Metal organic framework material composite catalyst and preparation method thereof
By loading transition metal oxide nanoparticles onto the metal-organic framework material UiO-66, a composite catalyst was constructed, which solved the problems of structural collapse and limited active sites in traditional molecular sieve composite materials in strongly alkaline amine solutions, and achieved more efficient CO2 capture and utilization.
Patent Information
- Application Number
- CN202511297757.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-11
- Publication Date
- 2026-01-16
AI Technical Summary
In existing technologies, traditional molecular sieve composite materials are prone to structural collapse in strongly alkaline amine solutions, have limited active sites, and insufficient cycle stability, resulting in high energy consumption for desorption of CO2-rich amine solutions.
Using metal-organic framework material UiO-66 as a support, a composite catalyst was constructed by loading transition metal oxide nanoparticles (Fe2O3, CoO, CeO2). ZrO2@C support was obtained by high-temperature pyrolysis, which enhanced the active site density and alkali resistance of the catalyst.
It significantly reduced the energy consumption of CO2-rich amine solution desorption, improved catalytic efficiency, and achieved more efficient CO2 capture and utilization.
Smart Images

Figure CN121338749A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts for CO2 capture and utilization, and more particularly to a metal-organic framework composite catalyst and its preparation method. Background Technology
[0002] In the field of CO2 capture in coal-fired power plants, chemisorption technology based on the alkanolamine method is widely used due to its maturity. However, the regeneration process of CO2-rich amine solutions suffers from excessive energy consumption. Studies have shown that solid acid catalysts can effectively reduce desorption energy consumption, but traditional molecular sieve composite materials are prone to structural collapse in strongly alkaline amine solutions and have defects such as limited active sites and insufficient cycle stability.
[0003] Chinese patent application CN109453801A discloses a method for desorbing Fe2O3 / ZrO2 / SO4 from CO2-rich amine solutions. 2- - A method for preparing a molecular sieve composite catalyst, wherein the composite catalyst is a Fe2O3-modified superstrong solid acid catalyst ZrO2 / SO4 2- The mixture is loaded onto a molecular sieve support; its preparation method includes the following steps: dissolving soluble iron salt and zirconium sulfate in methanol solution to obtain mixture A; heating mixture A at 50°C for 1 h to obtain mixture B; cooling mixture B to room temperature, adding molecular sieve powder and stirring for 5 h to obtain mixture C; subjecting mixture C to ultrasonic treatment for more than 0.5 h to obtain mixture D; drying and calcining mixture D to obtain Fe2O3 / ZrO2 / SO4. 2- - Molecular sieve composite catalyst. The composite catalyst in this scheme can reduce the energy consumption of desorption of CO2-rich amine solutions, but the catalytic effect needs to be improved. Summary of the Invention
[0004] To overcome the problems existing in the prior art, the present invention provides a metal-organic framework composite catalyst and its preparation method, which further reduces the energy consumption of desorption of CO2-rich amine solutions. The specific technical solution is as follows.
[0005] A method for preparing a metal-organic framework composite catalyst includes the following steps:
[0006] S1. Add a metal nitrate solution to a UiO-66 carrier, stir, let stand, and dry to obtain a UiO-66 carrier loaded with metal nitrates. The metal nitrate solution includes one or more of Fe(NO3)3·9H2O solution, Co(NO3)2·6H2O solution, and Ce(NO3)3·6H2O solution.
[0007] S2. The UiO-66 support loaded with metal nitrates described in S1 is calcined in an inert gas to obtain the xYO-ZrO2@C catalyst, wherein Y is one or more of Fe, Co, and Ce, and x represents the mass percentage content of Fe, Co, and Ce.
[0008] During the calcination process, the UiO-66 support loaded with metal nitrates forms a ZrO2@C support with stability and alkali resistance. The strong interaction between the metal oxide and the ZrO2@C support increases the density of active sites and improves the catalytic efficiency of desorption of CO2-rich amine solutions.
[0009] In one preferred embodiment, the metal nitrate solution in S1 is a Fe(NO3)3 solution, and the xYO-ZrO2@C catalyst in S2 is an xFe2O3-ZrO2@C catalyst, where x represents the mass percentage content of Fe. The xFe2O3-ZrO2@C catalyst has higher catalytic efficiency and can further reduce the energy consumption of desorption of carbon dioxide-rich amine solutions.
[0010] In one preferred embodiment, the iron content of the UiO-66 support is 2.5% to 7.5% by mass, preferably 2.5% to 5%. This range of iron content can further improve catalytic efficiency and reduce the energy consumption of desorption of carbon dioxide-rich amine solutions.
[0011] In one preferred embodiment, Fe(NO3)3·9H2O solution is added dropwise to the UiO-66 carrier in S1.
[0012] In one preferred embodiment, the inert gas in S2 is N. v The calcination temperature is 400–600℃, the heating rate is 4–6℃ / min, and the calcination time is 2–4 h. Calcination process parameters within this range are beneficial for forming a stable and alkali-resistant ZrO2@C support, increasing the density of active sites.
[0013] In one preferred embodiment, the stirring time in S1 is 15-45 min, and the settling time is 2-4 h.
[0014] In one preferred embodiment, the drying temperature in S1 is 70–90°C, and the drying time is 10–14 hours.
[0015] In one preferred embodiment, the preparation method of the UiO-66 carrier in S1 includes the following steps:
[0016] ZrCl4 was dissolved in dimethylformamide, and a mixture of phthalic acid, concentrated hydrochloric acid and benzoic acid was added. The mixture was ultrasonically mixed and reacted at 100–140 °C for 20–28 h. After cooling to room temperature, the product was collected by centrifugation.
[0017] The washing product was vacuum dried to obtain the UiO-66 carrier.
[0018] The UiO-66 carrier prepared by this method has a more regular shape and a larger particle size.
[0019] The molar ratio of ZrCl4 to phthalic acid is 1:1.
[0020] In one preferred embodiment, the mass-to-volume ratio of ZrCl4, phthalic acid, benzoic acid, and dimethylformamide is 3–5 mmol: 3–5 mmol: 70–90 mmol: 60–80 mL.
[0021] The present invention also discloses a composite catalyst comprising a calcined UiO-66 support, wherein the calcined UiO-66 support is loaded with a metal oxide, wherein the metal oxide is Fe2O3, CoO, or CeO2; preferably Fe2O3, wherein the Fe accounts for 2.5% to 7.5% of the mass percentage of the UiO-66 support; or a composite catalyst prepared by the preparation method described above.
[0022] Metal-organic frameworks (MOFs) have shown great potential in catalysis due to their tunable pore structure, high specific surface area, and excellent chemical stability. Zirconium-based MOFs, particularly UiO-66, possess excellent alkali resistance and thermal stability due to the strong Zr-O coordination bonds in their metal clusters [Zr6O4(OH)4]. Furthermore, MOFs can be synthesized in situ or modified post-synthesized to introduce functional active sites into organic ligands or metal clusters, providing abundant acidic sites for catalytic reactions.
[0023] Moderate calcination of MOF materials can yield derivative materials that significantly enhance alkali resistance while retaining the basic morphological characteristics and key properties of MOFs (such as high specific surface area). The calcination process, through the partial sacrifice of organic ligands, can expand the pore size of the material to some extent, facilitating the access of reactant molecules to internal active sites and enhancing mass transfer efficiency, while also increasing the surface acidity. However, the catalytic activity of single MOF-derived materials (such as ZrO2@C) still needs to be improved.
[0024] Compared with the prior art, the present invention has the following beneficial effects.
[0025] This invention uses ZrO2@C obtained from the high-temperature pyrolysis of UiO-66 as a support to construct a composite catalytic material by loading transition metal oxide nanoparticles (Fe2O3, CoO, CeO2). In this invention, the ZrO2@C support inherits the framework stability and alkali resistance of UiO-66, and the strong interaction between the metal oxide and the support increases the density of active sites, further regulating the metal loading and optimizing the catalytic efficiency. Attached Figure Description
[0026] Figure 1 The images are SEM images of the catalysts, where (a) UiO-66; (b) ZrO2@C; and (c) Fe2O3-ZrO2@C.
[0027] Figure 2 In the image, a is the HR-TEM image of the Fe2O3-ZrO2@C catalyst; b is the selected area electron diffraction (SAED) pattern; and c is the TEM-EDS pattern.
[0028] Figure 3 In the figure, a is the XRD pattern of the catalyst; b is the FT-IR pattern of the catalyst; c is the N2 adsorption-desorption curve of the catalyst; and d is the pore size distribution curve of the catalyst. Detailed Implementation
[0029] The present invention will now be described in further detail with reference to the accompanying drawings.
[0030] The CO2-rich amine solutions in the following examples and comparative examples were prepared by continuously passing pure CO2 gas through a prepared amine solution (MEA) to obtain a CO2-rich amine solution. The final loading was confirmed by titrating the CO2-rich amine solution with 1 mol / L dilute hydrochloric acid. To eliminate the influence of solution loading differences on desorption experiments, this application prepared a large batch of solutions at once to ensure that desorption experiments performed in the same amine solution were all under the same loading. The MEA solution concentration was 5 mol / L, and the CO2 loading in the amine solution was 5.3 mol CO2 / mol amine.
[0031] Comparative Example 1
[0032] Preparation of UiO-66 carrier material
[0033] 4 mmol ZrCl4 was dissolved in 72 mL DMF, and 4 mmol H2BDC, 8 mmol concentrated hydrochloric acid, and 80 mmol benzoic acid were added to the solution. After sonication until homogeneous, the solution was transferred to a reaction vessel and reacted at 120 °C for 24 h. After the reaction was completed, the mixture was cooled to room temperature, centrifuged to collect the solid product, and washed three times each with DMF and anhydrous ethanol to remove residual reactants. The obtained product was dried in a vacuum oven at 80 °C for 12 h to obtain the UiO-66 support material.
[0034] Preparation of ZrO2@C catalyst
[0035] The UiO-66 support material was placed in a tube furnace and heated to 500℃ at a heating rate of 5℃ / min under N2 atmosphere protection, and then calcined at a constant temperature for 3h to finally obtain the ZrO2@C catalyst.
[0036] Desorption of amine-rich solution
[0037] 200 mL of carbon-rich monoethanolamine (MEA) solution was placed in a three-necked flask, and 1.25 g of catalyst was added to the solution. The oil bath temperature was adjusted to 90 °C, and the magnetic stirrer was turned on. Before the experiment, nitrogen (N2) was introduced into the pipeline at a flow rate of 500 mL / min to purge any carbon dioxide (CO2) that might be present in the pipeline. The nitrogen gas was also used as a carrier gas, and after mixing with the CO2 released during the subsequent desorption process, the mixture was introduced into the CO2 analyzer for continuous measurement.
[0038] The experiment consisted of a heating phase and an isothermal phase. The heating phase involved gradually increasing the amine solution temperature from the initial temperature to a preset maximum temperature (90°C) to examine the catalyst's catalytic desorption performance at lower temperatures. The isothermal phase involved maintaining the solution temperature at the maximum temperature (90°C). Throughout the CO2 desorption process, the CO2 analyzer's detection signal showed an initial increase followed by a decrease, with a desorption time of 50 minutes. The three-necked flask was equipped with a condenser to maintain a stable concentration of the amine solution within the flask, and an ice cooler and a drying tube were connected sequentially before the CO2 analyzer inlet to prevent water vapor from entering the analyzer and causing damage.
[0039] Example 1
[0040] The preparation method of UiO-66 carrier material is the same as that of Comparative Example 1.
[0041] Preparation of Fe2O3-ZrO2@C catalyst
[0042] A pre-prepared Fe(NO3)3·9H2O solution, containing 2.5% iron by mass, was added dropwise to the UiO-66 support. The mixture was stirred thoroughly for 30 min, followed by standing at room temperature for 3 h. The treated mixture was then transferred to an 80℃ oven and dried for 12 h to obtain the precursor. This precursor was placed in a tube furnace and heated to 500℃ at a heating rate of 5℃ / min under a N2 atmosphere, and calcined at this temperature for 3 h to finally obtain the 2.5Fe2O3-ZrO2@C catalyst.
[0043] The desorption method for the carbon-rich amine solution is the same as that for Comparative Example 1.
[0044] First, the morphology of the prepared catalyst was analyzed. Figure 1 In the images, the morphologies of the UiO-66 precursor, the thermally decomposed ZrO2@C, and the Fe2O3-ZrO2@C catalyst can be clearly observed. The untreated UiO-66 precursor exhibits relatively sharp edges and a smooth surface, displaying a regular octahedral structure. While the ZrO2@C obtained after treatment under a high-temperature N2 atmosphere retains the octahedral outline, the edges become relatively blurred due to shrinkage during carbonization. For Fe2O3-ZrO2@C, the octahedral surface is observed to be modified by Fe2O3 particles.
[0045] The morphology of Fe2O3-ZrO2@C was determined by HR-TEM ( Figure 2 Further analysis revealed lattice fringes of 0.270 nm and 0.295 nm in the catalyst, corresponding to the (104) crystal plane of Fe2O3 and the (011) crystal plane of ZrO2, respectively. Furthermore, the nanoparticles with clearly defined lattice fringes were encapsulated by an amorphous carbon structure. Additionally, the selected region electron diffraction (SAED) results for Fe2O3-ZrO2@C showed… Figure 2 In (b), the three diffraction rings correspond to the (121), (112), and (011) crystal planes of ZrO2, respectively. Figure 2 As shown in (c), TEM-EDS further confirmed that Zr, O, Fe and C elements were uniformly distributed on the Fe2O3-ZrO2@C surface.
[0046] Example 2
[0047] The preparation method of UiO-66 carrier material is the same as that of Comparative Example 1.
[0048] Preparation of Fe2O3-ZrO2@C catalyst
[0049] A pre-prepared Fe(NO3)3·9H2O solution, containing 5% iron by mass, was added dropwise to the UiO-66 support. The mixture was stirred thoroughly for 30 min, followed by standing at room temperature for 3 h. The treated mixture was then transferred to an 80℃ oven and dried for 12 h to obtain the precursor. This precursor was placed in a tube furnace and heated to 500℃ at a heating rate of 5℃ / min under a N2 atmosphere, and calcined at this temperature for 3 h to finally obtain the 5Fe2O3-ZrO2@C catalyst.
[0050] The desorption method for the carbon-rich amine solution is the same as that for Comparative Example 1.
[0051] Example 3
[0052] The preparation method of UiO-66 carrier material is the same as that of Comparative Example 1.
[0053] Preparation of Fe2O3-ZrO2@C catalyst
[0054] A pre-prepared Fe(NO3)3·9H2O solution, containing 7.5% iron by mass, was added dropwise to the UiO-66 support. The mixture was stirred thoroughly for 30 min, followed by standing at room temperature for 3 h. The treated mixture was then transferred to an 80℃ oven and dried for 12 h to obtain the precursor. This precursor was placed in a tube furnace and heated to 500℃ at a heating rate of 5℃ / min under a N2 atmosphere, and calcined at this temperature for 3 h to finally obtain the 7.5Fe2O3-ZrO2@C catalyst.
[0055] The desorption method for the carbon-rich amine solution is the same as that for Comparative Example 1.
[0056] Table 1 Comparison of catalyst desorption energy consumption in the examples
[0057] catalyst Desorption energy consumption ratio % Desorption energy consumption reduced by %. blank 100% 0% Comparative Example 1 34.6% 65.4% Example 1 29.7% 70.3% Example 2 25.0% 75.0% Example 3 33.9% 66.1%
[0058] This application selects a heat transfer model to calculate the desorption energy consumption. The heat load is calculated by determining the ratio of steady-state heat transfer to the amount of CO2 removed during a certain time in the desorption process. The Fourier heat conduction equation is used to calculate the oil bath heating, and the calculation is performed using formula (1):
[0059]
[0060] In the formula, q is the steady-state heat transfer rate in J / s, k is the thermal conductivity of the heat-resistant glass used in the flask material in W / (m·K), and A is the cross-sectional area normal to the heat flow direction in m². 2 dT / dx is the temperature gradient (K·m) -1 The temperature difference dT is the difference between the oil temperature and the temperature of the inner wall of the flask, and dx is the glass wall thickness.
[0061] The desorption energy consumption of the solvent regeneration process is calculated as shown in formula (2):
[0062]
[0063] Since this device is carried out in a simple batch reactor without insulation measures, the calculated heat load is slightly higher than the actual value. Therefore, in order to better evaluate the catalyst performance, the parameter of relative heat load (%) is introduced, as shown in formula (3):
[0064]
[0065] Q blank Q represents the desorption energy consumption of the blank experimental group. catalyst The energy consumption for desorption of the amine system after the addition of a catalyst.
[0066] The experimental procedure for the blank experiment is the same as that for the desorption experiment with a catalyst, except that no catalyst is added.
[0067] The desorption energy consumption of each catalyst, ranked from highest to lowest, is: 5Fe2O3-ZrO2@C > 2.5Fe2O3-ZrO2@C > 7.5Fe2O3-ZrO2@C. Due to the excellent electrical conductivity of carbonaceous materials, the channels (Zr-OC) formed between them and metal ions can facilitate charge transfer and accelerate the reaction. Furthermore, the introduced metal oxides can form MO-Zr bonds (M = metal) with ZrO2, inducing interfacial charge redistribution. Among these, the 5Fe2O3-ZrO2@C catalyst showed the best catalytic effect, reducing desorption energy consumption by 75% compared to the control group.
[0068] Example 4
[0069] The preparation method of UiO-66 carrier material is the same as that of Comparative Example 1.
[0070] The preparation method of the CoO-ZrO2@C catalyst is the same as in Example 2, except that the CoO-ZrO2@C catalyst is prepared by replacing Fe(NO3)3·9H2O with an equal molar amount of Co(NO3)2·6H2O.
[0071] The desorption method for the carbon-rich amine solution is the same as that for Comparative Example 1.
[0072] Example 5
[0073] The preparation method of UiO-66 carrier material is the same as that of Comparative Example 1.
[0074] The preparation method of CeO2-ZrO2@C catalyst is the same as in Example 2, except that Fe(NO3)3·9H2O is replaced with an equal molar amount of Ce(NO3)3·6H2O to obtain CeO2-ZrO2@C catalyst.
[0075] The desorption method for the carbon-rich amine solution is the same as that for Comparative Example 1.
[0076] Table 2 Comparison of catalyst desorption energy consumption in the examples
[0077] catalyst Desorption energy consumption ratio % Desorption energy consumption reduced by %. blank 100% 0% Comparative Example 1 UiO-66 96.6% 3.4% Comparative Example 1 34.6% 65.4% Example 2 25% 75% Example 4 31.5% 68.5% Example 5 36.5% 63.5%
[0078] The order of decrease in desorption energy consumption for each catalyst, from highest to lowest, is: Fe2O3-ZrO2@C > CoO-ZrO2@C > ZrO2@C ≈ CeO2-ZrO2@C. Fe2O3-ZrO2@C showed the greatest reduction in CO2 desorption energy consumption, followed by CoO-ZrO2@C. However, compared to the Fe2O3 and CoO-supported samples, the introduction of CeO2 did not significantly improve the catalytic performance of the ZrO2@C composite material. This may be because Fe2O3 and CoO, as transition metal oxides, have stronger interactions with the ZrO2@C support, resulting in more uniform dispersion of the formed nanoparticles. CeO2, on the other hand, tends to aggregate more easily during high-temperature calcination, forming larger particles that cover the pore surface.
[0079] Table 3 Catalyst specific surface area and pore structure
[0080]
[0081] Figure 3 (a) XRD patterns of composite materials (ZrO2, ZrO2@C, and MxOy-ZrO2@C) based on the UiO-66 framework are shown. All catalysts exhibit broad diffraction peaks at 30.3°, 50.5°, and 60.2°, corresponding to the crystal planes of ZrO2 (JCPDS79-1764). However, no obvious characteristic diffraction peaks were observed, possibly due to the relatively uniform dispersion of metal nanoparticles on the support surface. To confirm the loading of metal oxides, further analysis of infrared spectra was performed ( Figure 3 (b)). Fe2O3-ZrO2@C, CeO2-ZrO2@C, and CoO-ZrO2@C were all found to be at 1080 cm⁻¹. -1 The presence of tensile vibration peaks for MOM (M = Fe, Ce, and Co) at 1620 cm⁻¹ indicates that Fe, Ce, or Co were successfully loaded onto the ZrO₂@C support. Furthermore, compared to ZrO₂@C and ZrO₂ supports, MxOy-ZrO₂@C exhibits higher tensile vibration peaks at 1620 cm⁻¹. -1 (OH bending vibration) and 3350cm -1 The absorption peak intensity at the (OH stretching vibration) was significantly enhanced, and these spectral features are attributed to the presence of coordinated and absorbed water in the sample. This confirms that the introduction of metal oxides can promote water adsorption and coordination, forming hydroxyl groups. N2 adsorption-desorption characterization determined information such as the specific surface area and pore structure of the catalyst. Figure 3As shown in (c)-(d) and Table 3, the specific surface area and pore size of CeO2-ZrO2@C show significant decreases and increases compared to the other three catalysts. This may be due to the large difference in lattice parameters between CeO2 and ZrO2, making it difficult to form stable chemical bonds, and thus they tend to exist on the support surface through physical adsorption. This results in the blockage of micropores on the support surface and the formation of new macropores. A small specific surface area limits the contact between the reaction products and the active sites. Compared to the original ZrO2@C, the catalysts with embedded Fe2O3 or CoO may have altered the original pore channel structure, resulting in an increase in specific surface area but a decrease in average pore size.
[0082] The embodiments of the present invention have been described above. Unless otherwise specified, the embodiments and features described in the embodiments can be combined with each other. The present invention is not limited to the specific embodiments described above; the specific embodiments described above are merely illustrative and not limiting. Those skilled in the art, under the guidance of the present invention, can make many modifications without departing from the spirit and scope of the claims, and all of these modifications fall within the scope of protection of the present invention.
Claims
1. A method for preparing a metal-organic framework composite catalyst, comprising the following steps: S1, adding a metal nitrate solution into a UiO-66 carrier, stirring, standing, and drying to obtain a UiO-66 carrier loaded with a metal nitrate, wherein the metal nitrate solution comprises one or more of Fe (NO3) 3·9H2O solution, Co (NO3) 2·6H2O solution, and Ce (NO3) 3·6H2O solution; S2, calcining the UiO-66 carrier loaded with the metal nitrate in an inert gas to obtain an xYO-ZrO2@C catalyst, wherein Y is one or more of Fe, Co, and Ce, and x represents the mass percentage content of Fe, Co, and Ce.
2. The preparation method of the composite catalyst according to claim 1, characterized in that, In S1, the metal nitrate solution is Fe (NO3) 3·9H2O solution, and in S2, the xYO-ZrO2@C catalyst is an xFe2O3-ZrO2@C catalyst, wherein x represents the mass percentage content of Fe.
3. The method of claim 2, wherein the composite catalyst is prepared by the steps of: The mass percentage of iron in the UiO-66 carrier is 2.5%-7.5%, preferably 2.5%-5%.
4. The method of claim 2, wherein the composite catalyst is prepared by the steps of: In S1, the Fe (NO3) 3 solution is added dropwise into the UiO-66 carrier.
5. The method of claim 1, wherein the composite catalyst is prepared by the steps of: In S2, the inert gas is N2, the calcination temperature is 400-600℃, the heating rate is 4-6℃ / min, and the calcination time is 2-4h.
6. The method of claim 1-5, wherein the composite catalyst is prepared by the steps of: In S1, the stirring time is 15-45min, and the standing time is 2-4h.
7. The method of claim 1-5, wherein the composite catalyst is prepared by the steps of: In S1, the drying temperature is 70-90℃, and the drying time is 10-14h.
8. The method of claim 1-5, wherein the composite catalyst is prepared by the steps of: The method for preparing the UiO-66 carrier in S1 comprises the following steps: dissolving ZrCl4 in dimethylformamide, adding a mixed solution of phthalic acid and concentrated hydrochloric acid, and benzoic acid thereto, ultrasonically mixing them uniformly, and reacting at 100-140℃ for 20-28h, and then centrifuging the product after cooling to room temperature; washing the product and vacuum drying to obtain the UiO-66 carrier.
9. The method of claim 8, wherein the composite catalyst is prepared by the steps of: The mass-volume ratio of ZrCl4, phthalic acid, benzoic acid, and dimethylformamide is 3-5mmol: 3-5mmol: 70-90mmol: 60-80mL.
10. A composite catalyst comprising a calcined UiO-66 support, characterized in that, The calcined UiO-66 carrier is loaded with metal oxides, and the metal oxides are Fe2O3, CoO, and CeO2; preferably Fe2O3, and the mass percentage of Fe in the UiO-66 carrier is 2.5%-7.5%; or a composite catalyst prepared by the method of any one of claims 1-9.
Citation Information
Patent Citations
Preparation method of molecular sieve composite catalyst Fe2O3 / ZrO2 / SO42 for desorbing CO2-rich amine solution
CN109453801A