A high-carbon self-lubricating graphite steel cutting tool material and its preparation method
By preparing ultra-high carbon self-lubricating graphite steel tool materials, and utilizing W, Mo, and V alloying and iron-mold sand-coating cooling processes, the material performance and cost issues of aluminum alloy cutting tools under complex working conditions were solved. This achieved a balance between high hardness, wear resistance, and self-lubricating properties, extending tool life and reducing production costs.
Patent Information
- Application Number
- CN202611036570.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-07-13
AI Technical Summary
Existing aluminum alloy cutting tool materials suffer from low material performance, high production costs, and difficulty in achieving high hardness, high wear resistance, and self-lubricating properties under complex working conditions.
Using ultra-high carbon self-lubricating graphite steel cutting tool material, high-hardness WC, MoC, and VC hard carbides are formed by adding W, Mo, and V alloying elements. Combined with iron mold sand cooling process and multiple small deformation forging, a self-lubricating graphite steel cutting tool with tempered martensite matrix and fine graphite particles is prepared.
It achieves high hardness, high wear resistance, low thermal friction coefficient, excellent thermal stability and impact resistance, solves the problem of tool sticking in the cutting process of aluminum alloys by traditional tool materials, extends tool life and reduces production costs.
Smart Images

Figure CN122522129B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cutting tool material preparation technology, specifically relating to an ultra-high carbon self-lubricating graphite steel cutting tool material and its preparation method. Background Technology
[0002] Aluminum alloys, with their advantages of low density, high specific strength, corrosion resistance, and ease of forming, are widely used in core fields such as aerospace, automotive manufacturing, and rail transportation. As high-end equipment manufacturing moves towards lightweighting and precision, stringent requirements are being placed on the accuracy, surface quality, processing efficiency, and tool life of aluminum alloy components during machining. Due to their inherent softness, high plastic deformation capacity, rapid thermal conductivity, and unstable cutting friction coefficient, aluminum alloys are prone to strong cutting friction and plastic adhesion effects under conditions such as high-speed dry cutting, precision mirror milling, complex curved surface forming cutting, and intermittent variable load cutting. This leads to tool sticking during aluminum alloy machining, resulting in built-up edge formation on the tool edge. This not only directly scratches the machined surface of the aluminum alloy workpiece, causing surface roughness, burrs, scratches, and other appearance defects, but also causes quality problems such as dimensional deviations and out-of-tolerance geometrical accuracy. Simultaneously, continuous tool sticking wear accelerates tool edge failure, significantly shortens tool life, and increases machining costs.
[0003] Currently, the main materials used for aluminum alloy cutting tools in the industry are high-speed steel and cemented carbide. High-speed steel tools have advantages such as excellent toughness, impact fracture resistance, easy grinding and forming, and low cost, and are widely used in low-speed, light-load aluminum alloy cutting scenarios. However, high-speed steel has relatively low overall hardness, poor wear resistance, and poor high-temperature mechanical properties. During continuous cutting of aluminum alloys, the accumulation of a large amount of cutting heat in the cutting zone causes the tool edge temperature to rise sharply, leading to high-temperature softening of the cutting edge, resulting in abrasive wear, adhesive wear, and ultimately failure problems such as edge dulling and chipping. Cemented carbide tools are prepared by powder metallurgy and have the characteristics of high hardness, excellent wear resistance at both room temperature and high temperature, good thermal stability, and high compressive strength. Compared with high-speed steel tools, they can effectively improve the machining efficiency and tool life of high-speed aluminum alloy cutting. However, cemented carbide materials have disadvantages such as high brittleness, low fracture toughness, and poor impact and vibration resistance. Under complex working conditions such as intermittent cutting and variable load impact cutting of aluminum alloys, the tool edge is easily subjected to alternating impact loads, frequently resulting in edge chipping. In addition, the raw materials for cemented carbide are expensive, the preparation process is complex, and the forming and processing are difficult, resulting in high production costs.
[0004] In summary, current aluminum alloy cutting tool materials and manufacturing technologies generally suffer from low material performance, high production costs, and difficulty in applying them to complex aluminum alloy cutting conditions. To address these technological bottlenecks in aluminum alloy cutting tools, this invention proposes a graphite steel material for aluminum alloy cutting tools and its manufacturing method that combines high hardness, high wear resistance, high thermal stability, and excellent self-lubricating and anti-sticking properties, providing a new material option for aluminum alloy cutting tools. Summary of the Invention
[0005] Therefore, the purpose of this invention is to provide an ultra-high carbon self-lubricating graphite steel cutting tool material and its preparation method, so as to solve the problems of low life and high cost of existing aluminum alloy cutting tool materials.
[0006] To achieve the above objectives, the following technical solution is adopted: A high-carbon self-lubricating graphite steel cutting tool material, comprising the following components by weight percentage: C: 1.2-2.0%; Cr: 1.0-2.0%; Mo: 0.5-1.0%; V: 0.2-0.5%; W: 0.5-2.0%; Si: 0.3-1.5%; The balance consists of Fe and unavoidable trace impurity elements.
[0007] Preferably, the C content is 1.3-1.6% and the Si content is 0.5-1.0%.
[0008] A method for preparing an ultra-high carbon self-lubricating graphite steel cutting tool material, comprising the following steps: S1: Weigh pig iron, scrap steel, ferrochrome, ferromolybdenum, ferrovanadium, ferrotungsten, and ferrosilicon according to the following mass percentages: C: 1.2-2.0%, Cr: 1.0-2.0%, Mo: 0.5-1.0%, V: 0.2-0.5%, W: 0.5-2.0%, Si: 0.3-1.5%, with the balance being Fe and unavoidable trace impurities. Add them to a medium-frequency induction furnace for smelting, thoroughly refining and removing impurities, removing gases and inclusions from the molten steel to obtain ultra-high carbon alloy steel liquid. S2: Casting is carried out using an iron mold with sand coating process. The thickness of the sand coating layer is adjusted according to the thickness of the tool blank to be prepared. The thicker the tool blank, the thinner the sand coating layer, in order to ensure its cooling rate. The thinner the tool blank, the thicker the sand coating layer, to slow down the cooling rate, avoid the risk of abnormal graphite precipitation in the matrix induced by silicon, and ensure that the matrix structure of the casting is dense, thus obtaining the as-cast tool blank. S3: The tool blank is heated and held at a high temperature before being forged at high temperature using a multi-fire and multi-forging process. Through multiple small deformation forgings, the continuous network of carbides in the as-cast structure is fully broken down, eliminating structural segregation, refining the matrix grains, and improving the material density and structural uniformity. S4: After cooling the forged tool blank to room temperature, it is sent to a heat treatment furnace for graphitization annealing below the eutectoid temperature and then slowly cooled to room temperature in the furnace. This allows the unstable carbides that have been broken down after forging to be fully decomposed and separated, forming spherical graphite particles with uniform size and a particle size of 1-2 μm, while stable hard carbides such as WC, MoC, and VC are completely retained in the matrix. S5: The tool blank is heated and held at a certain temperature, then quickly quenched in oil and tempered to obtain a self-lubricating graphite steel tool material with a microstructure of tempered martensite and fine graphite and hard carbides distributed on it.
[0009] Preferably, in step S1, the melting temperature is controlled at 1550-1650℃.
[0010] Preferably, in step S2, the thickness of the sand covering layer is controlled at 3-15mm.
[0011] Preferably, in step S3, the forging temperature range is 1000-1100℃, and the single forging reduction is controlled at 10-25%.
[0012] Preferably, in step S4, the annealing temperature is controlled at 600-750℃ and the holding time is 4-10h.
[0013] Preferably, in step S5, the tool blank is heated to a two-phase temperature of 780-920℃ and held for 0.5-1h, then quickly quenched in oil and tempered at 300-500℃ for 1-5h.
[0014] The beneficial effects of this invention are: 1. This invention adds W, Mo, and V alloying elements to form WC, MoC, and VC hard carbides with high hardness and high thermal stability, ensuring the tool matrix has high wear resistance and resistance to high-temperature softening. 2. The addition of silicon provides the conditions for graphitization precipitation, ultimately achieving the dual properties of high hardness and wear resistance of the matrix and friction reduction and self-lubrication of graphite particles, solving the problem that traditional tool materials cannot simultaneously achieve both hardness and self-lubricating performance. 3. The iron mold sand-coating cooling process was applied to the preparation of graphite steel for aluminum alloy cutting tools. By dynamically adjusting the thickness of the 3-15mm sand coating layer according to the thickness of the billet, the cooling rate was improved, which solved the problem of graphite precipitation during solidification caused by the presence of silicon in ultra-high carbon steel, and provided conditions for the subsequent precipitation of small-scale high-density graphite spheres. 4. Multiple small deformation forging fragmentation of network carbides can achieve fragmentation of network carbides and ensure that the sample does not undergo macroscopic cracking; 5. Graphitization annealing below the eutectoid temperature promotes the transformation of fragmented carbides into graphite, controlling the graphite particle size between 1-2 μm and the graphite number between 2000-5000 / mm. 2 And the distribution is uniform; 6. Compared with cemented carbide and high-speed steel tool materials, the ultra-high carbon self-lubricating graphite steel tool material prepared by this invention has a short production cycle, low raw material cost, simple and controllable preparation process, and can realize mass industrial production. 7. The ultra-high carbon self-lubricating graphite steel cutting tool prepared by this invention has the characteristics of high hardness, high wear resistance, low thermal friction coefficient, excellent thermal stability and impact resistance. Attached Figure Description
[0015] The accompanying drawings, which constitute a part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a microstructure image of the tool blank used in this invention; Figure 2 Macroscopic photograph of the cutting edge of the ultra-high carbon self-lubricating graphite steel tool prepared for this invention after continuous turning of aluminum alloy for 1 hour; Figure 3 Macroscopic photograph of the cutting edge after continuous turning of aluminum alloy with a high-speed steel tool for 1 hour; Figure 4 Macroscopic photograph of the cutting edge after continuous turning of aluminum alloy with carbide tool for 1 hour; Figure 5 Line graph comparing the changes in surface roughness of aluminum alloy after turning with cutting tools made of different materials. Detailed Implementation
[0016] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0017] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative effort should fall within the scope of protection of the present application.
[0018] Please refer to Figure 1-5This invention specifically discloses an ultra-high carbon self-lubricating graphite steel cutting tool material, comprising the following components by mass percentage: C: 1.2-2.0%; Cr: 1.0-2.0%; Mo: 0.5-1.0%; V: 0.2-0.5%; W: 0.5-2.0%; Si: 0.3-1.5%; balance is Fe and unavoidable trace impurity elements.
[0019] Preferably, the C content is 1.3-1.6% and the Si content is 0.5-1.0%.
[0020] The material's composition design principle: The synergistic proportions of the alloying elements in this invention precisely match the performance requirements of the cutting tool material, with the following specific effects: 1. Carbon (C): Ultra-high carbon content of 1.2-2.0%, providing sufficient carbon source for the precipitation of carbides and graphite. On the one hand, it ensures the amount of carbon required for the formation of hard carbides, ensuring the high hardness and high wear resistance of the material. On the other hand, it provides carbon atoms for the precipitation of self-lubricating graphite particles. 2. Tungsten (W): Content 0.5-2.0%, can preferentially combine with carbon elements in molten steel to form high-hardness WC hard carbides. WC has extremely high hardness and excellent wear resistance, which can significantly improve the hardness and wear resistance of the tool matrix and extend the cutting service life of the tool. 3. Molybdenum (Mo) and Vanadium (V): Mo content 0.5-1.0% and V content 0.2-0.5%. Both can combine with carbon to form MoC and VC carbides with extremely strong thermodynamic stability. These carbides have excellent high temperature resistance and softening resistance, and can exist stably under high temperature cutting conditions, ensuring the thermal stability and high temperature cutting performance of the tool material and avoiding tool softening at high temperature. 4. Silicon (Si): Content 0.3-1.5%, it is a graphitization promoting element and provides conditions for in-situ graphitization of carbides during graphitization annealing; however, silicon can easily induce abnormal graphite precipitation during room temperature and slow cooling. This defect can be precisely avoided by controlling the cooling rate of the iron mold sand coating process. 5. Chromium (Cr): Content 1.0-2.0%, can refine matrix grains, improve the hardenability and oxidation resistance of materials, and work synergistically with various hard carbides to improve the mechanical properties of the matrix, improve the corrosion resistance and high-temperature oxidation resistance of cutting tools. At the same time, the addition of Cr can inhibit the precipitation of graphite phase during solidification.
[0021] This invention combines defined chemical composition ranges, casting, forging, and heat treatment process parameters to set up three sets of examples. Example 1 is the optimal ratio and process scheme, while Examples 2 and 3 are comparison schemes of range boundary parameters. It can stably prepare graphite steel tool materials with high hardness, high wear resistance, high thermal stability, and excellent self-lubricating and anti-sticking properties, which can be applied to complex working conditions such as high-speed dry cutting of aluminum alloys and precision milling.
[0022] Example 1: A method for preparing an ultra-high carbon self-lubricating graphite steel cutting tool material, used to prepare the above-mentioned ultra-high carbon self-lubricating graphite steel cutting tool material. The thickness of the cutting tool blank prepared in this case is 20 mm, and includes the following steps: S1: The composition according to the above mass percentages is C: 1.5%, Cr: 1.5%, Mo: 0.8%, V: 0.35%, W: 1.2%, Si: 0.6%, with the balance being Fe and unavoidable trace impurity elements; where C comes from high-purity pig iron and scrap steel, Cr comes from ferrochrome, Mo comes from ferromolybdenum, V comes from ferrovanadium, W comes from ferrotungsten, and Si comes from ferrosilicon raw materials. The various alloy raw materials are weighed according to the proportions and placed into a medium-frequency induction furnace and heated to 1600℃. The furnace is then kept at a constant temperature for 15 minutes to fully remove the internal gas and oxide inclusions of the molten steel, homogenize the alloy composition, and obtain a pure, uniformly composed ultra-high carbon alloy molten steel without segregation or impurity aggregation. S2: According to the process matching principle, the thickness of the sand coating layer is set to 8mm, and the iron mold sand coating process is used for casting. By utilizing the rapid cooling characteristics of the iron mold and the buffer temperature control of the sand layer, the solidification and cooling rate of the molten steel is controlled, effectively avoiding the problem of abnormal graphite precipitation in the matrix induced by silicon element, ensuring that the casting has a dense structure, smooth surface, and no casting defects such as porosity, looseness, and cracks, and obtaining qualified cast tool blanks. S3: Preheat the tool blank to 1100℃ and hold it at that temperature for 30 minutes, then perform a multi-fire, multi-forging process. Employ a multi-stage small deformation process, controlling the deformation amount of each forging to 10%, and perform a total of 10 forging passes. Through multiple small deformation forging passes, the continuous network of carbides in the as-cast structure is fully broken down, the segregation of the microstructure is completely eliminated, the matrix grains are refined, and the overall density and mechanical property uniformity of the as-cast tool blank are improved. After forging, the blank has no macroscopic cracks and no microstructure damage. S4: After forging, the tool blank is air-cooled to room temperature, and then placed in a heat treatment furnace for graphitization annealing at a temperature of 660℃ for 5 hours. After holding, it is slowly cooled to room temperature with the furnace. This graphitization annealing process below the eutectoid temperature allows the unstable carbides that are fragmented after forging to be fully decomposed and transformed into spherical graphite particles in situ. At the same time, highly stable hard carbides such as WC, MoC, and VC are retained in the matrix. S5: The graphitized annealed tool blank is heated to 850℃ and held for 0.5h, then quickly quenched in room temperature oil and heated to 350℃ and held for 2h to obtain ultra-high carbon self-lubricating graphite steel tool material.
[0023] The graphite steel material for cutting tools prepared by the above process has a dense matrix structure, with spherical graphite particles uniformly controlled at a size of 1.2-1.6 μm and a particle count of 3800 particles / mm², evenly dispersed in the matrix without aggregation or large graphite particles. Hard carbides are uniformly distributed in the matrix, with no residual network carbides. The material has an overall hardness of HRC62-64, a low coefficient of friction, and excellent self-lubricating and anti-sticking properties, making it suitable for high-speed continuous cutting of aluminum alloys and precision milling of complex curved surfaces.
[0024] Figure 1 This is a microstructure image of the tool blank prepared using Example 1; Figure 2 This is a macroscopic photograph of the cutting edge of an ultra-high carbon self-lubricating graphite steel tool made in Example 1 after continuous turning of aluminum alloy for 1 hour; Figure 3 This is a macroscopic photograph of the cutting edge of a high-speed steel tool after continuous turning of an aluminum alloy for 1 hour using existing technology; Figure 4 This is a macroscopic photograph of the cutting edge of a cemented carbide tool after continuous turning of an aluminum alloy for 1 hour in the existing technology; Figure 5 This is a line graph comparing the changes in surface roughness of aluminum alloys after turning them with high-speed steel tools and cemented carbide tools in the prior art, and with the ultra-high carbon self-lubricating graphite steel tool made in Example 1.
[0025] Example 2: A method for preparing an ultra-high carbon self-lubricating graphite steel cutting tool material, used to prepare the above-mentioned ultra-high carbon self-lubricating graphite steel cutting tool material. The thickness of the cutting tool blank prepared in this case is 25 mm, and includes the following steps: S1: The composition according to the above mass percentages is C: 1.2%, Cr: 1.0%, Mo: 0.5%, V: 0.2%, W: 0.5%, Si: 0.3%, with the balance being Fe and unavoidable trace impurity elements; where C comes from high-purity pig iron and scrap steel, Cr comes from ferrochrome, Mo comes from ferromolybdenum, V comes from ferrovanadium, W comes from ferrotungsten, and Si comes from ferrosilicon raw materials. The various alloy raw materials are weighed according to the proportions and placed into a medium-frequency induction furnace and heated to 1580℃. The furnace is kept at a constant temperature and refined for 15 minutes to remove impurities and gases from the molten steel, resulting in a uniform and pure alloy molten steel. S2: The thickness of the tool blank is 25mm (thick blank). To match the process requirements, the thickness of the sand coating layer is reduced. The thickness of the sand coating layer is set to 3mm. The iron mold sand coating process is used for casting. Taking advantage of the rapid solidification of the iron mold, abnormal graphite precipitation is suppressed, and a dense cast tool blank is prepared. S3: Preheat the tool blank to 1050℃ and hold it for 30 minutes. Forge 15% deformation per forging, and forge a total of 6 passes to fully break down the network carbides, refine the matrix structure, and eliminate structural defects. S4: After forging, the tool blank is air-cooled to room temperature, and then placed in a heat treatment furnace for graphitization annealing at a temperature of 600℃ for 10 hours. The blank is then slowly cooled to room temperature in the furnace to complete the decomposition of carbides and the precipitation of graphite. S5: The graphitized annealed tool blank is heated to 780℃ and held for 1 hour, then quickly quenched into room temperature oil, and then heated to 300℃ and held for 4 hours to obtain ultra-high carbon self-lubricating graphite steel tool material.
[0026] The graphite steel material for cutting tools prepared by the above process has spherical graphite particles with a diameter of 1.0-1.3μm, a number of graphite particles of 2200 / mm², and uniform dispersion; the matrix has a moderate content of hard carbide, and the material has a hardness of HRC58-60, exhibiting good self-lubricating and anti-sticking properties and wear resistance.
[0027] Example 3: A method for preparing an ultra-high carbon self-lubricating graphite steel cutting tool material, used to prepare the above-mentioned ultra-high carbon self-lubricating graphite steel cutting tool material. The thickness of the cutting tool blank prepared in this case is 10 mm, and includes the following steps: S1: The composition according to the above mass percentages is C: 2.0%, Cr: 2.0%, Mo: 1.0%, V: 0.5%, W: 2.0%, Si: 1.5%, with the balance being Fe and unavoidable trace impurity elements; where C comes from high-purity pig iron and scrap steel, Cr comes from ferrochrome, Mo comes from ferromolybdenum, V comes from ferrovanadium, W comes from ferrotungsten, and Si comes from ferrosilicon raw materials. The various alloy raw materials are weighed according to the proportions and placed into a medium-frequency induction furnace and heated to 1620℃. The furnace is kept at a constant temperature and refined for 12 minutes to remove impurities and gases from the molten steel, resulting in a uniform and pure alloy molten steel. S2: The thickness of the tool blank is 10mm (thin blank). To match the process requirements, the thickness of the sand coating layer is increased. The thickness of the sand coating layer is set to 15mm to slow down the cooling rate. The iron mold sand coating process is used for casting to avoid structural stress defects caused by excessive cooling, so as to obtain a defect-free dense cast blank and prepare a dense cast tool blank. S3: Preheat the tool blank to 1000℃ and hold it for 30 minutes. Forge 15% deformation per forging, and forge 4 times in total to completely break down the network carbides, maximize the refinement of the matrix grains, and improve the material density. S4: After forging, the tool blank is air-cooled to room temperature, and then placed in a heat treatment furnace for graphitization annealing at a temperature of 720℃ for 4 hours. It is then slowly cooled to room temperature in the furnace to achieve full decomposition of unstable carbides and precipitation of uniform spherical graphite. S5: The graphitized annealed tool blank is heated to 920℃ and held for 0.5h, then quickly quenched into room temperature oil, and then heated to 500℃ and held for 1h to obtain ultra-high carbon self-lubricating graphite steel tool material.
[0028] The graphite steel material for cutting tools prepared by the above process has spherical graphite particles with a diameter of 1.5–2.0 μm and a number of 3500 graphite particles / mm², which are uniformly and densely distributed. The matrix has a high content of WC, MoC, and VC hard carbides, which are extremely stable. The material has a hardness of HRC58-60 and excellent wear resistance, impact resistance, and self-lubricating properties. It can be used for ultra-high speed dry cutting of aluminum alloys, heavy-duty intermittent cutting, and high-precision milling of complex curved surfaces.
[0029] Table of correspondence between tool blank thickness, sand coating thickness and molten iron residence time
[0030] The technological principle of a preparation method for ultra-high carbon self-lubricating graphite steel cutting tool material: 1. Iron mold sand coating process: Compared with traditional sand casting, the iron mold sand coating process has the dual advantages of rapid cooling of iron mold and buffer cooling of sand mold. It has a fast cooling rate, high production efficiency, low mold cost, and the surface quality of the prepared material is better than that of metal mold casting. By controlling the thickness of the sand coating layer from 3 to 15 mm, it can be used to prepare tool blanks of different thicknesses: for thick blanks, the sand coating thickness is reduced to utilize the strong cooling capacity of the iron mold to solidify quickly and inhibit graphite precipitation; for thin blanks, the sand coating thickness is increased to avoid structural stress defects caused by excessive cooling rate and ensure uniform and dense as-cast structure.
[0031] 2. High-temperature forging process with multiple passes and small deformations: The presence of continuous network carbides inside the cast billet leads to high brittleness of the material. High-temperature, multiple passes with small deformations can break down the network carbides without macroscopic cracks in the tool billet, avoiding billet cracking caused by a single large deformation, and laying a good microstructure foundation for subsequent graphitization precipitation.
[0032] 3. Low-temperature graphitization annealing process: Low-temperature annealing is carried out below the eutectoid temperature, which causes the fragmented unstable carbides to decompose in situ and form spherical graphite, while stable hard carbides such as WC, MoC, and VC are not affected by the annealing temperature; ultimately, a composite structure of high-hardness wear-resistant carbides in the matrix and dispersed fine spherical graphite is achieved, which takes into account both the wear resistance and self-lubricating friction-reducing properties of the material.
[0033] 4. Two-phase quenching and tempering process: The tool blank is heated to the two-phase region to dissolve the graphite back into the matrix, further reducing the graphite size and weakening its influence on strength and toughness. At the same time, the quenching and tempering treatment produces a tempered martensitic structure, ensuring the strength of the tool blank.
[0034] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-carbon self-lubricating graphite steel cutting tool material, characterized in that, Includes the following components by mass percentage: C:1.2-2.0%; Cr:1.0-2.0%; Mo: 0.5-1.0%; V:0.2-0.5%; W:0.5-2.0%; Si: 0.3-1.5%; The balance consists of Fe and unavoidable trace impurity elements; The matrix of the cutting tool material is tempered martensite, on which spherical graphite particles and hard carbide particles are dispersed. The particle size of the spherical graphite particles is 1-2 μm, and the number density is 2000-5000 particles / mm. 2 Hard carbide particles include WC, MoC, and VC.
2. The ultra-high carbon self-lubricating graphite steel cutting tool material according to claim 1, characterized in that, The C content is 1.3-1.6%, and the Si content is 0.5-1.0%.
3. A method for preparing an ultra-high carbon self-lubricating graphite steel cutting tool material, used to prepare the ultra-high carbon self-lubricating graphite steel cutting tool material as described in claim 1, characterized in that, Includes the following steps: S1: Weigh pig iron, scrap steel, ferrochrome, ferromolybdenum, ferrovanadium, ferrotungsten, and ferrosilicon according to the following mass percentages: C: 1.2-2.0%, Cr: 1.0-2.0%, Mo: 0.5-1.0%, V: 0.2-0.5%, W: 0.5-2.0%, Si: 0.3-1.5%, with the balance being Fe and unavoidable trace impurities. Add them to a medium-frequency induction furnace for smelting, thoroughly refining and removing impurities, removing gases and inclusions from the molten steel to obtain ultra-high carbon alloy steel liquid. S2: Casting is carried out using an iron mold with sand coating process. The thickness of the sand coating layer is adjusted according to the thickness of the tool blank to be prepared, and the thickness of the sand coating layer is controlled between 3-15mm. Among them, the thicker the tool blank, the thinner the sand coating layer, so as to ensure its cooling rate; the thinner the tool blank, the thicker the sand coating layer, so as to slow down the cooling rate, avoid the risk of abnormal graphite precipitation in the matrix induced by silicon element, and ensure that the matrix structure of the casting is dense, thus obtaining the as-cast tool blank. S3: After heating and holding the tool blank at a certain temperature, it is forged at a high temperature using a multi-fire and multi-forging process. The forging temperature range is 1000-1100℃, and the reduction in a single forging is controlled at 10-25%. Through multiple small deformation forgings, the continuous network carbides in the as-cast structure are fully broken down, the structure segregation is eliminated, the matrix grains are refined, and the material density and structure uniformity are improved. S4: After cooling the forged tool blank to room temperature, it is sent to a heat treatment furnace for graphitization annealing below the eutectoid temperature. The annealing temperature is controlled at 600-750℃, and the holding time is 4-10 hours. The blank is then slowly cooled to room temperature in the furnace. This process allows the unstable carbides that have fragmented after forging to be fully decomposed and separated, forming uniformly sized particles with a diameter of 1-2 μm and a number density of 2000-5000 particles / mm. 2 The spherical graphite particles, while the stable hard carbides WC, MoC, and VC are completely preserved in the matrix; S5: Heat the tool blank to a duplex temperature of 780-920℃ and hold for 0.5-1h, then quickly quench it in oil and temper it at 300-500℃ for 1-5h. Finally, a self-lubricating graphite steel tool material with a microstructure of tempered martensite matrix and fine graphite and hard carbides distributed on it is obtained.
4. The method for preparing an ultra-high carbon self-lubricating graphite steel cutting tool material according to claim 3, characterized in that, In step S1, the melting temperature is controlled at 1550-1650℃.
Citation Information
Patent Citations
Improvements in or relating to graphitic tool steels
GB1074012A