On-press developing lithographic printing plate precursor, method for producing lithographic printing plate, and lithographic printing method

By using polymer particles of specific size and composition in the on-machine developing lithographic printing plate original, combined with oxide coating and outer coating design, the problems of printing durability and developing residue are solved, achieving high printing durability and suppressing developing residue.

CN122094838APending Publication Date: 2026-05-26FUJIFILM CORP
View PDF 40 Cites 0 Cited by

Patent Information

Application Number
CN202480069016.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-10-31
Filing Date
2024-10-22
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

Existing in-machine developing lithographic printing plates are insufficient in terms of printing durability and developer residue suppression, making it difficult to meet the requirements of environmental protection and printing quality.

Method used

The image recording layer uses polymer particles with a median particle size of 50nm to 120nm and a content of 42% to 90%. The polymer particles are composed of acrylonitrile compounds and polyepoxide structural units. Combined with the design of oxide coating and outer coating on the support, the dispersion and uniformity of the polymer particles are improved.

Benefits of technology

It significantly improves printing durability and developer residue inhibition, ensuring printing quality and environmental performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present invention relates to an on-press developing lithographic printing plate precursor, a method for producing a lithographic printing plate using the on-press developing lithographic printing plate precursor, and a lithographic printing method, the on-press developing lithographic printing plate precursor having a support and an image recording layer on the support, the image recording layer contains a polymerizable compound and polymer particles, the median diameter of the polymer particles is 50-120 nm, the content of the polymer particles is 42-90 mass% relative to the total mass of the image recording layer, and after osmium dyeing treatment is performed on the thickness-direction cross section of the lithographic printing plate precursor, the thickness-direction cross section of the lithographic printing plate precursor is greater than the thickness-direction cross section of the lithographic printing plate precursor, and the thickness-direction cross section of the lithographic printing plate precursor is greater than the thickness-direction cross section of the lithographic printing plate precursor. In a cross-sectional image obtained by binarizing a cross-sectional image obtained by scanning electron microscope observation into a dyed section and a non-dyed section, the standard deviation of the area ratio of the non-dyed section is less than 6.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an on-machine developing type lithographic printing plate master, a method for manufacturing lithographic printing plates, and a lithographic printing method. Background Technology

[0002] Typically, a lithographic printing plate consists of an oleophilic image area that receives ink during the printing process and a hydrophilic non-image area that receives dampening solution. Lithographic printing is performed by utilizing the mutual repulsion between water and oil-based inks. The oleophilic image area of ​​the lithographic printing plate is used as the ink receiving area, and the hydrophilic non-image area is used as the dampening solution receiving area (ink non-receiving area). This creates a difference in ink adhesion on the surface of the lithographic printing plate, causing the ink to adhere only to the image area. The ink is then transferred to the substrate, such as paper, for printing.

[0003] In the past, to produce this lithographic printing plate, lithographic printing master plates (PS plates) were widely used, which consisted of an oleophilic photosensitive resin layer (image recording layer) placed on a hydrophilic support. Typically, a lithographic printing plate is obtained by exposing the lithographic printing master plate to an original image such as high-contrast film, leaving a portion of the image recording layer remaining as the image area. This remaining portion is then removed by dissolving it with an alkaline developer or organic solvent, thus exposing the surface of the hydrophilic support and forming the non-image area.

[0004] Furthermore, due to increasing concern for the Earth's environment, environmental problems related to waste liquids accompanying wet processing such as developing processes have become apparent.

[0005] To address the aforementioned environmental issues, there is a trend towards simplifying or eliminating the need for pretreatment in development or plate making. As one of the simplest manufacturing methods, a method called "in-machine development" has been developed. This involves exposing the original lithographic printing plate and then directly mounting it onto the printing press without the usual development process, removing unnecessary portions of the image recording layer at the initial stage of the typical printing process.

[0006] In this invention, the lithographic printing plate original that can be used for such on-machine development is referred to as an "on-machine developing type lithographic printing plate original".

[0007] As a previous lithographic printing original, for example, the lithographic printing original described in Patent Document 1 or Patent Document 2 can be cited.

[0008] Patent Document 1 discloses a lithographic printing plate original having an aluminum support and an image recording layer formed on the aluminum support. The image recording layer contains resin particles A having olefin unsaturated groups and a compound B having olefin unsaturated groups other than the resin particles A, and the olefin unsaturated bond valence is 1.5 mmol / g or more.

[0009] Patent Document 2 discloses particles for an on-machine developable lithographic printing plate and an on-machine developable lithographic printing plate. The particles for the on-machine developable lithographic printing plate contain a resin having structural units formed by aromatic vinyl compounds and structural units formed by acrylonitrile compounds. The particles are granulated by a surfactant. The image recording layer contains the particles for the on-machine developable lithographic printing plate.

[0010] Patent Document 1: International Publication No. 2020 / 262694

[0011] Patent Document 2: International Publication No. 2020 / 026809 Summary of the Invention

[0012] The technical problem to be solved by the invention

[0013] One embodiment of the present invention aims to solve the problem of providing an on-machine developing type lithographic printing plate with excellent printing durability and developer residue suppression.

[0014] Another embodiment of the present invention aims to solve the problem of providing a method for manufacturing a lithographic printing plate or a lithographic printing method using the above-described on-machine developing type lithographic printing plate master.

[0015] means for solving technical problems

[0016] The methods used to solve the above problems include the following approaches.

[0017] <1> An on-machine developing type lithographic printing plate master has a support and an image recording layer on the support. The image recording layer contains a polymeric compound and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles relative to the total mass of the image recording layer is 42% by mass or more and 90% by mass or less. After osmium staining is performed on the thickness direction section of the lithographic printing plate master, the standard deviation of the area ratio of the unstained part in the cross-sectional image obtained by binarizing the cross-sectional image obtained by observation by scanning electron microscopy into stained and unstained parts is less than 6.

[0018] <2> According to the machine-developable lithographic printing plate original described in <1>, the polymer particles are polymer particles having structural units formed by acrylonitrile compounds and polyepoxide structures.

[0019] <3> According to <2> the machine-developable lithographic printing plate original, wherein the polymer particles are polymer particles having structural units formed by aromatic vinyl compounds, structural units formed by acrylonitrile compounds, and structural units containing polyoxyalkylene structures.

[0020] <4> The original plate for machine-developable lithographic printing as described in <2> or <3>, wherein the above-mentioned polyoxyethylene structure is a polyoxyethylene structure.

[0021] <5> The original plate for machine-developable lithographic printing according to any one of <2> to <4>, wherein the number of repeating units of the above-mentioned polyoxyethylene structure is 3 to 10.

[0022] <6> The original plate for machine-developable lithographic printing according to any one of <2> to <5>, wherein the content of structural units containing polyoxyalkylene structures in the polymer particles is 10% by mass or more relative to the total mass of the polymer.

[0023] <7> The original plate for machine-developable lithographic printing according to any one of <1> to <6>, wherein the content of the polymer particles is 45% by mass or more relative to the total mass of the image recording layer.

[0024] <8> According to the machine-developable lithographic printing plate original described in <7>, the content of the polymer particles is 55% by mass or more relative to the total mass of the image recording layer.

[0025] <9> The original plate for machine-developable lithographic printing according to any one of <1> to <8>, wherein the median particle size of the polymer particles is 50 nm to 100 nm.

[0026] <10> The original plate for machine-developable offset printing as described in <9>, wherein the median particle size of the polymer particles is 50 nm to 90 nm.

[0027] <11> The original plate for machine-developable lithographic printing according to any one of <1> to <10>, wherein the polymeric compound includes oligomers.

[0028] <12> The original plate for machine-developable lithographic printing according to any one of <1> to <11>, wherein an intermediate layer is further provided between the support and the image recording layer, the intermediate layer containing a copolymer having support adsorption groups and hydrophilic groups.

[0029] <13> The original plate for machine-developable lithographic printing according to any one of <1> to <12>, wherein the image recording layer further comprises an outer coating containing an inorganic layered compound.

[0030] <14> The original plate for machine-developable lithographic printing according to any one of <1> to <13>, wherein the image recording layer further comprises an outer coating containing a water-soluble polymer, the thickness of the outer coating being greater than the thickness of the image recording layer.

[0031] <15> The on-machine developing type lithographic printing plate original according to any one of <1> to <14>, wherein the surface of the support has an oxide coating, and the oxide coating has micropores extending in the depth direction from the surface of the oxide coating on the image recording layer side, the micropores having: a large-diameter pore portion having an average pore diameter of 15 nm to 100 nm on the surface of the oxide coating; and a small-diameter pore portion communicating with the bottom of the large-diameter pore portion and extending further in the depth direction from the communication position, the small-diameter pore portion having an average pore diameter of 15 nm or less.

[0032] <16> The on-machine developing type lithographic printing plate original according to any one of <1> to <15>, wherein the surface of the support has an oxide coating, and the oxide coating has micropores extending in the depth direction from the surface of the oxide coating on the image recording layer side, wherein the maximum diameter inside the micropore is 1.2 to 10 times the average pore diameter of the surface relative to the average pore diameter of the oxide coating surface.

[0033] <17> An on-machine developing type lithographic printing plate master has a support and an image recording layer on the support. The image recording layer contains a polymeric compound and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles relative to the total mass of the image recording layer is 42% by mass or more and 90% by mass or less. The polymer particles are polymer particles that have 65% by mass or more of acrylonitrile compound structural units relative to the total mass of the polymer particles and have 10% by mass or more of polyepoxide structure structural units.

[0034] <18> A method for manufacturing a lithographic printing plate, comprising: a step of exposing an on-machine developing type lithographic printing plate master as described in any one of <1> to <17> in an image-like manner; and a step of supplying at least one of the group consisting of printing ink and dampening solution to a printing press to remove the non-image portion of the image recording layer.

[0035] <19> A lithographic printing method comprising: a step of exposing an on-machine developing type lithographic printing plate master as described in any one of <1> to <17> in an image-like manner; a step of supplying at least one of the group consisting of printing ink and dampening solution to a printing press to remove the non-image portion of an image recording layer to produce a lithographic printing plate; and a step of printing using the obtained lithographic printing plate.

[0036] Invention Effects

[0037] According to one embodiment of the present invention, an in-machine developing type lithographic printing plate master with excellent printing durability and developer residue suppression can be provided.

[0038] According to another embodiment of the present invention, a method for producing a lithographic printing plate or a lithographic printing method using the above-described on-machine developing type lithographic printing plate original can be provided. Attached Figure Description

[0039] Figure 1 This is a schematic cross-sectional view of one embodiment of the support.

[0040] Figure 2 This is a schematic cross-sectional view of another embodiment of the support.

[0041] Figure 3 This is a schematic diagram of an anodizing apparatus used for anodizing in a method for manufacturing a support with an anodized coating.

[0042] Figure 4 This is a side view illustrating the concept of a brushing process used for mechanical roughening in the fabrication of an aluminum support.

[0043] Figure 5 This is a diagram showing an example of an alternating current waveform used in electrochemical roughening treatment.

[0044] Figure 6 This is a side view showing an example of a radial cell in an electrochemical roughening process using alternating current. Detailed Implementation

[0045] The present invention will now be described in detail. The description of the constituent elements described below is sometimes based on representative embodiments of the invention, but the invention is not limited to these embodiments.

[0046] Furthermore, in this invention, the term "~" indicating a numerical range is used to encompass the numerical values ​​recorded before and after it as both a lower and upper limit.

[0047] Furthermore, in the marking of groups (atomic groups) in this invention, the markings without substitution and non-substitution include not only groups without substituents but also groups with substituents. For example, "alkyl" includes not only alkyl groups without substituents (unsubstituted alkyl) but also alkyl groups with substituents (substituted alkyl).

[0048] In this invention, "(meth)acrylic acid" is a term used to include both acrylic acid and methacrylic acid, and "(meth)acryloyl" is a term used to include both acryloyl and methacryloyl.

[0049] Furthermore, the term "process" in this invention includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process can be achieved.

[0050] In this invention, "mass%" and "weight%" have the same meaning, and "parts of mass" and "parts of weight" have the same meaning.

[0051] In this invention, unless otherwise specified, each component in the composition or each structural unit in the polymer may contain only one type, or two or more types may be used together.

[0052] In this invention, the amount of each component in the composition or each structural unit in the polymer, when there are multiple substances or structural units corresponding to each component in the composition or each structural unit in the polymer, unless otherwise specified, refers to the total amount of the corresponding multiple substances present in the composition or the corresponding multiple structural units present in the polymer.

[0053] In this invention, a combination of two or more preferred methods is a more preferred method.

[0054] Unless otherwise specified, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) in this invention are calculated using a gel permeation chromatography (GPC) analysis apparatus with columns of TSKgel GMHxL, TSKgel G4000HxL, and TSKgel G2000HxL (all trade names manufactured by Tosoh Corporation), and with THF (tetrahydrofuran) solvent and a differential refractometer, and with polystyrene as a standard substance.

[0055] In this invention, the term "lithographic printing plate original" includes not only lithographic printing plate originals but also discarded originals. Furthermore, the term "lithographic printing plate" includes not only lithographic printing plates made by exposing and developing lithographic printing plate originals as needed, but also discarded plates. In the case of discarded originals, exposure and development operations may not be required. Additionally, a discarded plate refers to, for example, a lithographic printing plate original used when a portion of a page is printed in monochrome or two colors in color newspaper printing, mounted on an unused printing cylinder.

[0056] In this invention, the "*" in the chemical structural formula indicates the bonding position with other structures.

[0057] <In-machine developing type lithographic printing plate original>

[0058] The first embodiment of the on-machine developing type lithographic printing plate (also simply referred to as "lithographic printing plate") involved in this invention has a support and an image recording layer on the support. The image recording layer contains a polymeric compound and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles relative to the total mass of the image recording layer is 42% by mass or more and 90% by mass or less. After performing osmium staining treatment on the thickness direction section of the lithographic printing plate, the standard deviation of the area ratio of the unstained portion in the cross-sectional image obtained by binarizing the cross-sectional image obtained by observation by scanning electron microscopy into stained and unstained portions is less than 6.

[0059] The second embodiment of the on-machine developing type lithographic printing plate original of the present invention has a support and an image recording layer on the support. The image recording layer contains a polymeric compound and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles relative to the total mass of the image recording layer is 42% by mass or more and 90% by mass or less. The polymer particles are polymer particles that are structural units formed of acrylonitrile compounds with 65% by mass or more relative to the total mass of the polymer particles and have structural units containing polyoxyalkylene structures with 10% by mass or more.

[0060] Furthermore, in this specification, unless otherwise specified, both the first embodiment and the second embodiment described above will be referred to as "the in-machine developing type lithographic printing plate original according to the present invention" or "the lithographic printing plate original according to the present invention". And, unless otherwise specified, the image recording layer of both the first embodiment and the second embodiment will be described as "image recording layer" or similar terms.

[0061] In conventional on-machine developing lithographic printing plates, if the image recording layer contains polymer particles with a median particle size of 50 nm to 120 nm, these small-sized polymer particles tend to aggregate, resulting in an image recording layer with a large number of polymer particles. Consequently, even if the image recording layer contains a large number of polymer particles from the viewpoint of improving print durability, a large number of these aggregates are still generated. These aggregates tend to accumulate as developing residue, and in the areas where these aggregates are generated, the strength of the image recording layer decreases, resulting in insufficient print durability and developing residue suppression.

[0062] In the first embodiment of the lithographic printing plate original involved in this invention, the image recording layer contains a polymeric compound and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm, and the content of the polymer particles relative to the total mass of the image recording layer is 42% by mass or more and 90% by mass or less. After performing osmium staining treatment on the thickness direction section of the lithographic printing plate original, the standard deviation of the unstained portion in the cross-sectional image obtained by binarizing the cross-sectional image obtained by observation by scanning electron microscopy into stained and unstained portions is less than 6. Therefore, it is considered that even an image forming layer containing a large number of small-sized polymer particles becomes an image recording layer with high polymer particle dispersion and uniformity, which suppresses the aggregation of the polymer particles. This provides an in-machine developing type lithographic printing plate original with excellent printing durability and developer residue suppression.

[0063] Furthermore, in the second embodiment of the lithographic printing plate original according to the present invention, the image recording layer contains a polymeric compound and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles relative to the total mass of the image recording layer is 42% by mass or more and 90% by mass or less. Relative to the total mass of the polymer particles, the polymer particles are polymer particles having 65% by mass or more of structural units formed by acrylonitrile compounds and 10% by mass or more of structural units containing polyoxyalkylene structures. Therefore, it is considered that even an image forming layer containing a large number of small-sized polymer particles becomes an image recording layer that suppresses the aggregation of the polymer particles and has high dispersion and uniformity of polymer particles. This enables the provision of an in-machine developing type lithographic printing plate original with excellent printing durability and developer residue suppression.

[0064] The following is a detailed description of each component of the original offset printing plate involved in this invention.

[0065] (Standard deviation of non-stained areas)

[0066] In the first embodiment of the on-machine developing type lithographic printing plate original according to the present invention, after osmium staining treatment is applied to the thickness direction cross section of the lithographic printing plate original, the standard deviation of the area ratio of the unstained portion in the cross section image obtained by binarizing the cross section image obtained by observation by scanning electron microscopy into stained and unstained portions is less than 6. From the viewpoint of printing durability and developer residue suppression, it is preferably less than 5.1, more preferably less than 4.2. The smaller the standard deviation, the more uniformly the non-polymerized portions exist in the film, thereby resulting in better printing durability and better developer residue suppression.

[0067] Furthermore, in the second embodiment of the on-machine developing type lithographic printing plate original according to the present invention, from the viewpoint of printing durability and development residue suppression, after performing osmium staining treatment on the thickness direction section of the lithographic printing plate original, the standard deviation of the area ratio of the unstained part in the cross-sectional image obtained by binarizing the cross-sectional image obtained by observing it by a scanning electron microscope into stained and unstained parts is preferably less than 6, more preferably less than 5.1, and particularly preferably less than 4.2.

[0068] As a specific method for setting a lithographic printing plate with a small standard deviation, improving the dispersibility of polymer particles contained in the image recording layer is effective. Details regarding particles with good dispersibility will be discussed later, but polymer particles having side groups containing hydrophilic poly(epoxy) segments are preferred.

[0069] The method for determining the standard deviation of the unstained portion in this invention is as follows.

[0070] -Osmium staining method-

[0071] The original lithographic printing plate was cut into approximately 10mm squares, and then subjected to vapor-phase staining using a 2% (w / w) osmium tetroxide aqueous solution. The staining was carried out at approximately 22°C for 24 hours.

[0072] -Scanning Electron Microscopy (SEM) Observation Methods-

[0073] After osmium staining, cross-sections were prepared using an argon (Ar) ion beam, followed by a carbon coating for conductivity treatment. Backscattered electron observation was then performed using a semi-in-lens SEM manufactured by Hitachi High-Tech Corporation at an accelerating voltage of 5 kV. The magnification was 50,000x, and N=10 fields of view were captured.

[0074] The obtained cross-sectional SEM images were binarized into stained and unstained areas using the image processing software imageJ (Fiji). An image recording layer was selected from the obtained cross-sectional SEM image, and noise was filtered using a Median filter (2 pixels) before binarization (Threshold). The Threshold setting was set to Auto (Li). After filtering noise using a Median filter (2 pixels) on the obtained binarized image, the area fraction of the unstained area was measured. The standard deviation of the area fraction of the unstained area was calculated based on N=10 field-of-view data points.

[0075] Furthermore, osmium staining is performed as follows: Osmium is bonded to the olefinic unsaturated bonds contained in the polymeric compound. The increased backscattering of electrons through the stained areas, due to the higher atomic number of osmium, makes them clearly visible. The stained areas (polymeric compounds) appear white in cross-sectional images using SEM, while the unstained areas (polymer particles and other non-polymeric additives) appear black.

[0076] (Image recording layer)

[0077] The image recording layer in the lithographic printing plate original involved in this invention is preferably a water-soluble or water-dispersible negative image recording layer.

[0078] Furthermore, regarding the image recording layer in the lithographic printing plate original involved in this invention, from the viewpoint of machine developability, it is preferable that the unexposed portion of the image recording layer can be removed by at least one of dampening solution and printing ink.

[0079] The following is a detailed explanation of the components contained in the image recording layer.

[0080] [Polymer particles]

[0081] The image recording layer contains polymer particles. These polymer particles help improve print durability and on-machine developability.

[0082] The polymer particles are preferably polymer particles that can convert the image recording layer into a hydrophobic state when heated. The polymer particles are preferably at least one selected from the group consisting of hydrophobic thermoplastic polymer particles and microcapsules containing hydrophobic compounds, with hydrophobic thermoplastic polymer particles being particularly preferred.

[0083] Specific examples of polymers constituting hydrophobic thermoplastic polymer particles include homopolymers or copolymers or mixtures thereof of monomers such as ethylene, styrene, vinyl chloride, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinylidene chloride, acrylonitrile, vinyl carbazole, acrylates or methacrylates having a polyalkylene structure.

[0084] As microcapsules, examples include those described in Japanese Patent Application Publications Nos. 2001-277740 and 2001-277742, which contain all or a portion of the components of an image recording layer within the microcapsule. The components of the image recording layer can also be contained outside the microcapsule. A preferred embodiment of the image recording layer containing microcapsules is one in which a hydrophobic component is contained within the microcapsule, while a hydrophilic component is contained outside the microcapsule.

[0085] The median particle size of the polymer particles is 50 nm to 120 nm. From the viewpoint of print durability and developer residue suppression, 50 nm to 100 nm is preferred, and 50 nm to 90 nm is more preferred. The smaller the polymer particle size, the better the print durability.

[0086] The method for determining the median particle size of polymer particles in this invention is obtained by measuring the particle size using dynamic light scattering. In the case of separating polymer particles from a plate and measuring their particle size, the obtained polymer particles are redispersed in a solvent using the following method before particle size measurement.

[0087] -Methods for separating polymer particles from a plate-

[0088] The plate coated with the image recording layer was immersed in a mixed solvent A of 40 / 30 / 20 / 10 (2-butanone / 1-methoxy-2-propanol / methanol / pure water), and ultrasonically irradiated for 10 seconds to prepare a dispersion of the image recording layer. The dispersion was then centrifuged at 5000 rpm for 10 minutes, yielding precipitate B at the bottom of the container. After discarding the supernatant, mixed solvent A was added again to redisperse the precipitate, which was then centrifuged at 5000 rpm for 10 minutes, yielding precipitate C at the bottom of the container. After discarding the supernatant, precipitate C was vacuum dried (50°C for 16 hours) to obtain polymer particle powder.

[0089] Furthermore, the median particle size of polymer particles can be determined by calculation based on images obtained using a semi-internal lens SEM. The specific determination method is as described below.

[0090] After dispersing and fixing the obtained polymer particle powder onto a carbon ribbon, it underwent conductive treatment and was observed using a semi-internal lens SEM manufactured by Hitachi High-Tech Corporation at an accelerating voltage of 2kV. The magnification was 100,000x. The number of fields of view was set to N=15 or more (the number of images with more than 400 particles extracted, as described later). Within the captured images, all polymer particles that do not overlap and whose outlines are discernible were extracted as much as possible, and the particle size was measured. The median particle size was calculated based on the obtained particle sizes (more than 400 particles).

[0091] Polymer particles can be used alone or in combination with two or more types.

[0092] Relative to the total mass of the image recording layer, the content of polymer particles in the lithographic printing plate original involved in this invention is 42% by mass or more and 90% by mass or less, and from the viewpoint of printing durability and development residue suppression, it is preferably 45% by mass or more, and more preferably 55% by mass or more.

[0093] Furthermore, from the viewpoint of print durability and developer residue suppression, the content of polymer particles in the lithographic printing plate original involved in this invention is preferably 45% to 85% by mass, more preferably 55% to 75% by mass, relative to the total mass of the image recording layer.

[0094] As a preferred embodiment, the hydrophobic thermoplastic polymer particles have a hydrophobic backbone and preferably contain the following two structural units:

[0095] i) Structural units having side-chain cyano groups directly bonded to the aforementioned hydrophobic main chain; and

[0096] ii) Structural units having side groups containing hydrophilic poly(epoxy) segments.

[0097] Acrylic resin chains are preferred as the hydrophobic backbone mentioned above.

[0098] Examples of the aforementioned side-chain cyano groups are preferably -[CH2CH(C≡N)-] or -[CH2C(CH3)(C≡N)-].

[0099] Furthermore, structural units with the aforementioned side-chain cyano groups can be readily derived from olefinic unsaturated monomers (e.g., acrylonitrile or methacrylonitrile) or combinations thereof.

[0100] Furthermore, the epoxide in the hydrophilic poly(epoxide) segment is preferably ethylene oxide or propylene oxide, and more preferably ethylene oxide.

[0101] The number of repeating units of the epoxy structure in the above-mentioned hydrophilic poly(epoxy) segment is preferably 2 to 100, more preferably 3 to 55, and particularly preferably 3 to 10.

[0102] As a resin particle having a hydrophobic main chain and containing i) a structural unit having a side chain cyano group directly bonded to the hydrophobic main chain and ii) a structural unit having a side group containing a hydrophilic poly(epoxy) segment, the particles described in paragraphs 0039 to 0068 of Japanese Patent Application Publication No. 2008-503365 are preferred examples.

[0103] Relative to the total mass of the polymer particles, the polymer particles in the second embodiment of the lithographic printing plate original according to the present invention are polymer particles having 65% or more of structural units formed of acrylonitrile compounds and 10% or more of structural units containing polyoxyalkylene structures. From the viewpoint of printing durability and developer residue suppression, it is preferable that they also have structural units formed of aromatic vinyl compounds.

[0104] Furthermore, from the viewpoint of printing durability and developer residue suppression, the polymer particles in the first embodiment of the lithographic printing plate original according to the present invention are preferably polymer particles having structural units formed of acrylonitrile compounds and structural units containing polyepoxide structures, and more preferably polymer particles having structural units formed of aromatic vinyl compounds, structural units formed of acrylonitrile compounds and structural units containing polyepoxide structures.

[0105] Furthermore, from the viewpoint of printing durability and developer residue suppression, relative to the total mass of polymer particles, the polymer particles in the first embodiment of the lithographic printing plate original according to the present invention are polymer particles having at least 65% by mass of structural units formed of acrylonitrile compounds and at least 10% by mass of structural units containing polyoxyalkylene structures.

[0106] In addition, unless otherwise specified, polymer particles having structural units formed of acrylonitrile compounds and structural units containing polyepoxide structures, as well as polymer particles having structural units formed of aromatic vinyl compounds, structural units formed of acrylonitrile compounds and structural units containing polyepoxide structures, are hydrophobic thermoplastic polymer particles.

[0107] Examples of acrylonitrile compounds include acrylonitrile and methacrylonitrile, with acrylonitrile being the preferred choice.

[0108] Examples of aromatic vinyl compounds include styrene, p-methylstyrene, p-methoxystyrene, β-methylstyrene, p-methyl-β-methylstyrene, α-methylstyrene, and p-methoxy-β-methylstyrene, with styrene being preferred.

[0109] As polymer particles having structural units formed from aromatic vinyl compounds and structural units formed from acrylonitrile compounds, the composition ratio (mass ratio) of structural units formed from aromatic vinyl compounds to structural units formed from acrylonitrile compounds is preferably 10:1 to 1:10.

[0110] From the viewpoint of printing durability and developer residue suppression, the polyoxyalkylene structure in the structural unit containing the polyoxyalkylene structure is preferably a polyoxyethylene structure, a polyoxypropylene structure, or a polyethylene / propylene oxide structure, and more preferably a polyoxyethylene structure.

[0111] Regarding the number of repeating units of the epoxy structure in the polyepoxide structure, from the viewpoints of machine developability, printing durability and developer residue suppression, the number of repeating units of the polyepoxide structure is preferably 2 to 100, more preferably 3 to 55.

[0112] From the viewpoint of print durability and developer residue suppression, the content of structural units formed by acrylonitrile compounds in the polymer particles of the first embodiment of the lithographic printing plate original according to the present invention is preferably 20% to 95% by mass, more preferably 50% to 95% by mass, further preferably 70% to 90% by mass, and particularly preferably 75% to 90% by mass, relative to the total mass of the polymer having structural units containing cyano groups.

[0113] In the second embodiment of the lithographic printing plate original involved in the present invention, the content of the structural unit formed by acrylonitrile compound in the polymer particles is 65% by mass or more. From the viewpoint of printing durability and development residue suppression, it is preferably 70% to 95% by mass, more preferably 70% to 90% by mass, and particularly preferably 75% to 90% by mass, relative to the total mass of the polymer having structural units containing cyano groups.

[0114] From the viewpoints of dispersibility, printing durability, and suppression of developing residue, the content of structural units containing polyoxyalkylene structures in the polymer particles of the first embodiment of the lithographic printing plate original according to the present invention is preferably 1% to 50% by mass, more preferably 5% to 30% by mass, further preferably 8% to 25% by mass, and particularly preferably 10% to 20% by mass, relative to the total mass of the polymer particles.

[0115] In the second embodiment of the lithographic printing plate original involved in this invention, the content of structural units containing polyoxyalkylene structures in the polymer particles is 10% by mass or more. From the viewpoints of dispersibility, printing durability and developer residue suppression, it is preferably 10% to 50% by mass relative to the total mass of polymer particles, more preferably 10% to 30% by mass, further preferably 10% to 25% by mass, and particularly preferably 10% to 20% by mass.

[0116] From the viewpoint of printing durability and developer residue suppression, the content of structural units formed by aromatic vinyl compounds in the polymer particles of the first embodiment of the lithographic printing plate original according to the present invention is preferably 50% by mass or less, more preferably 30% by mass or less, further preferably 20% by mass or less, and particularly preferably 5% by mass to 20% by mass, relative to the total mass of the polymer particles.

[0117] From the viewpoint of print durability and developer residue suppression, the content of structural units formed by aromatic vinyl compounds in the polymer particles of the second embodiment of the lithographic printing plate original according to the present invention is preferably 25% by mass or less, more preferably 20% by mass or less, and particularly preferably 5% by mass to 20% by mass, relative to the total mass of polymer particles.

[0118] From the perspective of print durability and chemical resistance, polymer particles can have structural units formed by N-vinyl heterocyclic compounds.

[0119] Examples of N-vinyl heterocyclic compounds include, for example, N-vinylpyrrolidone, N-vinylcarbazole, N-vinylpyrrole, N-vinylphenthiazide, N-vinylsuccinimide, N-vinylphthalimide, N-vinylcaprolactam and N-vinylimidazol, with N-vinylpyrrolidone being preferred.

[0120] From the viewpoint of print durability and chemical resistance, the content of structural units formed by N-vinyl heterocyclic compounds in the polymer particles of the first embodiment of the lithographic printing plate original involved in the present invention is preferably 5% to 50% by mass, more preferably 10% to 40% by mass, relative to the total mass of polymer particles.

[0121] From the viewpoint of print durability and chemical resistance, the content of structural units formed by N-vinyl heterocyclic compounds in the polymer particles of the second embodiment of the lithographic printing plate original involved in the present invention is preferably 5% to 25% by mass, more preferably 10% to 20% by mass, relative to the total mass of polymer particles.

[0122] Polymer particles may contain structural units with acidic groups, but from the viewpoint of machine developability and ink adhesion, it is preferable to avoid structural units with acidic groups.

[0123] Specifically, the content of structural units with acidic groups in the thermoplastic resin is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. The lower limit of the above content is not particularly limited and can be 0% by mass.

[0124] Furthermore, the acid value of the thermoplastic resin is preferably 160 mg KOH / g or less, more preferably 80 mg KOH / g or less, and even more preferably 40 mg KOH / g or less. The lower limit of the above acid value is not particularly limited and can be 0 mg KOH / g.

[0125] In this invention, the acid value is determined in accordance with the determination method of JIS K0070:1992.

[0126] From the perspective of ink adhesion, polymer particles can contain structural units that include hydrophobic groups.

[0127] Examples of hydrophobic groups include alkyl, aryl, and aralkyl groups.

[0128] The structural unit containing a hydrophobic group is preferably a structural unit formed from an alkyl (meth)acrylate compound, an aryl (meth)acrylate compound, or an alkyl (meth)acrylate compound, and more preferably a structural unit formed from an alkyl (meth)acrylate compound.

[0129] The alkyl group in the above-mentioned alkyl methacrylate compounds preferably has 1 to 10 carbon atoms. The alkyl group can be linear, branched, or cyclic. Examples of alkyl methacrylate compounds include methyl methacrylate, ethyl methacrylate, propyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, and dicyclopentyl methacrylate.

[0130] The aryl group in the above-mentioned aryl methacrylate compound preferably has 6 to 20 carbon atoms, more preferably phenyl. Furthermore, the aryl group may have known substituents. Phenyl methacrylate is a preferred example of an aryl methacrylate compound.

[0131] The alkyl group in the above-mentioned aralkyl methacrylate compound preferably has 1 to 10 carbon atoms. The alkyl group can be linear, branched, or cyclic. Furthermore, the aryl group in the above-mentioned aralkyl methacrylate compound preferably has 6 to 20 carbon atoms, more preferably phenyl. Benzyl methacrylate is a preferred example of an aralkyl methacrylate compound.

[0132] The content of structural units with hydrophobic groups in the polymer particles of the first embodiment of the lithographic printing plate original involved in the present invention is preferably 5% to 50% by mass, more preferably 10% to 30% by mass, relative to the total mass of the polymer particles.

[0133] The content of structural units with hydrophobic groups in the polymer particles of the second embodiment of the lithographic printing plate original involved in the present invention is preferably 5% to 25% by mass, more preferably 10% to 20% by mass, relative to the total mass of the polymer particles.

[0134] From the viewpoint of printability and machine developability, the resin contained in the polymer particles can have hydrophilic groups other than polyoxyalkylene structures.

[0135] As a hydrophilic group, there are no particular restrictions as long as the structure is hydrophilic; examples include acid groups such as carboxyl groups, hydroxyl groups, and amino groups.

[0136] Relative to the total mass of the polymer particles, the content of structural units having hydrophilic groups other than polyoxyalkylene structures in the polymer particles of the first embodiment of the lithographic printing plate original involved in the present invention is preferably 1% to 60% by mass, more preferably 5% to 30% by mass.

[0137] Relative to the total mass of the polymer particles, the content of structural units having hydrophilic groups other than polyoxyalkylene structures in the polymer particles of the second embodiment of the lithographic printing plate original involved in the present invention is preferably 1% to 25% by mass, more preferably 5% to 20% by mass.

[0138] The method of manufacturing the resin contained in the polymer particles is not particularly limited and can be manufactured by known methods.

[0139] For example, it can be obtained by polymerizing styrene compounds, acrylonitrile compounds, and at least one compound selected as needed from the group consisting of the above-mentioned N-vinyl heterocyclic compounds, compounds for forming the above-mentioned structural units having acidic groups, compounds for forming the above-mentioned structural units having hydrophobic groups, and compounds for forming the above-mentioned other structural units by a known method.

[0140] Furthermore, the introduction of polyepoxide structures can be achieved using monomers containing polyepoxide structures or through polymer reactions.

[0141] Specific examples of resins contained in polymer particles are shown in the table below, but the thermosetting resins used in this invention are not limited to these.

[0142] [Chemical Formula 1]

[0143]

[0144] [Chemical Formula 2]

[0145]

[0146] Furthermore, in the above specific examples, the content ratio of each structural unit can be appropriately changed according to the preferred range of the content of each structural unit.

[0147] Furthermore, the weight-average molecular weight of each compound shown in the above specific examples can be appropriately changed according to the preferred range of the weight-average molecular weight of the above thermoplastic resin.

[0148] [Polymerizing compounds]

[0149] The image recording layer contains polymeric compounds.

[0150] In this invention, a polymerizable compound refers to a compound having polymerizable groups.

[0151] The polymerizable group is not particularly limited and can be any known polymerizable group, but is preferably an olefinic unsaturated group. Furthermore, the polymerizable group can be a free radical polymerizable group or a cationic polymerizable group, but is preferably a free radical polymerizable group.

[0152] Examples of free radical polymerizable groups include (meth)acryloyl, allyl, vinylphenyl, and vinyl groups. From a reactivity point of view, (meth)acryloyl is preferred.

[0153] The molecular weight (weight-average molecular weight in the case of a molecular weight distribution) of the polymeric compound is preferably 50 or more and less than 2,500.

[0154] The polymerizable compound can be, for example, a free radical polymerizable compound or a cationic polymerizable compound, and is preferably an addition polymerizable compound (an olefinic unsaturated compound) having at least one olefinic unsaturated bond.

[0155] As an olefinically unsaturated compound, it is preferably a compound having at least one terminal olefinically unsaturated bond, and more preferably a compound having two or more terminal olefinically unsaturated bonds. The polymerizable compound may be in the chemical form of a monomer, prepolymer (i.e., dimer, trimer, or oligomer), or a mixture thereof.

[0156] Of these, from the viewpoint of print durability, polymeric compounds containing 3 or more functions are preferred, polymeric compounds containing 7 or more functions are more preferred, and polymeric compounds containing 10 or more functions are even more preferred. Furthermore, from the viewpoint of print durability in the obtained lithographic printing plate, the polymeric compounds preferably contain olefinically unsaturated compounds with 3 or more functions (preferably 7 or more functions, more preferably 10 or more functions), and even more preferably (meth)acrylate compounds with 3 or more functions (preferably 7 or more functions, more preferably 10 or more functions).

[0157] Furthermore, from the viewpoint of machine developability and stain inhibition, polymeric compounds containing two or fewer functions are preferred as polymeric compounds, more preferably containing two functional polymeric compounds, and particularly preferably containing two functional (meth)acrylate compounds.

[0158] From the viewpoints of print durability, machine developability, and contamination inhibition, the content of polymeric compounds with two or fewer functions (preferably difunctional polymeric compounds) is preferably 5% to 100% by mass, more preferably 10% to 100% by mass, and particularly preferably 15% to 100% by mass, relative to the total mass of the polymeric compounds in the aforementioned image recording layer.

[0159] -Oligomers-

[0160] As a polymeric compound contained in the image recording layer, it is preferable to contain a polymeric compound as an oligomer (hereinafter also simply referred to as "oligomer").

[0161] In this invention, oligomers refer to polymeric compounds with a molecular weight (weight-average molecular weight in the case of a molecular weight distribution) of 600 or more and 10,000 or less, and containing at least one polymeric group.

[0162] From the viewpoint of excellent chemical resistance and printability, the molecular weight of the oligomer is preferably 1,000 or more and 5,000 or less.

[0163] Furthermore, from the viewpoint of improving printability, the number of polymeric groups in one molecule of oligomer is preferably two or more, more preferably three or more, even more preferably six or more, and particularly preferably ten or more.

[0164] Furthermore, there is no particular upper limit to the number of polymerizable groups in the oligomer, but the number of polymerizable groups is preferably 20 or less.

[0165] From the viewpoint of printability and machine developability, the oligomer preferably has 7 or more polymeric groups and a molecular weight of 1,000 or more and 10,000 or less. More preferably, it has 7 or more and 20 or less polymeric groups and a molecular weight of 1,000 or more and 5,000 or less.

[0166] Alternatively, it may contain polymer components that may be generated during the manufacturing process of oligomers.

[0167] From the viewpoints of printability, visual recognizability and machine developability, the oligomer preferably contains at least one compound selected from the group consisting of compounds having urethane bonds, compounds having ester bonds and compounds having epoxy residues, and more preferably contains a compound having urethane bonds.

[0168] In this invention, an epoxy residue refers to a structure formed by an epoxy group, for example, representing a structure identical to that obtained by reacting an acid group (carboxylic acid group, etc.) with an epoxy group.

[0169] Examples of oligomers include compounds having urethane bonds, preferably compounds having at least a group represented by formula (Ac-1) or formula (Ac-2), more preferably compounds having at least a group represented by formula (Ac-1).

[0170] [Chemical Formula 3]

[0171]

[0172] In equations (Ac-1) and (Ac-2), L 1 ~L 4 Each group represents a divalent hydrocarbon group with 2 to 20 carbon atoms, and the wavy line indicates the bonding position with other structures.

[0173] As L 1 ~L 4 Each of the alkylene compounds is preferably an alkylene compound having 2 to 20 carbon atoms, more preferably an alkylene compound having 2 to 10 carbon atoms, and even more preferably an alkylene compound having 4 to 8 carbon atoms. Furthermore, the aforementioned alkylene compounds may have branched or cyclic structures, but are preferably straight-chain alkylene compounds.

[0174] The wavy line portion in the preferred formula (Ac-1) or formula (Ac-2) is independently bonded directly to the wavy line portion in the group represented by the following formula (Ae-1) or formula (Ae-2).

[0175] [Chemical Formula 4]

[0176]

[0177] In formulas (Ae-1) and (Ae-2), R independently represents acryloyloxy or methacryloyloxy, and the wavy line portion indicates the bonding position with the wavy line portion in formulas (Ac-1) and (Ac-2).

[0178] Furthermore, as a compound having urethane bonds, a compound in which polymerizable groups are introduced into a polyurethane obtained by reacting a polyisocyanate compound with a polyol compound can be used.

[0179] For example, a compound having urethane bonds can be obtained by reacting a compound having epoxy and polymerizable groups with a polyurethane oligomer, which is obtained by reacting a polyol compound having acid groups with a polyisocyanate compound.

[0180] The number of polymerizable groups in compounds having ester bonds, which are examples of oligomers, is preferably three or more, and more preferably six or more.

[0181] Examples of oligomers include compounds containing epoxy residues, preferably compounds containing hydroxyl groups within the compound.

[0182] Furthermore, the number of polymerizable groups in the compound having epoxy residues is preferably 2 to 6, more preferably 2 to 3.

[0183] As a compound having the aforementioned epoxy residues, it can be obtained, for example, by reacting acrylic acid with a compound having an epoxy group.

[0184] Specific examples of oligomers are shown in the table below, but the oligomers used in this invention are not limited thereto.

[0185] As oligomers, commercially available products can be used, such as UA510H, UA-306H, UA-306I, UA-306T (all manufactured by KYOEISHA CHEMICAL Co., LTD.), UV-1700B, UV-6300B, UV7620EA (all manufactured by NipponSynthetic Chemical Industry Co., Ltd.), U-15HA (manufactured by Shin-Nakamura Chemical Co., Ltd.), EBECRYL450, EBECRYL657, EBECRYL885, EBECRYL800, EBECRYL3416, and EBECRYL860 (all manufactured by DAICEL-ALLNEX LTD.), but are not limited to these.

[0186] From the viewpoint of improving chemical resistance, printing durability and inhibition of on-machine developing residue, the content of oligomers is preferably 30% to 100% by mass relative to the total mass of polymeric compounds in the image recording layer, more preferably 50% to 100% by mass, and even more preferably 80% to 100% by mass.

[0187] -Low molecular weight polymeric compounds-

[0188] Polymerizable compounds may also contain polymerizable compounds other than the oligomers mentioned above.

[0189] From the viewpoint of chemical resistance, low-molecular-weight polymeric compounds are preferred as polymeric compounds other than oligomers. These low-molecular-weight polymeric compounds can be in chemical forms such as monomers, dimers, trimers, or mixtures thereof.

[0190] Furthermore, from the viewpoint of chemical resistance, the preferred low-molecular-weight polymeric compound is at least one polymeric compound selected from the group consisting of polymeric compounds having three or more olefinic unsaturated groups and polymeric compounds having an isocyanurate ring structure.

[0191] In this invention, low molecular weight polymeric compounds refer to polymeric compounds with a molecular weight (weight-average molecular weight in the case of a molecular weight distribution) of 50 or more and less than 600.

[0192] From the viewpoint of excellent chemical resistance, printing durability, and inhibition of on-machine developing residue, the molecular weight of the low molecular weight polymeric compound is preferably 100 or more and less than 600, more preferably 300 or more and less than 600, and even more preferably 400 or more and less than 600.

[0193] When the polymeric compound includes low-molecular-weight polymeric compounds as polymeric compounds other than oligomers (the total amount when including two or more low-molecular-weight polymeric compounds), from the viewpoint of chemical resistance, printing durability, and inhibition of machine-developed residues, the ratio of the oligomer to the low-molecular-weight polymeric compound (oligomer / low-molecular-weight polymeric compound) is preferably 10 / 1 to 1 / 10 by mass, more preferably 10 / 1 to 3 / 7, and even more preferably 10 / 1 to 7 / 3.

[0194] Furthermore, as a low-molecular-weight polymerizable compound, the polymerizable compound described in paragraphs 0082 to 0086 of International Publication No. 2019 / 013268 is preferred.

[0195] The details of the polymeric compound's structure, whether it is used alone or in combination, the amount added, and other usage methods can be set arbitrarily.

[0196] From the perspective of printing durability, the image recording layer preferably contains two or more polymeric compounds.

[0197] The content of polymeric compounds (the total content of polymeric compounds when including two or more polymeric compounds) is preferably 5% to 75% by mass, more preferably 10% to 70% by mass, and even more preferably 15% to 60% by mass, relative to the total mass of the image recording layer.

[0198] [Polymerization initiator]

[0199] The image recording layer in this invention preferably contains a polymerization initiator.

[0200] Furthermore, from the viewpoints of sensitivity, printing durability, machine developability, and ink adhesion, the polymerization initiator preferably contains an electron-donating polymerization initiator, and more preferably contains both an electron-accepting polymerization initiator and an electron-donating polymerization initiator.

[0201] -Electron-received polymerization initiators-

[0202] The image recording layer described above preferably contains an electron-accepting polymerization initiator as a polymerization initiator.

[0203] Electron-accepting polymerization initiators are compounds that, when exposed to infrared light, excite the electrons of the infrared absorber and accept an electron through intermolecular electron movement, thereby generating free radicals and other polymerization initiators.

[0204] The electron-accepting polymerization initiator used in this invention is a compound that generates polymerization initiators such as free radicals or cations through the energy of light, heat or both, and can appropriately select and use known thermal polymerization initiators, compounds with bonds having low bond dissociation energy, photopolymerization initiators, etc.

[0205] As an electron-accepting polymerization initiator, a free radical polymerization initiator is preferred, and an onium salt compound is more preferred.

[0206] Furthermore, an infrared-sensitive polymerization initiator is preferred as the electron-receiving polymerization initiator.

[0207] Examples of electron-accepting free radical polymerization initiators include (a) organohalides, (b) carbonyl compounds, (c) azo compounds, (d) organic peroxides, (e) metallocene compounds, (f) azide compounds, (g) hexaaryl biimidazole compounds, (i) disulfone compounds, (j) oxime ester compounds, and (k) onium salt compounds.

[0208] (a) As an organohalide, the compounds described in paragraphs 0022 to 0023 of Japanese Patent Application Publication No. 2008-195018 are preferred, for example.

[0209] As for (b) carbonyl compounds, the compounds described in paragraph 0024 of Japanese Patent Application Publication No. 2008-195018 are preferred, for example.

[0210] As (c) azo compound, for example, the azo compound described in Japanese Patent Application Publication No. 8-108621 can be used.

[0211] As (d) organic peroxide, the compounds described in paragraph 0025 of Japanese Patent Application Publication No. 2008-195018 are preferred, for example.

[0212] As for (e) metallocene compounds, the compounds described in paragraph 0026 of Japanese Patent Application Publication No. 2008-195018 are preferred, for example.

[0213] Examples of (f) azide compounds include 2,6-bis(4-azidobenzylidene)-4-methylcyclohexanone.

[0214] As a (g) hexaaryl biimidazole compound, the compound described in paragraph 0027 of Japanese Patent Application Publication No. 2008-195018 is preferred.

[0215] As for (i) disulfone compounds, examples include those described in Japanese Patent Application Publication Nos. 61-166544 and 2002-328465.

[0216] (j) As an oxime ester compound, the preferred compounds are those described in paragraphs 0028 to 0030 of Japanese Patent Application Publication No. 2008-195018.

[0217] Among the aforementioned electron-accepting polymerization initiators, oxime ester compounds and onium salt compounds are preferred from the viewpoint of curability. Of these, iodonium salt compounds, sulfonium salt compounds, or azazine onium salt compounds are preferred from the viewpoint of print durability, iodonium salt compounds or sulfonium salt compounds are more preferred, and iodonium salt compounds are particularly preferred.

[0218] Examples of iodonium salt compounds and sulfonium salt compounds include the compounds described in paragraphs 0060 and 0061 of Japanese Patent Application Publication No. 2023-138231.

[0219] Furthermore, as counter anions for iodonium salt compounds and sulfonium salt compounds, sulfonamide anions or sulfonamide anions are preferred, and sulfonamide anions are more preferred.

[0220] As a sulfonamide anion, arylsulfonamide anion is preferred.

[0221] Furthermore, bis(aryl)sulfonamide anion is preferred as the sulfonamide anion.

[0222] As a specific example of a sulfonamide anion or a sulfonamide anion, the anion described in International Publication No. 2020 / 262692 is preferably cited.

[0223] Furthermore, from the viewpoint of developability and printing durability in the obtained lithographic printing plate, the aforementioned electron-accepted polymerization initiator may contain a compound represented by the following formula (II).

[0224] [Chemical Formula 5]

[0225]

[0226] In equation (II), X A R represents a halogen atom. A It represents an aryl group.

[0227] As X in equation (II) A Specifically, examples include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. Among these, chlorine atoms or bromine atoms are preferred due to their excellent sensitivity, and bromine atoms are particularly preferred.

[0228] Furthermore, in equation (II), as R A From the perspective of achieving an excellent balance between sensitivity and storage stability, aryl groups substituted with amide groups are preferred.

[0229] As a specific example of an electron-receiving polymerization initiator represented by the above formula (II), the polymerization initiator described in International Publication No. 2020 / 262692 can be preferred.

[0230] From the viewpoint of improving sensitivity and reducing wear, the minimum unoccupied molecular orbital (LUMO) of the electron-receiving polymerization initiator is preferably -3.00 eV or less, more preferably -3.02 eV or less.

[0231] Furthermore, as a lower limit, it is preferably -3.80 eV or higher, and more preferably -3.60 eV or higher.

[0232] Electron-accepting polymerization initiators can be used alone or in combination with two or more.

[0233] The content of the electron-receiving polymerization initiator is preferably 0.1% to 50% by mass relative to the total mass of the image recording layer, more preferably 0.5% to 30% by mass, and particularly preferably 0.8% to 20% by mass.

[0234] -Electron-donating polymerization initiator-

[0235] From the viewpoint of improving the chemical resistance and printing durability of offset printing plates, the polymerization initiator preferably includes an electron-donating polymerization initiator, and more preferably includes both an electron-donating polymerization initiator and the aforementioned electron-donating polymerization initiator.

[0236] Five examples of electron-donating polymerization initiators can be cited.

[0237] (i) Alkyl or arylate complexes: These are believed to be formed by the oxidative cleavage of carbon-heterobonds, generating active free radicals. Specifically, examples include borate compounds.

[0238] (ii) Glycine compounds: It is believed that an active free radical is generated by the cleavage of the CX bond on the carbon adjacent to nitrogen due to oxidation. Preferably, X is a hydrogen atom, a carboxyl group, a trimethylsilyl group, or a benzyl group. Specifically, examples include N-phenylglycine derivatives (which may have substituents in the phenyl group), N-phenyliminodiacetic acid (which may have substituents in the phenyl group), etc.

[0239] (iii) Sulfur-containing compounds: Compounds obtained by replacing the nitrogen atom of the above-mentioned aminoacetic acid compounds with a sulfur atom can generate active free radicals through the same process. Specifically, examples include phenylthioacetic acid (which may have substituents in the phenyl group), etc.

[0240] (iv) Tin-containing compounds: Compounds obtained by replacing the nitrogen atom of the above-mentioned glycine compound with a tin atom can generate active free radicals through the same action.

[0241] (v) Sulfites: These can generate reactive free radicals through oxidation. Examples include sodium arylsulfinates.

[0242] Among these electron-donating polymerization initiators, the image recording layer preferably contains a borate compound. As the borate compound, a tetraarylborate compound or a monoalkyltriarylborate compound is preferred; from the viewpoint of compound stability, a tetraarylborate compound is more preferred, and a tetraphenylborate compound is particularly preferred.

[0243] There are no particular limitations on the counter cations present in borate compounds, but alkali metal ions or tetraalkylammonium ions are preferred, and sodium ions, potassium ions or tetrabutylammonium ions are more preferred.

[0244] As a borate compound, sodium tetraphenylborate is particularly preferred.

[0245] Furthermore, from the viewpoint of chemical resistance and printability, the highest occupied molecular orbital (HOMO) of the electron-donating polymerization initiator used in this invention is preferably -6.00 eV or more, more preferably -5.95 eV or more, even more preferably -5.93 eV or more, and particularly preferably greater than -5.90 eV.

[0246] Furthermore, as an upper limit, it is preferably below -5.00 eV, and more preferably below -5.40 eV.

[0247] Hereinafter, as a preferred example of an electron-donating polymerization initiator, the polymerization initiator described in International Publication No. 2020 / 262692 is preferably cited.

[0248] Furthermore, from the viewpoints of visual recognition, print durability, and stability over time, the image recording layer preferably contains at least one compound selected from the group consisting of an onium salt compound as an electron-accepting polymerization initiator and a borate compound as an electron-donating polymerization initiator, and more preferably contains an onium salt compound as an electron-accepting polymerization initiator and a borate compound as an electron-donating polymerization initiator.

[0249] Furthermore, the image recording layer preferably contains a borate compound as the electron-donating polymerization initiator, more preferably contains a borate compound as the electron-donating polymerization initiator, and the HOMO value of the infrared absorber minus the HOMO value of the borate compound is 0.70 eV or less.

[0250] Electron-donating polymerization initiators can be added in single or multiple ways.

[0251] The content of the electron-donating polymerization initiator is preferably 0.01% to 30% by mass relative to the total mass of the image recording layer, more preferably 0.05% to 25% by mass, and even more preferably 0.1% to 20% by mass.

[0252] Furthermore, one of the preferred embodiments of the present invention is the formation of a salt by the above-mentioned electron-accepting polymerization initiator and the above-mentioned electron-donating polymerization initiator.

[0253] Specifically, for example, the aforementioned onium salt compound can be described as a salt of an onium ion and an anion (e.g., tetraphenylborate anion) in the aforementioned electron-donating polymerization initiator. More preferably, an iodonium borate compound is described, which is obtained by forming a salt from an iodonium cation (e.g., di-p-tolyliodonium cation) in the aforementioned iodonium salt compound and a borate anion in the aforementioned electron-donating polymerization initiator.

[0254] As a specific example of the formation of a salt by the aforementioned electron-accepting polymerization initiator and the aforementioned electron-donating polymerization initiator, the method described in International Publication No. 2020 / 262692 is preferably cited.

[0255] In this invention, when the image recording layer contains onium ions and the anions in the electron-donating polymerization initiator described above, the image recording layer contains an electron-accepting polymerization initiator and the electron-donating polymerization initiator described above.

[0256] Infrared absorber

[0257] The image recording layer in this invention preferably contains an infrared absorber.

[0258] There are no particular limitations on what can be used as an infrared absorber; for example, pigments and dyes can be cited.

[0259] As dyes that can be used as infrared absorbers, commercially available dyes and well-known dyes as described in publications such as "Dye Handbook" (The Society of Synthetic Organic Chemistry, Japan, 1955). Specifically, examples include azo dyes, metal complex salt azo dyes, pyrazolone azo dyes, naphthoquinone dyes, anthraquinone dyes, phthalocyanine dyes, carbonium dyes, quinone imine dyes, methylene dyes, anthocyanin dyes, squaric acid pigments, pyranium salts, and metal thiolate complexes.

[0260] Among these dyes, particularly preferred dyes include anthocyanins, squaric acid dyes, pyranonium salts, nickel thiol complexes, and indolinecyanine dyes. Additionally, anthocyanins and indolinecyanine dyes are also mentioned. Among these, anthocyanins are particularly preferred.

[0261] As an infrared absorber, a cationic polymethimide pigment having an oxygen or nitrogen atom at the meta position is preferred. Examples of cationic polymethimide pigments include anthocyanins, pyranonium pigments, thiopyranonium pigments, and azulenium pigments. From the viewpoints of availability and solvent solubility during the induction reaction, anthocyanins are preferred.

[0262] Specific examples of anthocyanins include compounds described in paragraphs 0017-0019 of Japanese Patent Application Publication No. 2001-133969, paragraphs 0016-0021 of Japanese Patent Application Publication No. 2002-023360, and paragraphs 0012-0037 of Japanese Patent Application Publication No. 2002-040638. Preferably, compounds described in paragraphs 0034-0041 of Japanese Patent Application Publication No. 2002-278057 and paragraphs 0080-0086 of Japanese Patent Application Publication No. 2008-195018 are listed. Particularly preferred are compounds described in paragraphs 0035-0043 of Japanese Patent Application Publication No. 2007-90850 and paragraphs 0105-0113 of Japanese Patent Application Publication No. 2012-206495.

[0263] Furthermore, compounds described in Japanese Patent Application Publication No. 5-5005, paragraphs 0008-0009, and Japanese Patent Application Publication No. 2001-222101, paragraphs 0022-0025, can be preferred.

[0264] As a pigment, compounds described in paragraphs 0072 to 0076 of Japanese Patent Application Publication No. 2008-195018 are preferred.

[0265] Furthermore, infrared absorbers may include infrared absorbers that decompose upon exposure to infrared light (decomposition-type infrared absorbers). Examples of decomposition-type infrared absorbers include decomposition-type chromogenic infrared absorbers.

[0266] It is speculated that the excellent printability is achieved by using a decomposable infrared absorber as an infrared absorber, whereby the infrared absorber or its decomposition products promote polymerization, and by the interaction between the decomposition products of the infrared absorber and the polymerizable compound.

[0267] The preferred type of decomposition infrared absorber is an infrared absorber that has the function of absorbing infrared rays through infrared exposure and decomposing them to produce color.

[0268] Hereinafter, the chromophore formed by the absorption and decomposition of infrared radiation by decomposition infrared absorbers through infrared exposure will also be referred to as the "chromophore of decomposition infrared absorbers".

[0269] Furthermore, the decomposition-type infrared absorber preferably has the function of absorbing infrared rays through infrared exposure and converting the absorbed infrared rays into heat.

[0270] Regarding decomposition-type infrared absorbers, it is sufficient to absorb at least a portion of the light in the infrared wavelength region (wavelength 750nm to 1mm) and decompose it. Preferably, it is an infrared absorber with a maximum absorption wavelength in the wavelength region of 750nm to 1,400nm, and more preferably, it is an infrared absorber with a maximum absorption wavelength in the wavelength region of 760nm to 900nm.

[0271] More specifically, the decomposition-type infrared absorber is preferably a compound that decomposes upon infrared exposure and generates a compound with a maximum absorption wavelength in the wavelength region of 500 nm to 600 nm.

[0272] The decomposable infrared absorber is preferably an infrared absorber that decomposes through thermal or electron transfer caused by infrared exposure, or both. More preferably, it is an infrared absorber that decomposes through electron transfer caused by infrared exposure. Here, "decomposition through electron transfer" means that electrons excited from the HOMO (highest occupied molecular orbital) to the LUMO (lowest unoccupied molecular orbital) of the decomposable infrared absorber by infrared exposure are transferred within the molecule to electron-accepting groups (groups with potential close to the LUMO), resulting in decomposition.

[0273] Furthermore, from the viewpoint of colorimetric properties, infrared absorbers preferably include compounds represented by the following formula (X) as decomposition-type infrared absorbers.

[0274] [Chemical Formula 6]

[0275]

[0276] In equation (X), Ar 11 and Ar 12 R represents the set of atoms required to form a substituted or unsubstituted aromatic ring, or a substituted or unsubstituted heteroaromatic ring, respectively. 11 and R 12 Each is an alkyl group, either substituted or unsubstituted, R. 13 R represents a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group. 14 Y represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group, and Y independently represents an oxygen atom, a sulfur atom, or a group consisting of >C(R) 15 R 16 R represents dialkylmethylene. 15 and R 16Each of the following groups independently represents an alkyl group having 1 to 4 carbon atoms, either substituted or unsubstituted. A1 and A2 independently represent substituted or unsubstituted alkyl groups, or groups of 2 or 3 carbon atoms required to form a substituted or unsubstituted 5- or 6-membered non-aromatic carbon ring. Za represents a counterion that neutralizes the charge.

[0277] The above Ar 11 and Ar 12 Each of these groups of atoms represents the set of atoms required to form a substituted or unsubstituted aromatic ring or a substituted or unsubstituted heteroaromatic ring, but examples of substituents for the aromatic or heteroaromatic ring include alkyl, alkoxy, halogen, cyano, -COOR, -SO3R, or -SO2R groups (where R represents a substituted or unsubstituted alkyl group), preferably alkyl or halogen atoms.

[0278] Furthermore, as mentioned above, Ar 11 and Ar 12 Preferably, it is the set of atoms required to form a substituted or unsubstituted aromatic ring, more preferably the set of atoms required to form a substituted or unsubstituted benzene ring or naphthalene ring.

[0279] As for Y mentioned above, each is preferably independently composed of >C(R) 15 R 16 The dialkylmethylene group represented by ) is preferably composed of >C(R 15 R 16 ) indicates that R 15 and R 16 The same dialkylmethylene. At this point, R... 15 and R 16 Each is preferably an alkyl group with 1 or 2 carbon atoms, either substituted or unsubstituted.

[0280] As for the aforementioned Y, it is particularly preferred to be >C(R) 15 R 16 ) indicates that R 15 and R 16 It is a dialkylmethylene group of methyl.

[0281] As mentioned above, R 11 and R 12 Each is preferably an alkyl group having 1 to 12 carbon atoms, either substituted or unsubstituted. Furthermore, the above-mentioned R... 11 and R 12 Ether bonds or ester bonds may be present in the middle of the carbon chain of alkyl groups with 1 to 12 carbon atoms, whether substituted or unsubstituted.

[0282] As mentioned above, R 13Preferably, it is an alkyl group having 1 to 12 carbon atoms, either substituted or unsubstituted; more preferably, it is a haloalkyl group having one or more hydrogen atoms of the alkyl group having 1 to 12 carbon atoms substituted with halogen atoms. In this case, chlorine or bromine atoms are preferred as halogen atoms.

[0283] Among them, as the above R 11 and R 12 Each of these is preferably a perfluoroalkyl group.

[0284] As mentioned above, R 14 Preferably, it is a hydrogen atom or an unsubstituted alkyl group having one or eight carbon atoms.

[0285] As for A1 and A2 above, they preferably represent substituted or unsubstituted alkyl groups, or groups of two or three carbon atoms that are bonded together to form a cyclopentene ring or a cyclohexene ring.

[0286] When Za is used as a counter anion, anions containing halogen atoms or boron atoms are preferred. Specifically, ClO4 can be cited as an example of Za. - PF6 - BF4 - SbF6 - CH3SO3 - CF3SO3 - C6H5SO3 - CH3C6H5SO3 - HOC6H5SO3 - ClC6H5SO3 - CH3C6H5SO3 - Tetraarylborate anions (e.g., tetraphenylborate anion), etc.

[0287] In the case where Za is the counter cation, examples include alkali metal ions, alkaline earth metal ions, tertiary ammonium ions, quaternary ammonium ions, and onium ions (iodonium ions, sulfonium ions, phosphonium ions, etc.).

[0288] The following are specific examples of compounds represented by formula (X), but the present invention is not limited to these. Additionally, Ph represents phenyl.

[0289] [Chemical Formula 7]

[0290]

[0291] As an infrared absorber and an infrared absorber that decomposes by infrared exposure, the infrared absorber described in International Publication No. 2020 / 262692 is preferred.

[0292] Furthermore, as an infrared absorber that decomposes through infrared exposure, the infrared absorber described in Japanese Patent Application Publication No. 2008-544322 or International Publication No. 2016 / 027886 is preferred.

[0293] Furthermore, as a decomposable infrared absorber, anthocyanin is preferably an infrared absorbing compound described in International Publication No. 2019 / 219560.

[0294] Infrared absorbers can be used in combination with one type or two or more types. In one embodiment, the image recording layer preferably contains two or more types of infrared absorbers. Furthermore, pigments and dyes can be used in combination as infrared absorbers.

[0295] The total content of infrared absorber in the image recording layer is preferably 0.1% to 10.0% by mass relative to the total mass of the image recording layer, and more preferably 0.5% to 7.5% by mass.

[0296] [The relationship between electron-donating polymerization initiators, electron-accepting polymerization initiators, and infrared absorbers]

[0297] The image recording layer of the present invention preferably contains two or more electron-donating polymerization initiators and electron-accepting polymerization initiators, and also contains an infrared absorber.

[0298] When the image recording layer contains two or more electron-donating polymerization initiators, electron-accepting polymerization initiators and infrared absorbers, it is more preferable that at least one of the two or more electron-donating polymerization initiators has a HOMO of -6.0 eV or more and the LUMO of the electron-accepting polymerization initiator is -3.0 eV or less.

[0299] More preferred methods for HOMO with two or more electron-donating polymerization initiators and LUMO with electron-accepting polymerization initiators are described above.

[0300] In the image recording layer of the present invention, it is presumed that at least one of two or more electron-donating polymerization initiators, an electron-accepting polymerization initiator, and an infrared absorber, for example, as described in the following chemical formula, perform energy transfer.

[0301] Therefore, it is believed that as long as at least one of the two or more electron-donating polymerization initiators has a HOMO of -6.0 eV or higher, and the LUMO of the electron-accepting polymerization initiator is below -3.0 eV, the free radical generation efficiency will be improved, thus making chemical resistance and printing durability more likely to be superior.

[0302] [Chemical Formula 8]

[0303]

[0304] From the viewpoint of printability and chemical resistance, the HOMO value of at least one of the HOMO-electron-donating polymerization initiators of the infrared absorber is preferably 1.0 eV or less, more preferably 0.70 eV or less, and particularly preferably 0.60 eV or less. Furthermore, from the same viewpoint, the HOMO value of at least one of the HOMO-electron-donating polymerization initiators of the infrared absorber is preferably -0.200 eV or more, more preferably -0.100 eV or more.

[0305] Additionally, a negative value indicates that the HOMO of at least one of the electron-donating polymerization initiators is higher than that of the infrared absorber.

[0306] Furthermore, from the viewpoint of printability and chemical resistance, the LUMO value of the LUMO-infrared absorber of the electron-accepting polymerization initiator is preferably 1.00 eV or less, more preferably 0.700 eV or less. Also from the same viewpoint, the LUMO value of the LUMO-infrared absorber of the electron-accepting polymerization initiator is preferably -0.200 eV or more, more preferably -0.100 eV or more.

[0307] Furthermore, from the same perspective, the LUMO value of the electron-accepting polymerization initiator versus the LUMO value of the infrared absorber is preferably 1.00 eV to -0.200 eV, more preferably 0.700 eV to -0.100 eV. Additionally, a negative value indicates that the LUMO of the infrared absorber is higher than that of the electron-accepting polymerization initiator.

[0308] [Coloring agent]

[0309] The image recording layer preferably contains a colorant, and more preferably contains an acid colorant.

[0310] The term "color-developing agent" as used in this invention refers to a compound that develops or decolorizes upon stimulation by light, acid, or the like, thereby changing the color of the image recording layer. Furthermore, "acid color-developing agent" refers to a compound that develops or decolorizes upon heating while in a state where it has received protons from an electron-accepting compound (e.g., an acid). As an acid color-developing agent, colorless compounds having partial skeletons such as lactones, lactams, sulfolactones, spiropyrans, esters, or amides are particularly preferred, and these partial skeletons rapidly undergo ring-opening or breakage upon contact with an electron-accepting compound.

[0311] An example of such an acid-based colorant is the acid-based colorant described in Japanese Patent Application Publication No. 2023-16860.

[0312] From the viewpoint of color development, the color-developing agent used in this invention is preferably at least one compound selected from the group consisting of spiropyran compounds, spiroxazine compounds, spironolactone compounds, and spironolactam compounds.

[0313] From a visibility point of view, the preferred hue of the pigment after color development is green, blue, or black.

[0314] Furthermore, from the viewpoint of color development and visual recognition of the exposed area, the aforementioned acid colorant is preferably a colorless pigment.

[0315] As for the aforementioned colorless pigment, there are no particular restrictions as long as it has a colorless structure, but it is preferred to have a helical structure, and more preferably to have a spironolactone ring structure.

[0316] Furthermore, from the viewpoint of colorimetric properties and visual recognition of the exposed portion, the colorless pigment described above is preferably a colorless pigment having a phthaloyl structure or a fluorane parent structure.

[0317] Furthermore, from the viewpoint of color development and visual recognition of the exposed portion, the aforementioned colorless pigment having a phthaloyl or fluorane structure is preferably a compound represented by any one of the following formulas (Le-1) to (Le-3), and more preferably a compound represented by the following formula (Le-2).

[0318] [Chemical Formula 9]

[0319]

[0320] In formulas (Le-1) to (Le-3), ERG independently represents an electron-donating group, X1 to X4 independently represent a hydrogen atom, a halogen atom, or a dialkylaniline group, and X5 to X 10 Each of the following groups independently represents a hydrogen atom, a halogen atom, or a monovalent organic group. Y1 and Y2 independently represent C or N. When Y1 is N, X1 does not exist. When Y2 is N, X4 does not exist. Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group. Rb1 to Rb4 independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0321] From the viewpoint of colorimetry and visual recognizability of the exposed portion, the electron-donating group in the ERG of formulas (Le-1) to (Le-3) is preferably amino, alkylamino, arylamino, heteroarylamino, dialkylamino, monoalkyl monoarylamino, monoalkyl monoheteroarylamino, diarylamino, diheteroarylamino, monoaryl monoheteroarylamino, alkoxy, aryloxy, heteroaryloxy, or alkyl. More preferably, it is amino, alkylamino, arylamino, heteroarylamino, dialkylamino, monoalkyl monoarylamino, monoalkyl monoheteroarylamino, diarylamino, diheteroarylamino, monoaryl monoheteroarylamino, alkoxy, or aryloxy. Even more preferably, it is monoalkyl monoarylamino, diarylamino, diheteroarylamino, or monoaryl monoheteroarylamino. Particularly preferred is monoalkyl monoarylamino.

[0322] Furthermore, from the viewpoint of color development and visual recognition of the exposed portion, the electron-donating group in the aforementioned ERG is preferably a disubstituted amino group having an aryl group with a substituent at at least one ortho position or a heteroaryl group with a substituent at at least one ortho position. More preferably, it is a disubstituted amino group having a phenyl group with a substituent at at least one ortho position and an electron-donating group at the para position. Even more preferably, it is an amino group having a phenyl group with a substituent at at least one ortho position and an electron-donating group at the para position and an aryl or heteroaryl group. Particularly preferred is an amino group having a phenyl group with a substituent at at least one ortho position and an electron-donating group at the para position and an aryl or heteroaryl group with an electron-donating group.

[0323] In addition, in this invention, the adjacent position in aryl or heteroaryl groups other than phenyl refers to the bonding position (e.g., position 2, etc.) adjacent to the aforementioned position 1 when the bonding position of aryl or heteroaryl group with other structures is set to position 1.

[0324] Furthermore, from the viewpoint of color development and visual recognition of the exposed portion, the electron-donating group of the aforementioned aryl or heteroaryl group is preferably amino, alkylamino, arylamino, heteroarylamino, dialkylamino, monoalkylmonoarylamino, monoalkylmonoheteroarylamino, diarylamino, diheteroarylamino, monoarylmonoheteroarylamino, alkoxy, aryloxy, heteroaryloxy, or alkyl, more preferably alkoxy, aryloxy, heteroaryloxy, or alkyl, and particularly preferably alkoxy.

[0325] From the viewpoint of color development and visual recognition of the exposed part, X1 to X4 in formulas (Le-1) to (Le-3) are each preferably hydrogen atoms or chlorine atoms, and more preferably hydrogen atoms.

[0326] From the perspective of color development and visual recognizability of the exposed area, X5 to X in formula (Le-2) or formula (Le-3) 10The atom is preferably hydrogen, halogen, alkyl, aryl, amino, alkylamino, arylamino, heteroarylamino, dialkylamino, monoalkylmonoarylamino, monoalkylmonoheteroarylamino, diarylamino, diheteroarylamino, monoarylmonoheteroarylamino, hydroxyl, alkoxy, aryloxy, heteroaryloxy, acyl, alkoxycarbonyl, aryloxycarbonyl, heteroaryloxycarbonyl, or cyano, more preferably hydrogen, halogen, alkyl, aryl, alkoxy, or aryloxy, further preferably hydrogen, halogen, alkyl, or aryl, and particularly preferably hydrogen.

[0327] From the viewpoint of color development and visual recognizability of the exposed part, Y1 and Y2 in formulas (Le-1) to (Le-3) are preferably at least one of them as C, and more preferably both Y1 and Y2 are C.

[0328] From the viewpoint of color development and visual recognizability of the exposed part, Ra1 in formulas (Le-1) to (Le-3) is preferably alkyl or alkoxy, more preferably alkoxy, and particularly preferably methoxy.

[0329] From the viewpoint of color development and visual recognizability of the exposed part, Rb1 to Rb4 in formulas (Le-1) to (Le-3) are each preferably hydrogen atoms or alkyl groups, more preferably alkyl groups, and particularly preferably methyl groups.

[0330] Furthermore, from the viewpoint of color development and visual recognition of the exposed portion, the aforementioned colorless pigment having a phthaloyl or fluorane structure is more preferably a compound represented by any one of the following formulas (Le-4) to (Le-6), and even more preferably a compound represented by the following formula (Le-5).

[0331] [Chemical Formula 10]

[0332]

[0333] In formulas (Le-4) to (Le-6), ERG independently represents an electron-donating group, X1 to X4 independently represent a hydrogen atom, a halogen atom, or a dialkylaniline group, Y1 and Y2 independently represent C or N, X1 is absent when Y1 is N, X4 is absent when Y2 is N, Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group, and Rb1 to Rb4 independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0334] The meanings of ERG, X1 to X4, Y1, Y2, Ra1 and Rb1 to Rb4 in equations (Le-4) to (Le-6) are the same as those in equations (Le-1) to (Le-3), and the preferred methods are also the same.

[0335] Furthermore, from the viewpoint of color development and visual recognition of the exposed portion, the aforementioned colorless pigment having a phthaloyl structure or a fluorane parent structure is further preferably a compound represented by any one of the following formulas (Le-7) to (Le-9), and particularly preferably a compound represented by the following formula (Le-8).

[0336] [Chemical Formula 11]

[0337]

[0338] In formulas (Le-7) to (Le-9), X1 to X4 independently represent hydrogen atoms, halogen atoms or dialkylaniline groups, Y1 and Y2 independently represent C or N, X1 does not exist when Y1 is N, X4 does not exist when Y2 is N, Ra1 to Ra4 independently represent hydrogen atoms, alkyl or alkoxy groups, Rb1 to Rb4 independently represent hydrogen atoms, alkyl, aryl or heteroaryl groups, and Rc1 and Rc2 independently represent aryl or heteroaryl groups.

[0339] The meanings of X1 to X4, Y1 and Y2 in equations (Le-7) to (Le-9) are the same as those in equations (Le-1) to (Le-3), and the preferred methods are also the same.

[0340] From the viewpoint of color development and visual recognizability of the exposed part, Ra1 to Ra4 in formula (Le-7) or formula (Le-9) are each preferably alkyl or alkoxy, more preferably alkoxy, and particularly preferably methoxy.

[0341] From the viewpoint of color development and visual recognition of the exposed part, Rb1 to Rb4 in formulas (Le-7) to (Le-9) are each preferably aryl groups substituted with hydrogen atoms, alkyl groups or alkoxy groups, more preferably alkyl groups, and particularly preferably methyl groups.

[0342] From the viewpoint of color development and visual recognizability of the exposed part, Rc1 and Rc2 in formula (Le-8) are preferably phenyl or alkylphenyl, and more preferably phenyl.

[0343] Furthermore, from the viewpoint of color development and visual recognizability of the exposed portion, Rc1 and Rc2 in formula (Le-8) are each preferably aryl groups having a substituent at at least one ortho position or heteroaryl groups having a substituent at at least one ortho position, more preferably aryl groups having a substituent at at least one ortho position, even more preferably phenyl groups having a substituent at at least one ortho position, and particularly preferably phenyl groups having a substituent at at least one ortho position and an electron-donating group at the para position. Examples of the substituents in Rc1 and Rc2 described later can be cited.

[0344] Furthermore, in formula (Le-8), from the viewpoint of color development and visual recognizability of the exposed part, it is preferable that X1 to X4 are hydrogen atoms and Y1 and Y2 are C atoms.

[0345] Furthermore, in formula (Le-8), from the viewpoint of color development and visual recognizability of the exposed portion, Rb1 and Rb2 are each preferably aryl groups substituted with alkyl or alkoxy groups.

[0346] Furthermore, in formula (Le-8), from the viewpoint of color development and visual recognizability of the exposed portion, Rb1 and Rb2 are each preferably aryl or heteroaryl, more preferably aryl, even more preferably aryl having an electron-donating group, and particularly preferably phenyl having an electron-donating group at the para position.

[0347] Furthermore, from the viewpoint of colorimetry and visual recognizability of the exposed portion, the electron-donating groups in Rb1, Rb2, Rc1, and Rc2 are preferably amino, alkylamino, arylamino, heteroarylamino, dialkylamino, monoalkylmonoarylamino, monoalkylmonoheteroarylamino, diarylamino, diheteroarylamino, monoarylmonoheteroarylamino, alkoxy, aryloxy, heteroaryloxy, or alkyl, more preferably alkoxy, aryloxy, heteroaryloxy, or alkyl, and particularly preferably alkoxy.

[0348] Furthermore, from the viewpoint of color development and visual recognition of the exposed area, it is preferable to use one or more compounds selected from the group consisting of compounds represented by the following formula (Le-10) and compounds represented by the following formula (Z-4).

[0349] That is, the image recording layer in the original lithographic printing plate involved in the present invention preferably further contains one or more compounds selected from the group consisting of compounds represented by the following formula (Le-10) and compounds represented by the following formula (Z-4).

[0350] [Chemical Formula 12]

[0351]

[0352] In formula (Le-10), Ar1 independently represents aryl or heteroaryl, and Ar2 independently represents aryl with substituents at at least one ortho position or heteroaryl with substituents at at least one ortho position.

[0353] The meaning of Ar1 in formula (Le-10) is the same as that of Rb1 and Rb2 in formulas (Le-7) to (Le-9), and the preferred method is also the same.

[0354] The meaning of Ar2 in formula (Le-10) is the same as that of Rc1 and Rc2 in formulas (Le-7) to (Le-9), and the preferred method is also the same.

[0355] The alkyl groups in formulas (Le-1) to (Le-9) can be straight chains, branched chains, or ring structures.

[0356] Furthermore, the number of carbon atoms of the alkyl group in formulas (Le-1) to (Le-9) is preferably 1 to 20, more preferably 1 to 8, even more preferably 1 to 4, and particularly preferably 1 or 2.

[0357] The number of carbon atoms in the aryl group in formulas (Le-1) to (Le-10) is preferably 6 to 20, more preferably 6 to 10, and particularly preferably 6 to 8.

[0358] As aryl groups in formulas (Le-1) to (Le-10), examples include phenyl, naphthyl, anthracene, and phenanthrene groups, which may have substituents.

[0359] As for the heteroaryl groups in formulas (Le-1) to (Le-10), examples include those that can have substituents, such as furanyl, pyridyl, pyrimidinyl, pyrazolyl, and phenylthioyl.

[0360] Furthermore, the monovalent organic groups, alkyl, aryl, heteroaryl, dialkylaniline, alkylamino, alkoxy, and other groups in formulas (Le-1) to (Le-10) can have substituents. Examples of substituents include alkyl, aryl, heteroaryl, halogen atoms, amino, alkylamino, arylamino, heteroarylamino, dialkylamino, monoalkylmonoarylamino, monoalkylmonoheteroarylamino, diarylamino, diheteroarylamino, monoarylmonoheteroarylamino, hydroxyl, alkoxy, aryloxy, heteroaryloxy, acyl, alkoxycarbonyl, aryloxycarbonyl, heteroaryloxycarbonyl, cyano, etc. Moreover, these substituents can be further replaced by these substituents.

[0361] [Chemical Formula 13]

[0362]

[0363] In formula (Z-4), Rza1 represents a hydrogen atom, alkyl or alkoxy group, Rzb1 to Rzb4 represent hydrogen atom, alkyl or aryl group respectively, Rzb1 and Rzb2, Rzb3 and Rzb4 can be linked to form a ring structure, X represents O or NR, R represents hydrogen atom, alkyl, aryl or heteroaryl group, and Y1 and Y2 represent CH or N respectively.

[0364] Rza1 in formula (Z-4) is preferably alkyl or alkoxy.

[0365] In formula (Z-4), Rzb1 and Rzb2 are each preferably alkyl groups.

[0366] In formula (Z-4), Rzb3 and Rzb4 are independently hydrogen atoms, alkyl groups or aryl groups, with one of them preferably being an aryl group.

[0367] In the preferred formula (Z-4), X is O, and Y1 and Y2 are CH.

[0368] The alkyl group in formula (Z-4) can be straight-chain, branched, or cyclic.

[0369] The alkyl group in formula (Z-4) preferably has 1 to 20 carbon atoms, more preferably 1 to 8, and even more preferably 1 to 5.

[0370] The number of carbon atoms in the aryl group in formula (Z-4) is preferably 6 to 20, more preferably 6 to 10, and particularly preferably 6 to 8.

[0371] The alkyl, aryl, and other groups in formula (Z-4) may have substituents. Examples of substituents include alkyl, aryl, halogen atoms, amino, alkylamino, arylamino, dialkylamino, monoalkylmonoarylamino, diarylamino, hydroxyl, alkoxy, aryloxy, acyl, alkoxycarbonyl, aryloxycarbonyl, and cyano. Furthermore, these substituents can be further replaced by other substituents.

[0372] The following compounds are examples of colorless pigments having a phthalide or fluorane parent structure that are preferred for use. Additionally, Me represents a methyl group.

[0373] [Chemical Formula 14]

[0374]

[0375] [Chemical Formula 15]

[0376]

[0377] [Chemical Formula 16]

[0378]

[0379] [Chemical Formula 17]

[0380]

[0381] [Chemical Formula 18]

[0382]

[0383] [Chemical Formula 19]

[0384]

[0385] [Chemical Formula 20]

[0386]

[0387] [Chemical Formula 21]

[0388]

[0389] As a color-developing agent, commercially available products can also be used, including ETAC, RED500, RED520, CVL, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, BLUE220, H-3035, BLUE203, ATP, H-1046, H-2114 (all manufactured by Fukui Yamada Chemical Co., Ltd.), ORANGE-DCF, Vermilion-DCF, PINK-DCF, RED-DCF, BLMB, CVL, GREEN-DCF, and TH-107 (all manufactured by HODOGAYA CHEMICAL). ODB, ODB-2, ODB-4, ODB-250, ODB-BlackXV, Blue-63, Blue-502, GN-169, GN-2, Green-118, Red-40, Red-8 (all manufactured by YAMAMOTO CHEMICALS INC.), crystal violet lactone (manufactured by Tokyo Chemical Industry Co., Ltd.), etc.

[0390] Among these commercially available products, the films formed by ETAC, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, H-3035, ATP, H-1046, H-2114, GREEN-DCF, Blue-63, GN-169, and crystal violet lactone have good visible light absorption rates and are therefore preferred.

[0391] These colorants can be used alone or in combination with two or more ingredients.

[0392] The content of the colorant is preferably 0.5% to 10% by mass relative to the total mass of the image recording layer, more preferably 1% to 7.5% by mass.

[0393] [Adhesive polymers]

[0394] The image recording layer may contain an adhesive polymer. As the adhesive polymer, the adhesive polymer used in the image recording layer of an on-machine developing type lithographic printing plate master can be used. Specifically, the adhesive polymer described in paragraphs 0288 to 0317 of International Publication No. 2022 / 019217 is preferably used.

[0395] In the image recording layer used in this invention, one type of adhesive polymer can be used alone, or two or more types can be used together.

[0396] The image recording layer can contain any amount of adhesive polymer, and the content of adhesive polymer relative to the total mass of the image recording layer is preferably 1% to 90% by mass, more preferably 5% to 80% by mass.

[0397] Furthermore, when the image recording layer in the present invention contains other adhesive polymers, the content of other adhesive polymers is preferably more than 0% by mass and less than 99% by mass relative to the total mass of the above-mentioned thermoplastic resin particles and other adhesive polymers, more preferably 20% by mass to 95% by mass, and even more preferably 40% by mass to 90% by mass.

[0398] [Oil-based]

[0399] Image recording layers may also contain oils.

[0400] The oil in this invention refers to a hydrophobic compound that is liquid at 80°C and separates without mixing when mixed with the same mass of water.

[0401] In addition, when using two or more oils, even if they contain compounds with a melting point of 80°C or higher, as long as they are in a liquid state at 80°C when mixed with two or more oils, it is acceptable.

[0402] Furthermore, from the viewpoint of machine developability and dampening solution turbidity suppression, the oil is preferably a compound with a molecular weight of less than 1,000, more preferably a compound with a molecular weight of 200 to 800, and particularly preferably a compound with a molecular weight of 300 to 500.

[0403] Furthermore, from the viewpoint of machine developability and dampening solution turbidity suppression, the oil is preferably a compound with a boiling point of 200°C or higher at 1 atmosphere, more preferably a compound with a boiling point of 250°C or higher at 1 atmosphere, even more preferably a compound with a boiling point of 300°C or higher at 1 atmosphere, and particularly preferably a compound with a boiling point of 400°C or higher and 500°C or lower at 1 atmosphere.

[0404] In addition, in this invention, unless otherwise specified, when referred to as "boiling point", it is the boiling point at 1 atmosphere.

[0405] Furthermore, from the viewpoint of machine developability and dampening solution turbidity suppression, the melting point of the oil at 1 atmosphere is preferably 50°C or less, more preferably 30°C or less, and particularly preferably -200°C or more and 25°C or less.

[0406] In addition, in this invention, unless otherwise specified, when referred to as "melting point", it is the melting point at 1 atmosphere.

[0407] Examples of oil-based agents include phosphate esters, aromatic hydrocarbons, glycerides, fatty acids, and aromatic esters.

[0408] From the viewpoints of UV printing durability, ink adhesion, on-machine developability, and dampening solution turbidity suppression, at least one compound is preferably selected from the group consisting of free phosphate ester compounds, aromatic hydrocarbon compounds, glycerol ester compounds, and aromatic ester compounds; more preferably, at least one compound is selected from the group consisting of free phosphate ester compounds, aromatic hydrocarbon compounds, and glycerol ester compounds; even more preferably, at least one compound is selected from the group consisting of free phosphate ester compounds and aromatic hydrocarbon compounds; and particularly preferably, phosphate ester compounds.

[0409] From the viewpoints of UV printing durability, ink adhesion, on-machine developability, and dampening solution turbidity suppression, phosphate triester compounds are preferred as phosphate compounds, more preferably triaryl phosphate compounds, and even more preferably tricresyl phosphate. A mixture of two or more of the ortho, meta, and para positions of tricresyl phosphate is particularly preferred.

[0410] From the viewpoint of machine developability and dampening solution turbidity suppression, compounds having two or more aromatic rings are preferred as aromatic hydrocarbon compounds, and compounds having two or more unfused benzene rings are more preferred.

[0411] From the viewpoint of machine developability and dampening solution turbidity suppression, triglyceride compounds are preferred as glyceride compounds, fatty oils are more preferred, and fatty oils such as castor oil that are liquid at 25°C are particularly preferred.

[0412] From the viewpoint of machine developability and dampening solution turbidity suppression, unsaturated fatty acids are preferred as fatty acid compounds, more preferably unsaturated fatty acids with 8 to 30 carbon atoms, and particularly preferably unsaturated fatty acids with 12 to 24 carbon atoms.

[0413] From the viewpoint of machine developability and dampening solution turbidity suppression, aromatic diester compounds are preferred as aromatic ester compounds, and aromatic diester compounds having aliphatic rings are more preferred.

[0414] From the viewpoint of machine developability and dampening solution turbidity suppression, aliphatic ester compounds having branched alkyl groups are preferred as aliphatic ester compounds, and aliphatic ester compounds having branched alkyl groups and having 10 to 24 carbon atoms are more preferred.

[0415] From the viewpoints of UV printing durability, ink adhesion, on-machine developability, and dampening solution turbidity suppression, oils containing phosphorus atoms are preferred as oils, and more preferably oils containing phosphorus atoms.

[0416] Furthermore, from the viewpoint of machine developability and dampening solution turbidity suppression, oils containing aromatic rings are preferred as oils, oils containing two or more aromatic rings are more preferred, and oils containing two or more unfused benzene rings are particularly preferred.

[0417] From the viewpoints of UV printing durability, ink adhesion, on-machine developability, and dampening solution turbidity suppression, the clogP value of the ink is preferably 5.0 or higher, more preferably 5.50 or higher, even more preferably 5.50 or higher and 10.0 or lower, and particularly preferably 5.60 or higher and 7.00 or lower.

[0418] The clogP value is the value obtained by calculating the common logarithm logP of the partition coefficient P between 1-octanol and water. Regarding the method or software used in calculating the clogP value, well-known methods or software can be used; unless otherwise specified, the ClogP program incorporated into Cambridge Soft's ChemBioDraw Ultra 12.0 is used in this invention.

[0419] As an oiling agent, examples include, for instance, tricresyl phosphate, dimethyl(1-phenylethyl)benzene, 2,4-diphenyl-4-methyl-1-pentene, dicyclohexyl phthalate, castor oil, α-linolenic acid, tri(2-ethylhexyl) phosphate, etc.

[0420] One type of oil can be used, or two or more types can be used together. However, from the viewpoint of machine developability and dampening solution turbidity suppression, the above-mentioned image recording layer preferably contains two or more types of oils with different structures.

[0421] The content of the oil relative to the total mass of the image recording layer is preferably 0.0001% to 10.0% by mass, more preferably 0.0002% to 1.0% by mass, even more preferably 0.0005% to 0.5% by mass, and particularly preferably 0.001% to 0.05% by mass.

[0422] [Chain transfer agent]

[0423] The image recording layer may contain a chain transfer agent. The chain transfer agent used in the image recording layer of a machine-developable lithographic printing plate can be used. Specifically, the chain transfer agent described in paragraphs 0388 to 0393 of International Publication No. 2022 / 019217 is preferred.

[0424] Chain transfer agents can be added in single or multiple ways.

[0425] The content of chain transfer agent relative to the total mass of the image recording layer is preferably 0.01% to 50% by mass, more preferably 0.05% to 40% by mass, and even more preferably 0.1% to 30% by mass.

[0426] [Lipid-sensitive agent]

[0427] To improve ink adhesion, the image recording layer may contain a lipophilic agent. As a lipophilic agent, the lipophilic agent used in the image recording layer of an on-machine developing type lithographic printing plate master can be used. Specifically, the lipophilic agent described in paragraphs 0395 to 0404 of International Publication No. 2022 / 019217 is preferred.

[0428] The content of the lipophilic agent is preferably 1% to 40.0% by mass relative to the total mass of the image recording layer, more preferably 2% to 25.0% by mass, and even more preferably 3% to 20.0% by mass.

[0429] The image recording layer may contain only one type of lipophilic agent, or it may use two or more types together.

[0430] One preferred embodiment of the image recording layer used in this invention is that it contains two or more compounds as lipophilic agents.

[0431] Specifically, in the image recording layer used in this invention, from the viewpoint of balancing on-machine developability and ink adhesion, phosphonium compounds, nitrogen-containing low molecular weight compounds and ammonium-containing polymers are preferably used as lipophilic agents, and more preferably phosphonium compounds, quaternary ammonium salts and ammonium-containing polymers are used.

[0432] [Development Accelerator]

[0433] The image recording layer preferably also contains a development accelerator.

[0434] Regarding the developer, the polarity value of the SP value is preferably 6.0 to 26.0, more preferably 6.2 to 24.0, even more preferably 6.3 to 23.5, and particularly preferably 6.4 to 22.0.

[0435] SP value (solubility parameter, unit: (cal / cm³)) in this invention 3 )1 / 2 The value of the polarity term is the value of the polarity term δp in the Hansen solubility parameter. Regarding the Hansen solubility parameter, the solubility parameter imported by Hildebrand is divided into three components: dispersion term δd, polarity term δp, and hydrogen bonding term δh, and is shown in three-dimensional space. However, the polarity term δp is used in this invention.

[0436] δp[cal / cm 3 [] is the Hansen solubility parameter dipole-dipole force term, V [cal / cm] 3 ] is the molar volume, and μ[D] is the dipole moment. As δp, the following simplified form by Hansen and Beerbower is usually used.

[0437] [Formula 1]

[0438]

[0439] As a developer promoter, a hydrophilic polymer or a hydrophilic low molecular weight compound is preferred.

[0440] In this invention, hydrophilicity refers to a polar value of SP ranging from 6.0 to 26.0. Hydrophilic macromolecules are compounds with a molecular weight (weight-average molecular weight in the case of molecular weight distribution) of 3,000 or more, and hydrophilic low molecular weight compounds are compounds with a molecular weight (weight-average molecular weight in the case of molecular weight distribution) of less than 3,000.

[0441] Examples of hydrophilic polymers include cellulose compounds, with cellulose compounds being the preferred choice.

[0442] Examples of cellulose compounds include compounds in which cellulose or at least a portion of cellulose is modified (modified cellulose compounds), with modified cellulose compounds being preferred.

[0443] As a modified cellulose compound, preferred examples are compounds in which at least a portion of the hydroxyl groups of cellulose are substituted with at least one group selected from the group consisting of alkyl and hydroxyalkyl groups.

[0444] The degree of substitution of the compound in which at least a portion of the hydroxyl groups of the cellulose are substituted by at least one group selected from the group consisting of alkyl and hydroxyalkyl groups is preferably 0.1 to 6.0, more preferably 1 to 4.

[0445] As the modified cellulose compound, alkyl cellulose compounds or hydroxyalkyl cellulose compounds are preferred, and hydroxyalkyl cellulose compounds are more preferred.

[0446] Methylcellulose is a preferred example of an alkylcellulose compound.

[0447] Hydroxypropyl cellulose is a preferred example of a hydroxyalkyl cellulose compound.

[0448] The molecular weight (weight-average molecular weight in the case of a molecular weight distribution) of the hydrophilic polymer is preferably 3,000 to 5,000,000, more preferably 5,000 to 200,000.

[0449] Examples of hydrophilic low-molecular-weight compounds include diols, polyols, organic amines, organic sulfonic acids, organic aminosulfonyl compounds, organic sulfuric acid compounds, organic phosphonic acid compounds, organic carboxylic acid compounds, and betaine compounds, with polyols, organic sulfonic acids, or betaine compounds being preferred.

[0450] Examples of diol compounds include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, and other diols, as well as their ether or ester derivatives.

[0451] Examples of polyol compounds include glycerol, pentaerythritol, and tris(2-hydroxyethyl) isocyanurate.

[0452] Examples of organic amine compounds include triethanolamine, diethanolamine, monoethanolamine, and their salts.

[0453] Examples of organic sulfonic acid compounds include alkyl sulfonic acids, toluene sulfonic acids, benzene sulfonic acids, and their salts, with alkyl sulfonic acids having 1 to 10 carbon atoms being preferred.

[0454] Examples of organic aminosulfonyl compounds include alkyl aminosulfonic acids and their salts.

[0455] Examples of organic sulfuric acid compounds include alkyl sulfuric acid, alkyl ether sulfuric acid, and their salts.

[0456] Examples of organophosphonic acid compounds include phenylphosphonic acid and its salts.

[0457] Examples of organic carboxylic acid compounds include tartaric acid, oxalic acid, citric acid, malic acid, lactic acid, gluconic acid, and their salts.

[0458] Examples of betaine compounds include phosphate betaine compounds, sulfobetaine compounds, and carboxybetaine compounds, with trimethylglycine being a preferred example.

[0459] The molecular weight (weight-average molecular weight in the case of a molecular weight distribution) of the hydrophilic low molecular weight compound is preferably 100 or more and less than 3,000, more preferably 300 to 2,500.

[0460] The developer is preferably a compound with a cyclic structure.

[0461] As a cyclic structure, it is not particularly limited, and examples include glucose rings, isocyanuride rings, aromatic rings that may have heteroatoms, aliphatic rings that may have heteroatoms, etc., at least part of the hydroxyl group can be replaced. Glucose rings or isocyanuride rings are preferred.

[0462] The aforementioned cellulose compounds are examples of compounds containing a glucose ring.

[0463] Examples of compounds containing an isocyanurate ring include the aforementioned tri(2-hydroxyethyl) isocyanurate.

[0464] Examples of compounds containing aromatic rings include toluenesulfonic acid and benzenesulfonic acid.

[0465] Examples of compounds having aliphatic rings include the aforementioned alkyl sulfuric acid compounds in which the alkyl group has a cyclic structure.

[0466] Furthermore, the compounds with the cyclic structure described above preferably have hydroxyl groups.

[0467] As compounds having hydroxyl groups and cyclic structures, the above-mentioned cellulose compounds and the above-mentioned tri(2-hydroxyethyl) isocyanurate are preferred examples.

[0468] Furthermore, onium salt compounds are preferred as development promoters.

[0469] Examples of onium salt compounds include ammonium compounds and sulfonium compounds, with ammonium compounds being preferred.

[0470] Examples of onium salt compounds, i.e., developer promoters, include trimethylglycine.

[0471] Furthermore, the onium salt compounds in the aforementioned electron-accepting polymerization initiators are compounds whose SP value polarity term is not 6.0 to 26.0 and are not included in the developer accelerators.

[0472] The image recording layer may contain only one type of development promoter, or it may use two or more types together.

[0473] In this invention, one preferred method for the image recording layer is to contain two or more compounds as development promoters.

[0474] Specifically, from the viewpoint of machine developability and ink adhesion, the image recording layer preferably contains the above-mentioned polyol compound and the above-mentioned betaine compound, the above-mentioned betaine compound and the above-mentioned organic sulfonic acid compound, or the above-mentioned polyol compound and the above-mentioned organic sulfonic acid compound as a development promoter.

[0475] The content of the developer relative to the total mass of the image recording layer is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.5% by mass or more and 15% by mass or less, and more preferably 1% by mass or more and 10% by mass or less.

[0476] [Other ingredients]

[0477] The image recording layer may contain surfactants, polymerization inhibitors, higher fatty acid derivatives, plasticizers, inorganic particles, inorganic layered compounds, etc., as other components. Specifically, please refer to paragraphs 0114 to 0159 of Japanese Patent Application Publication No. 2008-284817.

[0478] <<The Formation of Image Recording Layers>>

[0479] The image recording layer in the lithographic printing plate original involved in this invention can be formed, for example, by dispersing or dissolving the desired components in a known solvent to prepare a coating liquid, as described in paragraphs 0142-0143 of Japanese Patent Application Publication No. 2008-195018, applying the coating liquid onto a support using a known method such as bar coating, and then drying it. The coating amount (solid content) of the coated and dried image recording layer varies depending on the application, but is preferably 0.3 g / m². 2 ~3.0g / m 2 Within this range, good sensitivity and good coating properties of the image recording layer can be obtained.

[0480] As a solvent, known solvents can be used. Specifically, examples include water, acetone, methyl ethyl ketone (2-butanone), cyclohexane, ethyl acetate, dichloroethane, tetrahydrofuran, toluene, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, acetylacetone, cyclohexanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether acetate, 1-methoxy-2-propanol, 3-methoxy-1-propanol, methoxymethoxyethanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, 3-methoxypropyl acetate, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, methyl lactate, ethyl lactate, etc. One solvent may be used alone, or two or more may be used in combination. The concentration of solid components in the coating solution is preferably 1% to 50% by mass.

[0481] The coating amount (solid content) of the image recording layer after coating and drying varies depending on the application. From the viewpoint of obtaining good sensitivity and good coating properties of the image recording layer, 0.3 g / m² is preferred. 2 ~3.0g / m2 .

[0482] Furthermore, the thickness of the image recording layer in the lithographic printing plate original involved in this invention is preferably 0.1 μm to 3.0 μm, more preferably 0.3 μm to 2.0 μm.

[0483] In this invention, the film thickness of each layer in the lithographic printing plate original is confirmed by making a slice cut along a direction perpendicular to the surface of the lithographic printing plate original, and observing the cross-section of the slice using a scanning electron microscope (SEM).

[0484] (Support body)

[0485] The original lithographic printing plate involved in this invention has a support.

[0486] As a support, it can be appropriately selected from known supports for lithographic printing plates.

[0487] As a support, a support having a hydrophilic surface is preferred (hereinafter also referred to as "hydrophilic support").

[0488] As the support body in this invention, it is preferable to have an oxide coating, and more preferably an aluminum plate that has been roughened and anodized by a known method. That is, the support body in this invention preferably has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate.

[0489] Furthermore, it is preferable that the support has an aluminum plate and an anodized coating of aluminum disposed on the aluminum plate, and the anodized coating is located closer to the image recording layer side than the aluminum plate. The anodized coating has micropores extending from the surface of the image recording layer side in the depth direction, and the average diameter of the micropores at the surface of the anodized coating is more than 10 nm and less than 100 nm.

[0490] Furthermore, preferably, the micropores are composed of a large-diameter pore portion and a small-diameter pore portion. The large-diameter pore portion extends from the surface of the anodic oxide coating to a depth of 10 nm to 1,000 nm. The small-diameter pore portion is connected to the bottom of the large-diameter pore portion and extends from the connection position to a depth of 20 nm to 2,000 nm. The average diameter of the large-diameter pore portion in the surface of the anodic oxide coating is 15 nm to 100 nm, and the average diameter of the small-diameter pore portion at the connection position is 13 nm or less.

[0491] Furthermore, it is preferable that the support has an oxide coating on its surface, and the oxide coating has micropores extending from the surface of the oxide coating on the image recording layer side along the depth direction. The micropores have a large-diameter portion with an average pore diameter of 15 nm to 100 nm on the surface of the oxide coating and a small-diameter portion with an average pore diameter of 15 nm or less that communicates with the bottom of the large-diameter portion and extends further along the depth direction from the communication position.

[0492] Furthermore, it is preferable that the support has an oxide coating on its surface, and that the oxide coating has micropores extending along the depth direction from the surface of the oxide coating on the image recording layer side, wherein the maximum diameter of the micropores is 1.2 to 10 times the average pore diameter of the surface relative to the average pore diameter of the oxide coating.

[0493] Figure 1 This is a schematic cross-sectional view of one embodiment of the aluminum support 12a.

[0494] The aluminum support 12a has a laminated structure consisting of an aluminum plate 18 and an anodized aluminum coating 20a (hereinafter also simply referred to as "anodized coating 20a") stacked sequentially. Furthermore, the anodized coating 20a in the aluminum support 12a is located further towards the image recording layer than the aluminum plate 18. That is, the lithographic printing plate original according to the present invention preferably has at least an anodized coating, an image recording layer, and a water-soluble resin layer sequentially on the aluminum plate.

[0495] -Anodized Coating-

[0496] The preferred embodiment of the anodic oxide coating 20a will be described below.

[0497] The anodized coating 20a is a coating formed on the surface of the aluminum plate 18 by anodizing, and the coating has ultrafine micropores 22a that are approximately perpendicular to the coating surface and uniformly distributed. The micropores 22a extend from the surface of the anodized coating 20a on the image recording layer side (the surface of the anodized coating 20a on the side opposite to the aluminum plate 18 side) along the thickness direction (aluminum plate 18 side).

[0498] In the anodized coating 20a, the average diameter (average opening diameter) of the micropores 22a on the surface of the anodized coating is preferably greater than 10 nm and less than 100 nm. From the viewpoint of balancing print durability, stain resistance, and image visual recognizability, a diameter of 15 nm to 60 nm is more preferred, 20 nm to 50 nm is even more preferred, and 20 nm to 40 nm is particularly preferred. The diameter inside the pore can be wider or narrower than the surface layer.

[0499] Excellent printing durability and image visual recognition are achieved when the average diameter exceeds 10 nm. Furthermore, excellent printing durability is also achieved when the average diameter is below 100 nm.

[0500] The average diameter of the micropore 22a is as follows: the surface of the anodized coating 20a was observed using a field emission scanning electron microscope (FE-SEM) with a magnification of 150,000x in N=4 images. The diameter of 50 micropores existing in the range of 400nm×600nm was measured in the four images obtained and the average value was obtained.

[0501] In addition, when the shape of the micropore 22a is not circular, the equivalent diameter of the circle is used. The "equivalent diameter of the circle" refers to the diameter of the circle when the shape of the opening is assumed to be a circle with the same projected area as the opening.

[0502] The shape of the micropore 22a is not particularly limited, in Figure 1 The pore 22a is generally straight and tubular (generally cylindrical), but it can also be conical, with the diameter decreasing towards the depth direction (thickness direction). Furthermore, the shape of the bottom of the pore 22a is not particularly limited; it can be curved (convex) or planar.

[0503] In the support, the micropores can be composed of a large-diameter hole extending from the surface of the anodic oxide coating to a certain depth and a small-diameter hole communicating with the bottom of the large-diameter hole and extending from the communication position to a certain depth.

[0504] For example, such as Figure 2 As shown, the aluminum support 12b may include an aluminum plate 18 and an anodized coating 20b, which has micropores 22b consisting of large-diameter holes 24 and small-diameter holes 26.

[0505] For example, the micropores 22b in the anodic oxide coating 20b can be composed of large-diameter pores 24 and small-diameter pores 26, wherein the large-diameter pores 24 extend from the surface of the anodic oxide coating to a depth of 10 nm to 1000 nm (depth D: reference). Figure 2 The small-diameter hole 26 is connected to the bottom of the large-diameter hole 24, and extends further from the connection position to a depth of 20nm to 2,000nm.

[0506] Specifically, for example, the method described in paragraphs 0107 to 0114 of Japanese Patent Application Publication No. 2019-162855 can be used.

[0507] -Manufacturing method of support body-

[0508] As a method for manufacturing the support used in this invention, for example, a manufacturing method that sequentially performs the following steps is preferred.

[0509] • Roughening process: The process of roughening the surface of aluminum sheets.

[0510] • Anodizing process: The process of anodizing the roughened aluminum sheet.

[0511] • Hole enlargement process: This process involves contacting the aluminum plate with anodized coating obtained in the anodizing process with an acidic or alkaline aqueous solution to enlarge the diameter of the micropores in the anodized coating.

[0512] The following is a detailed description of the sequence of each process.

[0513] <<Roughening Process>>

[0514] The surface roughening process is a process of roughening the surface of an aluminum sheet, including electrochemical roughening. This process is preferably performed before the anodizing process described later; however, if the surface of the aluminum sheet already has a preferred surface shape, this process is not necessary. It can be performed using the method described in paragraphs 0086 to 0101 of Japanese Patent Application Publication No. 2019-162855.

[0515] <<Anodizing Process>>

[0516] The sequence of the anodizing process is not particularly restricted as long as the aforementioned micropores can be obtained, and well-known methods can be cited.

[0517] In the anodizing process, aqueous solutions of sulfuric acid, phosphoric acid, and oxalic acid can be used as electrolytes. For example, the concentration of sulfuric acid can range from 100 g / L to 300 g / L.

[0518] The conditions for anodizing can be appropriately set according to the electrolyte used, but examples include a electrolyte temperature of 5°C to 70°C (preferably 10°C to 60°C) and a current density of 0.5 A / dm³. 2 ~60A / dm 2 (Preferred 1A / dm) 2 ~60A / dm 2 The voltage is 1V to 100V (preferably 5V to 50V), the electrolysis time is 1 second to 100 seconds (preferably 5 seconds to 60 seconds), and the coating weight is 0.1g / m². 2 ~5g / m 2 (Preferred value: 0.2g / m) 2 ~3g / m 2 ).

[0519] <<Hole Enlargement Treatment>>

[0520] The pore enlargement process refers to the process of increasing the diameter (pore size) of the micropores present in the anodized coating formed by the above-mentioned anodizing process (pore size enlargement process).

[0521] Hole enlargement can be performed by contacting the aluminum plate obtained through the above-described anodizing process with an acidic or alkaline aqueous solution. The contact method is not particularly limited; examples include immersion and spraying.

[0522] The support may have a back coating on the side opposite to the image recording layer, as needed, containing an organic polymer compound as described in Japanese Patent Application Publication No. 5-45885 or a silicon alkoxy compound as described in Japanese Patent Application Publication No. 6-35174.

[0523] (Undercoat (Intermediate Layer))

[0524] The lithographic printing plate master according to the present invention preferably has a base coating (sometimes also called an intermediate layer) between the image recording layer and the support. The base coating enhances the adhesion between the support and the image recording layer in the exposed areas and facilitates the peeling of the image recording layer from the support in the unexposed areas. Therefore, the base coating helps to improve developability while suppressing a decrease in print durability. Furthermore, in the case of infrared laser exposure, the base coating acts as a heat insulation layer, preventing the heat generated by exposure from diffusing to the support and reducing sensitivity.

[0525] Examples of compounds used in the primer layer include polymers having adsorption groups (support adsorption groups) capable of adsorbing onto the surface of the support and hydrophilic groups. To improve adhesion to the image recording layer, polymers having adsorption groups, hydrophilic groups, and crosslinking groups are preferred. The compounds used in the primer layer can be low-molecular-weight compounds or polymers. Two or more compounds can be mixed as needed for use in the primer layer.

[0526] When the compound used in the primer is a polymer, copolymers of monomers having adsorption groups, monomers having hydrophilic groups, and monomers having crosslinking groups are preferred.

[0527] The preferred adsorption groups capable of adsorbing onto the support surface are phenolic hydroxyl groups, carboxyl groups, -PO3H2, -OPO3H2, -CONHSO2-, -SO2NHSO2-, and -COCH2COCH3. The preferred hydrophilic groups are sulfonyl groups or their salts, or carboxyl salts. The preferred crosslinking groups are acryloyl groups, methacryloyl groups, acrylamide groups, methacrylamide groups, allyl groups, etc.

[0528] The polymer may have crosslinking groups introduced by the polar substituents that form the polymer and the salt of a compound containing substituents having charges opposite to those of the polar substituents and olefinic unsaturated bonds, and may further copolymerize with monomers other than those described above, preferably hydrophilic monomers.

[0529] Specifically, preferred examples include silane coupling agents having olefinic double-bond reactive groups capable of addition polymerization as described in Japanese Patent Application Publication No. 10-282679, and phosphorus compounds having olefinic double-bond reactive groups as described in Japanese Patent Application Publication No. 2-304441. Low-molecular-weight or high-molecular-weight compounds having crosslinking groups (preferably olefinic unsaturated groups), functional groups interacting with the support surface, and hydrophilic groups as described in Japanese Patent Application Publication Nos. 2005-238816, 2005-125749, 2006-239867, and 2006-215263 are also preferred.

[0530] As a more preferred compound, examples include the polymers described in Japanese Patent Application Publication Nos. 2005-125749 and 2006-188038, which are adsorbent groups that can be adsorbed onto the surface of a support, and polymers having hydrophilic groups and crosslinking groups.

[0531] The content of olefinic unsaturated groups in the polymer used in the primer layer is preferably 0.1 mmol to 10.0 mmol per 1 g of polymer, more preferably 0.2 mmol to 5.5 mmol.

[0532] The weight-average molecular weight (Mw) of the polymer used in the base coating is preferably 5,000 or more, and more preferably 10,000 to 300,000.

[0533] In addition to the compounds used in the base coating, to prevent contamination over time, the base coating may also contain chelating agents, secondary or tertiary amines, polymerization inhibitors, and compounds with amino groups or functional groups that have polymerization inhibitory capabilities, or groups that interact with the surface of the support (e.g., 1,4-diazabicyclo[2.2.2]octane (DABCO), 2,3,5,6-tetrahydroxy-p-quinone, chloroquinone, sulfophthalic acid, hydroxyethylethylenediaminetriacetic acid, dihydroxyethylethylenediaminediacetic acid, hydroxyethyliminodiacetic acid, etc.).

[0534] From the viewpoint of print durability and machine developability, the lithographic printing plate original of the present invention preferably has an intermediate layer between the support and the image recording layer, wherein the intermediate layer contains a copolymer having support adsorption groups and hydrophilic groups.

[0535] The primer layer can be applied using known methods. The preferred coating weight (solid content) is 0.1 mg / m³. 2 ~100mg / m 2 More preferably 1 mg / m 2 ~30mg / m 2 .

[0536] <Outer Coating>

[0537] The lithographic printing plate of the present invention preferably has an outer coating (sometimes referred to as a "protective layer") on the side of the image recording layer opposite to the support side.

[0538] Furthermore, the original lithographic printing plate involved in this invention preferably has a support, an image recording layer, and an outer coating layer in sequence.

[0539] In addition to inhibiting the formation of the image by blocking oxygen, the outer coating can also prevent scratches in the image recording layer and prevent ablation during high-intensity laser exposure.

[0540] Such properties of the outer coating are described, for example, in U.S. Patent No. 3,458,311 and Japanese Patent Publication No. 55-49729. As the low-oxygen permeability polymer used in the outer coating, either a water-soluble polymer or a water-insoluble polymer can be appropriately selected, and two or more can be mixed as needed. However, from the viewpoint of machine developability, a water-soluble polymer is preferred.

[0541] In this invention, a water-soluble polymer refers to a polymer whose solubility in water at 25°C exceeds 5% by mass.

[0542] Examples of water-soluble polymers used in outer coatings include polyvinyl alcohol, modified polyvinyl alcohol, polyvinylpyrrolidone, cellulose derivatives, polyethylene glycol, and poly(meth)acrylonitrile.

[0543] Furthermore, the hydrophilic polymer preferably contains at least one selected from the group consisting of modified polyvinyl alcohol and cellulose derivatives.

[0544] As a modified polyvinyl alcohol, acid-modified polyvinyl alcohol having carboxyl or sulfonyl groups is preferred. Specifically, the modified polyvinyl alcohols described in Japanese Patent Application Publication Nos. 2005-250216 and 2006-259137 can be cited as examples.

[0545] Examples of cellulose derivatives include methylcellulose, hydroxypropyl methylcellulose, and carboxymethylcellulose.

[0546] The water-soluble polymers mentioned above preferably contain polyvinyl alcohol, and more preferably contain polyvinyl alcohol with a saponification degree of 50% or more.

[0547] The aforementioned degree of saponification is preferably 60% or higher, more preferably 70% or higher, and even more preferably 85% or higher. The upper limit of the degree of saponification is not particularly limited and can be below 100%.

[0548] The degree of saponification was determined according to the method described in JIS K 6726:1994.

[0549] Furthermore, as an outer coating, a preferred method is one containing polyvinyl alcohol and polyethylene glycol.

[0550] When the outer coating of the present invention contains a water-soluble polymer, the content of the water-soluble polymer relative to the total mass of the outer coating is preferably 1% to 99% by mass, more preferably 3% to 97% by mass, and even more preferably 5% to 95% by mass.

[0551] The aforementioned outer coating preferably contains a hydrophobic polymer.

[0552] Hydrophobic polymers are polymers that can dissolve less than 5g or not at all in 100g of pure water at 125℃.

[0553] Examples of hydrophobic polymers include, for example, polyethylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, alkyl poly(meth)acrylates (e.g., poly(meth)acrylate, poly(ethyl)acrylate, poly(butyl)acrylate, etc.), and copolymers formed by combining the raw material monomers of these resins.

[0554] Furthermore, it is preferable to use polyvinylidene chloride resin as a hydrophobic polymer.

[0555] Furthermore, it is preferable to contain styrene-propylene copolymer (also known as styrene-acrylic resin) as a hydrophobic polymer.

[0556] Furthermore, from the viewpoint of machine developability, hydrophobic polymers are preferably hydrophobic polymer particles.

[0557] Hydrophobic polymers can be used alone or in combination of two or more.

[0558] When the outer coating contains a hydrophobic polymer, the content of the hydrophobic polymer relative to the total mass of the outer coating is preferably 1% to 70% by mass, more preferably 5% to 50% by mass, and even more preferably 10% to 40% by mass.

[0559] In this invention, the area percentage of the hydrophobic polymer on the surface of the outer coating is preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more.

[0560] As an upper limit for the area ratio of hydrophobic polymers on the surface of the outer coating, for example, 90% area can be cited.

[0561] The area ratio of hydrophobic polymers on the surface of the outer coating can be determined as follows.

[0562] Using a PHI nano TOFII time-of-flight secondary ion mass spectrometer (TOF-SIMS) manufactured by ULVAC-PHI, Inc., Bi ion beams (primary ions) were irradiated onto the surface of the outer coating at an accelerating voltage of 30 kV. The peak values ​​of ions (secondary ions) corresponding to the hydrophobic regions released from the surface (i.e., the regions formed by the hydrophobic polymer) were measured, thereby mapping the hydrophobic regions and measuring the peak values ​​per 100 μm. 2 The area occupied by the hydrophobic part is calculated, and the area ratio of the hydrophobic part is used as the "area ratio of the hydrophobic polymer on the surface of the outer coating".

[0563] For example, when the hydrophobic polymer is an acrylic resin, according to C6H 13 O - The peak value was measured. Furthermore, in the case where the hydrophobic polymer is polyvinylidene chloride, the peak value was determined according to C2H2Cl. + The peak value was measured.

[0564] The aforementioned area ratio can be adjusted based on factors such as the amount of hydrophobic polymer added.

[0565] From the viewpoint of suppressing development defects, the outer coating preferably contains filler.

[0566] Examples of fillers include inorganic particles, organic resin particles, and inorganic layered compounds. Among these, inorganic layered compounds are preferred. By using inorganic layered compounds, it is possible to effectively suppress re-attachment from the roller surface to the image recording layer surface.

[0567] Examples of inorganic particles include silicon dioxide particles and other metal oxide particles.

[0568] Examples of organic resin particles include cross-linked resin particles.

[0569] Inorganic layered compounds are particles with thin, flat, plate-like shapes. Examples include natural mica, synthetic mica, talc, monzocarpite, montmorillonite, saponite, lithium montmorillonite, zirconium phosphate, etc., represented by the formula: 3MgO·4SiO·H2O.

[0570] Mica compounds are preferred inorganic layered compounds. Examples of mica compounds include those with the formula: A(B, C). 2-5 D4O 10 (OH, F, O)₂ [where A is any one of K, Na, Ca, B and C are any one of Fe(II), Fe(III), Mn, Al, Mg, V, and D is Si or Al.] represents the mica group including natural mica and synthetic mica.

[0571] Within the mica group, natural mica includes muscovite, sodium mica, phlogopite, biotite, and lepidolite. Synthetic mica includes fluorophlogopite KMg3(AlSi3O4). 10 F2, potassium tetrasilica KMg 2.5 (Si4O) 10 Non-swellable mica such as F2 and sodium tetrasilica (NaMg) 2.5 (Si4O) 10 F2, Na or Li with mica (Na, Li) Mg2Li (Si4O) 10 F2, montmorillonite series Na or Li lithium montmorillonite (Na, Li) 1 / 8 Mg 2 / 5 Li 1 / 8 (Si4O) 10 Swellable mica such as F2. In addition, synthetic smectite is also used.

[0572] Among the aforementioned mica compounds, fluorine-based swelling mica is particularly useful. Specifically, swelling synthetic mica possesses a layered structure consisting of unit lattice layers approximately 10 Å to 15 Å thick (1 Å = 0.1 nm), with significant metal atom substitution within the lattice compared to other clay minerals. Consequently, the lattice layers exhibit a lack of positive charge, which is compensated for by the adsorption of Li in the interlayer spaces. + Na + Ca 2+ Mg 2+ These interlayer cations are called exchangeable cations, capable of exchanging with various cations. In particular, the interlayer cation is Li. + Na + In this state, due to the small ionic radius, the bonding between the layered lattice is weak, resulting in significant swelling through water. When shear force is applied in this state, it easily splits, forming a stable sol in water. This tendency is strong in synthetic mica with high swelling properties, making it particularly preferred for use.

[0573] From the perspective of controlling diffusion, the thinner the mica compound, the better, and the larger the planar dimensions, the better, without hindering the smoothness of the coating surface or the transmissibility of activated light. Therefore, the aspect ratio is preferably 20 or more, more preferably 100 or more, and particularly preferably 200 or more. The aspect ratio is the ratio of the major axis of the particle to its thickness, and can be measured, for example, from the projection of a microscopic photograph of the particle. The larger the aspect ratio, the greater the effect obtained.

[0574] Regarding the particle size of the mica compound, its average major diameter is preferably 0.3 μm to 20 μm, more preferably 0.5 μm to 10 μm, and particularly preferably 1 μm to 5 μm. The average thickness of the particles is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.01 μm or less. Specifically, for example, when using a swellable synthetic mica as a representative compound, a preferred method is to have a thickness of about 1 nm to 50 nm and a surface size (major diameter) of about 1 μm to 20 μm.

[0575] The content of the inorganic layered compound relative to the total mass of the outer coating is preferably 1% to 60% by mass, more preferably 3% to 50% by mass. When multiple inorganic layered compounds are used together, the total amount of the inorganic layered compound is also preferably at the above-mentioned content. Within the above range, oxygen barrier properties are improved, and good sensitivity is obtained. Furthermore, it is possible to prevent a decrease in ink adhesion.

[0576] The outer coating may contain known additives such as plasticizers for imparting flexibility, surfactants for improving coatability, and inorganic particles for controlling surface lubricity. Furthermore, the outer coating may contain grease-sensitive agents described in the image recording layer.

[0577] The outer coating is applied using a known method. The coating weight (solid content) is preferably 0.01 g / m². 2 ~10g / m 2 More preferably 0.02 g / m 2 ~3g / m 2 The preferred value is 0.02 g / m 2 ~1g / m 2 .

[0578] The thickness of the outer coating in the lithographic printing plate original involved in this invention is preferably 0.1μm to 5.0μm, more preferably 0.3μm to 4.0μm.

[0579] From the viewpoint of printing durability and development residue suppression, the lithographic printing plate original involved in the present invention preferably has an outer coating containing an inorganic layered compound on the above-mentioned image recording layer.

[0580] Furthermore, from the viewpoint of printing durability and suppression of developing residue, the lithographic printing plate original according to the present invention preferably has an outer coating containing a water-soluble polymer on the image recording layer, and the thickness of the outer coating is thicker than the thickness of the image recording layer.

[0581] The original lithographic printing plate involved in this invention may have other layers besides those described above.

[0582] As other layers, there are no particular restrictions, and known layers can be used. For example, a back coating layer can be provided on the side of the support opposite to the image recording layer side, as needed.

[0583] (Methods for making offset printing plates and offset printing methods)

[0584] A lithographic printing plate can be produced by exposing an image to the original lithographic printing plate involved in this invention and performing a developing process.

[0585] The method for manufacturing the lithographic printing plate according to the present invention preferably includes: a step of exposing the on-machine developing type lithographic printing plate master of the present invention in an image state (hereinafter also referred to as the "exposure step"); and a step of supplying at least one of the group consisting of printing ink and dampening solution to a printing press to remove the non-image portion of the image recording layer (hereinafter also referred to as the "on-machine developing step").

[0586] The offset printing method of the present invention preferably includes the following steps: an exposure step (exposure step) of exposing the on-machine developing type offset printing plate of the present invention in an image state; an on-machine developing step (on-machine developing step) of supplying at least one of the group consisting of printing ink and dampening solution to a printing press to remove the image recording layer of non-image areas to produce an offset printing plate; and a printing step (printing step) of using the obtained offset printing plate.

[0587] Furthermore, the preferred method for manufacturing the lithographic printing plate according to the present invention includes the following steps: exposing an on-machine developable lithographic printing plate master to an image using an infrared laser; and supplying an image recording layer selected from a group consisting of printing ink and dampening solution to a printing press to remove non-image areas. The on-machine developable lithographic printing plate master has a support and an image recording layer on the support. The image recording layer contains an infrared absorber capable of donating electrons to the initiator and a chromophore precursor. The energy density of the infrared laser exposure at a wavelength of 830 nm is 110 mJ / cm². 2 When the image recording layer is exposed, the brightness change ΔL of the image recording layer before and after the exposure is 3.0 or more.

[0588] Furthermore, the preferred method for manufacturing the lithographic printing plate according to the present invention is as follows: a step of exposing an on-machine developing lithographic printing plate master in an image-like manner by means of an infrared laser; and a step of supplying at least one of a group consisting of printing ink and dampening solution to a printing press to remove non-image portions of an image layer, wherein the on-machine developing lithographic printing plate master has a support and an image recording layer on the support, the image recording layer containing an initiator, an infrared absorber and a chromophore precursor, and the image recording layer satisfies the following formula L.

[0589] 2.0≤L1-L0 (Equation L)

[0590] In formula L, L1 represents the visual recognition of the image recording layer, and L0 represents the visual recognition of the layer that is the same as the image recording layer except for the chromophore precursor.

[0591] Furthermore, regarding the offset printing method involved in this invention, it is preferable to exemplify methods that further include the aforementioned printing steps in these methods.

[0592] The preferred embodiments of each step in the following description are provided regarding the method for manufacturing the lithographic printing plate and the lithographic printing method involved in this invention. Furthermore, the original lithographic printing plate involved in this invention can also be developed using a developing solution.

[0593] The following describes the exposure and on-machine development processes in the method for making a lithographic printing plate. However, the exposure process in the method for making a lithographic printing plate of the present invention is the same as the exposure process in the lithographic printing method of the present invention, and the on-machine development process in the method for making a lithographic printing plate of the present invention is the same as the on-machine development process in the lithographic printing method of the present invention.

[0594] <Exposure Process>

[0595] The method for manufacturing the lithographic printing plate according to the present invention preferably includes an exposure step of exposing the original lithographic printing plate according to the present invention in an image-like manner to form an exposed portion and an unexposed portion. The original lithographic printing plate according to the present invention is preferably exposed in an image-like manner by laser exposure using a transparent original image having line images, halftone images, etc., or by laser beam scanning based on digital data.

[0596] A light source with a wavelength of 750 nm to 1,400 nm is preferably used. As a light source with a wavelength of 750 nm to 1,400 nm, solid-state lasers and semiconductor lasers that radiate infrared radiation are preferred. Regarding the infrared laser, the output power is preferably 100 mW or higher, the exposure time per pixel is preferably less than 20 microseconds, and the irradiation energy is preferably 10 mJ / cm². 2~300mJ / cm 2 Furthermore, multi-beam laser equipment is preferred to shorten the exposure time. The exposure mechanism can be any of the following: internal drum type, external drum type, and flat plate type.

[0597] Regarding image exposure, it can be performed using conventional methods such as plate-making machines. In the case of on-machine development, image exposure can be performed on the printing press after the lithographic printing plate is mounted on the printing press.

[0598] <On-machine developing process>

[0599] The method for manufacturing the lithographic printing plate according to the present invention preferably includes an on-machine developing process on a printing press to supply at least one of the group consisting of printing ink and dampening solution to remove the image recording layer of the non-image area.

[0600] The following is an explanation of the on-machine development method.

[0601] [In-machine development method]

[0602] In the on-machine development method, the following is preferred: for the lithographic printing plate original exposed to the image, oil-based ink and water-based components are supplied on the printing press to remove the image recording layer of the non-image area to produce the lithographic printing plate.

[0603] That is, when the lithographic printing plate is directly mounted on the printing press after image exposure without any development treatment, or when the lithographic printing plate is mounted on the printing press and image exposure is performed on the printing press, followed by the supply of oil-based ink and water-based components for printing, in the initial stage of printing, in the non-image section, the uncured image recording layer is dissolved or dispersed and removed by either or both of the supplied oil-based ink and water-based components, thereby exposing the hydrophilic surface in that area. On the other hand, in the exposure section, the image recording layer cured by exposure forms an oil-based ink receiving section with an oleophilic surface. Either oil-based ink or water-based components can be supplied to the plate first, but from the perspective of preventing the water-based components from being contaminated by the components of the removed image recording layer, it is preferable to supply oil-based ink first. In this way, the lithographic printing plate is developed on the printing press and can be directly used for multi-sheet printing. As the oil-based ink and water-based components, conventional lithographic printing inks and dampening solutions are preferred.

[0604] The laser used for image exposure of the lithographic printing plate master according to the present invention preferably has a wavelength of 300 nm to 450 nm or 750 nm to 1,400 nm. In the case of a 300 nm to 450 nm light source, a lithographic printing plate master containing sensitizing pigments with high absorption in this wavelength range in the image recording layer is preferably used. For a 750 nm to 1,400 nm light source, the aforementioned light sources are preferred. As a 300 nm to 450 nm light source, a semiconductor laser is preferred.

[0605] <Printing Process>

[0606] The lithographic printing method of the present invention includes a printing step of supplying printing ink to a lithographic printing plate to print on a recording medium.

[0607] There are no particular restrictions on printing inks; various well-known inks can be used as needed.

[0608] Furthermore, oil-based inks or ultraviolet-curable inks (UV inks) are preferred as printing inks.

[0609] Furthermore, dampening solution can be supplied as needed during the aforementioned printing process.

[0610] Furthermore, the above-mentioned printing process can be carried out continuously after the above-mentioned on-machine developing process without stopping the printing press.

[0611] As a recording medium, it is not subject to special restrictions and can use known recording media as needed.

[0612] In the method for producing a lithographic printing plate from the lithographic printing plate master according to the present invention, and in the lithographic printing method according to the present invention, the entire surface of the lithographic printing plate master can be heated as needed before exposure, during exposure, and from exposure to development. This heating promotes the image formation reaction in the image recording layer, resulting in advantages such as improved sensitivity and print durability, and stabilized sensitivity. Regarding heating before development, it is preferable to perform the heating under mild conditions below 150°C. This prevents problems such as curing of non-image areas. For heating after development, it is preferable to use very strong conditions, preferably within the range of 100°C to 500°C. Within this range, sufficient image enhancement can be obtained, and problems such as support degradation and thermal decomposition of the image area can be suppressed.

[0613] Example

[0614] The present invention will be described in detail below through examples, but the present invention is not limited thereto. In these examples, unless otherwise specified, "%" and "parts" refer to "mass %" and "parts by mass," respectively. Furthermore, unless otherwise specified, in polymer compounds, molecular weight is weight-average molecular weight (Mw), and the ratio of repeating structural units is molar percentage. The weight-average molecular weight (Mw) is a value determined by gel permeation chromatography (GPC) of polystyrene.

[0615] (Examples 1-20 and Comparative Examples 1 and 2)

[0616] <Fabrication of the Support Body>

[0617] - Fabrication of Support Body (1) -

[0618] The support body 1 was manufactured by performing the following treatments (Fa) to (Fg) on ​​an aluminum plate (aluminum alloy plate) of material 1S with a thickness of 0.3 mm. In addition, a water washing process was performed between all processing steps, and the liquid was drained using clamping rollers after the water washing process.

[0619] (Fa) Alkali etching treatment

[0620] An aqueous solution of caustic soda (26% by mass) and aluminum ions (6.5% by mass) was sprayed onto an aluminum plate at 70°C for etching. Subsequently, the aluminum dissolution rate on the surface after electrochemical roughening was 5 g / m². 2 .

[0621] (Fb) was treated with an acidic aqueous solution for decontamination.

[0622] The aluminum plate was treated by spraying an acidic aqueous solution at 30°C and with a sulfuric acid concentration of 150 g / L onto it for 3 seconds.

[0623] (Fc) Electrochemical roughening treatment

[0624] An electrolyte solution containing 14 g / L hydrochloric acid, 13 g / L aluminum ions, and 3 g / L sulfuric acid was used, and electrochemical roughening treatment was performed using alternating current. The electrolyte temperature was 30°C. Aluminum chloride was added to adjust the aluminum ion concentration.

[0625] The alternating current waveform is a symmetrical sine wave with positive and negative phases, and a frequency of 50 Hz. The ratio of the anode reaction time to the cathode reaction time in one cycle of the alternating current is 1:1. The current density, expressed as the peak current value of the alternating current waveform, is 75 A / dm³. 2 Furthermore, the charge, calculated as the total charge generated by the aluminum plate participating in the anode reaction, is 450 C / dm. 2 Regarding electrolytic treatment, each time at 112.5C / dm2 The energizing process was repeated four times, with a four-second interval between each energization. A carbon electrode was used as the counter electrode for the aluminum plate.

[0626] (Fd) Alkali etching treatment

[0627] An aqueous solution of caustic soda (5% by mass) and aluminum ions (0.5% by mass) was sprayed onto an aluminum plate at 45°C for etching. The aluminum dissolution rate on the surface after electrochemical roughening was 0.2 g / m². 2 .

[0628] (Fe) was treated with an acidic aqueous solution for decontamination.

[0629] The aluminum plate was treated by spraying an acidic aqueous solution at 35°C with a sulfuric acid concentration of 170 g / L and an aluminum ion concentration of 5 g / L onto the plate for 3 seconds.

[0630] (Ff) Stage 1 Anodizing Treatment

[0631] use Figure 3 The anodizing apparatus based on direct current electrolysis, as shown, was used for the first stage of anodizing. A 150 g / L aqueous phosphoric acid solution was used as the electrolyte, and the conditions were: a liquid temperature of 35 °C and a current density of 4.5 A / dm³. 2 Anodizing was performed under specific conditions to form a coating with a thickness of 1 g / m². 2 Anodized coating.

[0632] exist Figure 3 In the anodizing apparatus 610 shown, the aluminum plate 616 is as follows: Figure 3 The aluminum plate 616 is conveyed as indicated by the middle arrow. In the power supply tank 612 containing electrolyte 618, the aluminum plate 616 is charged (+) by the power supply electrode 620. Furthermore, the aluminum plate 616 is conveyed upwards in the power supply tank 612 by roller 622, and after being reversed downwards by clamping roller 624, it is conveyed to the electrolytic treatment tank 614 containing electrolyte 626, and its direction is reversed horizontally by roller 628. Next, the aluminum plate 616 is charged (-) by electrolytic electrode 630, thereby forming an anodized coating on its surface. The aluminum plate 616 leaving the electrolytic treatment tank 614 is conveyed to subsequent processes. In the anodizing apparatus 610, roller 622, clamping roller 624, and roller 628 constitute a direction-changing mechanism. In the inter-tank section between the power supply tank 612 and the electrolytic treatment tank 614, the aluminum plate 616 is conveyed in a mountain-shaped and inverted U-shaped manner by the aforementioned rollers 622, 624, and 628. The power supply electrode 620 and the electrolysis electrode 630 are connected to the DC power supply 634.

[0633] (Fg) Stage 2 Anodizing Treatment

[0634] use Figure 3 The anodizing apparatus based on direct current electrolysis, as shown, was used for the second stage of anodizing. A 170 g / L sulfuric acid aqueous solution was used as the electrolyte, and the conditions were: a liquid temperature of 50 °C and a current density of 13 A / dm³. 2 Anodizing was performed under specific conditions to form a coating with a thickness of 2.1 g / m². 2 The anodic oxide coating was then applied. Afterwards, it was washed with water using a spray gun. The average diameter of the micropores in support 1 is 40 nm.

[0635] L on the anodized coating surface of support 1 * a * b * Lightness (L) in the color system * The value is 83.7.

[0636] -Fabrication of Support Body 2-

[0637] The support body 2 was fabricated by performing the following treatments (Fa) to (Ff) on an aluminum plate (aluminum alloy plate) of material 1S with a thickness of 0.3 mm. In addition, a water washing process was performed between all processing steps, and the liquid was drained using clamping rollers after the water washing process.

[0638] (Fa) Alkali etching treatment

[0639] An aqueous solution of caustic soda (26% by mass) and aluminum ions (6.5% by mass) was sprayed onto an aluminum plate at 70°C for etching. Subsequently, the aluminum dissolution rate on the surface after electrochemical roughening was 5 g / m². 2 .

[0640] (Fb) was treated with an acidic aqueous solution for decontamination.

[0641] The aluminum plate was treated by spraying an acidic aqueous solution at 30°C and with a sulfuric acid concentration of 150 g / L onto it for 3 seconds.

[0642] (Fc) Electrochemical roughening treatment

[0643] An electrolyte solution containing 14 g / L hydrochloric acid, 13 g / L aluminum ions, and 3 g / L sulfuric acid was used, and electrochemical roughening treatment was performed using alternating current. The electrolyte temperature was 30°C. Aluminum chloride was added to adjust the aluminum ion concentration.

[0644] The alternating current waveform is a symmetrical sine wave with positive and negative phases, and a frequency of 50 Hz. The ratio of the anode reaction time to the cathode reaction time in one cycle of the alternating current is 1:1. The current density, expressed as the peak current value of the alternating current waveform, is 75 A / dm³. 2Furthermore, the charge, calculated as the total charge generated by the aluminum plate participating in the anode reaction, is 450 C / dm. 2 Regarding electrolytic treatment, each time at 112.5C / dm 2 The energizing process was repeated four times, with a four-second interval between each energization. A carbon electrode was used as the counter electrode for the aluminum plate.

[0645] (Fd) Alkali etching treatment

[0646] An aqueous solution of caustic soda (5% by mass) and aluminum ions (0.5% by mass) was sprayed onto an aluminum plate at 45°C for etching. The aluminum dissolution rate on the surface after electrochemical roughening was 0.2 g / m². 2 .

[0647] (Fe) was treated with an acidic aqueous solution for decontamination.

[0648] The aluminum plate was treated by spraying an acidic aqueous solution at 35°C with a sulfuric acid concentration of 170 g / L and an aluminum ion concentration of 5 g / L onto the plate for 3 seconds.

[0649] (Ff) Stage 1 Anodizing Treatment

[0650] use Figure 3 The anodizing apparatus based on direct current electrolysis, as shown, was used for the first stage of anodizing. A 150 g / L aqueous phosphoric acid solution was used as the electrolyte, and the conditions were: a liquid temperature of 35 °C and a current density of 4.5 A / dm³. 2 Anodizing was performed under specific conditions to form a coating with a thickness of 1 g / m². 2 Anodized coating.

[0651] The average diameter of the micropores in support 2 is 40 nm.

[0652] The value of lightness L* in the L*a*b* color system of the anodized coating surface of support 2 is 82.4.

[0653] - Fabrication of the support (3) -

[0654] The support 3 was manufactured according to the manufacturing method of the support in Example 5 of International Publication No. 2021 / 067054.

[0655] -Fabrication of Support Body 4-

[0656] The support body 4 was manufactured by performing the following (Ja) to (Jm) processes on an aluminum plate (aluminum alloy plate) of material 1S with a thickness of 0.3 mm. In addition, a water washing process was performed between all processing steps, and the liquid was drained using clamping rollers after the water washing process.

[0657] (Ja) Mechanical roughening treatment (brushing method)

[0658] Use such as Figure 4 The apparatus shown contains a pumice suspension (specific gravity 1.1 g / cm³). 3 The material was supplied as a grinding slurry to the surface of the aluminum plate, while a rotating bristle brush was used for mechanical roughening. Figure 4 In the diagram, 31 is an aluminum plate, 32 and 34 are roller brushes (in this embodiment, bristle brushes), 33 is a grinding slurry, and 35, 36, 37 and 38 are support rollers.

[0659] In the mechanical roughening process, the median particle size (μm) of the abrasive material was set to 30μm, the number of brushes was set to 4, and the brush rotation speed (rpm) was set to 250rpm. The bristle tuft brush was made of 6 / 10 nylon, with bristle diameter of 0.3mm and bristle length of 50mm. The brush was densely tufted by drilling holes in a φ300mm stainless steel sleeve. The distance between the two support rollers (φ200mm) at the bottom of the tuft brush was 300mm. The tuft brush was pressed until the load on the drive motor that rotated the brush increased by 10kW relative to the load before pressing the tuft brush against the aluminum plate. The rotation direction of the brush was the same as the movement direction of the aluminum plate.

[0660] (Jb) Alkali etching treatment

[0661] An aqueous solution of caustic soda (26% by mass) and aluminum ions (6.5% by mass) was sprayed onto an aluminum plate at 70°C for etching. Subsequently, the aluminum dissolution rate on the surface after electrochemical roughening was 10 g / m². 2 .

[0662] (Jc) used acidic aqueous solution for decontamination treatment.

[0663] The waste liquid of nitric acid, used in the next electrochemical roughening process at a liquid temperature of 35°C, was treated by spraying the aluminum plate with a sprayer for 3 seconds as an acidic aqueous solution.

[0664] (Jd) used electrochemical roughening treatment with nitric acid aqueous solution.

[0665] Electrochemical roughening treatment was performed continuously using a 60Hz AC voltage. The electrolyte used was an aqueous solution of 10.4 g / L nitric acid with aluminum nitrate added to adjust the aluminum ion concentration to 4.5 g / L, at a temperature of 35°C. The AC power supply waveform is as follows. Figure 5The waveform shown, using a trapezoidal rectangular alternating current with a current value reaching its peak value in 0.8 msec (tp), a duty cycle of 1:1, and a carbon electrode as the counter electrode, underwent electrochemical roughening treatment. Ferrite was used as the auxiliary anode. The electrolytic cell used... Figure 6 The electrolytic cell shown. The current density, expressed as peak current, is 30 A / dm³. 2 This causes 5% of the current flowing from the power source to be diverted to the auxiliary anode. (Electricity (C / dm³)) 2 The total charge during the reaction with the aluminum plate as the anode is 185 C / dm. 2 .

[0666] (Je) Alkali etching treatment

[0667] An aqueous solution of caustic soda (27% by mass) and aluminum ions (2.5% by mass) was sprayed onto an aluminum plate at 50°C using a sprayer for etching. The aluminum dissolution rate was 3.5 g / m². 2 .

[0668] (Jf) used acidic aqueous solution for decontamination treatment.

[0669] The aluminum plate was treated by spraying an acidic aqueous solution at 30°C with a sulfuric acid concentration of 170 g / L and an aluminum ion concentration of 5 g / L onto the plate for 3 seconds.

[0670] (Jg) underwent electrochemical roughening treatment using hydrochloric acid aqueous solution.

[0671] Electrochemical roughening treatment was performed continuously using an AC voltage of 60 Hz. The electrolyte used was an aqueous solution of 6.2 g / L hydrochloric acid with added aluminum chloride to adjust the aluminum ion concentration to 4.5 g / L at a temperature of 35°C. The AC power supply waveform is as follows. Figure 5 The waveform shown, using a trapezoidal rectangular alternating current with a current value reaching its peak value in 0.8 msec (tp), a duty cycle of 1:1, and a carbon electrode as the counter electrode, underwent electrochemical roughening treatment. Ferrite was used as the auxiliary anode. The electrolytic cell used... Figure 6 The electrolytic cell shown is operated at a current density of 25 A / dm³, expressed as the peak current. 2 The amount of electricity generated during hydrochloric acid electrolysis (C / dm³) 2 The total charge during the reaction with the aluminum plate as the anode is 63 C / dm. 2 .

[0672] (Jh) Alkali etching treatment

[0673] An aqueous solution of caustic soda (5% by mass) and aluminum ions (0.5% by mass) was sprayed onto an aluminum plate at 60°C using a sprayer for etching. The aluminum dissolution rate was 0.2 g / m³. 2 .

[0674] (Ji) used acidic aqueous solution for decontamination treatment.

[0675] The waste liquid (sulfuric acid concentration of 170 g / L and aluminum ion concentration of 5 g / L) generated during the anodizing process at a liquid temperature of 35°C was treated by spraying an acidic aqueous solution onto the aluminum plate for 4 seconds.

[0676] (Jj) Stage 1 Anodizing Treatment

[0677] use Figure 3 The anodizing apparatus based on direct current electrolysis, as shown, was used for the first stage of anodizing. A 170 g / L sulfuric acid aqueous solution was used as the electrolyte, and the conditions were: a liquid temperature of 50 °C and a current density of 30 A / dm³. 2 Anodizing was performed under specific conditions to form a coating with a thickness of 0.3 g / m². 2 Anodized coating.

[0678] (Jk) Hole Enlargement Treatment

[0679] The aluminum plate that had undergone anodizing was immersed in a caustic soda aqueous solution with a concentration of 5% by mass and an aluminum ion concentration of 0.5% by mass at 40°C for 3 seconds to perform a hole-enlarging treatment.

[0680] (Jl) Stage 2 Anodizing Treatment

[0681] use Figure 3 The anodizing apparatus based on direct current electrolysis, as shown, was used for the second stage of anodizing. A 170 g / L sulfuric acid aqueous solution was used as the electrolyte, and the conditions were: a liquid temperature of 50 °C and a current density of 13 A / dm³. 2 Anodizing was performed under specific conditions to form a coating with a thickness of 2.1 g / m². 2 Anodized coating.

[0682] (Jm) Hydrophilic treatment

[0683] To ensure the hydrophilicity of the non-image area, a silicate treatment was performed by immersing the aluminum plate in a 2.5% by mass sodium silicate solution (No. 3) for 7 seconds at 50°C. The Si deposition rate was 8.5 mg / m². 2 The average diameter of the micropores is 30 nm.

[0684] The value of lightness L* in the L*a*b* color system of the anodized coating surface of support 4 is 72.3.

[0685] <Formation of the base coating>

[0686] -Formation of base coating 1-

[0687] A primer coating liquid (1) with the following composition is applied to the support to achieve a dry coating weight of 0.03 g / m². 2 This forms the base coating 1.

[0688] <<Primer Coating Liquid (1)>>

[0689] • Aqueous solution of polyacrylic acid (40% by weight, Jurymer AC-10S, manufactured by TOAGOSEI CO., LTD.): 3.0 parts

[0690] Water: 27.0 parts

[0691] -Formation of base coating 2-

[0692] Apply a primer coating liquid (2) with the following composition to the support to achieve a dry coating weight of 0.1 g / m². 2 This forms the base coating 2.

[0693] <Coating liquid for primer layer (2)>

[0694] • Compound for primer coating (3): 0.010 parts

[0695] • CHELEST 400 (chelating agent; manufactured by CHELEST CORPORATION): 0.0280 parts

[0696] • CHELEST 3EAF (chelating agent; manufactured by CHELEST CORPORATION): 0.0499 parts

[0697] • Surfactant (EMALEX (registered trademark) 710, manufactured by NIHON EMULSION Co., Ltd.): 0.00159 parts

[0698] • Preservative (Biohope L, K·I Chemical Industry Co., LTD.): 0.00149 parts

[0699] Water: 2,8219 portions

[0700] [Chemical Formula 22]

[0701]

[0702] -Formation of base coating 3-

[0703] On the support, a primer coating liquid (3) with the following composition is applied to achieve a dry coating weight of 26 mg / m². 2 This forms the base coating 3.

[0704] <<Undercoat layer liquid (3)>>

[0705] • Compound (2) for primer coating (structure below): 0.013 parts

[0706] Hydroxyethyliminodiacetic acid: 0.005 parts

[0707] • Tetrasodium ethylenediaminetetraacetate: 0.005 parts

[0708] Polyoxyethylene lauryl ether: 0.0003 parts

[0709] Water: 3.15 parts

[0710] [Chemical Formula 23]

[0711]

[0712] The values ​​on the lower right side of the brackets of each structural unit in the above-mentioned primer coating compound (2) represent the mass ratio, and the values ​​on the lower right side of the brackets of the ethoxy group represent the number of repetitions.

[0713] <Formation of Image Recording Layers>

[0714] -Formation of image recording layers 1-14-

[0715] For image recording layers 1 to 14, each image recording layer coating solution (image recording layer coating solution (1) to (13)) with the following composition was applied by a rod, and dried at 110°C for 40 seconds to prepare samples with a dry weight of 0.8 g / m². 2 Image recording layer.

[0716] <<Image recording layer coating solution (1)~(14)>>

[0717] ·1-Propanol: 5,000 parts

[0718] ·2-Butanone: 2,500 parts

[0719] ·1-Methoxy-2-propanol: 4,200 parts

[0720] γ-Butyrolactone: 0.1500 parts

[0721] Water: 0.6600 parts

[0722] • Polymer particles (20% by mass) as recorded in Table 1: Amounts recorded in Table 1

[0723] ·KLUCEL E ※1 0.0070 copies

[0724] BYK 336 ※2 0.0720 copies

[0725] • Iodine salt (I-1): 0.9500 parts

[0726] • Infrared absorber (IR-1): 0.4500 parts

[0727] • Polymerizable compound (M-1): 0.4250 parts

[0728] • Polymerizable compound (M-2): 0.2125 parts

[0729] • Colorant (S-1): 0.0200 parts

[0730] ※1: Klucel E refers to hydroxypropyl cellulose that is available from Hercules.

[0731] ※2: A xylene / methoxypropyl acetate solution containing 25% by mass of modified polydimethylsiloxane copolymer (manufactured by BYK-Chemie).

[0732] [Chemical Formula 24]

[0733]

[0734] [Chemical Formula 25]

[0735]

[0736] M-1 is a urethane acrylate (40% by mass 2-butanone solution) obtained by reacting DESMODUR (registered trademark) N100 (manufactured by Bayer Corp., Milford, CT) with hydroxyethyl acetate and pentaerythritol triacrylate in a molar ratio of about 1:1.5:1.5.

[0737] M-2 is a bisphenol A ethoxylate (10 moles of ethylene oxide (EO) adduct) diacrylate (40% by mass 2-butanone solution).

[0738] -Formation of image recording layer 15-

[0739] Regarding image recording layer 15, a coating solution (15) with the following composition was applied by bar coating and dried at 120°C for 40 seconds to produce a dried weight of 1.0 g / m². 2 Image recording layer 15.

[0740] <<Coating solution for image recording layer (15)>>

[0741] • Infrared absorber (IR-2 below): 0.0200 parts

[0742] • Infrared absorber (IR-3 below): 0.0050 parts

[0743] • Colorant (S-2 below): 0.0300 parts

[0744] • Colorant (S-3 below): 0.0120 parts

[0745] • Onium-based polymerization initiator (I-2 below): 0.0980 parts

[0746] • Borate compound (sodium tetraphenylborate (TPB)): 0.0270 parts

[0747] • Polymerizable compound (M-3 below): 0.4363 parts

[0748] Fluorinated surfactant (1) (structure below): 0.004 parts

[0749] • Anionic surfactant (A-1 below, 30%): 0.1620 parts

[0750] ·2-Butanone: 6,000 parts

[0751] ·1-Methoxy-2-propanol: 3,7000 parts

[0752] Methanol: 2,300 parts

[0753] • Polymer particles (R-1, 20% by mass): 2.2500 parts (In addition, the amounts recorded in Table 1 are converted to the amounts in the image recording layer coating solutions (1) to (14).)

[0754] [Chemical Formula 26]

[0755]

[0756] [Chemical Formula 27]

[0757]

[0758] [Chemical Formula 28]

[0759]

[0760] [Chemical Formula 29]

[0761]

[0762] [Chemical Formula 30]

[0763]

[0764] <Synthetic methods of polymeric compound M-3>

[0765] A mixed solution of Takenate D-160N (polyisocyanate-trimethylolpropane adduct, manufactured by Mitsui Chemicals, Inc., 4.7 parts), ARONIX M-403 (manufactured by TOAGOSEI CO., LTD., in an amount where the NCO value of Takenate D-160N and the hydroxyl value of ARONIX M-403 are in a 1:1 ratio), tert-butylbenzoquinone (0.02 parts), and methyl ethyl ketone (11.5 parts) was heated to 65°C. NEOSTANN U-600 (bismuth-based polycondensation catalyst, manufactured by NITTO KASEI CO., LTD., 0.11 parts) was added to the reaction solution, and the mixture was heated at 65°C for 4 hours. The reaction solution was cooled to room temperature (25°C), and methyl ethyl ketone was added, thereby synthesizing a 70% by weight solution of urethane acrylate (polymeric M-3). Molecular weight fractionation of urethane acrylate solutions was performed using a reusable GPC (equipment: LC908-C60, columns: JAIGEL-1H-40 and 2H-40 (manufactured by Japan Analytical Industry)) and an eluent of tetrahydrofuran (THF). The weight-average molecular weight was 20,000.

[0766] <Formation of the outer coating>

[0767] -Formation of outer coating 1-

[0768] After bar-coating the image recording layer with the following outer coating solution (1), it was dried at 120°C for 60 seconds to form a dry coating weight of 0.1 g / m². 2 The outer coating 1.

[0769] <<Topical Coating Solution (1)>>

[0770] • Inorganic layered compound dispersion (1) (below): 0.625 parts

[0771] • Hydrophilic polymer (1) (structure below, Mw: 30,000): 0.03 parts

[0772] METOLOSE SM04: 0.0600 copies

[0773] • RAPISOL A-80 (80% aqueous solution): 0.0063 parts

[0774] Water: 2.0 parts

[0775] <<Preparation of Inorganic Layered Compound Dispersion (1)>>

[0776] 6.4 parts of synthetic mica SOMASIF ME-100 (manufactured by Co-op Chemical Co., Ltd.) were added to 193.6 parts of ion-exchanged water, and the mixture was dispersed using a homogenizer until the volume average particle size (laser scattering method) reached 3 μm. The aspect ratio of the obtained dispersed particles was greater than 100.

[0777] -Formation of outer coating 2-

[0778] An outer coating liquid (2) with the following composition is applied to the image recording layer to achieve a dry film thickness of 1.0 μm, and then dried at 100°C for 60 seconds to form an outer coating 2.

[0779] <External Coating Liquid (2)>

[0780] • POVAL PVA105 (polyvinyl alcohol, saponification degree = 98mol%~99mol%, manufactured by KURARAY CO., LTD.): 1.0 parts by weight

[0781] • PEG4000 (manufactured by Tokyo Chemical Industry Co., Ltd.): 0.39 parts by weight

[0782] Surfactant (RAPISOL A-80, manufactured by NOF CORPORATION): 0.01 parts by weight

[0783] Water: Amounting to 10 parts by mass

[0784] As described in Table 1, each support, base coating, image recording layer and outer coating as needed were formed to obtain the original lithographic printing plates of Examples 1 to 20 and Comparative Examples 1 and 2, respectively.

[0785] (Evaluation of printing durability)

[0786] Using a Kodak Magnus800 Quantum equipped with an infrared semiconductor laser, the original lithographic printing plate was exposed (equivalent to an irradiation energy of 110 mJ / cm²) at an output power of 27 W, an external drum speed of 450 rpm, and a resolution of 2,400 dpi (dots per inch, 1 inch is 2.54 cm). 2 This makes the exposed image include a solid image and an amplitude modulation screen with 10% dots.

[0787] The obtained exposed original was not developed and was directly mounted onto the cylinders of a Heidelberger Druckmaschinen AG printing press of SX-74 size. A 100L dampening solution circulation tank with a built-in nonwoven filter and temperature control was connected to the printing press. 80L of 3.5% dampening solution S-Z1 (manufactured by Fujifilm Corporation) was loaded into the circulation tank, and UV CORE TYPE-AJ ink GEM (manufactured by T&KTOKA Corporation) was used as the printing ink. After supplying the dampening solution and ink through a standard automatic printing start-up method, 1,000 sheets were printed on SHIRAOI paper (48.5kg ream, manufactured by Nippon Paper Industries Co., Ltd.) at a printing speed of 10,000 sheets per hour.

[0788] Next, printing was carried out. As the number of prints increased, the image area gradually wore down, resulting in a decrease in ink concentration on the printed material. Printing durability was evaluated as follows: the number of prints at which the dot area ratio of 10% halftone dots in the printed material, measured using an eXact spectrochromometer (manufactured by X-Rite), decreased by 3% compared to the measurement value of the 1,000th print was taken as the final print count. Relative printing durability was evaluated based on the following criteria, with 50,000 prints set as 100. A higher value indicates better printing durability.

[0789] Relative print durability = (Number of prints of the original offset printing plate) / 50,000) × 100

[0790] -Evaluation Criteria-

[0791] 5: The value for relative print durability exceeds 110.

[0792] 4: The value of relative printability is greater than 100 and less than 110.

[0793] 3: The value of relative printability is greater than 90 and less than 100.

[0794] 2: The relative printability value is greater than 75 and less than 90.

[0795] 1: The relative printability value is 75 or below.

[0796] (In-machine evaluation of developer residue inhibition (developer residue inhibition))

[0797] Using a LuxelPLATESETTER T-6000III manufactured by Fujifilm Corporation and equipped with an infrared semiconductor laser, the obtained lithographic printing plate master was exposed at an outer drum speed of 1,000 rpm, laser output of 70%, and a resolution of 2,400 dpi. The exposed image includes a solid image and a 50% dot map with 20 μm frequency-modulated halftone dots.

[0798] The obtained exposed originals were not developed and were directly mounted on the printing cylinder of the LITHRONE26 printing press manufactured by KOMORI Corporation. Using a dampening solution of Ecolity-2 (manufactured by Fujifilm Corporation) / tap water = 2 / 98 (volume ratio) and Space Color Fusion G yellow ink (manufactured by DIC GRAPHICS CORPRATION.), the dampening solution and ink were supplied to the press for on-machine development using the standard automatic printing start method of the LITHRONE26. After that, 500 sheets were printed on TOKUBISHI coated paper (manufactured by Mitsubishi Paper Mills Limited, ream weight: 76.5kg) at a printing speed of 10,000 sheets per hour.

[0799] After replacing the plate with a new one, the above on-machine developability evaluation was repeated three times to transfer the developing residue on the dampening roller in the printing press onto cellophane tape and attach it to OK Top Coat paper (manufactured by Oji Paper Co., Ltd., model: OK Top Coat+). The cyan density D (C) was measured using an X-Rite color density meter (manufactured by X-Rite Corporation).

[0800] -Evaluation Criteria-

[0801] Evaluation 1: D(C) is less than 0.1

[0802] Evaluation 2: D(C) is above 0.1 and less than 0.3.

[0803] Evaluation 3: D(C) is 0.3 or higher and less than 0.5.

[0804] Evaluation 4: D(C) is 0.5 or higher and less than 1.0.

[0805] Rating 5: D (C) is 1.0 or higher.

[0806] [Table 1]

[0807]

[0808] The details of each polymer particle recorded in Table 1 are shown in Table 2.

[0809] [Table 2]

[0810]

[0811] <Synthesis Example 1 (Synthesis of R-1)>

[0812] Under a nitrogen atmosphere, 218 g of 1-propanol and 5 g of polyethylene glycol monomethyl ether acrylate (Mn=232, number of repeating units in the polyethylene oxide structure: 3) were added to a three-necked flask, and the mixture was heated to 75 °C. 10 g of styrene and 35 g of acrylonitrile were mixed, and a liquid containing 0.35 g of azobisisobutyronitrile (0.3 mol% relative to the monomer) was added dropwise over 2 hours. The reaction was then carried out at 75 °C for 2 hours. The median particle size (R-1) obtained by dynamic light scattering was 75 nm.

[0813] <Synthesis Examples 2-10: Synthesis of R-2 to R-10>

[0814] The mass ratio of each structural unit, the molecular weight of polyethylene glycol monomethyl ether acrylate, and the amount of azobisisobutyronitrile added were changed to the amounts recorded in Table 2. Otherwise, each particle (R-2 to R-10) was synthesized in the same manner as R-1.

[0815] The abbreviations for each structural unit recorded in Table 2 are structural units formed from the parts shown below.

[0816] St: Styrene

[0817] AN: Acrylonitrile

[0818] PEGMA: Polyethylene glycol monomethyl ether acrylate

[0819] The results shown in Table 1 demonstrate that the lithographic printing plate originals involved in the embodiments exhibit excellent printing durability and developer residue suppression.

[0820] The entire contents of the invention of Japanese Patent Application No. 2023-187017, filed on October 31, 2023, are incorporated herein by reference.

[0821] All documents, patent applications and technical specifications set forth in this specification are incorporated herein by reference to the same extent as the individual documents, patent applications and technical specifications specifically and individually described and incorporated by reference.

[0822] Symbol Explanation

[0823] 12a, 12b - Aluminum support; 14 - Primer coating; 16 - Image recording layer; 18 - Aluminum plate; 20a, 20b - Anodized coating; 22a, 22b - Micropores; 24 - Large-diameter hole; 26 - Small-diameter hole; D - Depth of large-diameter hole; 30 - Original plate for lithography; 31 - Aluminum plate; 32, 34 - Roller brush; 33 - Grinding slurry; 35, 36, 37, 38 - Support rollers; 50 - Main electrolytic cell; 51 - AC power supply; 52 - Radial drum roller; 53a, 53b - Main electrode; 54 - Electrolyte supply port; 55 - Electrolyte; 56 - Auxiliary anode; 57 - Electrolyte channel; 58 - Auxiliary anode; 60 - Auxiliary anode Tank, 610 - Anodizing treatment device, 612 - Power supply tank, 614 - Electrolytic treatment tank, 616 - Aluminum plate, 618, 26 - Electrolyte, 620 - Power supply electrode, 622, 628 - Rollers, 624 - Clamping roller, 630 - Electrolytic electrode, 632 - Tank wall, 634 - DC power supply, W - Aluminum plate, S - Liquid supply direction, Ex - Electrolyte discharge direction, ta - Anode reaction time, tc - Cathode reaction time, tp - Time from 0 to peak current, Ia - Peak current on the anode circulation side, Ic - Peak current on the cathode circulation side, AA - Anode reaction current of the aluminum plate, CA - Cathode reaction current of the aluminum plate.

Claims

1. An on-machine developing type lithographic printing plate master, comprising a support and an image recording layer on the support, The image recording layer contains polymeric compounds and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles is 42% by mass or more and 90% by mass or less relative to the total mass of the image recording layer. After applying osmium staining to the thickness direction section of the original lithographic printing plate, the cross-sectional image obtained by observation through a scanning electron microscope is binarized into stained and unstained portions. The standard deviation of the area ratio of the unstained portion in the cross-sectional image is less than 6.

2. The on-machine developing type lithographic printing plate original according to claim 1, wherein, The polymer particles are polymer particles having structural units formed from acrylonitrile compounds and polyepoxide structures.

3. The on-machine developing type lithographic printing plate original according to claim 2, wherein, The polymer particles are polymer particles having structural units formed by aromatic vinyl compounds, structural units formed by acrylonitrile compounds, and structural units containing polyoxyalkylene structures.

4. The on-machine developing type lithographic printing plate original according to claim 2, wherein, The polyepoxide structure is a polyepoxide structure.

5. The on-machine developing type lithographic printing plate original according to claim 2, wherein, The number of repeating units in the polyepoxide structure is 3 to 10.

6. The on-machine developing type lithographic printing plate original according to claim 2, wherein, The content of structural units containing polyepoxide structures in the polymer particles is 10% by mass or more relative to the total mass of the polymer.

7. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The content of polymer particles is 45% by mass or more relative to the total mass of the image recording layer.

8. The on-machine developing type lithographic printing plate original according to claim 7, wherein, The content of polymer particles is 55% by mass or more relative to the total mass of the image recording layer.

9. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The median particle size of the polymer particles is 50 nm to 100 nm.

10. The on-machine developing type lithographic printing plate original according to claim 9, wherein, The median particle size of the polymer particles is 50 nm to 90 nm.

11. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The polymeric compounds include oligomers.

12. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, An intermediate layer is further provided between the support and the image recording layer, the intermediate layer containing a copolymer having support adsorption groups and hydrophilic groups.

13. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The image recording layer also has an outer coating containing an inorganic layered compound.

14. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The image recording layer also has an outer coating containing a water-soluble polymer, the thickness of which is greater than the thickness of the image recording layer.

15. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The surface of the support has an oxide coating, and the oxide coating has micropores extending along the depth direction from the surface of the oxide coating on the image recording layer side. The micropores have: large-diameter pores with an average pore diameter of 15 nm to 100 nm on the surface of the oxide coating; and small-diameter pores that communicate with the bottom of the large-diameter pores and extend further along the depth direction from the communication position, with an average pore diameter of less than 15 nm.

16. The on-machine developing type lithographic printing plate original according to claim 1 or 2, wherein, The support has an oxide coating on its surface, and the oxide coating has micropores extending along the depth direction from the surface of the oxide coating on the image recording layer side. The maximum diameter inside the micropore is 1.2 to 10 times the average pore diameter of the surface relative to the average pore diameter of the oxide coating surface.

17. An on-machine developing type lithographic printing plate master, comprising a support and an image recording layer on the support, The image recording layer contains polymeric compounds and polymer particles. The median particle size of the polymer particles is 50 nm to 120 nm. The content of the polymer particles is 42% by mass or more and 90% by mass or less relative to the total mass of the image recording layer. The polymer particles are polymer particles that have at least 65% by mass of structural units formed of acrylonitrile compounds relative to the total mass of the polymer particles and at least 10% by mass of structural units containing polyepoxide structures.

18. A method for producing a lithographic printing plate, comprising: The process of exposing the original on-machine developing type lithographic printing plate as described in claim 1 or 17 in an image-like manner; and A process of supplying at least one of the group consisting of printing ink and dampening solution to remove the image recording layer of a non-image section on a printing press.

19. A method for offset printing, comprising: The process of exposing the original on-machine developing type lithographic printing plate as described in claim 1 or 17 in an image-like manner; The process of supplying at least one of a group consisting of printing ink and dampening solution to a printing press to remove the image recording layer (excluding the image portion) to create a lithographic printing plate; and The process of printing using the obtained lithographic printing plate.

Citation Information

Patent Citations

  • JP1980049729B2

  • Photosolubilizable composition

    JP1986166544A

  • Electric discharge machine

    JP1988120037A

  • Heating cooking device

    JP1988220023A

  • Space heater with floor heating

    JP1988220025A