramic material are as follows: 200 parts by mass of anhydrous ethanol and water mixture with a volume ratio of 19:1 are mixed with 0.7 parts by mass of hydrophobic silane coupling agent, stirred at 65°C for 35 min, and then 22 parts by mass of alumina are added. Stirring is continued for 8 h, filtered and dried to obtain the hydrophobic modified ceramic material.

[0036] The preparation steps of the high-temperature resistant adhesive are as follows: 100 parts by mass of mixed acrylic monomers are added to 500 parts by mass of anhydrous ethanol; 3 parts by mass of ammonium persulfate are added, the temperature is set to 70°C, and the reaction is carried out for 12 hours under a nitrogen atmosphere to obtain the high-temperature resistant adhesive; wherein, the mass ratio of butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate in the mixed acrylic monomers is 1:1.2:0.6.

[0037] Comparative Example 1 The difference between Comparative Example 1 and Example 2 is that the low-moisture ceramic slurry uses ceramic material instead of hydrophobic modified ceramic material, while the other components and steps are the same as in Example 2.

[0038] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that the hydrophobic modified ceramic material is obtained by modifying alumina with γ-(methacryloyloxy)propyltrimethoxysilane, while the remaining components and steps are the same as in Example 2.

[0039] Comparative Example 3 The difference between Comparative Example 3 and Example 2 lies in the preparation of the low-moisture ceramic slurry, where the raw material components are directly mixed. The specific steps are as follows: (1) Weigh and mix the raw materials: 40 parts by mass of hydrophobic modified ceramic material, 5 parts by mass of thickener, 14 parts by mass of high temperature resistant binder, 0.07 parts by mass of wetting agent, 3 parts by mass of dispersant, and 40 parts by mass of solvent; (2) The solvent, dispersant, and hydrophobic modified ceramic material were stirred at 1400 r / min for 10 min, then the thickener was added and stirred at 1300 r / min for 1.5 h, followed by the addition of the high-temperature resistant binder and stirring at 1200 r / min for 1.5 h, then the wetting agent was added and the mixture was ground with a grinder and stirred at 50 r / min for 8 min to obtain a low-moisture ceramic slurry; the remaining components and steps were the same as in Example 2.

[0040] Comparative Example 4 The difference between Comparative Example 4 and Example 2 is that the binder used in the low-moisture ceramic slurry is obtained by polymerizing butyl acrylate and hydroxypropyl acrylate at a mass ratio of 1:0.5. The remaining components and steps are the same as in Example 2.

[0041] Example of effect Using a 9μm thick polyethylene film as the base film, the low-moisture ceramic slurry prepared in Examples 1-3 and Comparative Examples 1-4 was coated onto the base film to obtain a low-moisture ceramic diaphragm. The diaphragm was coated using a small coating machine and dried at 75°C to obtain a 9+4μm coated diaphragm.

[0042] Thermal stability: The low-moisture ceramic diaphragm was placed in an environment of 130℃ for 30 min and then removed. The dimensional changes of the diaphragm before and after heat treatment were observed and the thermal shrinkage rate (%) was calculated. The thermal shrinkage rate (%) = (diaphragm area before heat treatment - diaphragm area after heat treatment) * 100% / diaphragm area before heat treatment.

[0043] Ionic conductivity: The aforementioned low-moisture ceramic separator was immersed in electrolyte and sandwiched between stainless steel sheets. SS / Separator / SS cells were assembled, and the separator impedance was measured at a frequency range of 1×10⁻⁶. 6 Hz-10 Hz, AC amplitude of 10mV, the intercept of the curve on the X-axis in the Nyquist spectrum obtained by electrochemical impedance spectroscopy is the impedance of the diaphragm after being soaked in electrolyte. The ionic conductivity of the diaphragm = diaphragm thickness / (area of ​​stainless steel sheet * diaphragm impedance).

[0044] Table 1 below shows the performance test results of the low-moisture ceramic membranes prepared from the low-moisture ceramic slurries obtained in Examples 1-3 and Comparative Examples 1-4: Table 1

[0045] As shown in Table 1 above, the low-moisture ceramic membranes prepared from the low-moisture ceramic slurries obtained in Examples 1-3 and Comparative Examples 1-4 have low moisture content, good high-temperature resistance, and high ionic conductivity.

[0046] The difference between Comparative Example 1 and Example 2 is that the low-moisture ceramic slurry uses ceramic material instead of hydrophobic modified ceramic material, and the low-moisture ceramic membrane made from the obtained low-moisture ceramic slurry has a lower ionic conductivity.

[0047] The difference between Comparative Example 2 and Example 2 is that the hydrophobic modified ceramic material is obtained by modifying alumina with γ-(methacryloyloxy)propyltrimethoxysilane, and the low-moisture ceramic membrane made from the obtained low-moisture ceramic slurry has a lower ionic conductivity.

[0048] The difference between Comparative Example 3 and Example 2 is that in the preparation of the low-moisture ceramic slurry, the raw material components are directly mixed, and the low-moisture ceramic membrane made from the resulting low-moisture ceramic slurry has a higher ionic conductivity.

[0049] The difference between Comparative Example 4 and Example 2 is that the binder used in the low-moisture ceramic slurry is only obtained by polymerizing butyl acrylate and hydroxypropyl acrylate at a mass ratio of 1:0.5. The low-moisture ceramic diaphragm made from the obtained low-moisture ceramic slurry has weak high-temperature resistance and high ionic conductivity.

[0050] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A low-moisture ceramic slurry, characterized in that, By mass, the raw material components include 25-55 parts hydrophobic modified ceramic material, 1-10 parts thickener, 8-20 parts high-temperature resistant binder, 0.05-0.1 parts wetting agent, 1-5 parts dispersant, and 25-50 parts solvent.

2. The low-moisture ceramic slurry according to claim 1, characterized in that, The hydrophobic modified ceramic material is obtained by modifying alumina with a hydrophobic silane coupling agent.

3. The low-moisture ceramic slurry according to claim 2, characterized in that, The hydrophobic silane coupling agent is obtained by reacting 4-allyl-N,N-dimethylaniline with 3-mercaptopropyltrimethoxysilane.

4. The low-moisture ceramic slurry according to claim 1, characterized in that, The high-temperature resistant adhesive is obtained by polymerizing butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate.

5. The low-moisture ceramic slurry according to claim 1, characterized in that, The dispersant is one or more mixed solvents selected from methanol, propanol, n-butanol, isopropanol, ethylene glycol, methyl ether, diethyl ether, propylene glycol, glycerol, propanol, and butanone.

6. A method for preparing a low-moisture ceramic slurry as described in any one of claims 1 to 5, characterized in that, The preparation steps are as follows: (1) Under nitrogen protection, hydrophobic modified ceramic material and 80-160 parts by mass of n-butyllithium solution are mixed, water is removed by vacuum distillation, and the mixture is stirred at 80-90℃ for 11-13h. Then 100-120 parts by mass of dry diethyl ether is added and mixed, and then frozen with liquid nitrogen to obtain mixture A. High-temperature resistant binder is mixed with 50-70 parts by mass of diethyl ether and stirred for 55-65min. Then it is added dropwise to mixture A under nitrogen protection. After the addition is completed within 1h, the mixture is reacted at room temperature for 11-13h. Then the diethyl ether is removed by vacuum distillation to obtain premixed ceramic slurry. (2) Stir the solvent, dispersant and premixed ceramic slurry at 1000~1800r / min for 5~15min, then add the thickener and stir at 800~1500r / min for 1~2h, then grind with a grinder and add wetting agent, stirring at 30~80r / min for 5~10min to obtain low moisture ceramic slurry.

7. The method for preparing low-moisture ceramic slurry according to claim 6, characterized in that, The preparation steps of the hydrophobic modified ceramic material are as follows: 180-200 parts by weight of anhydrous ethanol and water in a volume ratio of 19:1 are mixed with 0.5-0.7 parts by weight of hydrophobic silane coupling agent. After stirring at 55-65°C for 25-35 minutes, 18-22 parts by weight of alumina are added and stirring is continued for 8 hours. The mixture is then filtered and dried to obtain the hydrophobic modified ceramic material.

8. The method for preparing low-moisture ceramic slurry according to claim 6, characterized in that, The preparation steps of the high-temperature resistant adhesive are as follows: 100 parts by weight of mixed acrylic monomers are added to 200-500 parts by weight of anhydrous ethanol; 1-3 parts by weight of ammonium persulfate are added, the temperature is set to 65-70℃, and the reaction is carried out for 10-12 hours under a nitrogen atmosphere to obtain the high-temperature resistant adhesive.

9. The method for preparing low-moisture ceramic slurry according to claim 8, characterized in that, The mass ratio of butyl acrylate, acryloyloxybenzophenone, and hydroxypropyl acrylate in the mixed acrylic monomers is 1:(0.8~1.2):(0.3~0.6).

10. A low-moisture ceramic membrane, characterized in that, The low-moisture ceramic diaphragm is prepared by coating the low-moisture ceramic slurry according to any one of claims 1 to 5 onto the surface of a base membrane and then drying it.