Mesoscopic porous core-shell dielectric resonant photothermal catalytic system, its preparation and application

By coating porous silica onto the surface of Cu2O nanoparticles to form a Cu2O@P-SiO2 structure, and utilizing dielectric resonance and photothermal synergy, the problems of rapid recombination of photogenerated carriers and heat dissipation in photocatalytic nitrogen fixation were solved, achieving efficient and low-cost green nitrogen fixation conversion.

CN122722249BActive Publication Date: 2026-11-17SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611184916.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17
Estimated Expiration
2046-08-06

AI Technical Summary

Technical Problem

Existing photocatalytic nitrogen fixation technologies suffer from problems such as rapid recombination of photogenerated carriers and easy dissipation of heat energy generated by photothermal conversion. Furthermore, traditional noble metal composite structures are costly and have complex interface mechanisms, making it difficult to achieve efficient and low-cost green nitrogen fixation.

Method used

A mesoscopic porous core-shell dielectric resonance photothermal catalytic system was adopted. Porous silica was coated in situ on the surface of Cu2O nanoparticles to form a Cu2O@P-SiO2 structure. The dielectric resonance effect was used to enhance photon capture and local electric field, and combined with the photothermal synergistic effect, nitrogen activation was promoted.

Benefits of technology

Achieving efficient interfacial nitrogen fixation conversion at room temperature and pressure significantly improves N2 mass transfer and the exposure of surface reaction sites, enhances photocatalytic performance, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122722249B_ABST
    Figure CN122722249B_ABST
Patent Text Reader

Abstract

This invention discloses a mesoscopic porous core-shell dielectric resonant photothermal catalytic system, its preparation method, and its application. The preparation method includes: [the process involves] forming a Cu-containing... 2+ Source, OH ‑ Cubic Cu₂O nanoparticles were prepared by reacting a mixture of source and L-ascorbic acid. An organosilicon precursor was then in-situ coated onto the surface of the cubic Cu₂O nanoparticles using a sol-gel method to obtain an amorphous organic SiO₂-uniformly coated Cu₂O core-shell composite. The amorphous organic SiO₂-uniformly coated Cu₂O core-shell composite was then immersed in an alkaline solution to obtain a mesoscopic porous core-shell dielectric resonant photothermal catalytic system. This invention, through a mesoscopic porous core-shell dielectric resonant photothermal catalytic system, achieves for the first time a synergistic effect of enhanced local field in the medium, Cu₂O photothermal effect, and photocatalytic interfacial nitrogen fixation, providing an innovative solution for developing efficient and low-cost green nitrogen fixation technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new chemical materials, specifically relating to a mesoscopic porous core-shell dielectric resonant photothermal catalytic system and its preparation and application. Background Technology

[0002] The efficient activation and utilization of nitrogen is of great significance to agricultural and industrial development. Although nitrogen (N2) constitutes 78% of the atmosphere, reactive nitrogen forms are extremely scarce in nature due to the extremely high bond energy of the N≡N triple bond (941.3 kJ / mol). While the traditional Haber-Bosch process achieves industrial nitrogen fixation, its harsh conditions of high temperature and high pressure (400-600℃, 15-25 MPa) result in huge consumption of fossil fuels and significant greenhouse gas emissions. Developing new green and sustainable nitrogen fixation technologies has become a research hotspot.

[0003] Photocatalytic nitrogen fixation technology has attracted much attention due to its room-temperature and ambient-pressure reaction characteristics and solar-driven advantages. However, it is limited by bottlenecks such as high recombination rate of photogenerated carriers and difficulty in nitrogen adsorption activation. Recent studies have found that the photothermal effect can effectively improve photocatalytic performance, and its mechanism of action includes: thermally induced increase in carrier mobility, generation of localized hot carriers, and promotion of surface reactant activation. However, conventional photothermal-photocatalytic systems mostly adopt noble metal composite structures, which have problems such as high cost and complex interface mechanisms. In order to further overcome the bottlenecks of energy conversion and molecular activation, developing non-noble metal catalytic systems based on the "dielectric resonance" effect has become a new approach to enhance the reaction kinetics of gas-solid-liquid three-phase interfaces.

[0004] Cuprous oxide (Cu₂O), as a p-type semiconductor with both a broad spectral response (band gap ~2.0 eV) and significant photothermal effects, exhibits unique advantages in the field of nitrogen fixation catalysis. More importantly, at a specific mesoscale formed by a high-refractive-index semiconductor and a dielectric, a significant dielectric resonance effect can be induced, thereby generating a strong local electric field, greatly improving photon capture efficiency and accelerating exciton dissociation. However, single Cu₂O materials suffer from drawbacks such as rapid recombination of photogenerated electrons and holes and easy dissipation of heat energy generated by photothermal conversion. Therefore, developing an efficient, low-cost, and green nitrogen fixation technology is an urgent problem to be solved. Summary of the Invention

[0005] To address the issues of high cost and complex interface mechanisms of conventional photothermal catalysts, as well as the drawbacks of rapid recombination of photogenerated carriers and easy dissipation of heat generated by photothermal conversion in single Cu2O materials, and to meet the need for developing high-performance photothermal catalysts, this invention provides a mesoscopic porous core-shell dielectric resonant photothermal catalytic system, its preparation method, and its application. The core of this system is a mesoscopic porous silica-coated cubic cuprous oxide nanoparticle core-shell structured photothermal catalytic material, with the general formula: Cu2O@P-SiO2.

[0006] To achieve the aforementioned objectives, the technical solution adopted by this invention includes: This invention provides a method for preparing a mesoscopic porous core-shell dielectric resonant photothermal catalytic system, comprising: Make Cu 2+ Source, OH - Cu2O nanoparticles were prepared by reacting a mixture of source and L-ascorbic acid. An organosilicon precursor was in situ coated onto the surface of cubic Cu2O nanoparticles using the sol-gel method to prepare a Cu2O core-shell composite uniformly coated with amorphous organic SiO2. Furthermore, the Cu2O core-shell structure composite uniformly coated with amorphous organic SiO2 is immersed in an alkaline solution to form a Cu2O nanoparticle core-shell structure composite uniformly coated with porous organic P-SiO2, thereby obtaining a mesoscopic porous core-shell dielectric resonant photothermal catalytic system.

[0007] The present invention also provides a mesoscopic porous core-shell dielectric resonant photothermal catalytic system prepared by the aforementioned preparation method, which includes: cubic Cu2O nanoparticles as the core and a porous organic P-SiO2 shell on the surface.

[0008] This invention also provides the application of the aforementioned mesoscopic porous core-shell dielectric resonant photothermal catalytic system in interfacial nitrogen fixation.

[0009] This invention also provides a method for interfacial photothermal catalytic nitrogen fixation, comprising: The aforementioned mesoscopic porous core-shell dielectric resonant photothermal catalytic system is provided; Furthermore, the mesoscopic porous core-shell dielectric resonant photothermal catalytic system is mixed with an ethanol solution and placed in a photocatalytic reaction device. Then, N2 is introduced at a constant rate to maintain the nitrogen saturation state of the system, and then the interfacial photothermal catalytic nitrogen fixation reaction is carried out under the irradiation of the solar spectrum simulated by a xenon lamp light source.

[0010] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention provides a design strategy for a mesoscopic porous core-shell dielectric resonant photothermal catalytic system and interfacial nitrogen fixation. In the porous core-shell Cu2O@P-SiO2 catalyst, the core Cu2O facilitates the absorption of incident photons, thereby generating photothermal conversion. The porous SiO2 shell on the surface slows down the thermal conduction of the core Cu2O to the surrounding environment. Furthermore, the porous organosilicon layer can also capture the infrared light radiated from the "hot" Cu2O core through absorption and scattering, thereby achieving the confinement of thermal energy on the catalyst surface and producing a significant heating effect similar to the "greenhouse effect" (e.g., Figure 2 As shown in the figure, this mesoporous structure significantly enhances the mass transfer of N2 and the exposure of surface nitrogen fixation reaction sites. (2) This invention constructs a dual-effect catalytic system of enhanced local field and photothermal synergy in the medium, and develops a highly selective reaction pathway; it breaks through the traditional high temperature and high pressure limitations and achieves efficient interfacial nitrogen fixation conversion under mild conditions. Attached Figure Description

[0011] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0012] Figure 1 This is a schematic diagram of the synthesis process of a mesoscopic porous core-shell dielectric resonant photothermal catalytic system (Cu2O@P-SiO2) in a typical embodiment of the present invention; Figure 2 This is a schematic diagram of the "greenhouse effect" of a mesoscopic porous core-shell dielectric resonant photothermal catalytic system (Cu2O@P-SiO2) in a typical embodiment of the present invention; Figure 3a The XRD patterns are of Cu2O@P-SiO2 in Specific Embodiment 1, Cu2O@SiO2 in Comparative Example 1, and Cu2O in Comparative Example 2 of the present invention. Figure 3b The Raman spectra of Cu2O@P-SiO2 in Specific Embodiment 1, Cu2O@SiO2 in Comparative Example 1, and Cu2O in Comparative Example 2 are shown below. Figure 4a This is a SEM image of Cu2O in Comparative Example 2 of the present invention; Figure 4b This is a SEM image of Cu2O@SiO2 in Comparative Example 1 of this invention; Figure 4c This is a SEM image of Cu2O@P-SiO2 in Example 1 of the present invention; Figure 5a This is a TEM image of Cu2O in Comparative Example 2 of the present invention; Figure 5b This is a TEM image of Cu2O@SiO2 in Comparative Example 1 of this invention; Figure 5c This is a TEM image of Cu2O@P-SiO2 in Example 1 of the present invention; Figure 5d In this invention Figure 5b A magnified TEM image of the yellow area; Figure 6aInfrared thermal images of Cu2O@SiO2 in Comparative Example 1, Cu2O in Comparative Example 2, and Cu2O@P-SiO2 in Example 1 of this invention; Figure 6b The above are multipath temperature diagrams of Cu2O@SiO2 in Comparative Example 1, Cu2O in Comparative Example 2, and Cu2O@P-SiO2 in Example 1 of this invention. Figure 7 The graphs show the photothermal catalytic ammonia production performance of Cu2O@SiO2 in Comparative Example 1, Cu2O in Comparative Example 2, and Cu2O@P-SiO2 in Example 1 of this invention. Detailed Implementation

[0013] In view of the deficiencies of the prior art, the applicant, through long-term research and extensive practice, has proposed the technical solution of this invention. The technical solution of this invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0014] This invention proposes a design strategy for a mesoscopic porous core-shell dielectric resonant structure: by coating cubic Cu2O nanoparticles (Cu2O@P-SiO2) with porous silica (P-SiO2), the following are achieved: (1) the photothermal localization and dielectric coupling effect of the SiO2 shell—utilizing the "light trapping effect" of the porous shell to synergistically enhance the dielectric resonance of the core, while suppressing heat loss and generating a "nano-greenhouse effect"; (2) the mesoscopic porous structure enhances N2 mass transfer and exposes surface reaction sites, constructing a highly active nitrogen fixation interface microenvironment; (3) the energy level matching of the core-shell interface promotes the directional migration of photogenerated carriers. This mesoscopic porous core-shell dielectric resonant system achieves for the first time the synergistic enhancement of localized dielectric field, Cu2O photothermal effect and photocatalytic interface nitrogen fixation, providing an innovative solution for developing efficient and low-cost green nitrogen fixation technology.

[0015] Specifically, as one aspect of the technical solution of this invention, the preparation method of a mesoscopic porous core-shell dielectric resonant photothermal catalytic system includes: Make Cu 2+ Source, OH - Cu2O nanoparticles were prepared by reacting a mixture of source and L-ascorbic acid. An organosilicon precursor was in situ coated onto the surface of cubic Cu2O nanoparticles using the sol-gel method to prepare a Cu2O core-shell composite uniformly coated with amorphous organic SiO2. Furthermore, the Cu2O core-shell structure composite uniformly coated with amorphous organic SiO2 is immersed in an alkaline solution to form a Cu2O nanoparticle core-shell structure composite uniformly coated with porous organic P-SiO2, thereby obtaining a mesoscopic porous core-shell dielectric resonant photothermal catalytic system.

[0016] In some preferred embodiments, the preparation method specifically includes: Cu 2+ The source is mixed with water and OH is added. - The source was then added with L-ascorbic acid under stirring and the reaction was continued for 30-60 min. After centrifugation, washing and vacuum drying, cubic Cu2O nanoparticles were obtained.

[0017] Furthermore, the Cu 2+ Cu in the source 2+ With OH - OH in the source - The molar ratio is 1:20 to 1:2.

[0018] Furthermore, the Cu 2+ Cu in the source 2+ The molar ratio with L-ascorbic acid is 1:1.

[0019] Furthermore, the Cu 2+ The source includes water-soluble divalent copper salts, which include any one or more combinations of CuCl2·2H2O, CuSO4·5H2O, and anhydrous CuSO4, and are not limited thereto.

[0020] Furthermore, the water-soluble divalent copper salt is CuCl2·2H2O.

[0021] Furthermore, the OH - Sources include, but are not limited to, NaOH and / or KOH.

[0022] Furthermore, the OH - The source is NaOH. In some preferred embodiments, the preparation method specifically includes: Cu2O nanoparticles were dispersed in ethanol to form a Cu2O nanoparticle dispersion. Ethanol and tetraethyl silicate are mixed to form the first mixed solution; Ethanol and water are mixed and the pH is adjusted to 4-6 using oxalic acid solution to form a second mixed solution; Furthermore, the second mixed solution, the epoxy-containing trialkoxysilane, and the first mixed solution are mixed and stirred for 3-5 hours. Then, Cu2O nanoparticle dispersion is added and the mixture is stirred and stirred for another 3-5 hours. Finally, the mixture is centrifuged, washed, and vacuum dried to obtain a Cu2O core-shell structured composite uniformly coated with amorphous organic SiO2.

[0023] Furthermore, the organosilicone ester includes any one or more combinations of methyl orthosilicate, ethyl orthosilicate (tetraethyl orthosilicate), and propyl orthosilicate, and is not limited thereto.

[0024] Furthermore, the organosilicone ester is tetraethyl orthosilicate (tetraethyl orthosilicate).

[0025] Furthermore, the epoxy-containing trialkoxysilane includes, but is not limited to, γ-glycidoxypropyltrimethoxysilane (GPTMS / KH-560).

[0026] Furthermore, the volume ratio of ethanol to tetraethyl silicate in the first mixed solution is 20:1 to 80:1.

[0027] Furthermore, the volume of ethanol in the first mixed solution is the same as that in the second mixed solution.

[0028] Furthermore, the volume ratio of water in the second mixed solution to tetraethyl silicate in the first mixed solution is 1:5; Furthermore, the concentration of the oxalic acid solution is 0.5~1.5 mol / L.

[0029] Furthermore, the volume of the epoxy-containing trialkoxysilane is the same as that of the water in the second mixed solution.

[0030] In some preferred embodiments, the preparation method specifically includes: immersing the amorphous organic SiO2-uniformly coated Cu2O core-shell composite in an alkaline solution with a pH of 8-10 for 1-3 hours, followed by centrifugation, washing, and drying to form a porous organic P-SiO2-uniformly coated Cu2O nanoparticle core-shell composite.

[0031] In some preferred embodiments, the preparation method of the mesoscopic porous core-shell dielectric resonant photothermal catalytic system (Cu2O@P-SiO2) includes the following steps: (1) Add CuCl2·2H2O solution to an appropriate amount of ultrapure water, followed by an appropriate amount of NaOH solution (1:20 ≤ CuCl2·2H2O). 2+ With OH The molar ratio of Cu is ≤ 1:2, and the mixture is stirred at a constant speed (300~600 r / min) using a magnetic stirrer. During stirring, an appropriate amount of L-ascorbic acid solution is added (its molar ratio is ≤ 1:2). 2+ The same amount of material was used, and stirring was continued for 30-60 minutes to ensure the reaction proceeded fully. After the reaction was complete, the brick-red precipitate was collected by high-speed centrifugation (3000-10000 r / min). The brick-red precipitate was washed multiple times with a 20%-50% ethanol solution to remove any reagent residues that may have remained during the reaction. The washed precipitate was then dried in a vacuum oven at 50℃-80℃ for 2-3 hours to obtain cubic Cu2O nanoparticles. (2) The cubic Cu2O nanoparticles synthesized in step (1) were coated with an organosilicon precursor in situ using the sol-gel method. After reaction and vacuum drying, a Cu2O@SiO2 core-shell composite with amorphous organosilicon SiO2 uniformly coated was obtained. Specifically: First, prepare mixture A: Take an appropriate volume of anhydrous ethanol and tetraethyl silicate, with a volume ratio of 20:1 to 80:1, and add them to a beaker and mix them evenly. Second, prepare mixture B: Take an equal volume of anhydrous ethanol to mixture A, and one-fifth the volume of ultrapure water to tetraethyl silicate in mixture A, mix them evenly, and then add 0.5 to 1.5 M oxalic acid solution to adjust the pH to 4 to 6. Add mixture B and an equal volume of γ-glycidoxypropyltrimethoxysilane to ultrapure water in mixture B to mixture A, and react for 3 to 5 hours. Weigh a certain mass of the cubic Cu2O nanoparticles prepared in step (1) above, uniformly disperse them in a certain volume of anhydrous ethanol, and slowly add them dropwise to mixture A. After the addition is complete, continue the reaction for 3-5 hours. All reactions are carried out under the condition of uniform stirring of the solution at a speed of 300-500 r / min. After the reaction is completed, collect the reaction product by centrifugation, wash it more than 3 times with ultrapure water, and dry it in a vacuum oven at 50℃-80℃ for 2-3 hours to obtain a Cu2O@SiO2 core-shell composite material uniformly coated with amorphous organic SiO2.

[0032] (3) Weigh a certain mass of the Cu2O@SiO2 core-shell structure complex synthesized in step (2), add it to an appropriate amount of alkaline sodium hydroxide solution (pH value: 8~10) and soak for 1~3 hours, centrifuge, wash and dry, and finally prepare Cu2O@P-SiO2 core-shell structure complex of Cu2O nanoparticles uniformly coated with porous organic P-SiO2.

[0033] A schematic diagram of the synthesis process of the mesoscopic porous core-shell dielectric resonant photothermal catalytic system (Cu2O@P-SiO2) of this invention is shown below. Figure 1 As shown.

[0034] Another aspect of the present invention provides a mesoscopic porous core-shell dielectric resonant photothermal catalytic system prepared by the aforementioned preparation method, comprising: cubic Cu2O nanoparticles as the core and a porous organic P-SiO2 shell on the surface.

[0035] Furthermore, the side length of the cubic Cu2O nanoparticles is 300–900 nm.

[0036] Furthermore, the thickness of the porous organic P-SiO2 shell is 10–150 nm.

[0037] Furthermore, the pore size of the pores contained in the porous organic P-SiO2 shell is 3 to 30 nm.

[0038] This invention provides a design strategy for a mesoscopic porous core-shell dielectric resonant system. It uses a porous SiO2 shell to coat Cu2O nanoparticles, avoiding the instability of the substrate material. Through the specific mesoscopic scale formed by the high-refractive-index semiconductor core and the porous medium shell, a significant dielectric resonance effect is induced, generating a strong local electric field. Simultaneously, utilizing its unique "light-trapping effect," a significant increase in the surface temperature of the core catalytic material and an enhancement in photon capture efficiency are achieved. Furthermore, the porous nature of the SiO2 shell facilitates contact between reactants and the active sites of the core catalytic material, constructing a highly active nitrogen-fixing interface microenvironment. This allows for the design and development of a dielectric resonant photothermal catalytic system with strong photoresponse, slow carrier recombination, fast interfacial reaction kinetics, and good stability.

[0039] Another aspect of the present invention provides the application of the aforementioned mesoscopic porous core-shell dielectric resonant photothermal catalytic system in interfacial nitrogen fixation.

[0040] Another aspect of the present invention provides a method for interfacial photothermal catalytic nitrogen fixation, comprising: The aforementioned mesoscopic porous core-shell dielectric resonant photothermal catalytic system is provided; Furthermore, the mesoscopic porous core-shell dielectric resonant photothermal catalytic system is mixed with an ethanol solution and placed in a photocatalytic reaction device. Then, N2 is introduced at a constant rate to maintain the nitrogen saturation state of the system, and then the interfacial photothermal catalytic nitrogen fixation reaction is carried out under the irradiation of the solar spectrum simulated by a xenon lamp light source.

[0041] In some preferred embodiments, the interfacial photothermal catalytic nitrogen fixation reaction includes: weighing 50 mg of photothermal catalytic material, using a photocatalytic reactor with a condensate jacket, and ultrasonically dispersing it with 50 mL of 20 vol.% ethanol solution for 2 hours in the dark to form a homogeneous catalytic system. Ethanol is used as a hole scavenger, and the reaction system uses high-purity N2 (99.999%) and water as the nitrogen and hydrogen sources, respectively. Before the reaction, the system is continuously purged with high-purity N2 for 1 hour to effectively remove dissolved oxygen and other impurity gases, creating an oxygen-free catalytic environment. During the reaction, N2 is introduced at a constant rate to maintain nitrogen saturation in the system. A xenon lamp source is used to simulate the solar spectrum (light intensity 100 mW / cm²). 2 The nitrogen reduction reaction is driven by dielectric resonance and photothermal synergy. The entire reaction takes place under ambient temperature and pressure conditions, producing only NH3 and NH4. + The product contained no other nitrogen-containing byproducts. A sampling and detection mechanism with 10-minute intervals was established. 1 mL of the clarified liquid was drawn using a syringe and reacted with Nessler's reagent for colorimetric analysis. Quantitative analysis was performed using UV-Vis spectroscopy with the characteristic absorption peak at 425 nm. Real-time monitoring of ammonia nitrogen concentration was achieved using a standard curve method.

[0042] The technical solution of the present invention will be further described in detail below with reference to several preferred embodiments and accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and provides detailed implementation methods and specific operation processes. However, the protection scope of the present invention is not limited to the following embodiments.

[0043] Unless otherwise specified, the experimental materials used in the examples below can be purchased from conventional biochemical reagent companies.

[0044] Example 1 (1) Add 1 mL of 0.1 M CuCl2·2H2O solution to 50 mL of ultrapure water, followed by 1 mL of 2 M NaOH solution (CuCl2·2H2O). 2+ With OH The mixture was stirred at a constant speed of 580 r / min using a magnetic stirrer (molar ratio of 1:20). During stirring, 1 mL of 0.1 M L-ascorbic acid solution was added, and stirring was continued for 30 min to ensure complete reaction. After the reaction was complete, the resulting brick-red precipitate was collected by high-speed centrifugation (10000 r / min). The brick-red precipitate was washed multiple times with 50% ethanol solution to remove any reagent residues that may have remained from the reaction. The washed precipitate was then dried in a vacuum oven at 50 °C for 3 hours to obtain cubic Cu₂O nanoparticles. (2) The cubic Cu2O nanoparticles synthesized in step (1) were coated with organosilicon precursors in situ using the sol-gel method. After reaction and vacuum drying, a Cu2O@SiO2 core-shell composite with amorphous organosilicon SiO2 uniformly coated was obtained. Specifically: First, mixture A was prepared: 15 mL of anhydrous ethanol and 300 μL of tetraethyl silicate were added to a beaker at a volume ratio of 50:1 and mixed evenly. Next, mixture B was prepared: 15 mL of anhydrous ethanol and 60 μL of ultrapure water were mixed evenly, and then 1 mol / L of oxalic acid solution was added to adjust the pH to 5. Mixture B and 60 μL of γ-glycidoxypropyltrimethoxysilane were added to mixture A and reacted for 3 hours. 100 mg of the cubic Cu2O nanoparticles prepared in step (1) were weighed and evenly dispersed in a certain volume of anhydrous ethanol. The ethanol was slowly added dropwise to mixture A, and the reaction was continued for 3 hours after the addition was completed. All reactions were carried out under uniform stirring of the solution at a speed of 400 r / min. After the reaction was completed, the reaction products were collected by centrifugation, washed more than three times with ultrapure water, and dried in a vacuum oven at 50°C for 3 hours to obtain a Cu2O@SiO2 core-shell composite material uniformly coated with amorphous organic SiO2.

[0045] (3) Weigh 30 mg of the Cu2O@SiO2 core-shell composite synthesized in step (2), add it to 30 mL of alkaline sodium hydroxide solution (pH: 9) and soak for 1 h, centrifuge, wash and dry, and finally prepare a mesoscopic porous core-shell dielectric resonant photothermal catalytic system (i.e., Cu2O nanoparticle core-shell composite Cu2O@P-SiO2 uniformly coated with porous organic P-SiO2, wherein the side length of the cubic Cu2O nanoparticle is about 400 nm, the thickness of the P-SiO2 shell is about 10 nm, the pore size distribution of the P-SiO2 shell is 3 to 30 nm, and the main peak pore size is about 3.8 to 4.0 nm).

[0046] (4) Weigh 50 mg of Cu2O@P-SiO2 and use a photocatalytic reactor with a cooling water jacket to disperse it with 50 mL of 20 vol.% ethanol solution in the dark for 2 hours to form a uniform catalytic system. Ethanol is used as a hole scavenger. The reaction system uses high-purity N2 (99.999%) and water as nitrogen and hydrogen sources. Before the reaction, the system is purged with high-purity N2 for 1 hour to effectively remove dissolved oxygen and other impurity gases, creating an oxygen-free catalytic environment. During the reaction, N2 is introduced at a constant rate to maintain the nitrogen saturation state of the system. A xenon lamp source is used to simulate the solar spectrum (light intensity 100 mW / cm²). 2 The nitrogen reduction reaction is driven by dielectric resonance and photothermal synergy. The entire reaction takes place under ambient temperature and pressure conditions, producing only NH3 and NH4. +The product contained no other nitrogen-containing byproducts. A sampling and detection mechanism with 10-minute intervals was established. 1 mL of the clarified liquid was drawn using a syringe and reacted with Nessler's reagent for colorimetric analysis. Quantitative analysis was performed using UV-Vis spectroscopy with the characteristic absorption peak at 425 nm. Real-time monitoring of ammonia nitrogen concentration was achieved using a standard curve method.

[0047] The obtained samples were characterized by XRD to analyze their structure and composition, and their microstructure was observed by SEM and TEM. The photothermal conversion effect of the samples was recorded by infrared thermal imaging, and the photothermal catalytic performance of the samples was characterized by photothermal catalytic nitrogen fixation performance test.

[0048] The XRD characterization of Cu2O@P-SiO2 obtained in Example 1 is as follows: Figure 3a As shown in (i), the diffraction peaks at 29.75°, 36.43°, 42.26°, 52.47°, 61.43°, 73.74° and 77.52° correspond to the (110), (111), (200), (211), (220), (311) and (222) crystal planes of cubic Cu2O, and no characteristic peaks of SiO2 are observed, indicating that SiO2 in the Cu2O@P-SiO2 sample appears in an amorphous form. Figure 3b The Raman spectrum in (i) further characterizes the bonding state of the material surface. In addition to the characteristic peak of Cu2O, the Raman spectrum of the Cu2O@P-SiO2 sample shows a peak at 1020 cm⁻¹. -1 The presence of an asymmetric vibrational peak in the Si-O-Si region further indicates the presence of organic silicon-oxygen compounds on the surface of the Cu2O substrate. The SEM characterization of Cu2O@P-SiO2 obtained in Example 1 is as follows: Figure 4c As shown, multiple overlapping mesopores are formed on the surface of the Cu2O core. This mesoporous shell structure protects the Cu2O core and ensures the transport of reactants and products during the interfacial nitrogen fixation reaction while achieving the "photothermal effect". The TEM characterization of Cu2O@P-SiO2 obtained in Example 1 is as follows: Figure 5c As shown, uneven coatings are clearly visible on the material surface, which is the result of cross-linking of multiple mesoporous phases. Figure 4c The corresponding SEM image. The infrared thermal image of Cu2O@P-SiO2 obtained in Example 1 is as follows. Figure 6a As shown in Figure (3), Cu2O@P-SiO2 has the highest apparent temperature, and the highest temperature value read by the infrared camera is 99 °C. Although the infrared camera measures the macroscopic temperature of the catalyst surface, which may be much lower than the local temperature of the core Cu2O, this trend clearly indicates that the prepared mesoscopic porous core-shell dielectric resonant structure has excellent photothermal effect. Figure 6bTo directly record the surface temperature changes of the sample using a multipath temperature recorder, the surface temperature of the Cu2O@P-SiO2 sample rapidly increased within 2 minutes, then stabilized, with an average surface temperature of 99 ℃. Figure 7 As shown, the mesoscopic porous core-shell dielectric resonant photothermal catalytic system (Cu2O@P-SiO2) exhibits the highest interfacial nitrogen fixation (ammonia production) efficiency, at 279.275 μmol / h. -1 g -1 .

[0049] Example 2 (1) Same as Specific Implementation Example 1; (2) The cubic Cu2O nanoparticles synthesized in step (1) were coated with an organosilicon precursor in situ using the sol-gel method. After reaction and vacuum drying, a Cu2O@SiO2 core-shell composite with amorphous organosilicon SiO2 uniformly coated was obtained. Specifically: First, mixture A was prepared: 15 mL of anhydrous ethanol and 500 μL of tetraethyl silicate were added to a beaker at a volume ratio of 30:1 and mixed evenly. Next, mixture B was prepared: 15 mL of anhydrous ethanol and 100 μL of ultrapure water were mixed evenly, and then 1 M of oxalic acid solution was added to adjust the pH to 5. Mixture B and 100 μL of γ-glycidoxypropyltrimethoxysilane were added to mixture A and reacted for 3 hours. 100 mg of the cubic Cu2O nanoparticles prepared in step (1) were weighed and evenly dispersed in a certain volume of anhydrous ethanol and slowly added dropwise to mixture A. After the addition was completed, the reaction was continued for 3 hours. All reactions were carried out under uniform stirring of the solution at a speed of 400 r / min. After the reaction was completed, the reaction products were collected by centrifugation, washed more than three times with ultrapure water, and dried in a vacuum oven at 50°C for 3 hours to obtain a Cu2O@SiO2 core-shell composite material uniformly coated with amorphous organic SiO2.

[0050] (3) In the same way as in Specific Example 1, a mesoscopic porous core-shell dielectric resonant photothermal catalytic system with a thicker P-SiO2 shell (i.e., Cu2O@P-SiO2 core-shell structure composite) was prepared.

[0051] Subsequent testing was performed as in Example 1.

[0052] Comparative Example 1 The step of soaking the SiO2 shell in alkaline sodium hydroxide solution to create pores in step (3) was not performed; all other operations were the same as in specific embodiment 1. (1) Same as Specific Implementation Example 1; (2) In the same way as in Specific Example 1, a Cu2O core-shell composite Cu2O@SiO2 with uniform SiO2 coating was prepared.

[0053] Subsequent testing is as described in Specific Example 1.

[0054] The XRD characterization of Cu2O@SiO2 obtained in Comparative Example 1 is as follows: Figure 3a As shown in (ii), the diffraction peaks at 29.75°, 36.43°, 42.26°, 52.47°, 61.43°, 73.74° and 77.52° correspond to the (110), (111), (200), (211), (220), (311) and (222) crystal planes of cubic Cu2O, and no characteristic peaks of SiO2 are present, indicating that SiO2 in the Cu2O@SiO2 sample appears in an amorphous form. Figure 3b The Raman spectrum in (ii) further characterizes the bonding state of the material surface. In addition to the characteristic peak of Cu2O, the Raman spectrum of the Cu2O@SiO2 sample shows a peak at 1020 cm⁻¹. -1 The presence of an asymmetric vibrational peak in the Si-O-Si region further indicates the presence of organic silicon-oxygen compounds on the surface of the Cu2O substrate. The SEM characterization of Cu2O@SiO2 obtained in Comparative Example 1 is as follows: Figure 4b As shown, a thin coating is visible on the surface of Cu2O@SiO2, indicating successful organosilicon coating. The TEM characterization of Cu2O@SiO2 obtained in Comparative Example 1 is as follows: Figure 5b As shown, after silicone coating, the material surface is uniformly covered with a thin layer of lighter color. Figure 5d enlarge Figure 5b The area marked by the yellow box in the middle is used to explore the thickness of the surface organosilicon layer. It can be observed that the thickness of the surface organosilicon layer is approximately 8 nm. The infrared thermal image of Cu2O@SiO2 obtained in Comparative Example 1 is shown below. Figure 6a As shown in Figure (1), Cu2O@SiO2 has the lowest apparent temperature, with the lowest temperature reading from the infrared camera being 45 °C. This may be because the surface-coated silicone is too uniform and dense, affecting the material's light absorption efficiency. Figure 6b The surface temperature of the Cu2O@SiO2 sample rapidly increased within 2 minutes, then stabilized, with an average surface temperature of 45 °C. Figure 7 As shown, Cu2O@SiO2 exhibits the lowest photothermal catalytic ammonia production efficiency, at 100.511 μmol / h. -1 g -1 This may be because the uniform and dense organosilicon coating on the surface not only affects the material's light absorption efficiency but also hinders the contact between the reactants nitrogen and water and the active sites on the Cu2O core surface. The photothermal catalytic ammonia production efficiency of Cu2O@P-SiO2 in Example 1 is 2.78 times that of Cu2O@SiO2.

[0055] Comparative Example 2 The steps of coating Cu2O with SiO2 in step (2) and creating pores by soaking the SiO2 shell in alkaline sodium hydroxide solution in step (3) were not performed. All other operations were the same as in specific embodiment 1. (1) In the same way as in Specific Example 1, cubic Cu2O nanoparticles were prepared; The XRD characterization of Cu2O obtained in Comparative Example 2 is as follows: Figure 3a As shown in (iii), the diffraction peaks at 29.75°, 36.43°, 42.26°, 52.47°, 61.43°, 73.74° and 77.52° correspond to the (110), (111), (200), (211), (220), (311) and (222) crystal planes of cubic Cu2O, indicating the successful synthesis of Cu2O. Figure 3b The Raman spectrum in (iii) further characterized the characteristic peaks of Cu₂O. The SEM characterization of Cu₂O obtained in Comparative Example 2 is as follows: Figure 4a As shown, Cu₂O exhibits a typical cubic morphology, consistent with the crystal form obtained from the XRD patterns described above. The TEM characterization of Cu₂O obtained in Comparative Example 2 is as follows: Figure 5a As shown, the Cu₂O sample exhibits a regular cubic structure. The infrared thermal image of the Cu₂O obtained in Comparative Example 2 is shown below. Figure 6a As shown in (2), the apparent temperature of Cu2O is moderate as read by the infrared camera. Corresponding to Figure 6b The surface temperature of the Cu₂O sample increased rapidly within 2 minutes, then stabilized, with an average surface temperature of 61.5 °C. Figure 7 As shown, the photothermal catalytic ammonia production efficiency of Cu2O is moderate, at 111.442 μmol / h. -1 g -1 The Cu2O@P-SiO2 in Example 1 is 2.50 times that of Cu2O.

[0056] In addition, the applicant also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.

[0057] It should be understood that the technical solutions of the present invention are not limited to the specific embodiments described above. Any technical modifications made to the technical solutions of the present invention without departing from the spirit and scope of the claims are within the scope of protection of the present invention.

Claims

1. A method for preparing a mesoscopic porous core-shell dielectric resonant photothermal catalytic system, characterized in that, include: Make Cu 2+ Source, OH - Cu2O nanoparticles were prepared by reacting a mixture of source and L-ascorbic acid. An organosilicon precursor was in situ coated onto the surface of cubic Cu2O nanoparticles using the sol-gel method to prepare a Cu2O core-shell composite uniformly coated with amorphous organic SiO2. Furthermore, the Cu2O core-shell structure composite uniformly coated with amorphous organic SiO2 is immersed in an alkaline solution to form a Cu2O nanoparticle core-shell structure composite uniformly coated with porous organic P-SiO2, thereby obtaining a mesoscopic porous core-shell dielectric resonant photothermal catalytic system.

2. The preparation method according to claim 1, characterized in that, Specifically, it includes: Cu 2+ The source is mixed with water and OH is added. - The source was then added with L-ascorbic acid under stirring and the reaction was continued for 30-60 min. After centrifugation, washing and vacuum drying, cubic Cu2O nanoparticles were obtained.

3. The preparation method according to claim 2, characterized in that: The Cu 2+ Cu in the source 2+ With OH - OH in the source - The molar ratio is 1:20 to 1:2; And / or, the Cu 2+ Cu in the source 2+ The molar ratio with L-ascorbic acid is 1:1; And / or, the Cu 2+ The source includes water-soluble divalent copper salts, wherein the water-soluble divalent copper salts include any one or more combinations of CuCl2·2H2O, CuSO4·5H2O, and anhydrous CuSO4; And / or, the OH - Sources include NaOH and / or KOH.

4. The preparation method according to claim 1, characterized in that, Specifically, it includes: Cu2O nanoparticles were dispersed in ethanol to form a Cu2O nanoparticle dispersion. Ethanol and organic orthosilicate are mixed to form a first mixed solution; Ethanol and water are mixed and the pH is adjusted to 4-6 using oxalic acid solution to form a second mixed solution; Furthermore, the second mixed solution, the epoxy-containing trialkoxysilane, and the first mixed solution are mixed and stirred for 3-5 hours. Then, Cu2O nanoparticle dispersion is added and the mixture is stirred and stirred for another 3-5 hours. Finally, the mixture is centrifuged, washed, and vacuum dried to obtain a Cu2O core-shell structured composite uniformly coated with amorphous organic SiO2.

5. The preparation method according to claim 4, characterized in that: The organosilicone esters include any one or more combinations of methyl orthosilicate, ethyl orthosilicate, and propyl orthosilicate; And / or, the epoxy-containing trialkoxysilane includes γ-glycidoxypropyltrimethoxysilane; And / or, the volume ratio of ethanol to organosilicone ester in the first mixed solution is 20:1 to 80:1; And / or, the volume of ethanol in the first mixed solution is the same as that in the second mixed solution; And / or, the volume ratio of water in the second mixed solution to the organosilicone ester in the first mixed solution is 1:5; And / or, the concentration of the oxalic acid solution is 0.5~1.5 mol / L; And / or, the epoxy-containing trialkoxysilane has the same volume as the water in the second mixed solution.

6. The preparation method according to claim 1, characterized in that, Specifically, it includes: The Cu2O core-shell structured composite uniformly coated with amorphous organic SiO2 was immersed in an alkaline solution with a pH of 8-10 for 1-3 hours, and then centrifuged, washed and dried to form a porous organic P-SiO2 uniformly coated Cu2O nanoparticle core-shell structured composite.

7. The mesoscopic porous core-shell dielectric resonant photothermal catalytic system prepared by the method according to any one of claims 1-6, characterized in that, include: The core consists of cubic Cu2O nanoparticles and a porous organic P-SiO2 shell on the surface.

8. The mesoscopic porous core-shell dielectric resonant photothermal catalytic system according to claim 7, characterized in that: The cubic Cu2O nanoparticles have a side length of 300–900 nm; And / or, the thickness of the porous organic P-SiO2 shell is 10–150 nm; And / or, the pore size of the pores contained in the porous organic P-SiO2 shell is 3 to 30 nm.

9. The application of the mesoscopic porous core-shell dielectric resonant photothermal catalytic system according to claim 7 or 8 in interfacial nitrogen fixation.

10. A method for interfacial photothermal catalytic nitrogen fixation, characterized in that, include: Provide the mesoscopic porous core-shell dielectric resonant photothermal catalytic system as described in claim 7 or 8; Furthermore, the mesoscopic porous core-shell dielectric resonant photothermal catalytic system is mixed with an ethanol solution and placed in a photocatalytic reaction device. Then, N2 is introduced at a constant rate to maintain the nitrogen saturation state of the system, and then the interfacial photothermal catalytic nitrogen fixation reaction is carried out under the irradiation of the solar spectrum simulated by a xenon lamp light source.

Citation Information

Patent Citations

  • Method for preparing Cu2O / SiO2 core-shell structure nano material

    CN102923755A

  • Supported yolk-eggshell structure nano-catalyst and preparation method thereof

    CN111215147A