A negative electrode active material, a preparation method thereof, a negative electrode sheet, a battery, and an electric device

By employing a core-shell structured carbon coating layer in the negative electrode active material and optimizing the interlayer spacing distribution, a fast ion channel is constructed, solving the problem of insufficient fast charging performance of secondary batteries and achieving efficient fast charging and stable cycling of the battery.

CN121237839BActive Publication Date: 2026-11-10BYD CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510318543.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-17
Publication Date
2026-11-10
Estimated Expiration
2045-03-17

AI Technical Summary

Technical Problem

The limited improvement in fast-charging performance of existing rechargeable batteries restricts battery development. Traditional methods may lead to increased specific surface area, exacerbated side reactions, or obstructed lithium-ion diffusion pathways.

Method used

The anode active material adopts a core-shell structure, with the core being the active material and the carbon coating layer composed of first and second carbon materials. The interlayer spacing is optimized to form a low-resistance diffusion channel and flexibly adjust the ion current density. By controlling the thickness and material ratio of the carbon coating layer, a fast ion channel is constructed.

Benefits of technology

It significantly improves the fast-charging performance and cycle stability of batteries, reduces interface impedance, increases initial coulombic efficiency, and meets the requirements of fast-charging batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121237839B_ABST
    Figure CN121237839B_ABST
Patent Text Reader

Abstract

The application provides a negative electrode active material and a preparation method thereof, a negative electrode sheet, a battery and an electric device. The negative electrode active material comprises an active material core and a carbon coating layer covering at least part of the surface of the active material core; the carbon coating layer comprises a first carbon material and a second carbon material, the interlayer spacing of the first carbon material is m, and the interlayer spacing of the second carbon material is n, wherein 0.345nm, 0.386nm. The negative electrode active material provided by the application has good fast charging performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a negative electrode active material, and more particularly to a negative electrode active material and its preparation method, a negative electrode sheet, a battery, and electrical equipment, belonging to the field of secondary batteries. Background Technology

[0002] With the rapid development of electric vehicles, portable electronic devices and renewable energy storage, secondary batteries (such as lithium-ion batteries) are facing increasingly stringent performance requirements as the core energy storage carrier.

[0003] Fast charging performance has become one of the key indicators for upgrading rechargeable battery technology. Fast charging capability directly impacts user experience, equipment operating efficiency, and the economics of the energy system. Currently, the fast charging performance of rechargeable batteries can be improved by reducing aggregate particle size to shorten the lithium-ion diffusion distance and by coating the surface with amorphous carbon to increase lithium-ion transport channels.

[0004] However, current improvements in the fast-charging performance of rechargeable batteries remain limited, hindering their development. Summary of the Invention

[0005] This invention provides a negative electrode active material, which includes an active material core and a carbon coating layer. By optimizing the interlayer spacing distribution of the carbon coating layer, the fast charging performance of the negative electrode active material can be significantly improved when it is used in a battery.

[0006] The present invention also provides a method for preparing a negative electrode active material, which is simple to operate and can prepare the above-mentioned negative electrode active material.

[0007] The present invention also provides a negative electrode sheet comprising the above-mentioned negative electrode active material, which, when used in a battery, can significantly improve the battery's fast charging performance.

[0008] The present invention also provides a battery comprising the above-mentioned negative electrode sheet, which has excellent fast charging performance.

[0009] The present invention also provides an electrical device that includes the aforementioned battery and has good performance.

[0010] The present invention provides a negative electrode active material, comprising an active material core and a carbon coating layer covering at least a portion of the surface of the active material core; the carbon coating layer comprises a first carbon material and a second carbon material, wherein the interlayer spacing of the first carbon material is m and the interlayer spacing of the second carbon material is n, wherein 0.345≤m<0.386nm and 0.386≤n<0.429nm.

[0011] In an optional embodiment, the carbon coating layer includes an inner coating layer extending outward from the core of the active material.

[0012] and, an outer coating extending inward from the outer surface of the carbon coating;

[0013] Furthermore, in the inner coating layer, the ratio of the first carbon material to the second carbon material is (85-100):(0-15);

[0014] In the outer coating layer, the ratio of the first carbon material to the second carbon material is (60-85):(15-40).

[0015] In an optional embodiment, the first carbon material comprises a transition carbon material with an interlayer spacing of 0.35 nm to 0.37 nm;

[0016] In the inner coating layer, the transition carbon material accounts for 10% to 40% of the amount of the first carbon material;

[0017] And / or, in the outer coating layer, the proportion of the transition carbon material to the first carbon material is 0-10%.

[0018] In one alternative embodiment, the active material core comprises graphite;

[0019] And / or, the carbon coating layer includes at least one of soft carbon, hard carbon, and heteroatom-doped carbon materials.

[0020] In an optional embodiment, the negative electrode active material I D / I G Let z be the integer part of the equation, and 0.7 ≤ z ≤ 2.1.

[0021] In one optional embodiment, the thickness of the coating layer is h, where 5nm < h ≤ 50nm;

[0022] And / or, the specific surface area of ​​the negative electrode active material is 0.5–2 m². 2 / g.

[0023] In another aspect, the present invention provides a method for preparing a negative electrode active material as described above, comprising the following steps:

[0024] 1) The carbon source and the active material are stirred to coat at least a portion of the surface of the active material with the carbon source, thereby obtaining a first precursor;

[0025] 2) The first precursor is heat-treated in a protective atmosphere to obtain the negative electrode active material.

[0026] In an optional embodiment, the heat treatment includes the following process: the first precursor is subjected to heat treatment in a protective atmosphere at a heating rate of 2-20°C / min to 900-1200°C for 6-48 hours to obtain the negative electrode active material.

[0027] In an alternative embodiment, the heat treatment includes the following process:

[0028] The first precursor is subjected to a first heat treatment in a protective atmosphere, with the temperature increased to 500-700℃ at a rate of 2-20℃ / min for 1-6 hours, and then subjected to a second heat treatment in a temperature increased to 900-1200℃ at a rate of 2-20℃ / min for 6-48 hours to obtain the negative electrode active material.

[0029] In an optional embodiment, the carbon source includes at least one of bitumen, heavy oil, and resin;

[0030] And / or, the stirring treatment of the carbon source and the active material specifically includes: stirring the organic solvent in which the carbon source is dispersed with the active material.

[0031] In another aspect, the present invention provides a negative electrode sheet, comprising the negative electrode active material as described above or the negative electrode active material prepared by the preparation method described above.

[0032] In another aspect, the present invention provides a battery comprising the negative electrode sheet as described above.

[0033] In another aspect, the present invention provides an electrical device comprising the battery described above.

[0034] The negative electrode active material provided by the present invention includes an active material core with different interlayer spacing distributions and a carbon coating layer. By limiting the interlayer spacing of the core and the carbon coating layer, a gradient distribution of the interlayer spacing of the negative electrode active material is achieved, which significantly reduces the diffusion barrier for the insertion and extraction of active metal ions, effectively regulates the lithium ion diffusion dynamics, and thus improves the fast charging performance of the battery. Attached Figure Description

[0035] Figure 1 This is a schematic diagram of the structure of the negative electrode active material provided in a specific embodiment of the present invention;

[0036] Figure 2 This is a schematic diagram of the structure of the negative electrode active material provided in a specific embodiment of the present invention;

[0037] Figure 3 This is a TEM image of the negative electrode active material according to a specific embodiment of the present invention;

[0038] Figure 4A statistical distribution histogram is generated for the interlayer spacing values ​​of the negative electrode active material in a specific embodiment of the present invention.

[0039] Explanation of reference numerals in the attached figures:

[0040] 1-Active material core; 2-Carbon coating layer; 21-Inner coating layer; 22-Outer coating layer; A-First carbon material; B-Second carbon material. Detailed Implementation

[0041] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0042] Currently, in order to improve the fast-charging performance of negative electrode active materials, the common methods are to reduce the aggregate particle size or to coat the surface of the negative electrode active material with amorphous carbon to increase the active metal ion transport channels, so as to adapt to the rapid insertion and extraction of active metal ions.

[0043] However, reducing the particle size of graphite aggregate leads to a significant increase in specific surface area and surface energy. The proportion of surface atoms in nano- or submicron-sized particles increases, enhancing chemical activity and exacerbating side reactions. This results in the electrolyte decomposing on the surface to form a thicker SEI film, leading to a decrease in initial efficiency. Furthermore, when the surface of the negative electrode active material is coated with amorphous carbon, the structure of the amorphous carbon may hinder the lithium-ion diffusion path, limiting the rapid migration of lithium ions.

[0044] like Figure 1 As shown, one aspect of the present invention provides a negative electrode active material, including an active material core 1 and a carbon coating layer 2 covering at least a portion of the surface of the active material core 1; the carbon coating layer includes a first carbon material A and a second carbon material B, the interlayer spacing of the first carbon material A is m, and the interlayer spacing of the second carbon material B is n, wherein 0.345≤m<0.386nm, 0.386≤n<0.429nm.

[0045] The negative electrode active material provided by the present invention has a core-shell structure, and the core of the active material refers to a material that can embed and release active metal ions.

[0046] The carbon coating layer in this invention refers to an amorphous carbon layer.

[0047] The first carbon material A and the second carbon material B are randomly distributed in the carbon coating layer, wherein the interlayer spacing of the first carbon material A includes, but is not limited to, 0.345nm, 0.350nm, 0.355nm, 0.360nm, 0.365nm, 0.370nm, 0.375nm, 0.380nm, 0.385nm or any range greater than or equal to 0.345nm and less than 0.368nm.

[0048] The interlayer spacing of the second carbon material B includes, but is not limited to, 0.386 nm, 0.390 nm, 0.395 nm, 0.400 nm, 0.405 nm, 0.410 nm, 0.415 nm, 0.420 nm, 0.425 nm, 0.428 nm, or any range greater than or equal to 0.386 nm and less than 0.429 nm.

[0049] In some embodiments, the interlayer spacing of the first carbon material A and the second carbon material B in the carbon coating layer of the present invention can be analyzed using Gatan Digital Micrograph software, and the interlayer spacing can be calculated by Fast Fourier Transform (FFT).

[0050] The negative electrode active material provided by this invention can significantly improve the initial coulombic efficiency of a battery, thereby enhancing its fast-charging performance. On one hand, the carbon coating layer forms a low-resistance surface diffusion channel, accelerating the transport of active lithium ions at the electrode / electrolyte interface and constructing a fast ion channel. On the other hand, the different interlayer spacing distributions in the first and second carbon materials break the directional arrangement limitations of traditional single interlayer spacing, flexibly adjusting the local ion current density, eliminating transport bottlenecks, and thus improving the battery's fast-charging performance.

[0051] In one specific implementation, such as Figure 2 As shown, the carbon coating layer 2 includes an inner coating layer 21 extending outward from the core of the active material.

[0052] and an outer coating layer 22 extending inward from the outer surface of the carbon coating layer;

[0053] Furthermore, in the inner coating layer 21, the ratio of the first carbon material to the second carbon material is (85-100):(0-15);

[0054] In the outer coating layer 22, the ratio of the first carbon material to the second carbon material is (60-85):(15-40).

[0055] The ratio of the first carbon material to the second carbon material can be detected by the following method:

[0056] The analysis was performed using a Malvern Mastersizer 3000 with a wet dispersion-laser derivatization method: 0.20±0.01g of the negative electrode active material sample was weighed into a 100mL beaker, 3ml of surfactant was added, and deionized water was added to a final volume of 20.0±0.1mL. The beaker was sealed with a sealing film and placed in an ultrasonic machine (40KHz / 210W, 70% output power) for 5min. The laser intensity was 70-90%, and the detector light energy was <100. When the light shielding reached 5-15%, the test was started. The particle size distribution and bulk density distribution curve of the negative electrode active material were obtained, and the Dv50 value of the negative electrode active material was then output.

[0057] Graphite particles with a particle size close to Dv50 were selected as the object. Using a high-resolution TEM as the origin, images were taken at four angles (45°, 135°, 225°, and 315°) on the upper left, upper right, lower left, and lower right sides, resulting in four images. The core of the active material has a continuous and regular interlayer spacing of less than 0.338 nm, while the carbon coating layer has an interlayer spacing greater than 0.338 nm. Within the carbon coating layer, the interlayer spacing is mainly concentrated between 0.345 nm and 0.429 nm. The first carbon material has an interlayer spacing greater than or equal to 0.345 nm and less than 0.386 nm, while the second carbon material has an interlayer spacing greater than or equal to 0.386 nm and less than 0.429 nm. The first carbon material also includes transition carbon material with an interlayer spacing greater than or equal to 0.35 nm and less than or equal to 0.37 nm.

[0058] The following method was used to measure the ratio of the first carbon material, the second carbon material, and the ratio of the transition carbon material in the first carbon material: The straight-line distance from the active material core to the outer surface of the carbon coating layer was measured, which is the thickness of the carbon coating layer. The straight-line distance from the active material core to the outer surface of the carbon coating layer was also measured, which is the thickness *h* of the carbon coating layer. The region with a carbon coating layer thickness of *y* nm in the direction from the outer surface of the carbon coating layer to the active material core was designated as the outer coating layer. The region with a carbon coating layer thickness of *x* nm in the direction from the outer surface of the active material core to the carbon coating layer was designated as the inner coating layer. Then, the images of the inner and outer coating layers were analyzed separately. Specifically, the data was analyzed using Gatan Digital Micrograph software: the image was converted to integer mode, the scale was measured (using a dashed line of the same length as the scale – input the corresponding length 5 nm), 40 measurement areas were randomly selected, and a 3*0.5 nm range was selected along the vertical direction of the interlayer spacing in each selected area. The results were obtained through Fast Fourier Transform (FFT). Figure 3The distance between two adjacent peaks is defined as one inter-layer spacing. Five inter-layer spacing values ​​are randomly selected for each bounded area. Finally, a statistical distribution histogram is generated based on the 800 measured inter-layer spacing values. (See [link to relevant documentation]). Figure 4 After fitting and generating the distribution curve, the ratio of the first carbon material to the second carbon material and the proportion of the transition carbon material in the inner and outer coating layers are calculated based on the area of ​​the corresponding regions of the first carbon material, the second carbon material and the transition carbon material on the distribution curve.

[0059] For example, the ratio of the first carbon material to the second carbon material in the inner coating layer includes, but is not limited to, 85:15, 86:14, 88:12, 90:10, 92:8, 94:6, 96:4, 98:2, 100:0, or any combination thereof; the ratio of the first carbon material to the second carbon material in the outer coating layer includes, but is not limited to, 60:40, 62:38, 64:36, 66:34, 68:32, 70:30, 72:28, 74:26, 76:24, 78:22, 80:20, 82:18, 84:16, 85:15, or any combination thereof.

[0060] By limiting the distribution ratio of the first and second carbon materials in the inner and outer coating layers of the negative electrode active material, the high-binding region of the inner coating layer is tightly connected to the graphite bulk, with an interlayer spacing close to that of graphite (0.335nm±0.02nm). This reduces interfacial impedance, absorbs volume expansion during charge and discharge, and avoids mechanical stripping. Meanwhile, the higher proportion of the first carbon material in the outer coating layer facilitates rapid lithium-ion diffusion, while the second carbon material provides stress buffering, preventing cycle cracking and the formation of a continuous conductive network, thus improving rate performance. This approach achieves structural-electrochemical synergistic stability while maintaining high ion conductivity, making it particularly suitable for fast-charging battery requirements and improving battery cycle stability and rate performance.

[0061] By way of example and not limitation, the thickness of the carbon coating is h, the thickness of the inner coating is x, and the thickness of the outer coating is y, where x + y ≤ h.

[0062] In one specific embodiment, the first carbon material includes a transition carbon material with an interlayer spacing of 0.35 nm to 0.37 nm;

[0063] In the inner coating layer, the transition carbon material accounts for 10% to 40% of the amount of the first carbon material.

[0064] In detail, the interlayer spacing of the transition carbon material includes, but is not limited to, a range of 0.350 nm, 0.355 nm, 0.360 nm, 0.365 nm, 0.370 nm, or any two thereof.

[0065] Similarly, the interlayer spacing and frequency ratio of carbon materials were determined using the methods described above, and will not be repeated here.

[0066] For ease of understanding, the portion of the first carbon material that does not conform to the interlayer spacing of transition carbon materials can be defined as non-transition carbon material.

[0067] In detail, in the inner coating layer, the proportion of transition carbon material to the first carbon material includes, but is not limited to, 10%, 15%, 20%, 25%, 30%, 35%, 40%, or any combination thereof.

[0068] The interlayer spacing (0.35–0.37 nm) of the transition carbon material is between that of the core and the first carbon material in the inner coating layer (0.345–0.386 nm). When the ratio of the transition carbon material to the first carbon material is within the above range, a continuous interlayer spacing gradient can be formed, reducing the lattice mismatch stress between the core and the coating layer, suppressing the generation of interface cracks. Moreover, the transition region acts as a "flexible buffer zone," absorbing the drastic volume change of the active material core during fast charging, preventing the coating layer from cracking and causing the electronic pathway to be interrupted, and further ensuring the fast charging performance, rate performance, and cycle stability of the battery.

[0069] In another specific embodiment, the transition carbon material in the outer coating layer accounts for 0 to 10% of the amount of the first carbon material.

[0070] In detail, in the outer coating layer, the proportion of the transition carbon material to the first carbon material includes, but is not limited to, 0%, 2%, 4%, 6%, 8%, 10%, or any combination thereof.

[0071] As described above, since the proportion of transition carbon materials in the outer coating layer is low, it can be ensured that the outer coating layer is mainly composed of non-transition carbon materials. This is conducive to the formation of low-resistance ion channels, further ensuring rate performance and fast charging performance. Moreover, the dense structure of transition carbon materials may increase the contact area between the electrolyte and the active material. The low proportion design reduces side reaction sites, inhibits excessive growth of the SEI film, and improves the cycle performance of the battery.

[0072] In one specific embodiment, the active material core comprises graphite.

[0073] Graphite, with its good conductivity and stable cycle performance, is relatively inexpensive and therefore more suitable for use in batteries for consumer electronics such as smartphones and laptops.

[0074] In another specific embodiment, the carbon coating layer includes at least one of soft carbon, hard carbon, and heteroatom-doped carbon materials.

[0075] As described above, by introducing heteroatoms (such as nitrogen, boron, phosphorus, sulfur, etc.) into the carbon coating layer, the electronic structure of the carbon coating layer can be changed, and its conductivity can be improved. This helps to further accelerate the electron transport rate, thereby improving the rate performance of the battery.

[0076] In one specific embodiment, the negative electrode active material I D / I G Let z be the integer part of the equation, and 0.7 ≤ z ≤ 2.1.

[0077] Among them, the negative electrode active material I D / I G It can reflect the degree of its defects, when the I of the negative electrode active material D / I G Within the above range, it can accelerate ion diffusion, improve fast charging performance, reduce interface impedance, regulate SEI film formation, suppress side reaction buffer volume expansion, and extend cycle life.

[0078] For example, the I of the negative electrode active material D / I G The measurement can be performed as follows: Take 0.5g of the negative electrode active material of this invention and place it on a glass slide, then flatten it with another glass slide to form a flat test surface. Before the test begins, use a single-crystal silicon wafer (520nm). -1 Calibration wavenumber error (accuracy < 1 cm) -1 The laser beam was examined, and its focusing state was checked. The laser wavelength was 532 nm, the attenuation power was 10%, and the scanning range was 100-3000 cm. -1 Exposure time was 10 seconds, and tests were performed three times. The sample was observed under a 100x objective lens, and 100 well-focused test points were selected. Subsequently, intelligent polynomial baseline fitting was used to remove the test substrate, and peak fitting was performed on the accumulated peaks in the Raman spectrum of the negative electrode active material. The peak value was 1355±5 cm⁻¹. -1 The peaks corresponding to D on the left and right are I. D 1582±5cm -1 The left and right sides correspond to peak G. Peak G can be fitted as peak G1 and peak G2. The sum of the peak intensities of G1 and G2 is I. G I D / I G =I D / (I G1 +I G2 ).

[0079] In detail, the I of the negative electrode active material D / I GIncluding but not limited to 0.7, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, or any combination thereof.

[0080] In one specific embodiment, the thickness of the coating layer is h, where 5nm < h ≤ 50nm.

[0081] In detail, the coating thickness can be detected using conventional methods in the field, such as FIB slicing followed by TEM testing.

[0082] The coating thickness includes, but is not limited to, a range of 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, or any combination thereof.

[0083] The aforementioned coating thickness not only provides space for the distribution of the first and second carbon materials, but also maintains good electrical conductivity while ensuring structural stability, thereby improving the battery's fast charging performance, rate performance, and cycle performance.

[0084] In another specific embodiment, the average particle size of the active material core is 10-20 μm; the average particle size of the active material core refers to the average diameter of the active material core, which can be controlled by adjusting the particle size distribution of the active material core during the preparation process.

[0085] In detail, the average particle size of the active material core includes, but is not limited to, a range of 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, or any two of these.

[0086] In another specific embodiment, the specific surface area of ​​the negative electrode active material is 0.5–2 m². 2 / g.

[0087] The specific surface area of ​​the negative electrode active material can be tested using methods commonly used in the field, such as gas adsorption.

[0088] Specifically, the specific surface area of ​​the negative electrode active material includes, but is not limited to, 0.5 m². 2 / g, 1m 2 / g, 1.5m 2 / g、2m 2 / g or a range consisting of any two of them.

[0089] A moderate specific surface area reduces the contact area between the material and the electrolyte, suppresses side reactions (such as excessive growth of the SEI film), reduces lithium loss, reduces irreversible lithium consumption during the first charge and discharge cycle, improves the first coulombic efficiency, and can also reduce the risk of local dendrite formation and improve the cycle stability of the material.

[0090] In another aspect, the present invention provides a method for preparing the negative electrode active material as described above, comprising the following steps:

[0091] 1) The carbon source and the active material are stirred to coat at least a portion of the surface of the active material with the carbon source, thereby obtaining a first precursor;

[0092] 2) The first precursor is heat-treated in a protective atmosphere to obtain the negative electrode active material.

[0093] Specifically, in step 1), the carbon source and the active material are stirred to achieve carbon source coating, thereby obtaining the first precursor.

[0094] Among them, common petroleum by-product carbon sources or resins can be selected according to the actual situation. Among them, petroleum by-product carbon sources include at least one of asphalt and heavy oil.

[0095] In one specific embodiment, in order to ensure the coating effect and improve the uniformity of coating, the carbon source is dispersed in an organic solvent to obtain a carbon source dispersion with a solid content of 5% to 15%.

[0096] The present invention does not limit the specific type of solvent. In one specific embodiment, the solvent includes at least one of tetrahydrofuran, toluene, ethylene glycol, and cyclohexane.

[0097] Understandably, in order to ensure that the carbon source and organic solvent are fully mixed and to avoid the influence of undissolved particles on subsequent steps, the carbon source and organic solvent can be mixed and stirred in a water bath for 2 hours, and then the undissolved particles can be removed by passing them through a 200-mesh metal sieve.

[0098] When mixing the carbon source solution and the active material, a high-speed disperser can be used with gradient stirring to ensure uniform mixing. For example, stir at a low speed of 300-700 rpm for 20 minutes for initial dispersion, then stir at a high speed of 2500-4000 rpm for 40 minutes for forced coating, and finally stir at a low speed of 700-900 rpm for 60 minutes to eliminate slurry stress. The temperature should be maintained at 50±2℃ throughout the process to prevent solvent evaporation, which would affect the mixing effect.

[0099] When a carbon source is mixed with an organic solvent to obtain a carbon source solution, the solvent needs to be removed after impregnation and coating. This invention does not limit the specific method of solvent removal; methods commonly used in the art can be selected for solvent removal, such as heating evaporation, vacuum evaporation, and spray drying.

[0100] In one specific embodiment, the heat treatment includes the following process: the first precursor is subjected to heat treatment in a protective atmosphere at a heating rate of 2-20℃ / min to 900-1200℃ for 6-48 hours to obtain the negative electrode active material.

[0101] In detail, the heat treatment temperature includes, but is not limited to, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C or any combination thereof, and the time includes, but is not limited to, 6h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 48h or any combination thereof.

[0102] To prevent the structure of the negative electrode active material from collapsing, heat treatment is required under appropriate pressure, such as 50 Pa to 100 Pa. Furthermore, to avoid adverse effects from other substances on the heat treatment, the process must be carried out under an inert atmosphere, such as nitrogen.

[0103] In another specific embodiment, the heat treatment includes the following process:

[0104] In step 2), the first precursor is heat-treated at 500-700℃ for 1-6 hours in a protective atmosphere at a heating rate of 2-20℃ / min, and then heat-treated at 900-1200℃ for 6-48 hours at a heating rate of 2-20℃ / min to obtain the negative electrode active material.

[0105] For example, the temperature of a single heat treatment includes, but is not limited to, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C, 660°C, 680°C, 700°C or any combination thereof, and the time includes, but is not limited to, 1h, 2h, 3h, 4h, 5h, 6h or any combination thereof.

[0106] For example, the temperature of the secondary heat treatment includes, but is not limited to, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C or any combination thereof, and the time includes, but is not limited to, 6h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 48h or any combination thereof.

[0107] When a carbon source is mixed with an organic solvent to obtain a carbon source solution, the solvent needs to be removed after impregnation and coating. This invention does not limit the specific method of solvent removal; methods commonly used in the art can be selected for solvent removal, such as heating evaporation, vacuum evaporation, and spray drying.

[0108] To prevent the structure of the negative electrode active material from collapsing, heat treatment is required under appropriate pressure, such as 50 Pa to 100 Pa. Furthermore, to avoid adverse effects from other substances on the heat treatment, the process must be carried out under an inert atmosphere, such as nitrogen.

[0109] It is understandable that, in order to control the particle size, specific surface area, etc. of the negative electrode material, the negative electrode material obtained after heat treatment can also be post-processed, for example: using an air jet mill (grading wheel speed 3000-5000 rpm) for crushing and shaping, and then screening through a 325 mesh vibrating screen (coating thickness uniformity CV value < 8%).

[0110] The preparation method provided by this invention is simple to operate and can prepare a negative electrode active material with good fast charging performance.

[0111] In another aspect, the present invention provides a negative electrode sheet, comprising the negative electrode active material as described above or the negative electrode active material prepared by the preparation method described above.

[0112] Since the negative electrode sheet provided by the present invention includes the above-mentioned negative electrode active material, it has good fast charging performance.

[0113] It is understood that the negative electrode sheet provided by the present invention includes a negative electrode current collector and a negative electrode active layer covering at least a portion of the surface of the negative electrode current collector, wherein the negative electrode active material is located in the negative electrode active layer.

[0114] The negative electrode active material layer may contain one or more negative electrode active materials. When multiple negative electrode active materials are contained, they may also include one or more of the following: graphite (artificial graphite, natural graphite), soft carbon, hard carbon, mesophase carbon microspheres, silicon carbide, etc.

[0115] In this invention, the negative electrode active layer may include a binder in addition to the negative electrode active material. In some cases, it may also include a conductive agent and other additives. The binder and conductive agent are conventional choices in the battery field. Exemplary binders include, but are not limited to, one or more of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polyimide (PI), polyacrylic acid (PAA), polyacrylates (such as polymethyl methacrylate, polymethyl acrylate, polyethyl acrylate, etc.), polyolefins (such as polypropylene, polyethylene, etc.), carboxymethyl cellulose (CMC), sodium alginate, etc. Conductive agents include, but are not limited to, one or more of carbon nanotubes, carbon black, graphene, carbon fibers, acetylene black, Ketjen black, graphite flakes, etc. Other additives include, but are not limited to, one or more of mesoporous silica, mesoporous alumina, silica microspheres, alumina nanoparticles, etc.

[0116] The aforementioned negative electrode sheet can be obtained by sequentially coating a slurry containing negative electrode material, binder, and optionally conductive agent onto a negative electrode current collector according to the present invention, followed by drying and rolling. The negative electrode current collector can be coated on one side or both sides. In other words, one side surface of the negative electrode current collector may have a negative electrode active coating, or both opposite sides of the negative electrode current collector may have a negative electrode active material coating.

[0117] When the negative electrode current collector is double-sided coated, the negative electrode active material layer on either side only needs to meet the aforementioned scheme of this invention. The current collector carrying the negative electrode active material layer can include, but is not limited to, any one of the following: copper foil, composite copper foil, carbon-coated copper foil, aluminum foil, composite aluminum foil, carbon-coated aluminum foil, stainless steel foil, copper alloy foil, copper-plated film, etc.

[0118] In another aspect, the present invention provides a battery comprising the negative electrode sheet as described above.

[0119] The battery provided by this invention further includes a positive electrode, a separator, and an electrolyte disposed between the positive electrode and the negative electrode. This battery can use any battery with the negative electrode provided by this invention, including but not limited to lithium-ion secondary batteries, sodium-ion secondary batteries, and potassium-ion secondary batteries.

[0120] The positive electrode sheet includes a positive current collector and a positive active layer disposed on the positive current collector. The positive active layer includes a positive active material, a binder, and an optional conductive agent. The positive active material can be selected according to the active ions on which the energy storage of the specific secondary battery depends. Active ions can include lithium ions, sodium ions, potassium ions, magnesium ions, aluminum ions, zinc ions, etc. For lithium-ion batteries, the positive active material can be one or more of the following, including but not limited to lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), and olivine-structured lithium phosphates (such as lithium iron phosphate (LFP) and lithium manganese iron phosphate (LFMP)). For sodium-ion batteries, the positive active material includes, but is not limited to, one or more of the following: transition metal oxides, polyanionic compounds, organic polymers, and Prussian blue materials.

[0121] The system also includes a separator, which is positioned between the positive and negative electrodes to isolate them. This application does not limit the type of separator; any separator material from existing batteries can be used. Exemplary separators include, but are not limited to, single-layer PP (polypropylene) films, single-layer PE (polyethylene) films, double-layer PP / PE films, double-layer PP / PP films, and triple-layer PP / PE / PP films. The electrolyte includes electrolyte salts and organic solvents, the specific types and compositions of which are conventional choices in the battery field and can be selected according to actual needs.

[0122] The battery also includes an electrolyte, which consists of electrolyte salts and solvents. The specific types and components of the electrolyte salts and organic solvents are not specifically limited and can be selected according to actual needs.

[0123] In another aspect, the present invention provides a battery pack comprising the battery as described above.

[0124] This battery pack has advantages corresponding to the aforementioned negative electrode active materials, which will not be elaborated further.

[0125] Generally, a battery pack includes multiple batteries as individual cells, which are connected to form the battery pack. These batteries can be electrically connected using methods conventional in the art, such as series connection, parallel connection, or a combination of these connection methods, without any particular limitation.

[0126] In another aspect, the present invention provides an electrical device comprising a battery as described above or a battery pack as described above.

[0127] The electrical equipment in the embodiments of the present invention can be conventional electrical equipment in the art, such as power equipment (e.g., electric vehicles, electric cars), electronic equipment (e.g., mobile phones, tablets, laptops, digital cameras, etc.), wearable devices (e.g., watches, bracelets, VR glasses, etc.), energy storage power stations, etc., and there are no particular limitations.

[0128] The negative electrode active material provided by the present invention will be described in detail below through specific embodiments.

[0129] Example 1

[0130] The method for preparing the negative electrode active material provided in this embodiment includes the following steps:

[0131] 1. Mix coal tar pitch (coking value 45%) with tetrahydrofuran (THF) at a mass ratio of 1:3 (45℃ water bath, magnetic stirring for 2 hours), remove undissolved particles by passing through a 200-mesh metal sieve; adjust the solid content of the solution to 10±0.5% (concentrate under reduced pressure using a rotary evaporator) to obtain the asphalt solution;

[0132] 2. Add the artificial graphite with a Dv50 of 15μm and the above asphalt solution into a high-speed disperser at a mass ratio of 1:2. First, stir at 500rpm for 20min for premixing, then stir at 2000rpm for 40min for coating, and finally stir at 800rpm for 60min to relieve stress. Temperature control: maintain 50±2℃ throughout the process (to avoid THF volatilization).

[0133] 3. Use a spray dryer: inlet air temperature 180℃, outlet air temperature 90℃, atomization pressure 0.3MPa, then perform programmed temperature rise: 2℃ / min to 300℃ (air atmosphere), hold for 2h to obtain the first precursor.

[0134] 4. Under N2 protection, the first precursor is heated to 600℃ at 5℃ / min and held for 1 hour for the first heat treatment. Then, it is heated to 1100℃ at 3℃ / min and held for 8 hours for the second heat treatment. Finally, it is cooled to room temperature at 10℃ / min. During the first and second heat treatments, a slight positive pressure of 50-100Pa is maintained in the carbonization furnace to prevent structural collapse.

[0135] 5. The particle size distribution is controlled by using an air jet mill (grading wheel speed 4000 rpm), and finally the material is obtained by passing it through a 325 mesh vibrating screen (coating thickness uniformity CV value < 8%).

[0136] The particle size distribution of the negative electrode active material and the ratio of the first carbon material to the second carbon material were tested using the following steps:

[0137] The analysis was performed using a Malvern Mastersizer 3000 with a wet dispersion-laser derivatization method: 0.20±0.01g of the negative electrode active material sample was weighed into a 100ml beaker, 3mL of surfactant was added, and deionized water was added to a final volume of 20.0±0.1mL. The beaker was sealed with a sealing film and placed in an ultrasonic machine (40KHz / 210W, 70% output power) for 5min. The laser intensity was 70-90%, and the detector light energy was <100. When the light shielding reached 5-15%, the test was started, and the particle size distribution and bulk density distribution curve of the negative electrode active material were obtained. The Dv50 value of the negative electrode active material was then output.

[0138] Graphite particles with a particle size close to Dv50 were selected as the target. Using the center of these particles as the origin, high-resolution TEM images were taken at four angles (45°, 135°, 225°, and 315°) on the upper left, upper right, lower left, and lower right sides. The instrument parameters were: accelerating voltage 200 kV, electron beam current density 10 pA / cm². 2The exposure time was 1.5 seconds, and the magnification was 730k, resulting in four images. The interlayer spacing must be clearly visible. The layers with a spacing less than 0.338 nm and arranged continuously and regularly constitute the active material core. Layers with a spacing greater than 0.338 nm constitute the carbon coating layer. Within the carbon coating layer, the interlayer spacing is mainly concentrated between 0.345 nm and 0.429 nm. Layers with a spacing greater than or equal to 0.345 nm and less than 0.386 nm constitute the first carbon material, and layers with a spacing greater than or equal to 0.386 nm and less than 0.429 nm constitute the second carbon material. The first carbon material also includes transition carbon materials with an interlayer spacing greater than or equal to 0.35 nm and less than or equal to 0.37 nm. The quantity ratios of the first carbon material, the second carbon material, and the transition carbon material in the first carbon material were measured using the following method: The straight-line distance from the active material core to the outer surface of the carbon coating layer was measured; this is the thickness of the carbon coating layer. The straight-line distance from the active material core to the outer surface of the carbon coating layer was also measured in the direction extending from the outer surface of the carbon coating layer to the active material core; this is the thickness *h* of the carbon coating layer. The region with a carbon coating layer thickness of *y* nm in the direction extending from the outer surface of the carbon coating layer to the active material core was designated as the outer coating layer. The region with a carbon coating layer thickness of *x* nm in the direction extending from the outer surface of the active material core to the carbon coating layer was designated as the inner coating layer. Then, the images of the inner and outer coating layers were analyzed separately using Gatan Digital. Micrograph software analyzes the data: The image is converted to integer mode. A scale bar is measured (a dashed line of the same length as the scale bar is drawn – input the corresponding length 5nm). Forty measurement regions are randomly selected. A 3*0.5nm range is selected along the vertical direction of the interlayer spacing in each selected region. A Fast Fourier Transform (FFT) is used to obtain an image. The distance between two adjacent peaks in the image is measured as one interlayer spacing. Five interlayer spacing values ​​are randomly selected for each selected region. Finally, a statistical distribution histogram is generated based on the 800 measured interlayer spacing values. After fitting and generating a distribution curve, the ratio of the first carbon material to the second carbon material in the inner and outer cladding layers, as well as the proportion of the transition carbon material to the first carbon material, are calculated based on the area of ​​the corresponding regions of the first carbon material, the second carbon material, and the transition carbon material on the distribution curve.

[0139] Example 2

[0140] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0141] In step 4 of the preparation process, the second heat treatment temperature is 900℃ and the holding time is 24h.

[0142] Example 3

[0143] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0144] In step 1 of the preparation process, the asphalt is replaced with oil-based asphalt with a coking value of 30%.

[0145] Example 4

[0146] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0147] In step 1 of the preparation process, the asphalt is replaced with asphalt with a coking value of 67%; in step 2, the mass ratio of graphite to asphalt solution is 2:1.

[0148] Example 5

[0149] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0150] In step 2 of the preparation process, the graphite is replaced with graphite with a Dv50 of 17 μm.

[0151] Example 6

[0152] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0153] In step 1 of the preparation process, THF is replaced with toluene.

[0154] Example 7

[0155] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0156] In step 1 of the preparation process, the asphalt is replaced with asphalt with a coking value of 67%; in step 2, the mass ratio of graphite to asphalt solution is 5:1.

[0157] Example 8

[0158] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0159] The preparation process does not use solvent to disperse the asphalt in step 1. Instead, asphalt with a coking value of 45% is directly mixed with graphite for coating.

[0160] Example 9

[0161] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that the asphalt in the preparation process is replaced with phenolic resin and the solvent is replaced with water.

[0162] Example 10

[0163] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that 3 wt% melamine is mixed into the asphalt during the preparation process.

[0164] Example 11

[0165] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0166] In step 1 of the preparation process, asphalt is replaced with acetylene.

[0167] Example 12

[0168] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0169] In step 4 of the preparation process, there is no first heat treatment stage.

[0170] Comparative Example 1

[0171] The negative electrode active material is the artificial graphite of Example 1.

[0172] Comparative Example 2

[0173] The negative electrode active material provided in this embodiment includes an active material core and a carbon coating layer covering at least a portion of the surface of the active material core; the carbon coating layer does not include a second carbon material.

[0174] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that:

[0175] The first precursor is heated to 1100℃ at 3℃ / min and held at that temperature for 55h for the second heat treatment. Finally, it is cooled to room temperature at 10℃ / min. During the heat treatment, a slight positive pressure of 50-100Pa is maintained in the carbonization furnace to prevent structural collapse.

[0176] Comparative Example 3

[0177] The negative electrode active material provided in this embodiment includes an active material core and a carbon coating layer covering at least a portion of the surface of the active material core; the carbon coating layer does not include a first carbon material.

[0178] The preparation method of the negative electrode active material provided in this embodiment is basically the same as that in Example 1, except that there is no second heat treatment stage in step 4.

[0179] The relevant parameters of the negative electrode active materials provided in all embodiments and comparative examples are shown in Table 1.

[0180] Table 1

[0181]

[0182]

[0183] Test case

[0184] The battery is prepared by sequentially using the negative electrode active materials provided in all the embodiments and comparative examples, including the following steps:

[0185] 1) Preparation of negative electrode:

[0186] The above-mentioned negative electrode active material, conductive agent carbon black, thickener CMC and binder SBR are mixed in a solid mass ratio of 100:1:1.6:1.8. The mixed powder is placed in a homogenizer, and deionized water is added as a solvent to mix and stir evenly to obtain a negative electrode slurry. The negative electrode secondary active material is selected according to the claims of this scheme. The negative electrode slurry is sieved (200 mesh screen) and then coated onto the negative electrode current collector aluminum foil. After drying in an oven at 105°C, it is then rolled and cut to obtain a negative electrode sheet.

[0187] 2) Preparation of the positive electrode:

[0188] The positive electrode active material, conductive agent carbon black, and binder PVDF are mixed in a mass ratio of 96:2:2. The mixed powder is placed in a vacuum mixer, and solvent N-methylpyrrolidone (NMP) is added and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry is sieved (through a 200-mesh sieve) and coated onto a positive electrode current collector aluminum foil. After drying in an oven at 150°C, it is then rolled and slit to obtain a positive electrode sheet.

[0189] 3) Electrolyte preparation:

[0190] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent. 1 wt% of vinylene carbonate (VC) is added to the mixed solvent, and then dry lithium salt LiPF6 is added to prepare an electrolyte with a LiPF6 concentration of 1 mol / L.

[0191] 4) Assemble the battery:

[0192] In an argon-filled glove box, the positive electrode, separator (specifically a polyethylene film), and negative electrode are stacked in sequence to obtain a battery cell. The separator must completely isolate the positive and negative electrode cells. The stacked battery cell is then placed into an aluminum-plastic film soft package and injected with the electrolyte. After vacuum sealing, settling, formation, cutting, and sealing, a lithium-ion battery is obtained.

[0193] 1. Initial effectiveness test:

[0194] In a constant temperature environment of 25℃, the battery was subjected to a 0.1C / 0.1C cycle test with a voltage range of 2.0V-3.8V (charged at 0.1C to a voltage of 3.8V, rested for 10 minutes, and then discharged at a 0.1C rate to a voltage of 2.0V, which is one cycle). The specific capacity of the battery during the first charge and the specific capacity during the first discharge were recorded, and the first charge and discharge efficiency of the battery was calculated based on these. The battery's first discharge efficiency (%) = first charge specific capacity / first discharge specific capacity * 100%. The specific test data are shown in Table 2.

[0195] 2. Charging rate test:

[0196] The battery was charged at 25℃ to 3.8V at 4C, left to stand for 30 minutes, and then discharged at 0.1C to 2.0V. This cycle was repeated 3 times. The charging efficiency of the battery was calculated using the charging and discharging data from the 3rd cycle. The battery charging rate (%) = 3rd discharge specific capacity (0.1C) / 3rd charge specific capacity (4C) * 100%. Specific test data are shown in Table 2.

[0197] 3. Loop testing:

[0198] In a constant temperature environment of 25℃, the battery was charged to 3.8V at 1C constant current and left to stand for 10 minutes; then discharged to 2.0V at 1C constant current and left to stand for 10 minutes; the cycle was terminated after 1000 cycles or when the capacity retention rate was less than 60%. Specific test data are shown in Table 2.

[0199] Table 2

[0200]

[0201]

[0202] As shown in Table 2, compared with the comparative example, the negative electrode active material of the embodiment helps to further improve the rate and cycle performance of the battery.

[0203] Furthermore, the data from Examples 1-7 and Examples 8-12 show that the schemes in Examples 1-7 can further improve the cycle performance of the battery by reasonably controlling the distribution of the first carbon material and the second carbon material.

[0204] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A negative electrode active material, characterized in that, It includes an active material core and a carbon coating layer covering at least a portion of the surface of the active material core; the carbon coating layer includes a first carbon material and a second carbon material, the interlayer spacing of the first carbon material is m, and the interlayer spacing of the second carbon material is n, wherein 0.345≤m<0.386nm, 0.386≤n<0.429nm; The carbon coating layer includes an inner coating layer extending outward from the core of the active material. and, an outer coating extending inward from the outer surface of the carbon coating; Furthermore, in the inner coating layer, the ratio of the first carbon material to the second carbon material is (85~100):(0~15). In the outer coating layer, the ratio of the first carbon material to the second carbon material is (60~85):(15~40).

2. The negative electrode active material according to claim 1, characterized in that, The first carbon material includes a transition carbon material with an interlayer spacing of 0.35 nm to 0.37 nm; In the inner coating layer, the transition carbon material accounts for 10% to 40% of the amount of the first carbon material; And / or, in the outer coating layer, the proportion of the transition carbon material to the first carbon material is 0 to 10%.

3. The negative electrode active material according to any one of claims 1-2, characterized in that, The negative electrode active material I D / I G Let z be the integer part of the equation, and 0.7 ≤ z ≤ 2.

1.

4. The negative electrode active material according to any one of claims 1-2, characterized in that, The active material core includes graphite; And / or, the carbon coating layer includes at least one of soft carbon, hard carbon, and heteroatom-doped carbon materials.

5. The negative electrode active material according to claim 3, characterized in that, The active material core includes graphite; And / or, the carbon coating layer includes at least one of soft carbon, hard carbon, and heteroatom-doped carbon materials.

6. The negative electrode active material according to any one of claims 1-2 and 5, characterized in that, The thickness of the carbon coating layer is h, where 5nm < h ≤ 50nm; And / or, the specific surface area of ​​the negative electrode active material is 0.5~2 m². 2 / g.

7. The negative electrode active material according to claim 3, characterized in that, The thickness of the carbon coating layer is h, where 5nm < h ≤ 50nm; And / or, the specific surface area of ​​the negative electrode active material is 0.5~2 m². 2 / g.

8. The negative electrode active material according to claim 4, characterized in that, The thickness of the carbon coating layer is h, where 5nm < h ≤ 50nm; And / or, the specific surface area of ​​the negative electrode active material is 0.5~2 m². 2 / g.

9. A method for preparing a negative electrode active material as described in any one of claims 1-8, characterized in that, Includes the following steps: 1) The carbon source and the active material are stirred to coat at least a portion of the surface of the active material with the carbon source, thereby obtaining a first precursor; 2) The first precursor is heat-treated in a protective atmosphere to obtain the negative electrode active material; The heat treatment includes the following process: a first heat treatment at a heating rate of 2-20℃ / min to 500-700℃ for 1-6 hours, followed by a second heat treatment at a heating rate of 2-20℃ / min to 900-1200℃ for 6-48 hours to obtain the negative electrode active material; during the first and second heat treatments, a slight positive pressure of 50-100 Pa is maintained in the carbonization furnace; the carbon source includes at least one of asphalt, heavy oil, and resin.

10. The preparation method according to claim 9, characterized in that, The process of stirring the carbon source and the active material specifically includes: stirring the organic solvent containing the carbon source with the active material.

11. A negative electrode sheet, characterized in that, Includes the negative electrode active material according to any one of claims 1-8 or the negative electrode active material prepared by the preparation method according to any one of claims 9-10.

12. A battery, characterized in that, Includes the negative electrode sheet as described in claim 11.

13. An electrical appliance, characterized in that, Includes the battery as described in claim 12.

Citation Information

Patent Citations

  • Preparation method of carbon-coated graphite anode material

    CN109638260A

  • Graphite negative electrode material and preparation method and application thereof

    CN115566152A

  • Negative active material, method for preparing same, and electrochemical device including same

    CN115775877A

  • Method for preparing a carbon cathode material of lithium ion battery

    CN1567617A