Secondary battery, power utilization device, pole piece and preparation method of pole piece

By using ultraviolet light curing adhesive technology, the problem of slow drying speed of the active layer in the preparation of secondary battery electrodes was solved, realizing the efficient production of active layers with uniform thickness and improving the adhesion and conductivity of the electrodes.

CN121688048APending Publication Date: 2026-03-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411295348.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2026-03-17

AI Technical Summary

Technical Problem

Existing methods for preparing secondary battery electrodes are difficult to achieve rapid drying of a thick active layer, resulting in low production efficiency, poor adhesion, and high film resistance.

Method used

By using ultraviolet light-curing adhesives instead of traditional adhesives, the active layer can be cured in fractions of a second using ultraviolet light curing technology, forming an active layer with a thickness of not less than 300 micrometers, thereby improving electrode production efficiency and adhesion.

Benefits of technology

It significantly improves the coating efficiency of the electrode, forms a thicker active layer with good performance, and enhances the adhesion of the electrode and the film resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121688048A_ABST
    Figure CN121688048A_ABST
Patent Text Reader

Abstract

The invention discloses a secondary battery, a power utilization device, a pole piece and a preparation method of the pole piece. The pole piece comprises a current collector and an active layer located on the surface of the current collector, the active layer comprises an active material and an ultraviolet curing binder, and the total thickness of the active layer is not smaller than 300 micrometers. The active layer of the pole piece comprises the active material and the ultraviolet light curing binder, and the ultraviolet light curing binder can achieve a bonding effect in an ultraviolet light curing mode, so that the thickness of the active layer can be increased, and the production efficiency of the pole piece and the battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of batteries, specifically to secondary batteries, electrical devices, electrodes, and their preparation methods. Background Technology

[0002] Secondary batteries are a clean and renewable resource that can be used as a driving energy source or storage unit in fields such as automobiles and energy storage.

[0003] With the continuous development of science and technology, the requirements for battery performance are becoming increasingly stringent, especially the need to improve battery energy density. Increasing the thickness of the active layer on the battery electrode sheets is an effective way to improve battery energy density. Increasing the thickness of the active layer on the electrode sheets can correspondingly reduce the number of electrode layers inside the battery, reduce the space occupied by the current collector and separator, provide more space for the active material, increase the energy of the active material carried per unit area of ​​the electrode sheet surface, and thus improve the specific capacity of the battery.

[0004] However, current secondary batteries, electrical devices, electrodes, and their preparation methods still need improvement. Summary of the Invention

[0005] In view of the above problems, the present invention provides a secondary battery, an electrical device, an electrode, and a method for preparing the same. The secondary battery has an active layer containing active materials and a UV-curable binder. The active layer can be prepared by UV curing, which can improve the production efficiency of the electrode and the battery.

[0006] In one aspect of this application, an electrode is provided. The electrode includes a current collector and an active layer located on the surface of the current collector, the active layer comprising an active material and a UV-curable adhesive, the total thickness of the active layer being not less than 300 micrometers.

[0007] In the technical solution of this application embodiment, an ultraviolet light curing adhesive is used to replace the traditional adhesive to form the active layer. This allows for the preparation of the active layer using a more efficient light curing process. The light curing process can penetrate to a depth of millimeters and has a fast curing speed, which is beneficial for increasing the thickness of the active layer and improving the production efficiency of the electrode sheet.

[0008] In some embodiments, the content of the UV-curable adhesive in the active layer is 2.5 wt% to 5 wt%.

[0009] In some embodiments, the total thickness of the active layer is 300 micrometers to 1500 micrometers.

[0010] In some embodiments, the raw materials forming the UV-curable adhesive include a polymerizable compound and a photoinitiator, wherein the polymerizable compound includes at least one of a monomer and a prepolymer, and / or the photoinitiator includes at least one of a pyrolysis-type free radical photoinitiator and a hydrogen-abstracting free radical photoinitiator.

[0011] In some embodiments, the monomer comprises at least one of alkyl acrylates, hydroxy methacrylates, glycidyl methacrylates, isobornyl acrylates, tetrahydrofuran methyl acrylate, styrene, 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and dipentaerythritol pentaacrylate; and / or,

[0012] The prepolymer includes at least one of polyurethane acrylate, polyester acrylate, epoxy resin acrylate, and polyether resin acrylate.

[0013] In some embodiments, the polymerizable compound includes a monomer and a prepolymer, and the photoinitiator is a pyrolytic free radical photoinitiator. Based on the total mass of the raw materials forming the UV-curable adhesive, the raw materials forming the UV-curable adhesive include: 60wt%-80wt% of the prepolymer, 15wt%-35wt% of the monomer, and 1wt%-5wt% of the photoinitiator.

[0014] In some embodiments, the active layer further includes a conductive agent, which includes at least one of acetylene black, carbon black, Ketjen black, and carbon nanotubes, and / or the content of the conductive agent in the active layer is 1wt%-5wt%.

[0015] In some embodiments, the film resistance of the electrode is 0.2Ω-0.8Ω, and / or the adhesion force of the electrode is 15N / m-22N / m.

[0016] In some embodiments, the electrode includes a positive electrode and / or a negative electrode.

[0017] In another aspect of this application, a method for preparing an electrode sheet is provided. The method includes: mixing an active material and a UV-curable binder and coating them onto the surface of a current collector to obtain an active pre-layer; and subjecting the current collector having the active pre-layer to UV curing treatment to form an active layer on the surface of the current collector, wherein the total thickness of the active layer is not less than 300 micrometers.

[0018] In some embodiments, the method includes: mixing an active material and a UV-curable adhesive, and applying the mixture to the surfaces of both sides of the current collector by melt extrusion to form two active pre-fabricated layers, and / or

[0019] The photocuring process includes irradiating the active preform with ultraviolet light.

[0020] In some embodiments, the coating speed is 80m / min-120m / min.

[0021] In another aspect of this application, a secondary battery is provided. The secondary battery includes the electrode sheet described above or the electrode sheet prepared by the method described above.

[0022] In another aspect of this application, an electrical device is provided. This electrical device includes the aforementioned secondary battery, which is used to provide electrical energy.

[0023] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0024] To more clearly illustrate the technical solution of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without any creative effort.

[0025] Figure 1 This is a schematic diagram of the electrode structure according to one embodiment of this application;

[0026] Figure 2 This is a schematic diagram of a square secondary battery structure according to an embodiment of this application;

[0027] Figure 3 This is a schematic diagram of the outer packaging structure of a secondary battery according to one embodiment of this application;

[0028] Figure 4 This is a schematic diagram of the electrical device structure according to one embodiment of this application.

[0029] Figure Labels

[0030] 100. Electrode; 110. Current collector; 120. Active layer;

[0031] 1. Secondary battery; 2. Electrical device;

[0032] 11. Housing; 12. Electrode assembly; 13. Cover plate.

[0033] To better describe and illustrate embodiments and / or examples of the inventions disclosed herein, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed inventions, the currently described embodiments and / or examples, or the best mode of these inventions as currently understood. Detailed Implementation

[0034] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are intended to cover non-exclusive inclusion.

[0036] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0037] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0038] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0039] In the description of the embodiments of this application, the technical terms "upper", "lower", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0040] Unless otherwise stated, the terms used in this application have their common meanings as commonly understood by those skilled in the art. Unless otherwise stated, the values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this application).

[0041] As mentioned earlier, thicker electrodes can significantly improve the energy density of batteries. However, as the thickness of the active layer in the electrode sheet increases, the coating thickness also increases. Traditional binders are prepared by first dissolving them in liquid solvents such as N-methylpyrrolidone (NMP), then mixing them with the active material, coating them onto the current collector, and finally drying them to obtain the active layer. Therefore, it is difficult to obtain a thick film layer in a single coating process. Furthermore, the increased thickness of the active layer also leads to longer drying times. Longer drying times result in reduced production efficiency. During the drying process, components such as binders and conductive agents are also prone to migration with the solvent, leading to uneven distribution of the binder in the coating. This, in turn, results in poor adhesion of the produced electrode sheet and high film resistance.

[0042] Although the above problems can be alleviated to some extent by applying multiple coatings, multiple coatings involve coating the slurry onto the surface of the dried electrode film, which inevitably leads to the phenomenon of the dried material dissolving again, affecting the electrode's electronic conductivity and pore distribution. At the same time, multiple coatings require multiple drying and rolling processes, which are cumbersome and have high energy consumption.

[0043] Therefore, if a component capable of rapidly drying a thick active film layer could be provided, the aforementioned problems would be significantly alleviated or even solved. To address these issues, this application employs an adhesive with photocurable capabilities, which can significantly improve the drying speed of the active layer and increase the thickness of the electrode.

[0044] The electrode and secondary battery proposed in this application utilize ultraviolet light to cure the adhesive, which polymerizes under ultraviolet light to achieve the adhesive effect. The curing can be completed in a fraction of a second or a little longer, which can significantly improve the coating efficiency of the electrode. Therefore, it is easy to obtain a high-performance and thick active layer.

[0045] refer to Figure 1 The electrode 100 proposed in this application includes a current collector 110 and an active layer 120 located on the surface of the current collector. The total thickness of the active layer on the surface of the current collector is not less than 300 micrometers, and the active layer 120 includes an active material and a UV-curable adhesive. The UV-curable adhesive can achieve bonding by UV curing, and the curing speed is fast.

[0046] In this application, the specific details of the active materials in the electrode 100 and the active layer 120 can be selected as needed. For example, the electrode can be an electrode for electrochemical components such as lithium-ion secondary batteries, and can be either a positive electrode or a negative electrode. In some embodiments, the electrode includes a positive electrode and / or a negative electrode, both of which have a current collector and an active layer located on the surface of the current collector. The active layer of the positive electrode and / or negative electrode includes an active material and an ultraviolet-cured binder. When the electrode 100 is a positive electrode, the active material is a positive active material, such as lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, ternary materials, etc. As another example, the electrode 100 can be a negative electrode, in which case the active material can include graphite, such as natural graphite and / or artificial graphite, and silicon-based materials, such as silicon-carbon materials. The specific number of active layers 120 can also be adjusted as needed. For example, only one active layer 120 can be provided on the current collector 110, or, as Figure 1 As shown, active layers 120 can also be provided on both sides of the current collector 110, that is, the electrode 100 may include two active layers 120.

[0047] In some embodiments, the raw materials forming the UV-curable adhesive include a polymerizable compound and a photoinitiator. The photoinitiator can initiate a reaction of the polymerizable compound through free radical polymerization under UV light irradiation, thereby achieving the purpose of adhesion and UV curing. For example, the polymerizable compound may include at least one of a monomer and a prepolymer, and the photoinitiator may include at least one of a pyrolysis-type free radical photoinitiator and a hydrogen-abstracting free radical photoinitiator.

[0048] In some embodiments, medium- and short-wave ultraviolet radiation can be used to cause a photoinitiator to form free radicals (or cations), thereby initiating polymerization of monomers and / or prepolymers that can undergo polymerization.

[0049] monomer

[0050] A monomer is a small organic molecule containing one or more polymerizable functional groups. In this application, it can also act as an active diluent, mainly to adjust viscosity and participate in polymerization reactions.

[0051] prepolymer

[0052] Prepolymers are reactive low-molecular-weight polymers that can provide a skeleton structure for photocurable adhesives in this application. The main functions of prepolymers are to provide viscosity, tensile strength, shear strength, hardness, and flexibility.

[0053] Monomers can be classified into monofunctional monomers, difunctional monomers, and polyfunctional monomers based on their functionality. In some embodiments, the monomer may be selected from at least one of monofunctional, difunctional, and polyfunctional monomers. For example, it may be selected from at least one of monofunctional, difunctional, and trifunctional monomers. Monofunctional monomers have only one polymerizable functional group and can be cured to form a linear polymer, which is beneficial for improving the flexibility and adhesion of the formed active layer. Difunctional and trifunctional monomers both have multiple polymerizable functional groups, acting not only as reactive diluents but also as crosslinking agents, enabling crosslinking to form three-dimensional polymer structures, which significantly influence the hardness, toughness, and strength of the formed active layer. Furthermore, increasing the functionality of the monomer can accelerate the curing process; therefore, mixtures of monofunctional, difunctional, and polyfunctional monomers are often used. The monomers used in free radical curing systems mainly include (meth)acrylates, vinyl groups, and vinyl ethers, such as styrene, butyl acrylate, isooctyl acrylate, isobornyl acrylate, tripropylene glycol diacrylate, hexanediol diacrylate, and trimethylolpropane triacrylate.

[0054] In some embodiments, the chemical composition of the monomer may be adjusted as needed. In some embodiments, the monomer may include at least one of alkyl acrylates, hydroxy methacrylates, glycidyl methacrylate (GMA), isobornyl acrylate, tetrahydrofuran methyl acrylate, styrene, 1,6-hexanediol diacrylate (HDDA), dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate (TMPTA), pentaerythritol triacrylate (PETA), and dipentaerythritol pentaacrylate (DPPA). The structural formula of the alkyl acrylate monomer is as follows:

[0055]

[0056] In this application, the prepolymer can be an unsaturated polymer containing double bonds, mainly including polyacrylates, epoxy acrylates, polyurethane acrylates, unsaturated polyesters, polyolefins / thiols, etc. For example, at least one of epoxy acrylates and polyurethane acrylates can be selected as the prepolymer, which has the advantages of high reactivity, abundant raw materials, many varieties, and moderate price. In some embodiments, the prepolymer may include at least one of polyurethane acrylates, polyester acrylates, epoxy resin acrylates, and polyether resin acrylates.

[0057] The structural formula of polyurethane acrylate can be as follows:

[0058]

[0059] Photoinitiator

[0060] Photoinitiators play a decisive role in the sensitivity (curing rate) of UV curing systems. Photoinitiators include free radical photoinitiators and cationic photoinitiators, applied to free radical and cationic systems respectively. Commonly used free radical initiators include carbonyl compounds, azo compounds, organosulfur compounds, redox substances, halogen compounds, organometallic compounds, and salting dyes. Carbonyl compounds are widely used and perform well, mainly including bibenzoyl, benzophenone, benzoin and its ether compounds such as benzoin ethyl ether and benzoin butyl ether.

[0061] Cracked free radical photoinitiators

[0062] After absorbing light energy, the cleavage-type photoinitiator transitions to the excited singlet state and then jumps to the excited triplet state via intersystem crossing. In the excited singlet or triplet state, the molecular structure is unstable, and the weak bonds undergo homolytic cleavage, generating active free radicals that initiate the polymerization and crosslinking of oligomers and monomers.

[0063] For example, cleavage-type photoinitiators can include styrene derivatives, aromatic ketones, and nitrobenzenes. Cleavage-type photoinitiators can undergo cleavage under ultraviolet light induction, producing free radicals as follows:

[0064]

[0065] Hydrogen-abstracting free radical photoinitiators

[0066] For example, hydrogen-abstracting photoinitiators can include benzophenone, thioxanthone (TX), and their derivatives. After absorbing light energy, the hydrogen-abstracting photoinitiator molecule is excited and undergoes intersystem crossing to the excited triplet state (as shown in the *-shaped benzophenone structure below), where it undergoes a bimolecular interaction with a hydrogen donor, generating active free radicals via electron transfer, initiating oligomer and monomer polymerization and crosslinking. Hydrogen donors can include triethylamine, triisopropylamine, and triisobutylamine. For example, hydrogen-abstracting photoinitiators can undergo cleavage under ultraviolet light induction, producing free radicals as follows:

[0067]

[0068] In this application, by adjusting the proportions of raw materials such as prepolymer, monomer, and photoinitiator, the flowability of the raw materials forming the UV-curable adhesive can be controlled, allowing it to be mixed with the active material of the electrode through a process such as melting. This helps to reduce or even eliminate the liquid solvent in the active layer, thereby further improving the efficiency and effect of curing.

[0069] In some embodiments, based on the total mass of the raw materials forming the UV-curable adhesive, the raw materials forming the UV-curable adhesive include: 60 wt%-80 wt% of a prepolymer, 15 wt%-35 wt% of a monomer, and 1 wt%-5 wt% of a photoinitiator. Specifically, the mass percentage of the prepolymer can be one of 60 wt%, 62 wt%, 64 wt%, 66 wt%, 68 wt%, 70 wt%, 72 wt%, 74 wt%, 76 wt%, 78 wt%, or 80 wt%, or any value satisfying the above range. The mass percentage of the monomer can be one of 15 wt%, 18 wt%, 20 wt%, 22 wt%, 25 wt%, 28 wt%, 30 wt%, 32 wt%, or 35 wt%, or any value satisfying the above range. The mass percentage of the photoinitiator can be one of 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt%, or any value satisfying the above range. When the contents of prepolymer, monomer, and photoinitiator meet the above requirements, the resulting UV-curable adhesive has good bonding properties.

[0070] In some embodiments, the content of UV-curable adhesive in the active layer is 2.5 wt%-5 wt%. This further enhances the electrode adhesion. Specifically, the content of UV-curable adhesive can be one of 2.5 wt%, 2.8 wt%, 3 wt%, 3.2 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, and 5 wt%, or any value satisfying the above range. The UV-curable adhesive content described above can effectively form an active layer with a total thickness of not less than 300 micrometers, improving the electrode adhesion of the formed active layer and ensuring that the active layer contains a sufficient amount of active material to guarantee the electrode capacity.

[0071] In some embodiments, the total thickness of the active layer is 300 micrometers to 1500 micrometers. When the thickness of the active layer is within the above range, the photoinitiator in the raw material can better receive ultraviolet light. Specifically, the active layer can be provided only on one side of the current collector, in which case the total thickness of the active layer is the thickness of the active layer on one side. Alternatively, the active layer can be provided on both sides of the electrode, and the thickness of the active layer provided on one side of the electrode can be half of the total thickness. Exemplarily, the total thickness of the active layer can be one of 300 micrometers, 400 micrometers, 500 micrometers, 600 micrometers, 700 micrometers, 800 micrometers, 900 micrometers, 1000 micrometers, 1100 micrometers, 1200 micrometers, 1300 micrometers, 1400 micrometers, and 1500 micrometers, or any value satisfying the above range. The above thickness can advantageously increase the capacity of the secondary battery using this electrode, and the electrode formed by a single photocuring process also has good adhesion.

[0072] In some embodiments, due to the use of a fast-curing adhesive, the adhesion strength and membrane resistance of the electrode with the active layer can be significantly improved, with the membrane resistance reaching 0.2Ω-0.8Ω and the adhesion strength of the electrode reaching 15N / m-22N / m.

[0073] In some embodiments, the active layer further includes a conductive agent, which includes at least one of acetylene black, carbon black, Ketjen black (Super P), and carbon nanotubes.

[0074] In some embodiments, the content of the conductive agent in the active layer is 1%-5%. This allows for the realization of electrode sheets with even better conductivity. Specifically, the content of the conductive agent can be one of 1%, 2%, 3%, 4%, or 5%, or any value within the aforementioned range.

[0075] In another aspect of this application, a method for preparing an electrode sheet is proposed. This method includes: mixing an active material and a UV-curable binder and coating them onto the surface of a current collector to obtain an active pre-layer; and subjecting the current collector with the active pre-layer to UV curing treatment to form an active layer on the surface of the current collector. The active material and UV-curable binder can be the same active material and UV-curable binder included in the electrode active layer described above. The UV-curable binder can promote cross-linking of the binder through UV curing to achieve an adhesive effect on the active material. The slurry can be rapidly cured under UV light, significantly improving production efficiency. This method can easily provide thick electrodes with all the aforementioned characteristics of electrodes, which will not be elaborated further here. This method has advantages such as ease of operation and low cost.

[0076] In some embodiments, the active material and the UV-curable adhesive are mixed and applied to the surfaces on both sides of the current collector by melt extrusion to form two active prefabricated layers.

[0077] In some embodiments, the thickness of the active prefabricated layer can be adjusted to achieve the desired thickness of the active layer. The thickness of the active prefabricated layer can be slightly greater than the thickness of the active layer. For example, the total thickness of the active prefabricated layer can be 300 micrometers to 1600 micrometers. Specifically, the total thickness of the active prefabricated layer can be one of 300 micrometers, 500 micrometers, 700 micrometers, 900 micrometers, 1000 micrometers, 1200 micrometers, 1400 micrometers, and 1600 micrometers, or any value within the range described above.

[0078] In some embodiments, the coating speed is 80 m / min to 120 m / min. Due to the faster photocuring speed, faster coating can be achieved. Specifically, the coating speed can be one of 80 m / min, 90 m / min, 100 m / min, 110 m / min, or 120 m / min, or any value within the above range.

[0079] In some embodiments, the photocuring process includes irradiating the active preform layer with ultraviolet light. This allows the mid- and high-wavelength radiation of ultraviolet light to excite a photoinitiator to form free radicals or cations, thereby initiating the polymerization of monomers and prepolymers containing active functional groups to form an electrode.

[0080] In another aspect, this application provides a secondary battery. The secondary battery includes a positive electrode, a negative electrode, and a separator, with the separator located between the positive and negative electrodes. Both the positive and negative electrodes have a current collector and an active layer on the surface of the current collector. The active layer of the positive and / or negative electrode includes an active material and a UV-curable binder. The UV-curable binder polymerizes under UV light to achieve its binding effect, offering advantages such as high production efficiency, improved membrane resistance, and enhanced adhesion. The total thickness of the active layer is not less than 300 micrometers, thereby achieving thick electrodes for the positive and negative electrodes of the battery. This battery offers advantages such as high production efficiency, improved membrane resistance, and enhanced adhesion.

[0081] In some embodiments, the total thickness of the active layer is 300 micrometers to 1500 micrometers. Specifically, the total thickness of the active layer can be one of 300 micrometers, 500 micrometers, 700 micrometers, 900 micrometers, 1000 micrometers, 1200 micrometers, 1400 micrometers, and 1500 micrometers, or any value that satisfies the above range.

[0082] In some embodiments, the raw materials forming the UV-curable adhesive include polymerizable compounds and photoinitiators. The polymerizable compounds include at least one of monomers and prepolymers, and the photoinitiators include at least one of pyrolytic radical photoinitiators and hydrogen-abstracting radical photoinitiators.

[0083] In some embodiments, the polymerizable compound includes monomers and prepolymers, and the photoinitiator is a pyrolytic free radical photoinitiator. Based on the total mass of the raw materials forming the UV-curable adhesive, the raw materials forming the UV-curable adhesive include: 60wt%-80wt% of prepolymer, 15wt%-35wt% of monomer, and 1wt%-5wt% of photoinitiator.

[0084] In some embodiments, the active layer further includes a conductive agent, which includes at least one of acetylene black, carbon black, Super P, and carbon nanotubes.

[0085] In some embodiments, the content of the conductive agent in the active layer is 1%-5%. Specifically, the content of the conductive agent can be one of 1%, 2%, 3%, 4%, 5%, or any value that meets the above range.

[0086] In some embodiments, the film resistance of the positive and / or negative electrodes having a UV-curable adhesive is 0.2Ω-0.8Ω. Specifically, the film resistance can be one of 0.2Ω, 0.3Ω, 0.4Ω, 0.5Ω, 0.6Ω, 0.7Ω, 0.8Ω or any value satisfying the above range.

[0087] In this application, the diaphragm resistance can be tested using the four-probe method. Four probes are used to contact the sample under test and measure its resistance. The diaphragm resistance can be measured using the Yuaneng Technology BER2100 device. The electrode or diaphragm is placed on the testing device with its surface flat, and the pressure gauge is adjusted to fix the test sample, ensuring good contact between the probes and the sample. The testing device is turned on, and current is introduced into the sample under test through the circuit connection, and the voltage change is recorded. The resistance value of the sample is calculated according to Ohm's law.

[0088] In some embodiments, the electrode bonding force of the positive and / or negative electrodes is 15 N / m to 22 N / m. Specifically, the electrode bonding force can be one of 15 N / m, 16 N / m, 17 N / m, 18 N / m, 19 N / m, 20 N / m, 21 N / m, and 22 N / m, or any value satisfying the above range.

[0089] In this application, the electrode adhesion strength can be evaluated by applying a peel force. The electrode adhesion strength can be measured using a lithium battery electrode adhesion strength tester (model: MX-0580). A test sample is prepared, the electrode is fixed, and a peel force perpendicular to the contact surface, i.e., the screen where the current collector is located, is applied. The electrode adhesion strength is evaluated by measuring the maximum value of the applied peel force.

[0090] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process. For example, Figure 2 This is an example of a square-structured secondary battery 1.

[0091] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the aforementioned electrode assembly and electrolyte. In some embodiments, refer to... Figure 3The outer packaging may include a shell 11 and a cover plate 13. The shell 11 may include a bottom plate and side plates connected to the bottom plate, the bottom plate and side plates forming a receiving cavity. The shell 11 has an opening communicating with the receiving cavity, and the cover plate 13 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator can be formed into an electrode assembly 12 by a winding process or a stacking process. The electrode assembly 12 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 12. The secondary battery 1 may contain one or more electrode assemblies 12, which can be selected by those skilled in the art according to specific practical needs.

[0092] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, aluminum shell, or steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate. This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. In another aspect of this application, an electrical device is proposed. This electrical device includes a secondary battery as described above, which is used to provide electrical energy.

[0093] In this application, the electrical device can be such as a mobile phone, tablet, laptop, electric toy, power tool, electric vehicle, electric car, ship, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.

[0094] As for the aforementioned electrical device, a rechargeable battery can be selected according to its usage requirements. For example, Figure 4 This is an example of an electrical appliance 2.

[0095] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0096] Example 1

[0097] Preparation of positive electrode sheet

[0098] The mass ratio of lithium iron phosphate:carbon black:UV-curable adhesive is 8:1:1, where the UV-curable adhesive is based on the total mass of monomers, prepolymers, and initiators. The lithium iron phosphate, carbon black, and UV-curable adhesive are mixed and then dry-mixed using a dual-blade grinder. The UV-curable adhesive is composed of polyurethane acrylate (weight average molecular weight 400,000-500,000), methyl methacrylate (weight average molecular weight 300,000-400,000), and benzophenone, with a mass ratio of polyurethane acrylate:methyl methacrylate:photoinitiator of 8:1.5:0.5.

[0099] The mixture is heated to a molten state (temperature 250℃-400℃) and coated onto both sides of aluminum foil by melt extrusion at a coating speed of 100m / min. Then, it is cold-pressed to obtain an active pre-coated layer.

[0100] An aluminum foil with the two active pre-layers is placed in an oven irradiated with ultraviolet light to obtain a positive electrode sheet. The two active layers of the positive electrode sheet have equal thicknesses, and the total thickness of the active layers is 350 micrometers.

[0101] Example 2

[0102] Preparation of positive electrode sheet

[0103] The remaining operations are the same as in Example 1, except that the amount of coating is controlled to obtain two active layers of the positive electrode sheet with equal thickness, and the total thickness of the active layer is 500 micrometers.

[0104] Example 3

[0105] Preparation of positive electrode sheet

[0106] The remaining operations are the same as in Example 1, except that the amount of coating is controlled to obtain two active layers of the positive electrode with equal thickness, and the total thickness of the active layer is 1000 micrometers.

[0107] Example 4

[0108] Preparation of positive electrode sheet

[0109] The remaining operations are the same as in Example 1, except that the lithium iron phosphate: carbon black: UV-curable adhesive is mixed in a mass ratio of 7:1:2.

[0110] Example 5

[0111] Preparation of positive electrode sheet

[0112] The remaining operations are the same as in Example 1, except that the lithium iron phosphate: carbon black: UV-cured adhesive is mixed in a mass ratio of 8.5:1:0.5.

[0113] Example 6

[0114] Preparation of positive electrode sheet

[0115] The remaining operations are the same as in Example 1, except that the prepolymer is an epoxy resin acrylate.

[0116] Comparative Example 1

[0117] The remaining operations are the same as in Example 1, except that lithium iron phosphate, carbon black and PVDF are mixed according to a mass ratio of lithium iron phosphate: carbon black: PVDF of 8:1:1, and then N-methylpyrrolidone solvent is added. The mixture is coated on both sides of aluminum foil at a coating speed of 50 m / min. After cold pressing and cutting, a positive electrode sheet is obtained. The two active layers of the positive electrode sheet have equal thickness, and the total thickness of the active layer is 350 micrometers.

[0118] Secondary batteries were fabricated using the electrodes obtained in the above embodiments and comparative examples. The fabrication process of the secondary batteries is as follows:

[0119] Negative electrode sheet: The active layer of the electrode is made of a slurry containing graphite, sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR), with a mass ratio of graphite:sodium carboxymethyl cellulose:styrene-butadiene rubber of 97:2:1, obtained by cold pressing;

[0120] Separator: PE film is used as the battery separator;

[0121] Electrolyte: Lithium bis(fluorosulfonyl)imide (LiFSI) with a concentration of 1 mol / L is used as the lithium salt, and ethylene carbonate (EC) is used as the solvent.

[0122] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. The stacked electrodes are then stacked to form small stacks. The bare cell is placed in the outer packaging of the lithium battery. After drying, electrolyte is injected into the outer packaging of the battery. After vacuum sealing, settling, formation, and shaping, a secondary battery is obtained.

[0123] Performance testing

[0124] Adhesion test

[0125] The tensile test method was used for testing.

[0126] The specific procedure for the tensile test is as follows:

[0127] The peel strength was quantitatively determined using the 180° peel method. The free end of the electrode was folded 180°, and the free end of the electrode and the test plate were clamped on the upper and lower clamps respectively. The electrode and the coating were continuously peeled using a tensile testing machine in the same environment until the electrode and the coating were completely separated. The peel strength value could be read directly.

[0128] The adhesive strength is assessed by measuring the maximum applied tensile force.

[0129] Electrode and diaphragm resistance testing

[0130] The four-probe method was used for testing.

[0131] The specific procedure for testing resistance using the four-probe method is as follows:

[0132] Place the electrode on the testing device and make its surface flat.

[0133] Adjust the pressure gauge to fix the test sample and ensure good contact between the probe and the sample.

[0134] Turn on the testing device, introduce current into the sample under test through the circuit connection, and record the voltage change.

[0135] The resistance of the sample is calculated using Ohm's law.

[0136] The test results are shown in Table 1.

[0137] Table 1 Summary of experimental results from Examples 1-6 and Comparative Example 1

[0138]

[0139]

[0140] As shown in Table 1, the adhesion strength and film resistance of the positive electrode sheets prepared in this application are significantly improved compared to the positive electrode sheets in the comparative examples. Specifically, by replacing the adhesive in the existing positive electrode sheets with the photocurable adhesive of this application, the adhesion strength of the electrode sheets is significantly improved; for example, in Example 1, the adhesion strength increased from 10 N / m to 20 N / m, and the film resistance decreased from 1.5 Ω to 0.4 Ω. Furthermore, compared to the conventional process in the comparative examples, which requires drying at around 100°C, affecting the coating speed, the photocuring speed in this application is faster, allowing for quicker coating and higher production efficiency.

[0141] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A pole piece, characterized in that, The electrode plate comprises: a current collector, and an active layer on the surface of the current collector, the active layer comprises an active material and an ultraviolet light-cured binder, and the total thickness of the active layer is not less than 300 microns.

2. The pole piece of claim 1, wherein The content of the ultraviolet light-cured binder in the active layer is 2.5wt%-5wt%.

3. The pole piece according to claim 1 or 2, characterized in that The total thickness of the active layer is 300 microns-1500 microns.

4. The pole piece according to any one of claims 1 to 3, characterized in that The raw materials for forming the ultraviolet light-cured binder comprise a polymerizable compound and a photoinitiator, the polymerizable compound comprises at least one of a monomer and a prepolymer, and / or the photoinitiator comprises at least one of a cleavage-type free radical photoinitiator and a hydrogen abstraction-type free radical photoinitiator.

5. The pole piece of claim 4, wherein The monomer comprises at least one of an alkyl acrylate, a hydroxyl methacrylate, a glycidyl methacrylate, an isobornyl acrylate, a tetrahydrofurfuryl acrylate, a styrene, a 1,6-hexanediol diacrylate, a dipropylene glycol diacrylate, a tripropylene glycol diacrylate, a trihydroxymethyl propane triacrylate, a pentaerythritol triacrylate, and a dipentaerythritol pentaacrylate; and / or The prepolymer comprises at least one of a polyurethane acrylate, a polyester acrylate, an epoxy resin acrylate, and a polyether resin acrylate.

6. The pole piece of claim 5, wherein The polymerizable compound comprises a monomer and a prepolymer, the photoinitiator is a cleavage-type free radical photoinitiator, and based on the total mass of the raw materials for forming the ultraviolet light-cured binder, the raw materials for forming the ultraviolet light-cured binder comprise 60wt%-80wt% of the prepolymer, 15wt%-35wt% of the monomer, and 1wt%-5wt% of the photoinitiator.

7. The pole piece of any of claims 1-6, wherein, The active layer further comprises a conductive agent, the conductive agent comprises at least one of acetylene black, carbon black, ketjen black, and a carbon nanotube, and / or the content of the conductive agent in the active layer is 1wt%-5wt%.

8. The pole piece of any of claims 1-7, wherein, The sheet resistance of the electrode plate is 0.2Ω-0.8Ω, and / or The adhesion of the electrode plate is 15N / m-22N / m.

9. The pole piece of any of claims 1-8, wherein, The electrode plate comprises a positive electrode plate and / or a negative electrode plate.

10. A method of making a pole piece, characterized by, The method comprises: mixing an active material and an ultraviolet light-cured binder, and coating the mixture on the surface of a current collector by a melt extrusion method to form two active preformed layers, and / or The light curing treatment comprises irradiating the active preformed layer with ultraviolet light.

11. The method of claim 10, wherein, The coating speed of the coating is 80m / min-120m / min. The electrode plate is prepared by the method of any one of claims 10-12. The electrical device comprises the secondary battery of claim 13, and the secondary battery is used to provide electrical energy.

12. The method according to claim 10 or 11, characterized in that, ​ 13. A secondary battery characterized by comprising: ​ 14. An electrical device, characterized by ​

Citation Information

Cited By

  • Resin composition, pole piece, method for manufacturing same, and single battery, battery device, and power using equipment

    CN122278429A