Shell, manufacturing method thereof and electronic equipment

By introducing a layered structure into the shell and adjusting the raw material composition ratio of the adhesive layer, the problem of cracking caused by internal stress during the curing process of fiber composite shells was solved, achieving a rich and colorful appearance and improved impact resistance.

CN122094042APending Publication Date: 2026-05-26BEIJING XIAOMI MOBILE SOFTWARE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411708576.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-26
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

During the curing process, the internal stress caused by the volume shrinkage of the film structure in the fiber composite shell can easily lead to cracks when dropped or impacted, affecting the appearance and impact resistance.

Method used

The structure consists of a shell substrate, an inner textured layer, a coating layer, and an outer textured layer, all stacked together. The outer textured layer includes an adhesive layer, a connecting layer, and a first textured layer. By adjusting the raw material composition ratio of the adhesive layer, curing shrinkage stress is released, thereby improving interfacial bonding and impact resistance.

Benefits of technology

It achieves a rich and colorful appearance effect on the shell from different viewing angles, and significantly reduces the probability of cracks in the outer texture layer when dropped or impacted, thus improving the shell's impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122094042A_ABST
    Figure CN122094042A_ABST
Patent Text Reader

Abstract

The invention provides a shell, a manufacturing method thereof and electronic equipment. The shell comprises a shell base material, an inner texture layer, a coating layer and an outer texture layer which are arranged in a stacked mode. The outer texture layer comprises a bonding layer, a connecting layer and a first texture layer which are stacked, and the bonding layer covers the coating layer; the bonding layer comprises the following raw material components in percentage by mass: 20-40% of polyester resin; 40%-70% of an oxygen-containing solvent; 6%-15% of an aromatic solvent; and 5%-10% of isocyanate. The inner texture layer, the coating layer and the outer texture layer are arranged in a stacked mode, so that the shell can provide light rays of different colors at different observation angles, and the shell has a good and rich colorful appearance effect. The outer texture layer and the coating layer can be tightly combined through the bonding layer, the bonding layer has good crosslinking density, the curing shrinkage stress of the first texture layer can be released in the slow curing process of the bonding layer, the internal stress of the outer texture layer is reduced, and the impact resistance of the shell is improved; and the probability that the outer texture layer cracks when the shell falls or is impacted is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of electronic device components technology, and in particular to a housing and its manufacturing method, and an electronic device. Background Technology

[0002] With the development of technology and the improvement of living standards, electronic devices have become necessities. When choosing electronic devices, their appearance is one of the important factors for users. The appearance of electronic devices is mainly reflected in the casing. Fiber composite materials, due to their lightness, thinness, and high strength, have gradually become the main material for casings. However, the appearance of fiber composite materials is monotonous, and their appearance needs to be improved.

[0003] In related technologies, a film structure consisting of an inner texture, a physical vapor deposition coating, and an outer texture is formed on the surface of a fiber composite material to achieve a dazzling textured effect on the casing. However, since the coatings forming the inner and outer textures in the film structure on the surface of the fiber composite material are both photocurable coatings, the volume shrinkage during the curing process causes internal stress in the film structure. When the electronic device formed by the casing is dropped or subjected to an impact, the film structure on the casing is prone to cracking. Summary of the Invention

[0004] To overcome the problems existing in the related technologies, this disclosure provides a housing, a method for manufacturing the same, and an electronic device.

[0005] According to a first aspect of the present disclosure, a housing is provided, the housing comprising a housing substrate, an inner textured layer, a coating layer and an outer textured layer stacked together; the outer textured layer comprising an adhesive layer, a connecting layer and a first textured layer stacked together, the adhesive layer covering the coating layer;

[0006] The adhesive layer comprises the following raw material components by mass fraction: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%.

[0007] In some embodiments of this disclosure, the oxygen-containing solvent includes at least one of ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents.

[0008] In some embodiments of this disclosure, the adhesive layer comprises the following raw material components in the following mass fractions: polyester resin: 20%-40%; ketone solvent: 8%-15%; ester solvent: 14%-22%; alcohol solvent: 5%-10%; alcohol ether solvent: 13%-21%; aromatic solvent: 8%-14%; isocyanate: 5%-10%.

[0009] In some embodiments of this disclosure, the adhesive layer comprises the following raw material components in the indicated mass fractions: polyester resin: 25%-35%; methyl ethyl ketone (MEK): 10%-15%; butyl acetate: 10%-12%; ethyl acetate: 5%-8%; isopropanol: 5%-8%; propylene glycol methyl ether acetate: 15%-20%; toluene: 8%-10%; xylene: 1%-3%; isocyanate: 5%-10%.

[0010] In some embodiments of this disclosure, the thickness of the adhesive layer is 8 μm-12 μm; and / or,

[0011] The thickness of the connecting layer is 9μm-12μm; and / or,

[0012] The thickness of the first texture layer is 20μm-25μm.

[0013] In some embodiments of this disclosure, the first textured layer comprises the following raw material components in weight fractions: polypropylene ester: 45%-65%; polyurethane acrylate: 10%-15%; solvent: 23%-45%; photoinitiator: 2%-4%.

[0014] In some embodiments of this disclosure, the first textured layer comprises the following raw material components in the indicated mass fractions: polypropylene ester: 50%-60%; polyurethane acrylate: 11%-13%; ethyl acetate: 10%-15%; ethylene glycol butyl ether: 5%-10%; isopropanol: 5%-10%; n-butanol: 3%-5%; methyl isobutyl ketone: 1%-2%; and photoinitiator: 2%-4%.

[0015] In some embodiments of this disclosure, the material of the coating layer includes at least one of elemental silicon, silicon dioxide, titanium dioxide, zirconium dioxide, and niobium pentoxide.

[0016] In some embodiments of this disclosure, the inner texture layer includes an adhesive layer, a color layer, and a second texture layer stacked together, the adhesive layer covering the housing substrate.

[0017] In some embodiments of this disclosure, the thickness of the adhesive layer is 8 μm-12 μm; and / or,

[0018] The thickness of the color layer is 22μm-27μm; and / or,

[0019] The thickness of the second texture layer is 20μm-25μm.

[0020] In some embodiments of this disclosure, the housing further includes an anti-fouling layer that covers the first textured layer.

[0021] According to a second aspect of this disclosure, a method for manufacturing a housing is provided, the method comprising:

[0022] An inner texture layer is formed on the surface of the housing substrate;

[0023] A coating layer is formed on the surface of the inner texture layer;

[0024] An adhesive layer, a connecting layer, and a first texture layer are sequentially formed on the surface of the coating layer, and the adhesive layer, the connecting layer, and the first texture layer are stacked to form an outer texture layer;

[0025] The adhesive layer comprises the following raw material components by mass fraction: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%.

[0026] In some embodiments of this disclosure, the adhesive layer comprises the following raw material components in the indicated mass fractions: polyester resin: 25%-35%; methyl ethyl ketone (MEK): 10%-15%; butyl acetate: 10%-12%; ethyl acetate: 5%-8%; isopropanol: 5%-8%; propylene glycol methyl ether acetate: 15%-20%; toluene: 8%-10%; xylene: 1%-3%; isocyanate: 5%-10%.

[0027] In some embodiments of this disclosure, the first textured layer comprises the following raw material components in the indicated mass fractions: polypropylene ester: 50%-60%; polyurethane acrylate: 10%-15%; ethyl acetate: 10%-15%; ethylene glycol butyl ether: 5%-10%; isopropanol: 5%-10%; n-butanol: 3%-5%; methyl isobutyl ketone: 1%-2%; and photoinitiator: 2%-4%.

[0028] In some embodiments of this disclosure, forming an inner texture layer on the surface of the housing substrate includes:

[0029] An adhesive layer, a color layer, and a second texture layer are sequentially formed on the surface of the housing substrate, and the adhesive layer, the color layer, and the second texture layer form the inner texture layer.

[0030] According to a third aspect of this disclosure, an electronic device is provided, the electronic device comprising the housing provided in the first aspect.

[0031] The technical solutions provided by the embodiments of this disclosure can include the following beneficial effects: the shell has a stacked structure of an inner texture layer, a coating layer, and an outer texture layer, which allows the shell to provide different colored light under different viewing angles, and the shell has a good and rich dazzling appearance effect. By setting the content ratio of each raw material component in the adhesive layer of the outer texture layer of the shell, the adhesive layer can tightly bond the connecting layer and the first texture layer to the coating layer, and the adhesive layer has a good cross-linking density. During the curing process of the adhesive layer, the curing shrinkage stress of the first texture layer can be released, thereby reducing the internal stress of the outer texture layer, improving the impact resistance of the shell, and reducing the probability of cracks in the outer texture layer when the shell is dropped or impacted.

[0032] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit this disclosure. Attached Figure Description

[0033] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0034] Figure 1 This is a schematic diagram of the structure of the housing according to an exemplary embodiment.

[0035] Figure 2 This is a schematic diagram of the structure of the housing according to another exemplary embodiment.

[0036] Figure 3 This is a schematic diagram of the structure of the housing according to another exemplary embodiment.

[0037] Figure 4 This is a flowchart illustrating a method for manufacturing a housing according to an exemplary embodiment. Detailed Implementation

[0038] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numerals in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples of apparatuses and methods consistent with some aspects of the invention as detailed in the appended claims.

[0039] The appearance of electronic devices is primarily determined by their casing. Fiber-reinforced composites, due to their thinness and high strength, are increasingly becoming the main material for casings. However, their appearance is often monotonous, necessitating improvements. One related technology involves creating an internal texture-physical vapor deposition (PVD) coating-external texture layer structure on the surface of the fiber-reinforced composite material to achieve vibrant textured effects. However, since the coatings forming the internal and external textures in this film structure are photocurable, the volume shrinkage during curing causes internal stress in the film structure. When the electronic device is dropped or subjected to impact, the film structure on the casing is prone to cracking.

[0040] In view of this, the present disclosure provides a housing comprising a housing substrate, an inner textured layer, a coating layer, and an outer textured layer stacked together; the outer textured layer comprising an adhesive layer, a connecting layer, and a first textured layer stacked together, the adhesive layer covering the coating layer; the adhesive layer comprising the following raw material components by mass fraction: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%. The stacked inner textured layer, coating layer, and outer textured layer enable the housing to provide different colored light under different viewing angles, resulting in a rich and vibrant visual effect. By setting the content ratio of each raw material component in the adhesive layer of the outer textured layer, the adhesive layer can tightly bond the connecting layer and the first textured layer to the coating layer, and the adhesive layer has a good cross-linking density. During the slow curing process of the adhesive layer, the curing shrinkage stress of the first textured layer can be released, thereby reducing the internal stress of the outer textured layer, improving the impact resistance of the housing, and reducing the probability of cracks in the outer textured layer when the housing is dropped or impacted.

[0041] In one exemplary embodiment of this disclosure, a housing is provided, see [link to example]. Figure 1 As shown, Figure 1 This is a schematic diagram of the structure of a housing shown in an exemplary embodiment. The housing 100 includes a housing substrate 10, an inner texture layer 20, a coating layer 30 and an outer texture layer 40 stacked together. The outer texture layer 40 includes an adhesive layer 41, a connecting layer 42 and a first texture layer 43 stacked together. The adhesive layer 41 covers the coating layer 30.

[0042] To avoid affecting the appearance provided by the inner texture layer 20, the coating layer 30, and the outer texture layer 40, the appearance stack structure consisting of the inner texture layer 20, the coating layer 30, and the outer texture layer 40 is disposed on the outer surface of the housing substrate 10, that is, the surface that the user directly touches and sees. This allows the vibrant appearance effect provided by the appearance stack structure consisting of the inner texture layer 20, the coating layer 30, and the outer texture layer 40 to be directly visible to the human eye, making the vibrant appearance effect more pronounced. In other words, the inner texture layer 20 is a texture layer farther away from the user, while the outer texture layer 40 is a texture layer closer to the user.

[0043] The shell substrate 10 is the main structure of the shell 100. It can be formed of inorganic materials such as glass, microcrystalline glass, ceramic, and sapphire glass, or it can be formed by laminating one or more plastic materials such as PMMA (poly(methyl methacrylate), PC (polycarbonate), ABS (acrylonitrile butadiene styrene copolymer), PET (poly(ethylene terephthalate), and PVC (polyvinyl chloride). It can also be formed of fiber composite materials such as glass fiber composites, carbon fiber composites, and aramid fiber composites. In some examples, the shell substrate 10 is formed by hot pressing at least one layer of glass fiber composite prepreg. In some examples, the shell substrate 10 is formed by 3D hot pressing at least five layers of glass fiber composite prepreg.

[0044] The inner texture layer 20 covers the shell substrate 10. The inner texture layer 20 ensures a tight bond between the coating layer 30 and the shell substrate 10, providing good adhesion between the layered structure (inner texture layer 20, coating layer 30, and outer texture layer 40) and the shell substrate 10, preventing the layered structure from detaching. The inner texture layer 20 also provides a texture, such as a pyramidal texture or a prism texture, to create a three-dimensional effect. When light reaches the inner texture layer 20, the three-dimensional texture refracts and reflects the light. The reflected light then passes through the high-gloss texture provided by the coating layer 30, resulting in a bright and dazzling appearance. Due to the three-dimensional texture provided by the inner texture layer 20, the glossy glare effect shifts with the viewing angle, creating a good light and shadow effect. For example, the inner texture layer 20 can be formed using processes such as transfer printing, imprinting, or screen printing.

[0045] In some examples, reference Figure 2As shown, the inner texture layer 20 may include a laminated adhesive layer 21, a color layer 22, and a second texture layer 23, with the adhesive layer 21 covering the housing substrate 10. The adhesive layer 21 ensures good interfacial adhesion between the inner texture layer 20 and the housing substrate 10, and can be formed by printing, coating, or spraying a material with good adhesion. In some examples, the thickness of the adhesive layer 21 can be between 8 μm and 12 μm. In some examples, the main material of the adhesive layer 21 may include chlorinated polypropylene resin, polyurethane resin, etc.

[0046] Color layer 22 is used to provide color so that the inner texture layer 20 can provide the base color of the housing 100. Color layer 22 can be formed by printing, coating, or spraying with colored paint or ink. It is understood that color layer 22 is opaque so that the wavelength of light reflected by color layer 22 can present the color provided by color layer 22. In some examples, the thickness of color layer 22 can be between 22 μm and 27 μm to ensure that color layer 22 is opaque. In some examples, color layer 22 can be formed of polyurethane colored coating.

[0047] The second texture layer 23 is used to provide a three-dimensional texture, such as a pyramid texture, prism texture, or other textures with a three-dimensional effect. In some examples, the thickness of the second texture layer 23 can be between 20μm and 25μm to ensure that it can provide a good and clear texture effect.

[0048] For example, the second textured layer 23 can be formed using a photosensitive resin (e.g., a UV resin) through a transfer or imprinting process. For instance, when forming the second textured layer 23 using a transfer process, a texture mold can be used to coat or spray the UV resin onto the texture mold. The housing substrate 10, which is provided with the adhesive layer 21 and the color layer 22, is then placed on the surface of the texture mold with the color layer 22 facing the texture mold. After rolling, the color layer 22 is adhered to the texture mold. After initial curing, the housing substrate 10 is peeled off from the texture mold and then irradiated with a UV lamp or Hg lamp to completely cure the UV resin, thereby forming the second textured layer 23. For example, when forming the second texture layer 23 using the imprinting process, UV resin is coated or sprayed onto the color layer 22. After the UV resin surface dries, the texture film is used to imprint the texture on the texture film onto the incompletely cured UV resin under vacuum and pressure. After the UV resin is initially cured, the texture film is removed and then irradiated with a UV lamp or Hg lamp to completely cure the UV resin and form the second texture layer 23.

[0049] Understandably, the second textured layer 23 formed by UV resin will generate stress due to volume shrinkage during the curing process, especially when the second textured layer 23 is fully cured by subsequent irradiation with a UV lamp or Hg lamp. The stress generated in the second textured layer 23 increases with the degree of curing. At the same time, in order to ensure the color of the color layer 22, the thickness of the color layer 22 supporting the second textured layer 23 is relatively large. The curing process of the thicker color layer 22 can release the curing shrinkage stress of the second textured layer 23, thereby reducing the risk of the inner textured layer 20 peeling off.

[0050] refer to Figure 1 and Figure 2 As shown, the coating layer 30 is disposed between the inner texture layer 20 and the outer texture layer 40. Specifically, the coating layer 30 is disposed on the surface of the second texture layer 23, and the texture provided by the second texture layer 23 can also provide good adhesion for the formation of the coating layer 30. The coating layer 30 can be formed using materials such as oxides, metals, and rare earth materials through processes such as evaporation deposition, plasma sputtering, ion beam sputtering, atomic layer deposition, and magnetron sputtering. In some examples, the material of the coating layer 30 can include, but is not limited to, elemental silicon, silicon dioxide, titanium dioxide, zirconium dioxide, and niobium pentoxide. In some examples, the thickness of the coating layer 30 can be between 200 nm and 250 nm. The coating layer 30 can be multilayered. Based on the requirements of the transmission and reflection properties of the coating layer 30, the number of coating layers 30, as well as the material and thickness of each layer, can be set.

[0051] Under natural light, the coating layer 30 can reflect colored light, creating a bright and dazzling effect. Simultaneously, the coating layer 30 has a certain degree of light transmittance, allowing the light reflected from the color layer 22 in the inner texture layer 20 to pass through the second texture layer 23, the coating layer 30, and the outer texture layer 40 and be observed. The coating layer 30 enables the shell 100 to achieve a dazzling high-gloss effect, allowing observers to visually perceive different colors of light from multiple viewing angles, creating a dazzling color-changing effect.

[0052] The outer texture layer 40 covers the coating layer 30. The outer texture layer 40 includes an adhesive layer 41, a connecting layer 42, and a first texture layer 43 stacked together, with the adhesive layer 41 covering the coating layer 30. The adhesive layer 41 ensures good interfacial adhesion between the outer texture layer 40 and the coating layer 30. The connecting layer 42 serves as the interface between the adhesive layer 41 and the first texture layer 43, and provides the outer texture layer 40 with a certain degree of toughness, improving its impact resistance. The first texture layer 43 forms the outer surface of the housing 100, and the texture provided by the first texture layer 43 contributes to a better appearance of the housing 100 and provides a certain tactile feel to its surface. In some examples, the texture provided by the first texture layer 43 may be, for example, a glittery texture, an anti-glare texture, etc.

[0053] It should be noted that, since the outer texture layer 40 is disposed on the outer surface of the coating layer 30, the adhesive layer 41, the connecting layer 42, and the first texture layer 43 in the outer texture layer 40 are all translucent, and the adhesive layer 41, the connecting layer 42, and the first texture layer 43 all need to be of relatively small thickness to avoid affecting the texture effect of the coating layer 30. In some examples, the thickness of the adhesive layer 41 can be between 8μm and 12μm, the thickness of the connecting layer 42 can be between 9μm and 12μm, and the thickness of the first texture layer 43 can be between 20μm and 25μm.

[0054] refer to Figure 2 As shown, since the forming material of the first texture layer 43 is similar to that of the second texture layer 23 (both are UV resins), and the texture forming process is also similar, the first texture layer 43 will also experience volume shrinkage and generate significant stress during curing. However, the thickness of the connecting layer 42 adjacent to the first texture layer 43 is relatively small, making it unable to release the shrinkage stress generated by the first texture layer 43. Therefore, by setting the raw material composition and content ratio of the adhesive layer 41, while ensuring good adhesion between the outer texture layer 40 and the coating layer 30, the curing process of the adhesive layer 41 can release the curing shrinkage stress generated by the first texture layer 43, thereby reducing the internal stress of the outer texture layer 40, improving the overall impact resistance of the shell 100, and reducing the probability of cracks in the outer texture layer 40 when the shell 100 is dropped or impacted.

[0055] In some examples, the raw material components contained in the adhesive layer 41 are expressed in mass fractions as follows: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%.

[0056] Isocyanate serves as a curing agent in the raw material components of adhesive layer 41. The isocyanate contains -N=C=O groups and can react with compounds containing active hydrogen atoms, such as hydroxyl groups in polyester resins. When the oxygen-containing solvent includes hydroxyl compounds, the isocyanate can also react with the hydroxyl compounds to generate polyurethane. Exemplarily, the isocyanate may include monoisocyanate, diisocyanate, or polyisocyanate. In some examples, the isocyanate includes at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and lysine diisocyanate (LDI). In some examples, the mass fraction of isocyanate in the raw material components of adhesive layer 41 is 5%-10%. In some examples, the mass fraction of isocyanate in the raw material components of adhesive layer 41 is 6%-8%.

[0057] Polyester resin, as the main component of the adhesive layer 41, is a polymer compound formed by the condensation polymerization of alcohol and acid. The polyester resin can be a saturated polyester containing hydroxyl groups. The polyester resin provides polymer segments, and the hydroxyl groups in the polyester resin can undergo a cross-linking and curing reaction with isocyanate to generate polyester-type polyurethane. Because polyester contains ester groups with extremely strong covalent bonds, these ester groups can further form hydrogen bonds, acting as elastic cross-linking points. Therefore, the adhesive layer 41 formed by polyester-type polyurethane has good adhesion, mechanical properties, abrasion resistance, and tear resistance. Furthermore, saturated polyester has a low shrinkage rate during curing. During the slow curing process of the polyester resin and isocyanate in the adhesive layer 41, the curing shrinkage stress of the first textured layer 43 can be continuously released. In some examples, the mass fraction of polyester resin in the raw material components of the adhesive layer 41 is 20%-40%. In some examples, the mass fraction of polyester resin in the raw material components of the adhesive layer 41 is 25%-35%.

[0058] Oxygen-containing solvents are solvents containing oxygen atoms in their molecules. They possess high polarity, allowing them to dissolve polyester resins and resulting in a resin system forming the adhesive layer 41 with good flowability and low viscosity. Exemplarily, oxygen-containing solvents may include at least one of ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents. Ketone solvents may include, but are not limited to, acetone, butanone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. Ester solvents may include, but are not limited to, ethyl acetate, butyl acetate, isopropyl acetate, etc. Alcohol solvents may include, but are not limited to, ethanol, n-butanol, isopropanol, etc. Alcohol ether solvents may include, but are not limited to, ethylene glycol butyl ether, propylene glycol methyl ether acetate, etc. In some examples, the mass fraction of the oxygen-containing solvent in the raw material components of the adhesive layer 41 is 40%-70%. In some examples, the mass fraction of the oxygen-containing solvent in the raw material components of the adhesive layer 41 is 45%-65%.

[0059] When the oxygen-containing solvent includes alcohols and / or alcohol ethers, it can also react with isocyanates and participate in the curing reaction. When the oxygen-containing solvent includes ketones, the presence of the carbonyl group makes ketones hydrogen bond acceptors, resulting in excellent solubility. When the oxygen-containing solvent includes esters, although esters are less polar than alcohols, they still exhibit good solubility for polyester resins.

[0060] When the oxygen-containing solvent includes ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents, the mixed solvent obtained by combining multiple solvents has a greater dissolving capacity than a single solvent, and makes the resin system have good fluidity and low viscosity. In addition, some solvents can also participate in the curing reaction, resulting in the formed adhesive layer 41 having a high crosslinking density.

[0061] Aromatic solvents can also effectively dissolve polyester resins, and their cost is lower than that of oxygen-containing solvents. Blending aromatic solvents with oxygen-containing solvents can adjust the viscosity, leveling, and volatility of the resin system. Aromatic solvents can include toluene, xylene, mixed aromatics S-100, mixed aromatics S-150, mixed aromatics S-200, etc. In some examples, the mass fraction of aromatic solvents in the raw material components of the adhesive layer 41 is 6%-15%. In other examples, the mass fraction of aromatic solvents in the raw material components of the adhesive layer 41 is 8%-14%.

[0062] In some examples, the oxygen-containing solvents include ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents. The raw material components contained in the adhesive layer 41 are expressed in mass fraction as follows: polyester resin: 20%-40%; ketone solvents: 8%-15%; ester solvents: 14%-22%; alcohol solvents: 5%-10%; alcohol ether solvents: 13%-21%; aromatic solvents: 5%-15%; isocyanate: 5%-10%. Among them, ketone solvents can be butanone, acetone, etc.; ester solvents can be ethyl acetate, butyl acetate, isopropyl acetate, etc.; alcohol solvents can be n-butanol, isopropanol, etc.; and alcohol ethers can be propylene glycol methyl ether acetate.

[0063] In some examples, the ketone solvent may be butanone, the ester solvent may include butyl acetate and ethyl acetate, the alcohol solvent may be isopropanol, and the alcohol ether solvent may be propylene glycol methyl ether acetate. The raw material components contained in the adhesive layer 41 are expressed in mass fraction as follows: polyester resin: 25%-35%; butanone: 10%-15%; butyl acetate: 10%-12%; ethyl acetate: 5%-8%; isopropanol: 5%-8%; propylene glycol methyl ether acetate: 15%-20%; aromatic solvent: 5%-15%; isocyanate: 5%-10%.

[0064] In some examples, ketone solvents may be butanone (MEK), ester solvents may include butyl acetate and ethyl acetate, alcohol solvents may be isopropanol, alcohol ether solvents may be propylene glycol methyl ether acetate, and aromatic solvents may include toluene and xylene. The raw material components contained in the adhesive layer 41 are expressed in mass fractions as follows: polyester resin: 25%-35%; MEK: 10%-15%; butyl acetate: 10%-12%; ethyl acetate: 5%-8%; isopropanol: 5%-8%; propylene glycol methyl ether acetate: 15%-20%; toluene: 8%-10%; xylene: 1%-3%; isocyanate: 5%-10%.

[0065] Since the first textured layer 43 serves as the outer surface of the housing 100, it needs to possess good toughness to ensure the housing 100 has good impact resistance and reduce the probability of cracking upon impact. In some examples, the raw material components of the first textured layer 43, expressed as mass fractions, are: polypropylene ester: 45%-65%; polyurethane acrylate: 10%-15%; solvent: 23%-45%; photoinitiator: 2%-4%.

[0066] Polypropylene ester, as the main resin in the raw material component of the first textured layer 43, forms a first textured layer 43 with good flexibility, resistance to yellowing, weather resistance, and adhesion. The first textured layer 43 also has good gloss, giving the shell 100 a good appearance and feel. In some examples, the mass percentage of polypropylene ester in the raw material component of the first textured layer 43 is 45%-65%. In some examples, the mass percentage of polypropylene ester in the raw material component of the first textured layer 43 is 50%-60%.

[0067] Polyurethane acrylate, as a prepolymer in the raw material components of the first textured layer 43, gives the first textured layer 43, formed by a resin system containing polyurethane acrylate, good mechanical abrasion resistance and toughness. This results in a high elongation at break in the first textured layer 43, giving the shell 100 good impact resistance and reducing the probability of cracking upon drop. Furthermore, polyurethane acrylate can reduce stress shrinkage of the first textured layer 43 during curing and reduce internal stress in the outer textured layer 40, further preventing cracking of the shell 100. In some examples, the mass percentage of polyurethane acrylate in the raw material components of the first textured layer 43 is 10%-15%. In other examples, the mass percentage of polyurethane acrylate is 11%-13%.

[0068] The solvent is used to disperse and dissolve the polypropylene ester, polyurethane acrylate, and photoinitiator, and to adjust the viscosity and rheological properties of the resin system, making it easy to coat and form the first textured layer 43. Simultaneously, selecting a suitable solvent can improve the appearance of the first textured layer 43, such as gloss and fullness. The solvent in the first textured layer 43 can include oxygen-containing solvents such as ketone solvents, ester solvents, alcohol solvents, etc., and can also include aromatic solvents. In some examples, the solvent accounts for 23%-45% of the raw material components of the first textured layer 43 by mass. In some examples, the solvent accounts for 24%-42% of the first textured layer 43 by mass.

[0069] Photoinitiators are used to absorb the energy of light of a certain wavelength under illumination, generating active substances such as free radicals and cations. These active substances can initiate cross-linking reactions of monomers or prepolymers, allowing the liquid resin system to cure. This results in the formation of a clearly defined texture in the first textured layer 43, thus achieving a certain aesthetic effect. Photoinitiators can be free radical photoinitiators, cationic photoinitiators, etc. In some examples, photoinitiators may include, but are not limited to, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylbenzophenone, 2-hydroxy-2-methyl-1-phenylpropanone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, α-hydroxyalkylbenzophenone, α-aminealkylbenzophenone, etc. In some examples, the photoinitiator has a mass percentage of 2%-4% in the raw material components of the first textured layer 43.

[0070] It is understandable that the raw material components of the first textured layer 43 may also include reactive diluents. Reactive diluents are used to adjust the viscosity of the resin system and participate in the curing reaction of the resin system, becoming part of the cross-linked network structure of the resin system. Reactive diluents are monomers with C=C unsaturated double bonds, such as monomers containing acryloyloxy, methacryloyloxy, vinyl, or allyl groups. In some examples, reactive diluents may include styrene, vinylpyrrolidone, vinyl acetate, butyl acrylate, isooctyl acrylate, hydroxy methacrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, trimethylolpropane triacrylate, etc.

[0071] In some examples, the solvent may include ethyl acetate, ethylene glycol butyl ether, isopropanol, n-butanol, methyl isobutyl ketone, etc. The raw material components contained in the first texture layer 43 are expressed in mass fraction as follows: polypropylene ester: 50%-60%; polyurethane acrylate: 11%-13%; ethyl acetate: 10%-15%; ethylene glycol butyl ether: 5%-10%; isopropanol: 5%-10%; n-butanol: 3%-5%; methyl isobutyl ketone: 1%-2%; photoinitiator: 2%-4%.

[0072] Since the first texture layer 43 serves as the outer surface of the housing 100, and the first texture layer 43 has a texture, when a user touches the housing 100, the texture in the first texture layer 43 easily traps dirt and grime. Therefore, in some examples, [referencing...] Figure 3As shown, in addition to the stacked shell substrate 10, inner texture layer 20, coating layer 30, and outer texture layer 40, the shell 100 also includes an anti-fouling layer 50, which covers the first texture layer 43 of the outer texture layer 40. That is, the anti-fouling layer 50 serves as the outer surface of the shell 100. The anti-fouling layer 50 can be formed of an organic fluorine material. An anti-fouling layer 50 formed of organic fluorine material with a thickness at the nanometer level can achieve good anti-fouling effects, giving the surface of the shell 100 a large water contact angle. Dirt and fingerprints are less likely to remain on the surface of the shell 100, and the shell 100 is easy to clean. Furthermore, the relatively thin anti-fouling layer 50 does not affect the appearance of the stacked inner texture layer 20, coating layer 30, and outer texture layer 40, nor does it affect the textured feel provided by the first texture layer 43, resulting in a good user experience.

[0073] The housing provided in this disclosure, after production, was randomly sampled into 20 units. After a 50cm drop ball test, no cracks or peeling of the laminated structure were observed in the housing. Furthermore, after assembling the drop ball-tested housing with the main structure of the electronic device, a roller drop test was conducted. After 100 rounds of roller drop testing, none of the 20 samples showed any cracks. In contrast, in existing housing comparison models, when 10 housing comparison models were used for roller drop testing, one model cracked in the fifth round, and all models cracked after 65 rounds. Therefore, it can be demonstrated that the housing provided in this disclosure has excellent impact resistance and effectively improves the problem of housing cracking.

[0074] In one exemplary embodiment, this disclosure also provides a method for manufacturing a housing. This method can be used to manufacture the housing provided in the above embodiments of this disclosure. (Refer to...) Figure 4 The method for manufacturing the shell includes the following steps:

[0075] Step S100: Form an inner texture layer on the surface of the shell substrate;

[0076] Step S200: Form a coating layer on the surface of the inner texture layer;

[0077] Step S300: An adhesive layer, a connecting layer and a first texture layer are sequentially formed on the surface of the coating layer, and the stacked adhesive layer, connecting layer and first texture layer form an outer texture layer.

[0078] In step S100, refer to Figure 1As shown, an inner texture layer 20 can be formed on the surface of the shell substrate 10 using UV resin through texturing processes such as stencil printing and transfer printing. The material of the shell substrate 10 can be glass, microcrystalline glass, ceramic, PMMA, PC, ABS, glass fiber composite material, carbon fiber composite material, aramid fiber composite material, etc.

[0079] In some examples, reference Figure 2 As shown, the inner texture layer 20 may include an adhesive layer 21, a color layer 22, and a second texture layer 23 stacked together. The adhesive layer 21 ensures good interfacial adhesion between the inner texture layer 20 and the housing substrate 10; the color layer 22 provides color, allowing the inner texture layer 20 to provide the underlying color of the housing 100; the second texture layer 23 provides a three-dimensional texture, so that when light reaches the second texture layer 23, the three-dimensional texture provided by the second texture layer 23 can refract and reflect the light. When forming the inner texture layer 20, the adhesive layer 21, color layer 22, and second texture layer 23 may be sequentially formed on the surface of the housing substrate 10.

[0080] In some examples, the adhesive layer 21 can be formed using a chlorinated polypropylene resin primer or a polyurethane resin primer, and the viscosity of the primer for forming the adhesive layer 21 can be as low as 9.2 μm. 2 / s-9.8m 2 Between / s, the primer is applied or sprayed onto the surface of the housing substrate 10 and dried or cured at 60℃-70℃ to form an adhesive layer 21. The thickness of the adhesive layer 21 can be between 8μm and 12μm.

[0081] In some examples, polyurethane colored coatings can be used to form color layer 22, and the viscosity of the color paint used to form color layer 22 can be as low as 8.5 m. 2 / s-9.5m 2 Between / s, the paint is applied or sprayed onto the surface of the cured adhesive layer 21 and cured at 60℃-70℃ to form the color layer 22, the thickness of which can be between 22μm and 27μm.

[0082] In some examples, the second textured layer 23 can be formed using a UV coating. The main resin of the UV coating can be polypropylene, so that the formed second textured layer 23 has good flexibility. The viscosity of the UV coating used to form the second textured layer 23 can be 9.0 μL. 2 / s-10.0m 2The thickness of the second texture layer 23 can be between 20μm and 25μm, with a speed between [value missing]. The second texture layer 23 can be formed using a printing process. UV coating is applied or sprayed onto the surface of the cured color layer 22. The surface of the UV coating layer is dried at 45℃-55℃. The texture film is pressed onto the coating layer, and the coating layer is irradiated with an LED light source with 25% curing energy under a vacuum of 17s and a pressure of 150Kg to allow the UV coating to initially cure. The texture on the texture film is then completely transferred onto the incompletely cured coating layer. Next, the texture film is released and exposed to a UV lamp at 700mj / cm [value missing]. 2 -900mj / cm 2 The UV coating is irradiated under curing energy to fully cure, thereby forming the second texture layer 23.

[0083] Although the second texture layer 23 formed by the UV coating will generate stress due to volume shrinkage during the curing process, especially when the second texture layer 23 is fully cured by subsequent UV lamp irradiation, the stress generated by the second texture layer 23 increases with the degree of curing. At the same time, in order to ensure the color of the color layer 22, the color layer 22 adjacent to the second texture layer 23 is thicker. The curing process of the thicker color layer 22 can release the curing shrinkage stress of the second texture layer 23, thereby preventing the inner texture layer 20 from peeling off.

[0084] In step S200, the coating layer 30 can be formed using materials such as oxides, metals, and rare earth materials through processes such as evaporation deposition, plasma sputtering, ion beam sputtering, atomic layer deposition, and magnetron sputtering. In some examples, the material of the coating layer 30 can include, but is not limited to, elemental silicon, silicon dioxide, titanium dioxide, zirconium dioxide, and niobium pentoxide. In some examples, the thickness of the coating layer 30 can be between 200 nm and 250 nm. The coating layer 30 can be multilayered. Based on the requirements of the transmission and reflection properties of the coating layer 30, the number of layers, the material of each layer, the thickness, etc., can be set.

[0085] In some examples, the coating layer 30 can be formed by evaporation deposition of elemental silicon, and the vacuum value of the evaporation chamber can be controlled at 4*10. -2 -6*10 -2The evaporation deposition process includes a preheating section, a pre-melting section, a pre-melting holding section, and an evaporation section. In the preheating section, the voltage is maintained between 3.0V and 3.4V for 15-25 seconds; in the pre-melting section, the voltage is maintained between 3.2V and 3.6V for 35-45 seconds; in the pre-melting holding section, the voltage is maintained between 3.4V and 3.8V for 35-45 seconds; and in the evaporation section, the voltage is maintained between 3.6V and 4.0V for 10-20 seconds, thus forming the coating layer 30.

[0086] In step S300, the outer texture layer 40 includes an adhesive layer 41, a connecting layer 42, and a first texture layer 43 stacked together, with the adhesive layer 41 covering the coating layer 30. The adhesive layer 41 ensures good interfacial adhesion between the outer texture layer 40 and the coating layer 30; the connecting layer 42 serves as the interface between the adhesive layer 41 and the first texture layer 43, and provides the outer texture layer 40 with a certain degree of toughness, improving its impact resistance; the first texture layer 43 serves as the outer surface of the housing 100, and the texture provided by the first texture layer 43 contributes to a better appearance of the housing 100 and gives the surface of the housing 100 a certain tactile feel. When forming the outer texture layer 40, the adhesive layer 41, the connecting layer 42, and the first texture layer 43 can be formed sequentially on the surface of the coating layer 30.

[0087] In some examples, the raw material components comprising the adhesive layer 41 are expressed as follows by mass fraction: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%. When forming the adhesive layer 41, the above raw materials can be prepared according to the specified proportions and mixed uniformly to obtain a viscosity of 8.2 m. 2 / s-8.8m 2 A resin composition with a thickness between 8 μm and 12 μm is applied or coated onto the surface of the coating layer 30 and cured at 65°C-75°C to form an adhesive layer 41. The adhesive layer 41 has a thickness between 8 μm and 12 μm. In the resin composition, polyester resin provides polymer segments, and the hydroxyl groups in the polyester resin can undergo a cross-linking curing reaction with isocyanate to generate polyester-type polyurethane. Because the polyester resin contains ester groups with extremely strong covalent bonds, these ester groups can further form hydrogen bonds with the hard segments, acting as elastic cross-linking points. Therefore, the adhesive layer 41 formed by the polyester-type polyurethane has good adhesion, mechanical properties, abrasion resistance, and tear resistance. Furthermore, the saturated polyester has a low shrinkage rate during curing, and the slow curing process of the polyester resin and isocyanate in the adhesive layer 41 can continuously release the curing shrinkage stress of the subsequently formed first textured layer 43.

[0088] The isocyanate may include monoisocyanates, diisocyanates, or polyisocyanates. In some examples, the isocyanate includes at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate. The oxygen-containing solvent may include at least one of ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents. Ketone solvents may include, but are not limited to, acetone, butanone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. Ester solvents may include, but are not limited to, ethyl acetate, butyl acetate, isopropyl acetate, etc. Alcohol solvents may include, but are not limited to, ethanol, n-butanol, isopropanol, etc. Alcohol ether solvents may include, but are not limited to, ethylene glycol butyl ether, propylene glycol methyl ether acetate, etc. Aromatic solvents may include toluene, xylene, mixed aromatic hydrocarbons S-100, mixed aromatic hydrocarbons S-150, mixed aromatic hydrocarbons S-200, etc.

[0089] In some examples, the oxygen-containing solvents include ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents. The raw material components contained in the adhesive layer 41 are expressed in mass fraction as follows: polyester resin: 20%-40%; ketone solvents: 8%-15%; ester solvents: 14%-22%; alcohol solvents: 5%-10%; alcohol ether solvents: 13%-21%; aromatic solvents: 5%-15%; isocyanate: 5%-10%. Among them, ketone solvents can be butanone, acetone, etc.; ester solvents can be ethyl acetate, butyl acetate, isopropyl acetate, etc.; alcohol solvents can be n-butanol, isopropanol, etc.; and alcohol ethers can be propylene glycol methyl ether acetate.

[0090] In some examples, the ketone solvent may be butanone, the ester solvent may include butyl acetate and ethyl acetate, the alcohol solvent may be isopropanol, and the alcohol ether solvent may be propylene glycol methyl ether acetate. The raw material components contained in the adhesive layer 41 are expressed in mass fraction as follows: polyester resin: 25%-35%; butanone: 10%-15%; butyl acetate: 10%-12%; ethyl acetate: 5%-8%; isopropanol: 5%-8%; propylene glycol methyl ether acetate: 15%-20%; aromatic solvent: 5%-15%; isocyanate: 5%-10%.

[0091] In some examples, ketone solvents may be butanone (MEK), ester solvents may include butyl acetate and ethyl acetate, alcohol solvents may be isopropanol, alcohol ether solvents may be propylene glycol methyl ether acetate, and aromatic solvents may include toluene and xylene. The raw material components contained in the adhesive layer 41 are expressed in mass fractions as follows: polyester resin: 25%-35%; MEK: 10%-15%; butyl acetate: 10%-12%; ethyl acetate: 5%-8%; isopropanol: 5%-8%; propylene glycol methyl ether acetate: 15%-20%; toluene: 8%-10%; xylene: 1%-3%; isocyanate: 5%-10%.

[0092] By setting the raw material composition and content ratio of the adhesive layer 41, the adhesive layer 41 can achieve good adhesion between the outer texture layer 40 and the coating layer 30. At the same time, the curing process of the adhesive layer 41 can release the curing shrinkage stress generated during the curing process of the subsequently formed first texture layer 43, thereby reducing the internal stress of the outer texture layer 40, improving the overall impact resistance of the shell 100, and reducing the probability of cracks in the outer texture layer 40 when the shell 100 is dropped or impacted.

[0093] In some examples, the connecting layer 42 can be formed using a transparent polyurethane coating, and the viscosity of the coating forming the connecting layer 42 can be as low as 7.5 μm. 2 / s-8.5m 2 Between / s, a transparent coating is applied or sprayed onto the surface of the cured adhesive layer 41 and cured at 60℃-70℃ to form a bonding layer 42. The thickness of the bonding layer 42 can be between 9μm and 12μm.

[0094] In some examples, the first textured layer 43 can be formed using a UV coating. Since the first textured layer 43 serves as the outer surface of the housing 100, it needs to possess good toughness to ensure the housing 100 has good impact resistance and reduces the probability of cracking upon drop. In some examples, the raw material components of the first textured layer 43, expressed as mass fractions, are: polypropylene ester: 45%-65%; polyurethane acrylate: 10%-15%; solvent: 23%-45%; photoinitiator: 2%-4%.

[0095] The viscosity of the UV resin system forming the first textured layer 43 can be 9.0 m. 2 / s-10.0m 2 The thickness of the first textured layer 43 can be between 20μm and 25μm, with a speed between [value missing]. The first textured layer 43 can be formed using a printing process. A UV resin system is coated or sprayed onto the surface of the cured connecting layer 42. The surface of the UV resin coating is dried at 45℃-55℃. The textured film forming the first textured layer 43 is pressed onto the coating. The coating is then irradiated with an LED light source with 25% curing energy under a vacuum of 17s and a pressure of 150Kg to allow the UV resin system to initially cure, completely transferring the texture from the textured film onto the incompletely cured coating. Next, the textured film is released and exposed to a UV lamp at 700mj / cm [value missing]. 2 -900mj / cm 2 The UV resin system is irradiated under curing energy to completely cure the UV resin system, thereby forming the first texture layer 43.

[0096] In the raw material components of the first textured layer 43, polypropylene ester serves as the main resin. The resulting first textured layer 43 exhibits good flexibility, resistance to yellowing, weather resistance, and adhesion, and also possesses good gloss, giving the shell 100 a pleasant appearance and feel. Polyurethane acrylate, as the prepolymer in the raw material components of the first textured layer 43, provides good mechanical abrasion resistance and toughness, resulting in a high elongation at break. This enhances the impact resistance of the shell 100 and reduces the probability of cracking upon drop. Furthermore, polyurethane acrylate can reduce stress shrinkage during the curing process of the first textured layer 43 and decrease the internal stress of the outer textured layer 40, further preventing cracking of the shell 100. Solvents are used to disperse and dissolve the polypropylene ester, polyurethane acrylate, and photoinitiator, and to adjust the viscosity and rheological properties of the resin system. Photoinitiators are used to absorb the energy of light of a certain wavelength under light irradiation, generating active substances such as free radicals and cations, which can then initiate cross-linking reactions of monomers or prepolymers.

[0097] In some examples, the solvent may include ethyl acetate, ethylene glycol butyl ether, isopropanol, n-butanol, methyl isobutyl ketone, etc. The resin system forming the first textured layer 43 contains the following raw material components expressed by mass fraction: polypropylene ester: 50%-60%; polyurethane acrylate: 11%-13%; ethyl acetate: 10%-15%; ethylene glycol butyl ether: 5%-10%; isopropanol: 5%-10%; n-butanol: 3%-5%; methyl isobutyl ketone: 1%-2%; photoinitiator: 2%-4%. The first textured layer 43 formed by this resin system has good flexibility, yellowing resistance, weather resistance, gloss, abrasion resistance, and toughness, giving the shell 100 good impact resistance.

[0098] In one exemplary embodiment, the method for manufacturing the housing includes the following steps:

[0099] Step S101: Form an inner texture layer on the surface of the shell substrate;

[0100] Step S102: Form a coating layer on the surface of the inner texture layer;

[0101] Step S103: An adhesive layer, a connecting layer, and a first texture layer are sequentially formed on the surface of the coating layer, and the stacked adhesive layer, connecting layer, and first texture layer form an outer texture layer;

[0102] Step S104: Form an anti-fouling layer on the surface of the first texture layer.

[0103] In this embodiment, the implementation methods of steps S101 to S103 are the same as or similar to steps S100 to S300 in the above embodiments, and will not be described in detail here.

[0104] In step S104, refer to Figure 3 As shown, an anti-fouling layer 50 can be formed using AF (Anti-Finger Print) pellets made of organic fluorine materials through processes such as electron beam evaporation and vacuum evaporation. The thickness of the formed anti-fouling layer 50 is in the nanometer range, giving the surface of the shell 100 a large water contact angle, making it difficult for dirt and fingerprints to remain on the surface of the shell 100, and making the shell 100 easy to clean. In addition, the relatively small thickness of the anti-fouling layer 50 does not affect the appearance of the composite layer formed by the inner texture layer 20, the coating layer 30, and the outer texture layer 40, nor does it affect the textured feel provided by the first texture layer 43, resulting in a good user experience.

[0105] In one exemplary embodiment, this disclosure also provides an electronic device, such as a mobile phone, tablet computer, watch, or bracelet. The electronic device includes the housing provided in the above embodiments, which is tightly attached to the main body structure of the electronic device and can serve as a back cover. Because the housing has a good glossy and vibrant effect, it has a good appearance. At the same time, because the housing has good impact resistance and low internal stress, it provides high durability for the user when using the electronic device. The appearance provided by the housing maintains its good lifespan, resulting in a good user experience.

[0106] Other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This application is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope and spirit of the invention are indicated by the following claims.

[0107] It should be understood that the present invention is not limited to the precise structure described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A housing, characterized in that, The housing includes a housing substrate, an inner texture layer, a coating layer, and an outer texture layer stacked together; the outer texture layer includes an adhesive layer, a connecting layer, and a first texture layer stacked together, and the adhesive layer covers the coating layer. The adhesive layer comprises the following raw material components by mass fraction: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%.

2. The housing according to claim 1, characterized in that, The oxygen-containing solvent includes at least one of ketone solvents, ester solvents, alcohol solvents, and alcohol ether solvents.

3. The housing according to claim 1, characterized in that, The adhesive layer comprises the following raw material components in the indicated mass fractions: polyester resin: 20%-40%; ketone solvents: 8%-15%; ester solvents: 14%-22%; alcohol solvents: 5%-10%; alcohol ether solvents: 13%-21%; aromatic solvents: 8%-14%; and isocyanate: 5%-10%.

4. The housing according to claim 1, characterized in that, The adhesive layer comprises the following raw material components in the indicated mass fractions: polyester resin: 25%-35%; methyl ethyl ketone (MEK): 10%-15%; butyl acetate: 10%-12%; Ethyl acetate: 5%-8%; Isopropanol: 5%-8%; Propylene glycol methyl ether acetate: 15%-20%; Toluene: 8%-10%; Xylene: 1%-3%; Isocyanates: 5%-10%.

5. The housing according to any one of claims 1-4, characterized in that, The thickness of the adhesive layer is 8μm-12μm; and / or, The thickness of the connecting layer is 9μm-12μm; and / or, The thickness of the first texture layer is 20μm-25μm.

6. The housing according to any one of claims 1-4, characterized in that, The first textured layer comprises the following raw material components by mass fraction: polypropylene ester: 45%-65%; polyurethane acrylate: 10%-15%; Solvent: 23%-45%; Photoinitiator: 2%-4%.

7. The housing according to claim 6, characterized in that, The first textured layer comprises the following raw material components by mass fraction: polypropylene ester: 50%-60%; Polyurethane acrylate: 11%-13%; Ethyl acetate: 10%-15%, ethylene glycol butyl ether: 5%-10%, isopropanol: 5%-10%, n-butanol: 3%-5%, methyl isobutyl ketone: 1%-2%; Photoinitiator: 2%-4%.

8. The housing according to claim 1, characterized in that, The material of the coating layer includes at least one of elemental silicon, silicon dioxide, titanium dioxide, zirconium dioxide, and niobium pentoxide.

9. The housing according to claim 1, characterized in that, The inner texture layer includes an adhesive layer, a color layer, and a second texture layer stacked together, with the adhesive layer covering the housing substrate.

10. The housing according to claim 9, characterized in that, The thickness of the adhesive layer is 8μm-12μm; and / or, The thickness of the color layer is 22μm-27μm; and / or, The thickness of the second texture layer is 20μm-25μm.

11. The housing according to claim 1, characterized in that, The housing also includes an anti-fouling layer that covers the first textured layer.

12. A method for manufacturing a shell, characterized in that, The method for manufacturing the shell includes: An inner texture layer is formed on the surface of the housing substrate; A coating layer is formed on the surface of the inner texture layer; An adhesive layer, a connecting layer, and a first texture layer are sequentially formed on the surface of the coating layer, and the adhesive layer, the connecting layer, and the first texture layer are stacked to form an outer texture layer; The adhesive layer comprises the following raw material components by mass fraction: polyester resin: 20%-40%; oxygen-containing solvent: 40%-70%; aromatic solvent: 6%-15%; isocyanate: 5%-10%.

13. The method for manufacturing the shell according to claim 12, characterized in that, The adhesive layer comprises the following raw material components in the indicated mass fractions: polyester resin: 25%-35%; methyl ethyl ketone (MEK): 10%-15%; butyl acetate: 10%-12%; Ethyl acetate: 5%-8%; Isopropanol: 5%-8%; Propylene glycol methyl ether acetate: 15%-20%; Toluene: 8%-10%; Xylene: 1%-3%; Isocyanates: 5%-10%.

14. The method for manufacturing the shell according to claim 12, characterized in that, The first textured layer comprises the following raw material components by mass fraction: polypropylene ester: 50%-60%; polyurethane acrylate: 10%-15%; Ethyl acetate: 10%-15%, ethylene glycol butyl ether: 5%-10%, isopropanol: 5%-10%, n-butanol: 3%-5%, methyl isobutyl ketone: 1%-2%; Photoinitiator: 2%-4%.

15. The method for manufacturing the shell according to claim 12, characterized in that, The process of forming an inner texture layer on the surface of the housing substrate includes: An adhesive layer, a color layer, and a second texture layer are sequentially formed on the surface of the housing substrate, and the adhesive layer, the color layer, and the second texture layer form the inner texture layer.

16. The method for manufacturing the shell according to claim 12, characterized in that, The method for manufacturing the shell further includes: An anti-fouling layer is formed on the surface of the first texture layer.

17. An electronic device, characterized in that, The electronic device includes the housing as described in any one of claims 1-11.