High-temperature-resistant adhesive for bonding low-surface-energy materials, preparation method of high-temperature-resistant adhesive and cotton paper double-sided tape
By controlling the polarity and molecular weight of polyacrylate adhesive, and combining it with tackifying resin and silane coupling agent, an organic-inorganic bonding layer is formed, solving the bonding problem of low surface energy materials and achieving high-temperature resistance and multi-material applicability of high-performance adhesives.
Patent Information
- Application Number
- CN202512027774.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-30
- Publication Date
- 2026-04-03
AI Technical Summary
Existing adhesives are difficult to bond effectively to low surface energy materials such as polypropylene (PP), polyethylene (PE), and polytetrafluoroethylene (PTFE), and conventional methods sacrifice the temperature resistance of the adhesives.
Using polyacrylate as the main monomer, tackifying resin and silane coupling agent are added. By controlling the polarity and molecular weight, EVA and EAA long-chain polymers are combined, and epoxy and isocyanate curing agents are used to form an organic matrix-silane coupling agent-inorganic matrix bonding layer, which reduces the polarity of the adhesive and improves the bonding performance.
We offer high-temperature resistant adhesives and double-sided cotton paper tapes suitable for low surface energy materials, with excellent bonding performance, temperature resistance, and weather resistance, suitable for bonding needs of a variety of materials.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of adhesive materials, and particularly to a high-temperature resistant adhesive for bonding low surface energy materials, its preparation method, and a cotton paper double-sided adhesive tape. Background Technology
[0002] With the development of technology, all industries are moving towards lighter, simpler, and more environmentally friendly designs. In the construction, automotive, and home appliance markets, some large and heavy metal parts are gradually being replaced by polymer materials. While maintaining their basic performance, people prefer lightweight materials that are easier to transport and use. Some polymer materials, like metals, have high surface energy, making them easy to bond; however, many materials still have extremely low surface energy, making bonding and fixing a significant challenge. Examples include polypropylene (PP), polyethylene (PE), and polytetrafluoroethylene (PTFE).
[0003] Currently, the adhesives used for bonding and fixing on the market mainly include acrylic, epoxy, and polyurethane adhesives. Among them, acrylic adhesives have the widest range of applications, and with their excellent bonding performance and superior temperature and weather resistance, they have a promising future in the adhesive field. However, commonly used acrylic adhesives are not very effective at bonding materials with low surface energy, such as PP, PE, and PTFE.
[0004] Given the current problem, most adhesive manufacturers, especially those producing water-based adhesives, address the issue by adding surfactants to their adhesives to lower the overall surface energy and facilitate bonding of low-surface-energy materials. However, this approach reduces the overall performance of the adhesive, particularly its temperature resistance. Sacrificing many other excellent properties for the sake of bonding low-surface-energy materials is ultimately counterproductive.
[0005] Therefore, it is necessary to provide a high-temperature resistant adhesive and a method for preparing an adhesive tape suitable for bonding low surface energy materials. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a high-temperature resistant adhesive for bonding low surface energy materials, its preparation method, and cotton paper double-sided adhesive tape, in order to address the shortcomings of the prior art.
[0007] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: In its first aspect, the present invention provides a high-temperature resistant adhesive for bonding low surface energy materials, comprising the following raw materials in parts by weight: 100 parts polyacrylate, 30-40 parts tackifying resin A, 5-8 parts tackifying resin B, 5-10 parts tackifying resin C, 0.02-0.05 parts curing agent A, and 0.1-0.5 parts curing agent B; The raw materials for preparing the polyacrylate include, by weight, 25-35 parts of isooctyl acrylate, 5-10 parts of butyl acrylate, 0.02-0.05 parts of hydroxyethyl acrylate, 2-5 parts of acrylic acid, 1-4 parts of methyl acrylate, 0.0008-0.0012 parts of initiator, 1-3 parts of silane coupling agent, 10-20 parts of modified resin, and 50-60 parts of solvent.
[0008] Preferably, the raw materials for preparing the polyacrylate include, by weight, 25 parts isooctyl acrylate, 5 parts butyl acrylate, 0.05 parts hydroxyethyl acrylate, 2 parts acrylic acid, 2 parts methyl acrylate, 0.001 parts initiator, 1 part silane coupling agent, 10 parts modified resin, and 55 parts ethyl acetate solvent.
[0009] Preferably, the modified resin is a mixture of EVA and EAA in a mass ratio of (0.5-2):(0.5-2).
[0010] Preferably, the polyacrylate is prepared by the following method: ① After mixing the monomers (isooctyl acrylate, butyl acrylate, hydroxyethyl acrylate, acrylic acid, methyl acrylate) and solvents in a certain proportion, a monomer mixture is obtained. The monomer mixture is divided into a first monomer mixture and a second monomer mixture in a mass ratio of 6:4. ② Mix EVA and EAA monomers in a reaction vessel at a mass ratio of 1.5:1 and control the temperature above 80℃. Add 4 times the total mass of EVA and EAA of butanone and mix evenly. Then add 15 parts per ten thousand of the total mass of EVA and EAA of initiator and let it react fully for more than 6 hours. Pour it out to obtain the modified resin. ③ Add the first monomer mixture to the reactor, purge with nitrogen, and add 0.06% (by weight of 0.06%) of the initiator at 64-65°C. After reacting for 2.5 hours, add 1.2% (by weight of 0.01%) of the initiator and heat to 78°C for 30 minutes. Add the second monomer mixture dropwise to the reactor over 90 minutes, maintaining the temperature at 78-80°C. After the dropwise addition is complete, keep the temperature at 80°C for 30 minutes. Add 0.2% (by weight of 0.02%) of the initiator and continue to keep the temperature above 80°C for 1 hour. Add 10-20 parts of the modified resin and continue the reaction for 1.5 hours. After the reaction is complete, the polyacrylate is obtained.
[0011] Preferably, the polyacrylate is prepared by the following method: ①Weigh and mix the monomers (isooctyl acrylate, butyl acrylate, hydroxyethyl acrylate, acrylic acid, methyl acrylate) and solvents according to the proportion to obtain a monomer mixture. Divide the monomer mixture into a first monomer mixture and a second monomer mixture according to a mass ratio of 6:4. ② Mix EVA and EAA monomers in a reaction vessel at a mass ratio of 1.5:1 and control the temperature above 80℃. Add 4 times the total mass of EVA and EAA butanone and mix evenly. Then add 15 parts per ten thousand of the initiator benzoyl peroxide and let it react fully for more than 6 hours. Pour it out to obtain the modified resin. ③ Add the first monomer mixture to the reactor, purge with nitrogen, and add 0.06% (0.06%) of the initiator azobisisobutyltrimethylammonium (AIBJ) at 64-65°C. After reacting for 2.5 hours, add 12% (0.01%) of the initiator azobisisobutyltrimethylammonium (AIBJ) again. Raise the temperature to 78°C for 30 minutes. Add the second monomer mixture dropwise to the reactor over 90 minutes, maintaining the temperature at 78-80°C. After the dropwise addition is complete, keep the temperature at 80°C for 30 minutes. Add 0.2% (0.02%) of the initiator azobisisobutyltrimethylammonium (AIBJ) and continue to keep the temperature above 80°C for 1 hour. Add 10 parts of the modified resin and continue the reaction for 1.5 hours. After the reaction is complete, the polyacrylate is obtained.
[0012] Preferably, the silane coupling agent is vinyltriethoxysilane.
[0013] Preferably, the tackifying resin A is one of rosin glycerol ester, disproportionated rosin resin, and hydrogenated rosin resin, with a softening point of 80-90℃ and an acid value of 4-15 mgKOH / g.
[0014] Preferably, the tackifying resin B is one of pentaerythritol ester, petroleum resin, or hydrogenated petroleum resin, with a softening point of 85-105℃ and an acid value of 8-20 mg KOH / g.
[0015] Preferably, the tackifying resin C is one of hydrogenated rosin resin, modified rosin resin, and terpene resin, with a softening point of 115-125℃ and an acid value of 20-30 mgKOH / g.
[0016] Preferably, the curing agent A is one of a metal salt curing agent, an isocyanate curing agent, or an epoxy curing agent; The curing agent B is one of epoxy curing agents, metal salt curing agents, or isocyanate curing agents.
[0017] In a second aspect, the present invention provides a high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials, comprising a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked sequentially, wherein the first adhesive layer and the second adhesive layer are both obtained by coating and curing with a high-temperature resistant adhesive as described above, and the substrate layer is cotton paper.
[0018] A third aspect of the present invention provides a method for preparing a high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials as described above, comprising the following steps: S1. Mix polyacrylate, tackifying resin A, tackifying resin B, tackifying resin C, curing agent A, and curing agent B, and stir evenly to obtain a high-temperature resistant adhesive. S2. Apply a high-temperature resistant adhesive to the first side of the double-sided release layer, bake and cure to form the first adhesive layer, then bond the first adhesive layer to the first side of the substrate layer and roll it up to form a semi-finished product. S3. Apply a high-temperature resistant adhesive to the second side of the double-sided release layer, bake and cure to form a second adhesive layer, peel off the double-sided release layer and the second adhesive layer on it, and then attach the second adhesive layer to the second side of the substrate layer to obtain the high-performance cotton paper double-sided tape suitable for bonding low surface energy materials.
[0019] The beneficial effects of this invention are: This invention provides a high-temperature resistant adhesive for bonding low surface energy materials, its preparation method, and a double-sided cotton paper tape. In synthesizing polyacrylate adhesives, this invention uses monomers with little or no hydroxyl and carboxyl groups as the main monomers, introducing fewer polar monomers. Furthermore, the synthesis time is relatively increased while the temperature is slightly decreased, resulting in a main adhesive with low overall surface energy and a high molecular weight. Tackifying resins are then added to the polyacrylate adhesive to improve its overall bonding performance. This invention selects three synergistic tackifying resins, improving bonding performance to low surface energy materials without significantly sacrificing other properties. A small amount of silane coupling agent is added to the formulation of this invention. The silane coupling agent, situated between the inorganic and organic interfaces, can form a bonding layer between the organic matrix, silane coupling agent, and the matrix-free matrix, reducing the polarity of the adhesive. The subsequently added EVA (ethylene-vinyl acetate copolymer) and EAA (ethylene-acrylic acid copolymer) are both long-chain polymers containing a large amount of -CH2-, while having very little content of polar groups such as hydroxyl and carboxyl groups, further reducing the polarity of the adhesive itself. Detailed Implementation
[0020] The present invention will be further described in detail below with reference to embodiments, so that those skilled in the art can implement it based on the description.
[0021] It should be understood that terms such as “having,” “comprising,” and “including” as used herein do not exclude the presence or addition of one or more other elements or combinations thereof.
[0022] Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, the materials and reagents used in the following examples are commercially available. For examples where specific conditions are not specified, conventional conditions or conditions recommended by the manufacturer are followed. For reagents or instruments whose manufacturers are not specified, they are all commercially available products.
[0023] This invention provides a high-temperature resistant adhesive for bonding low surface energy materials, comprising the following raw materials in parts by weight: 100 parts polyacrylate, 30-40 parts tackifying resin A, 5-8 parts tackifying resin B, 5-10 parts tackifying resin C, 0.02-0.05 parts curing agent A, and 0.1-0.5 parts curing agent B.
[0024] In a preferred embodiment, the raw materials for preparing polyacrylate include, by weight: 25-35 parts isooctyl acrylate, 5-10 parts butyl acrylate, 0.02-0.05 parts hydroxyethyl acrylate, 2-5 parts acrylic acid, 1-4 parts methyl acrylate, 0.0008-0.0012 parts initiator, 1-3 parts silane coupling agent, 10-20 parts modified resin, and 50-60 parts solvent.
[0025] In a preferred embodiment, the raw materials for preparing the polyacrylate include, by weight: 25 parts isooctyl acrylate, 5 parts butyl acrylate, 0.05 parts hydroxyethyl acrylate, 2 parts acrylic acid, 2 parts methyl acrylate, 0.001 parts initiator, 1 part silane coupling agent, 10 parts modified resin, and 55 parts ethyl acetate solvent.
[0026] In a preferred embodiment, the polyacrylate solid content is 40%-50%; the viscosity is 9000-18000 cps; the weight-average molecular weight is 450,000-650,000; and the glass transition temperature is -20 to 10°C.
[0027] In a preferred embodiment, the modified resin is a mixture of EVA (ethylene-vinyl acetate copolymer) and EAA (ethylene-acrylic acid copolymer) in a mass ratio of (0.5-2):(0.5-2). Adding the modified resin at the final stage after the main adhesive synthesis better reduces the polarity of the adhesive, making it more suitable for bonding low surface energy materials.
[0028] In a preferred embodiment, the polyacrylate is prepared by the following method: ① After mixing the monomers (isooctyl acrylate, butyl acrylate, hydroxyethyl acrylate, acrylic acid, methyl acrylate) and solvents in a certain proportion, a monomer mixture is obtained. The monomer mixture is divided into a first monomer mixture and a second monomer mixture in a mass ratio of 6:4. ② Mix EVA and EAA monomers in a reaction vessel at a mass ratio of 1.5:1 and control the temperature above 80℃. Add 4 times the total mass of EVA and EAA of butanone and mix evenly. Then add 15 parts per ten thousand of the total mass of EVA and EAA of initiator and let it react fully for more than 6 hours. Pour it out to obtain the modified resin. ③ Add the first monomer mixture to the reactor, purge with nitrogen at 64-65℃, add 0.06% (by weight of the total monomer mixture) of initiator, react for 2.5 hours, then add 12% (by weight of the total monomer mixture) of initiator again, heat to 78℃ for 30 minutes, add the second monomer mixture dropwise to the reactor, complete the dropwise addition in 90 minutes, control the temperature at 78-80℃, after the dropwise addition is complete, keep at 80℃ for 30 minutes, add 0.2% (by weight of the total monomer mixture) of initiator, continue to keep at above 80℃ for 1 hour, add 10-20 parts of modified resin, continue to react for 1.5 hours, and obtain the polyacrylate after the reaction is completed.
[0029] In a preferred embodiment, the polyacrylate is prepared by the following method: ①Weigh and mix the monomers (isooctyl acrylate, butyl acrylate, hydroxyethyl acrylate, acrylic acid, methyl acrylate) and solvents according to the proportion to obtain a monomer mixture. Divide the monomer mixture into a first monomer mixture and a second monomer mixture according to a mass ratio of 6:4. ② Mix EVA and EAA monomers in a reaction vessel at a mass ratio of 1.5:1 and control the temperature above 80℃. Add 4 times the total mass of EVA and EAA butanone and mix evenly. Then add 15 parts per ten thousand of the initiator benzoyl peroxide and let it react fully for more than 6 hours. Pour it out to obtain the modified resin. ③ Add the first monomer mixture to the reactor, purge with nitrogen at 64-65°C, add 0.06% (by weight) of the initiator azobisisobutyltrimonium (DIB), react for 2.5 h, then add 12% (by weight) of the initiator azobisisobutyltrimonium (DIB) again, heat to 78°C for 30 min, add the second monomer mixture dropwise into the reactor over 90 min, control the temperature at 78-80°C, hold at 80°C for 30 min, add 0.2% (by weight) of the initiator azobisisobutyltrimonium (DIB), continue holding at above 80°C for 1 h, add 10 parts of modified resin, and continue reacting for 1.5 h. After the reaction is complete, the polyacrylate is obtained.
[0030] In a preferred embodiment, the silane coupling agent is vinyltriethoxysilane.
[0031] In a preferred embodiment, the tackifying resin A is one of rosin glycerol ester, disproportionated rosin resin, and hydrogenated rosin resin, with a softening point of 80-90℃ and an acid value of 4-15 mgKOH / g.
[0032] In a preferred embodiment, the tackifying resin B is one of pentaerythritol ester, petroleum resin, or hydrogenated petroleum resin, with a softening point of 85-105℃ and an acid value of 8-20 mgKOH / g.
[0033] In a preferred embodiment, the tackifying resin C is one of hydrogenated rosin resin, modified rosin resin, or terpene resin, with a softening point of 115-125℃ and an acid value of 20-30 mg KOH / g.
[0034] In a preferred embodiment, curing agent A is one of a metal salt curing agent, an isocyanate curing agent, or an epoxy curing agent.
[0035] In a preferred embodiment, curing agent B is one of epoxy curing agents, metal salt curing agents, or isocyanate curing agents.
[0036] The adhesive composed of the above components has excellent bonding properties; the addition of some hydrogenated resins results in a low surface energy; and the further cross-linking by the post-curing agent further enhances its bonding performance and cohesion to low surface energy materials, giving it good temperature resistance and weather resistance.
[0037] The present invention also provides a high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials, comprising a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked in sequence. The first adhesive layer and the second adhesive layer are both obtained by coating and curing the above-mentioned high-temperature resistant adhesive, and the substrate layer is cotton paper.
[0038] In a preferred embodiment, the thickness of both the first adhesive layer and the second adhesive layer is 50μm-70μm.
[0039] In a preferred embodiment, the substrate layer thickness is 20μm-40μm and the basis weight is 12g-14g.
[0040] This invention also provides a method for preparing high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials, comprising the following steps: S1. Mix polyacrylate, tackifying resin A, tackifying resin B, tackifying resin C, curing agent A, and curing agent B, and stir evenly to obtain a high-temperature resistant adhesive. S2. Apply a high-temperature resistant adhesive to the first side of the double-sided release layer, bake and cure to form the first adhesive layer, then bond the first adhesive layer to the first side of the substrate layer and roll it up to form a semi-finished product. S3. Apply a high-temperature resistant adhesive to the second side of the double-sided release layer, bake and cure to form a second adhesive layer, peel off the double-sided release layer and the second adhesive layer on it, and then attach the second adhesive layer to the second side of the substrate layer to obtain a high-performance cotton paper double-sided tape suitable for bonding low surface energy materials.
[0041] In a preferred embodiment, the ratio of the release force of the second side to the first side of the double-sided release layer is 1-3:1.
[0042] The adhesive tape prepared by this invention has excellent adhesion to low surface energy materials, and also has excellent temperature resistance and weather resistance.
[0043] For bonding low-surface-energy and high-surface-energy or irregular low-surface-energy materials, some problems still exist; for example, some pipes, curved surface bonding, and even curved surface bonding under high environmental temperature requirements. Some tapes can only meet one of the performance requirements and are difficult to be all-encompassing. Sometimes they can bond very firmly at room temperature, but as the temperature rises, the adhered object and the tape will separate, or even break completely. Furthermore, for bonding low-surface-energy and high-surface-energy materials, some tapes are specifically designed for bonding low-surface-energy materials, but have problems bonding conventional materials, and often the tape will separate from the high-surface-energy material. Therefore, the purpose of this invention is to provide a high-temperature resistant double-sided cotton paper tape suitable for bonding low-surface-energy materials, which has good adhesion to low-surface-energy materials, excellent temperature resistance, and good adhesion performance to conventional materials.
[0044] This invention uses monomers with little or no hydroxyl and carboxyl groups as the main monomers in the synthesis of polyacrylate adhesives, minimizing the introduction of polar monomers. The synthesis time is relatively increased while the temperature is slightly decreased, aiming to obtain a main adhesive with low overall surface energy and a high molecular weight. Tackifying resins are then added to the polyacrylate adhesive to improve its overall bonding performance. Tackifying resins with low acid values are selected to ensure the adhesive maintains a low overall surface energy. Experiments show that adding only one tackifying resin is insufficient to achieve the desired bonding strength for PE and PP. Although sometimes quantity can lead to quality improvement, adding more resin may result in some improvement, but this comes at the cost of some cohesive strength, which is not ideal. To balance bonding performance and cohesive strength, this invention selects three tackifying resins that work synergistically, improving bonding performance to low surface energy materials without significantly sacrificing other properties. Experiments show that adding tackifying resins A, B, and C to the main adhesive yields the best results.
[0045] This invention relates to a self-made suitable acrylic adhesive for bonding low surface energy materials. The key feature of this self-made adhesive is that it contains almost no polar monomers and includes a small amount of silane coupling agent. The silane coupling agent, situated between the inorganic and organic interfaces, forms a bonding layer between the organic matrix, the silane coupling agent, and the matrix-free substrate, thus reducing the adhesive's polarity. Furthermore, the subsequently added EVA (ethylene-vinyl acetate copolymer) and EAA (ethylene-acrylic acid copolymer), both long-chain polymers containing a significant amount of -CH2- groups, have very low levels of polar groups such as hydroxyl and carboxyl groups, further reducing the adhesive's inherent polarity.
[0046] Because this invention incorporates various types of tackifying resins, the selection of curing agents must be very careful. The type and amount of curing agent have a significant impact on the final performance of the adhesive; even a slight difference can lead to drastic consequences. Experimental verification has shown that using a mixture of epoxy and isocyanate curing agents achieves the best expected results. This invention adds tackifying resins A, B, and C to the main adhesive, and then cures it using two different types of curing agents. This combination of the three tackifying resins and the main adhesive produces a high-performance adhesive suitable for bonding low surface energy materials.
[0047] The above is the general concept of the present invention. Based on this, detailed embodiments and comparative examples are provided below to further illustrate the present invention.
[0048] In the following examples and comparative examples: The silane coupling agent is vinyltriethoxysilane, specifically KH-151 from Hangzhou Jessica Chemical Co., Ltd. EVA (ethylene-vinyl acetate copolymer) and EAA (ethylene-acrylic acid copolymer) are from Chuangli New Materials Co., Ltd.
[0049] Polyacrylates are prepared by the following method: The raw materials for preparing the polyacrylate include, by weight, 25 parts isooctyl acrylate, 5 parts butyl acrylate, 0.05 parts hydroxyethyl acrylate, 2 parts acrylic acid, 2 parts methyl acrylate, 0.001 parts initiator, 1 part silane coupling agent, 10 parts modified resin, and 55 parts ethyl acetate solvent.
[0050] ①Weigh and mix the monomers (isooctyl acrylate, butyl acrylate, hydroxyethyl acrylate, acrylic acid, methyl acrylate) and solvent (ethyl acetate) in a certain proportion to obtain a monomer mixture. Divide the monomer mixture into a first monomer mixture and a second monomer mixture in a mass ratio of 6:4. ② Mix EVA and EAA monomers in a reaction vessel at a mass ratio of 1.5:1 and control the temperature above 80℃. Add 4 times the total mass of EVA and EAA butanone and mix evenly. Then add 15 parts per ten thousand of the initiator benzoyl peroxide and let it react fully for more than 6 hours. Pour it out to obtain the modified resin. ③ Add the first monomer mixture to the reactor, purge with nitrogen, and add 0.06% (by weight) of the initiator azobisisobutyl at 65°C. After reacting for 2.5 hours, add 12% (by weight) of the initiator azobisisobutyl at 30% (by weight) of the monomer mixture again. Raise the temperature to 78°C for 30 minutes. Add the second monomer mixture dropwise to the reactor over 90 minutes, maintaining the temperature at 80°C. After the dropwise addition is complete, keep the temperature at 80°C for 30 minutes. Add 0.2% (by weight) of the initiator azobisisobutyl at 3000, and continue to keep the temperature above 80°C for 1 hour. Add 10 parts of the modified resin and continue the reaction for 1.5 hours. After the reaction is complete, the polyacrylate is obtained.
[0051] The polyacrylate has a solid content of 42%, a viscosity of 18,000 cps, a weight-average molecular weight of 500,000, and a glass transition temperature of -1℃.
[0052] Example 1 A high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials includes a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked sequentially. The first adhesive layer and the second adhesive layer are both obtained by coating and curing with a high-temperature resistant adhesive. The thickness of the first adhesive layer and the second adhesive layer is 65μm. The substrate layer is made of 14g cotton paper (thickness 30μm).
[0053] The method for preparing this high-performance cotton paper double-sided adhesive tape is characterized by comprising the following steps: S1. Preparation of high-temperature resistant adhesive: By weight fraction, 100 parts of polyacrylate, 40 parts of tackifying resin A, 5 parts of tackifying resin B, 10 parts of tackifying resin C, 0.035 parts of curing agent A, and 0.2 parts of curing agent B are mixed and stirred evenly to obtain a high-temperature resistant adhesive.
[0054] Among them, tackifying resin A is hydrogenated rosin resin with a softening point of 85℃ and an acid value of 7mgKOH / g; specifically, it is AS-5085F from Guangzhou Yabiao Technology Co., Ltd. Tackifying resin B is a hydrogenated petroleum resin with a softening point of 101℃ and an acid value of 12mgKOH / g; specifically, it is C-8010 from Nanjing Yangzi Eastman Chemical Co., Ltd. The tackifying resin C is a modified rosin resin with a softening point of 118℃ and an acid value of 25mgKOH / g; specifically, it is GA-100A from Guangxi Wuzhou Huangchuan Chemical Industry Co., Ltd.
[0055] Curing agent A is an epoxy curing agent, specifically the epoxy curing agent ETERAC EC-97 produced by Changxing Chemical. Curing agent B is an isocyanate curing agent, specifically Bayer's isocyanate curing agent L-75.
[0056] S2. Apply a high-temperature resistant adhesive to the first side of the double-sided release layer, bake at 120°C for 2-3 minutes to cure and form the first adhesive layer, then bond the first adhesive layer to the first side of the substrate layer and roll it up to form a semi-finished product. S3. Apply a high-temperature resistant adhesive to the second side of the double-sided release layer, bake at 120°C for 2-3 minutes to cure and form a second adhesive layer. Peel off the double-sided release layer and the second adhesive layer on it, then attach the second adhesive layer to the second side of the substrate layer, roll it up, and cure it at 55°C for 2 days to obtain a high-performance cotton paper double-sided tape suitable for bonding low surface energy materials.
[0057] The ratio of the release force of the second side to the first side of the double-sided release layer is 2:1.
[0058] Example 2 A high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials includes a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked sequentially. The first adhesive layer and the second adhesive layer are both obtained by coating and curing with a high-temperature resistant adhesive. The thickness of the first adhesive layer and the second adhesive layer is 52μm. The substrate layer is made of 14g cotton paper (thickness 30μm).
[0059] The method for preparing this high-performance cotton paper double-sided adhesive tape is characterized by comprising the following steps: S1. Preparation of high-temperature resistant adhesive: By weight fraction, 100 parts of polyacrylate, 35 parts of tackifying resin A, 5 parts of tackifying resin B, 8 parts of tackifying resin, 0.035 parts of curing agent A, and 0.15 parts of curing agent B are mixed and stirred evenly to obtain a high-temperature resistant adhesive.
[0060] Among them, tackifying resin A is hydrogenated rosin resin with a softening point of 85℃ and an acid value of 7mgKOH / g; specifically, it is AS-5085F from Guangzhou Yabiao Technology Co., Ltd. Tackifying resin B is a hydrogenated petroleum resin with a softening point of 101℃ and an acid value of 12mgKOH / g; specifically, it is C-8010 from Nanjing Yangzi Eastman Chemical Co., Ltd. The tackifying resin C is a modified rosin resin with a softening point of 118℃ and an acid value of 25mgKOH / g; specifically, it is GA-100A from Guangxi Wuzhou Huangchuan Chemical Industry Co., Ltd.
[0061] Curing agent A is an epoxy curing agent, specifically the epoxy curing agent ETERAC EC-97 produced by Changxing Chemical. Curing agent B is an isocyanate curing agent, specifically Bayer's isocyanate curing agent L-75.
[0062] Steps S2 and S3 are the same as in Example 1.
[0063] The ratio of the release force of the second side to the first side of the double-sided release layer is 2:1.
[0064] Example 3 A high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials includes a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked sequentially. The first adhesive layer and the second adhesive layer are both obtained by coating and curing with a high-temperature resistant adhesive. The thickness of the first adhesive layer and the second adhesive layer is 43μm. The substrate layer is made of 14g cotton paper (thickness 30μm).
[0065] The method for preparing this high-performance cotton paper double-sided adhesive tape is characterized by comprising the following steps: S1. Preparation of high-temperature resistant adhesive: By weight fraction, 100 parts of polyacrylate, 30 parts of tackifying resin A, 5 parts of tackifying resin B, 8 parts of tackifying resin C, 0.035 parts of curing agent A, and 0.1 parts of curing agent B are mixed and stirred evenly to obtain a high-temperature resistant adhesive.
[0066] Among them, tackifying resin A is hydrogenated rosin resin with a softening point of 85℃ and an acid value of 7mgKOH / g; specifically, it is AS-5085F from Guangzhou Yabiao Technology Co., Ltd. Tackifying resin B is a hydrogenated petroleum resin with a softening point of 101℃ and an acid value of 12mgKOH / g; specifically, it is C-8010 from Nanjing Yangzi Eastman Chemical Co., Ltd. The tackifying resin C is a modified rosin resin with a softening point of 118℃ and an acid value of 25mgKOH / g; specifically, it is GA-100A from Guangxi Wuzhou Huangchuan Chemical Industry Co., Ltd.
[0067] Curing agent A is an epoxy curing agent, specifically the epoxy curing agent ETERAC EC-97 produced by Changxing Chemical. Curing agent B is an isocyanate curing agent, specifically Bayer's isocyanate curing agent L-75.
[0068] Steps S2 and S3 are the same as in Example 1.
[0069] The ratio of the release force of the second side to the first side of the double-sided release layer is 2:1.
[0070] Comparative Example 1 A high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials includes a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked sequentially. The first adhesive layer and the second adhesive layer are both obtained by coating and curing with a high-temperature resistant adhesive. The thickness of the first adhesive layer and the second adhesive layer is 65μm. The substrate layer is made of 14g cotton paper (thickness 30μm).
[0071] The method for preparing this high-performance cotton paper double-sided adhesive tape is characterized by comprising the following steps: S1. Preparation of high-temperature resistant adhesive: By weight fraction, 100 parts of polyacrylate, 40 parts of tackifying resin A, 5 parts of tackifying resin B, 10 parts of tackifying resin C, 0.035 parts of curing agent A, and 0.2 parts of curing agent B are mixed and stirred evenly to obtain a high-temperature resistant adhesive.
[0072] Among them, tackifying resin A is a common rosin resin with a softening point of 85℃ and an acid value of 7mgKOH / g; specifically, it is AS-5085F from Guangzhou Yabiao Technology Co., Ltd. Tackifying resin B is a hydrogenated petroleum resin with a softening point of 101℃ and an acid value of 12mgKOH / g; specifically, it is C-8010 from Nanjing Yangzi Eastman Chemical Co., Ltd. The tackifying resin C is a modified rosin resin with a softening point of 118℃ and an acid value of 25mgKOH / g; specifically, it is GA-100A from Guangxi Wuzhou Huangchuan Chemical Industry Co., Ltd.
[0073] Curing agent A is an epoxy curing agent, specifically the epoxy curing agent ETERAC EC-97 produced by Changxing Chemical. Curing agent B is an isocyanate curing agent, specifically Bayer's isocyanate curing agent L-75.
[0074] Steps S2 and S3 are the same as in Example 1.
[0075] The ratio of the release force of the second side to the first side of the double-sided release layer is 2:1.
[0076] Comparative Example 2 A high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials includes a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked sequentially. The first adhesive layer and the second adhesive layer are both obtained by coating and curing with a high-temperature resistant adhesive. The thickness of the first adhesive layer and the second adhesive layer is 65μm. The substrate layer is made of 14g cotton paper (thickness 30μm).
[0077] The method for preparing this high-performance cotton paper double-sided adhesive tape is characterized by comprising the following steps: S1. Preparation of high-temperature resistant adhesive: By weight fraction, 100 parts of polyacrylate, 40 parts of tackifying resin A, 5 parts of tackifying resin B, 0.035 parts of curing agent A, and 0.2 parts of curing agent B are mixed and stirred evenly to obtain a high-temperature resistant adhesive.
[0078] Among them, tackifying resin A is hydrogenated rosin resin with a softening point of 85℃ and an acid value of 7mgKOH / g; specifically, it is AS-5085F from Guangzhou Yabiao Technology Co., Ltd. Tackifying resin B is a hydrogenated petroleum resin with a softening point of 101℃ and an acid value of 12mgKOH / g; specifically, it is C-8010 from Nanjing Yangzi Eastman Chemical Co., Ltd. Curing agent A is an epoxy curing agent, specifically the epoxy curing agent ETERAC EC-97 produced by Changxing Chemical. Curing agent B is an isocyanate curing agent, specifically Bayer's isocyanate curing agent L-75.
[0079] Steps S2 and S3 are the same as in Example 1.
[0080] The ratio of the release force of the second side to the first side of the double-sided release layer is 2:1.
[0081] Performance testing The adhesive tapes prepared in the examples and comparative examples were subjected to the following performance tests: (1) The peel force performance of different boards was tested according to GB / T 2792-2014 standard for peel force test of pressure sensitive tape.
[0082] (2) Initial tack performance was tested according to GBT4853-2002 pressure-sensitive tape initial tack (rolling ball method).
[0083] (3) The holding force performance was tested in accordance with GB / T 4851-2014 pressure-sensitive tape holding force test standard.
[0084] The test results are shown in Table 1 below: Table 1 Test results show that by using two different types of hydrogenated resins in combination, the surface energy of the overall adhesive can be further controlled, resulting in better adhesion to materials with low surface energy. The hydrogenated resin primarily utilizes hydrogenation to treat the double bonds in the original resin, transforming them into more stable saturated single bonds, thus exhibiting higher resistance to yellowing and temperature variations. Finally, a modified rosin resin, pentaerythritol ester, containing four hydroxymethyl groups, is added, exhibiting high symmetry. After esterification, pentaerythritol triacrylate is obtained, which is compatible with the main adhesive, acrylic acid, and can be better dispersed on various branches, resulting in stronger dispersibility. This significantly improves the adhesive's bonding and temperature resistance properties compared to the original method.
[0085] The formulation in Comparative Example 1 is basically the same as that in Example 1, except that the tackifying resin A in Comparative Example 1 is not hydrogenated rosin resin. The test data shows that although Comparative Example 1 has good adhesion strength and temperature resistance to SUS, it does not have good adhesion to PP and PE materials. In Comparative Example 2, the final modified rosin resin (tackifying resin C) was not added, and only two hydrogenated resins were added. The data shows that the adhesion performance of Comparative Example 2 to PP and PE materials is not much different from that of Example 1, but there is a slight loss in adhesion and initial tack performance to SUS. The overall performance is worse than that of Example 1.
[0086] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details.
Claims
1. A high-temperature resistant adhesive for bonding low surface energy materials, characterized in that, The ingredients include the following parts by weight: 100 parts polyacrylate, 30-40 parts tackifying resin A, 5-8 parts tackifying resin B, 5-10 parts tackifying resin C, 0.02-0.05 parts curing agent A, and 0.1-0.5 parts curing agent B; The raw materials for preparing the polyacrylate include, by weight, 25-35 parts of isooctyl acrylate, 5-10 parts of butyl acrylate, 0.02-0.05 parts of hydroxyethyl acrylate, 2-5 parts of acrylic acid, 1-4 parts of methyl acrylate, 0.0008-0.0012 parts of initiator, 1-3 parts of silane coupling agent, 10-20 parts of modified resin, and 50-60 parts of solvent.
2. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The modified resin is obtained by mixing and reacting EVA and EAA in a mass ratio of (0.5-2):(0.5-2).
3. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The raw materials for preparing the polyacrylate include, by weight, 25-35 parts of isooctyl acrylate, 5-10 parts of butyl acrylate, 0.02-0.05 parts of hydroxyethyl acrylate, 2-5 parts of acrylic acid, 1-4 parts of methyl acrylate, 0.0008-0.0012 parts of initiator, 1-3 parts of silane coupling agent, 10-20 parts of modified resin, and 50-60 parts of solvent. The polyacrylate is prepared by the following method: ①Isooctyl acrylate, butyl acrylate, hydroxyethyl acrylate, acrylic acid, methyl acrylate, and solvent are mixed evenly in a certain proportion to obtain a monomer mixture. The monomer mixture is divided into a first monomer mixture and a second monomer mixture in a mass ratio of 6:
4. ② Mix EVA and EAA monomers in a reaction vessel at a mass ratio of 1.5:1 and control the temperature above 80℃. Add 4 times the total mass of EVA and EAA of butanone and mix evenly. Then add 15 parts per ten thousand of the total mass of EVA and EAA of initiator and let it react fully for more than 6 hours. Pour it out to obtain the modified resin. ③ Add the first monomer mixture to the reactor, purge with nitrogen, and add 0.06% (by weight of 0.06%) of the initiator at 64-65°C. After reacting for 2.5 hours, add 1.2% (by weight of 0.01%) of the initiator and heat to 78°C for 30 minutes. Add the second monomer mixture dropwise to the reactor over 90 minutes, maintaining the temperature at 78-80°C. After the dropwise addition is complete, keep the temperature at 80°C for 30 minutes. Add 0.2% (by weight of 0.02%) of the initiator and continue to keep the temperature above 80°C for 1 hour. Add 10-20 parts of the modified resin and continue the reaction for 1.5 hours. After the reaction is complete, the polyacrylate is obtained.
4. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The silane coupling agent is vinyltriethoxysilane.
5. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The tackifying resin A is one of rosin glycerol ester, disproportionated rosin resin, and hydrogenated rosin resin, with a softening point of 80-90℃ and an acid value of 4-15 mgKOH / g.
6. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The tackifying resin B is one of pentaerythritol ester, petroleum resin, or hydrogenated petroleum resin, with a softening point of 85-105℃ and an acid value of 8-20 mgKOH / g.
7. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The tackifying resin C is one of hydrogenated rosin resin, modified rosin resin, and terpene resin, with a softening point of 115-125℃ and an acid value of 20-30 mgKOH / g.
8. The high-temperature resistant adhesive for bonding low surface energy materials according to claim 1, characterized in that, The curing agent A is one of a metal salt curing agent, an isocyanate curing agent, or an epoxy curing agent; The curing agent B is one of epoxy curing agents, metal salt curing agents, or isocyanate curing agents.
9. A high-performance double-sided cotton paper tape suitable for bonding low surface energy materials, characterized in that, It includes a first adhesive layer, a substrate layer, a second adhesive layer and a double-sided release layer stacked in sequence. The first adhesive layer and the second adhesive layer are both obtained by coating and curing the high-temperature resistant adhesive as described in any one of claims 1-8. The substrate layer is cotton paper.
10. A method for preparing a high-performance cotton paper double-sided adhesive tape suitable for bonding low surface energy materials as described in claim 9, characterized in that, Includes the following steps: S1. Mix polyacrylate, tackifying resin A, tackifying resin B, tackifying resin C, curing agent A, and curing agent B, and stir evenly to obtain a high-temperature resistant adhesive. S2. Apply a high-temperature resistant adhesive to the first side of the double-sided release layer, bake and cure to form the first adhesive layer, then bond the first adhesive layer to the first side of the substrate layer and roll it up to form a semi-finished product. S3. Apply a high-temperature resistant adhesive to the second side of the double-sided release layer, bake and cure to form a second adhesive layer, peel off the double-sided release layer and the second adhesive layer on it, and then attach the second adhesive layer to the second side of the substrate layer to obtain the high-performance cotton paper double-sided tape suitable for bonding low surface energy materials.