Corrosion inhibition inhibitor for hydrochloric acid pickling as well as preparation method and application of corrosion inhibition inhibitor
By preparing a hydrochloric acid pickling corrosion inhibitor containing hexamethylenetetramine, ferric chloride and other components, a protective film is formed to prevent metal corrosion, which solves the problems of poor corrosion inhibitor performance and poor environmental performance in the existing technology, and achieves efficient metal protection and acid conservation.
Patent Information
- Application Number
- CN202511502447.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-21
- Publication Date
- 2026-01-16
AI Technical Summary
In the existing hydrochloric acid pickling process, the concentration of corrosion inhibitors is high, the inhibition effect is limited, and the environmental performance is poor, resulting in metal surface corrosion, large acid consumption, and serious acid mist emissions.
A hydrochloric acid pickling corrosion inhibitor composed of hexamethylenetetramine, ferric chloride, ethyl silicate, glacial acetic acid, dibutyl phthalate, sodium hydroxide, and ethylenediaminetetraethanol is used to form a protective film to prevent the metal from contacting H+ ions and inhibit the corrosion reaction.
It significantly reduces metal corrosion and acid consumption, improves the surface finish of strip steel, reduces acid mist emissions, is environmentally friendly, has a low concentration, and high thermal stability.
Smart Images

Figure CN121344612A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal surface treatment technology, specifically relating to a corrosion inhibitor for hydrochloric acid pickling, its preparation method, and its application. Background Technology
[0002] In the hydrochloric acid pickling process of hot-rolled strip steel, high-temperature hydrochloric acid and shallow-tank jet turbulent pickling technology are commonly used to thoroughly remove the iron oxide scale from the surface of the hot-rolled strip steel. When the hot-rolled steel plate is immersed in the acid solution, the actual pickling reaction does not begin immediately. As a first step, the acid solution must come into contact with the metallic iron through the cracks in the iron oxide scale to generate an electromotive force. Only when the chemical reaction has progressed to a certain extent can it be considered that the actual pickling has begun. In a turbulent pickling system, the rapidly flowing acid solution helps the acid solution penetrate into the cracks in the oxide scale more quickly, thereby accelerating the chemical reaction of pickling. After the iron oxide scale is dissolved, the acid solution will directly corrode the metal surface, causing metal dissolution, which is undesirable. To prevent the acid solution from corroding the metal surface and to reduce the consumption of pickling solution, it is necessary to add a suitable pickling corrosion inhibitor to the pickling solution. The biggest feature of pickling corrosion inhibitors is that they provide effective protection for the metal surface without affecting the pickling efficiency. Although existing corrosion inhibitors can partially inhibit corrosion, they have problems such as high concentration, limited inhibition effect, and poor environmental friendliness. Summary of the Invention
[0003] To address the problems in the prior art, this invention provides a corrosion inhibitor for hydrochloric acid pickling, its preparation method, and its application. It can significantly inhibit the corrosion of the metal substrate by the acid solution while ensuring pickling efficiency, and reduce iron loss, hydrogen embrittlement, and acid mist emissions.
[0004] The technical solution of this invention is: A corrosion inhibitor for hydrochloric acid pickling, comprising the following components by mass percentage: Hexamethylenetetramine 10%~20%; 2% ferric chloride; Ethyl silicate 3%~5%; 2% glacial acetic acid; Dibutyl phthalate 3%~5%; Sodium hydroxide 10%; 1%~3% ethylenediaminetetraethanol; The remainder is demineralized water.
[0005] Furthermore, in the aforementioned hydrochloric acid pickling corrosion inhibitor, the density of the inhibitor is 1.000~1.150 g / cm³. 3 The pH value is 3~6.
[0006] Furthermore, in the above-mentioned hydrochloric acid pickling corrosion inhibitor, the concentration of the inhibitor added to the hydrochloric acid pickling solution is 0.5~1‰ (corrosion inhibitor weight g / regenerated acid weight g).
[0007] Furthermore, the above-mentioned hydrochloric acid pickling corrosion inhibitor has an inhibition rate of 70-90%.
[0008] This invention also discloses a method for preparing the above-mentioned corrosion inhibitor for hydrochloric acid pickling, comprising the following steps: Add demineralized water to the reaction vessel; Add dibutyl phthalate, sodium hydroxide solution, hexamethylenetetramine, ethyl silicate, glacial acetic acid, ethylenediaminetetraethanol and ferric chloride in sequence; Shake or stir after each addition until a clear, dark red liquid is formed.
[0009] The present invention also discloses the application of the above-mentioned corrosion inhibitor for hydrochloric acid pickling in the hydrochloric acid pickling process of hot-rolled strip steel.
[0010] The mechanism of action of this invention is as follows: No pickling inhibitor is added to the pickling solution, and the H in the acid solution + The ions will react directly with the metallic iron matrix to produce ferrous chloride and H2: Fe + 2HCl → FeCl2 + H2.
[0011] After adding pickling corrosion inhibitor to the acid solution, the NH4+ in the corrosion inhibitor... 3+ The complex R forms a "protective film" with the metal ions through coordination bonds, preventing the metal matrix from coming into contact with H+ ions and undergoing a chemical reaction. This inhibits the redox reaction of iron ions, avoiding further localized corrosion. (R-NH) 2+ H + →R-NH 3+ .
[0012] Advantages and beneficial effects of the present invention: 1. Using the inhibitor of this invention reduces the direct corrosion of metals by acid, reduces iron loss by about 90%, reduces acid consumption by 10%, and increases efficiency by about 20 yuan per ton of steel. 2. The inhibitor of this invention effectively suppresses the generation of acid mist, reduces the amount of acid volatilization, and effectively improves the on-site working environment; 3. When the inhibitor of the present invention is added to the acid solution of the hydrochloric acid pickling unit, the surface smoothness and brightness of the strip steel will be improved by 30%, avoiding corrosion spots and hydrogen bubble scars on the metal surface, minimizing surface stains, and preventing hydrogen embrittlement. 4. Compared with other similar corrosion inhibitors, the inhibitor added in this invention has a low concentration (0.5~1‰), good thermal stability, and is environmentally friendly and safe. Attached Figure Description
[0013] Figure 1 Flowchart of hydrochloric acid pickling process for hot-rolled strip steel; Figure 2 This is a comparison diagram of the reaction of hot-rolled strip steel in pickling solution with and without corrosion inhibitor in Example 1; Figure 3 Comparison of hot-rolled strip steel from Example 1 after immersion in pickling solution with and without corrosion inhibitor for 30 minutes; Figure 4 This is a diagram from the experiment in Example 2; Figure 5 This is a graph showing the test results of the corrosion inhibition rate in Example 2; Figure 6 The graph shows the iron loss weight results for Example 2. Detailed Implementation
[0014] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and should not be used to limit the scope of the present invention.
[0015] Example 1 This embodiment discloses a corrosion inhibitor for hydrochloric acid pickling, which is composed of the following components by mass percentage: hexamethylenetetramine 10%; ferric chloride 2%; ethyl silicate 3%; glacial acetic acid 2%; dibutyl phthalate 3%; sodium hydroxide 10%; ethylenediaminetetraethanol 1%; and the balance being demineralized water.
[0016] The preparation method is as follows: add dibutyl phthalate, sodium hydroxide solution, hexamethylenetetramine, ethyl silicate, glacial acetic acid, ethylenediaminetetraethanol and ferric chloride in sequence according to the above percentages; shake or stir after each addition until a transparent dark red liquid is formed.
[0017] The process flow chart for hydrochloric acid pickling of hot-rolled strip steel is as follows: Figure 1 As shown, in this embodiment, two hot-rolled strips were respectively placed in acid solutions containing the corrosion inhibitor of this embodiment and those without the corrosion inhibitor of this embodiment. The corrosion inhibitor was added to the 80°C pickling solution at a concentration of 1‰. Figure 2 As shown, no obvious chemical reaction occurred in the beaker containing the corrosion inhibitor, while the reaction in the other beaker was vigorous. Figure 3 As shown, after soaking for 30 minutes, the surface whiteness of hot-rolled strip steel containing corrosion inhibitor is brighter. The surface whiteness of strip steel using this corrosion inhibitor is 84.2 degrees, while the surface whiteness of strip steel without corrosion inhibitor is 60.3 degrees.
[0018] Example 2 This embodiment discloses a corrosion inhibitor for hydrochloric acid pickling, which is composed of the following components by mass percentage: hexamethylenetetramine 20%; ferric chloride 2%; ethyl silicate 5%; glacial acetic acid 2%; dibutyl phthalate 5%; sodium hydroxide 10%; ethylenediaminetetraethanol 3%; and the balance being demineralized water.
[0019] The preparation method is as follows: add dibutyl phthalate, sodium hydroxide solution, hexamethylenetetramine, ethyl silicate, glacial acetic acid, ethylenediaminetetraethanol and ferric chloride in sequence according to the above percentages; shake or stir after each addition until a transparent dark red liquid is formed.
[0020] like Figure 4 As shown in the figure, in this embodiment, four hot-rolled strip steels were respectively placed in acid solutions containing the corrosion inhibitor of this embodiment, and in acid solutions containing the corrosion inhibitor of this embodiment, an imported corrosion inhibitor, and a domestic corrosion inhibitor. The corrosion inhibitor was added to the pickling solution at a concentration of 1‰ at 80°C. After soaking for 30 minutes, the surface whiteness of the hot-rolled strip steel containing the corrosion inhibitor was 84.2 degrees, the surface whiteness of the strip steel using the imported corrosion inhibitor was 84.3 degrees, the surface whiteness of the strip steel using the domestic corrosion inhibitor was 70.8 degrees, and the surface whiteness of the strip steel without the added corrosion inhibitor was 60.3 degrees.
[0021] The iron loss was calculated by weighing the samples separately, and the results are as follows: Figure 6 As shown, the steel loss rate of hot-rolled strip containing this corrosion inhibitor is 0.41%, the steel loss rate of using a certain imported corrosion inhibitor strip is 0.40%, the steel loss rate of using a certain domestic corrosion inhibitor strip is 0.61%, and the steel loss rate of strip without added corrosion inhibitor is 1.41%.
[0022] To verify the effectiveness of this pickling corrosion inhibitor, four steel grades—DC01 / DC51D+Z, B170P, DP590, and CR340—were selected. The corrosion inhibitor from this embodiment was added to an 80°C pickling solution at concentrations of 0.5‰, 1‰, and 2‰, respectively, and immersion tests were conducted for 3 minutes, 5 minutes, 10 minutes, 15 minutes, 30 minutes, and 60 minutes to test the corrosion inhibition rate. The test results are as follows: Figure 5 As shown.
Claims
1. An inhibitor for hydrochloric acid pickling characterized by comprising: consists of the following components in percentage by mass: Hexamethylenetetramine 10%~20%; Iron chloride 2%; Ethyl silicate 3%~5%; Ice acetic acid 2%; Dibutyl phthalate 3%~5%; Sodium hydroxide 10%; Ethylenediamine tetraethanol 1%~3%; The balance is desalted water.
2. The corrosion inhibitor for hydrochloric acid pickling according to claim 1, characterized by, The density of the inhibitor is 1.000 to 1.150 g / cm 3 pH is 3 to 6.
3. The corrosion inhibitor for hydrochloric acid pickling according to claim 1, characterized by, The inhibitor is added in the concentration of 0.5~1‰ in the hydrochloric acid pickling solution.
4. The corrosion inhibitor for hydrochloric acid pickling according to claim 1, characterized by, The inhibition rate of the inhibitor is 70~90%.
5. A process for the preparation of the corrosion inhibitor for hydrochloric acid pickling according to any one of claims 1 to 4, characterized by, The method comprises the following steps: Desalted water is added into a reaction container; Dibutyl phthalate, sodium hydroxide solution, hexamethylenetetramine, ethyl silicate, ice acetic acid, ethylenediamine tetraethanol and iron chloride are added in sequence; After each step, shaking or stirring is performed until a transparent dark red liquid is formed.
6. Application of the inhibitor for hydrochloric acid pickling according to any one of claims 1~4 in the hydrochloric acid pickling process of hot-rolled strip steel.