Preparation method and application of a composite functional catalytic material
The Pd-FeWO4-HZSM-5 composite catalytic material was prepared in one step, which solved the safety and high energy consumption problems of low-concentration organic waste gas treatment and achieved low-cost and high-efficiency adsorption and catalytic degradation effects.
Patent Information
- Application Number
- CN202611361477.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-09-03
AI Technical Summary
Existing technologies are insufficient for efficiently and cost-effectively treating low-concentration, low-value-added organic waste gases, especially those containing pollutants such as chlorobenzene and toluene. Furthermore, traditional methods pose safety risks and high energy consumption issues.
A one-step method was used to prepare Pd-FeWO4-HZSM-5 composite functional catalytic material. The mixture was mechanically ground and calcined to form a catalyst with a special pore structure and acid properties, which was used for the adsorption and catalytic degradation of organic waste gas.
It achieves efficient adsorption, concentration, and deep mineralization of low-concentration organic waste gas, with lower degradation temperature, higher safety, lower cost, and better performance than traditional methods.
Smart Images

Figure CN122850248B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalytic materials technology, and more specifically, to a method for preparing and applying a composite functional catalytic material. Background Technology
[0002] The catalytic effects of catalytic materials mainly include acid-base catalysis, redox catalysis, coordination catalysis, and bioenzyme catalysis. Each type of catalytic material has its own unique application area and is specific. However, some catalytic reactions require the joint participation of different catalytically active sites. For example, the chemical process of converting n-hexane to cyclohexene requires a dehydrogenation catalyst to form a double bond, and simultaneously requires acid centers to achieve carbon skeleton isomerization and form a cyclic structure. This is usually achieved using a Pd / γ-Al2O3 bifunctional catalyst, where Pd provides redox active centers and γ-Al2O3 provides surface acidic centers. With the rapid development of the chemical industry and the increasing demand for new materials, the research and development of composite functional materials integrating multiple functions has become increasingly urgent. In addition, many chemical reaction processes often involve harsh operating conditions such as high temperature, high pressure, and strong acid corrosion, thus placing higher demands on the research and development of high-performance catalytic materials.
[0003] Polyurethane materials are widely used due to their superior performance and are hailed as the "sixth largest plastic." During their synthesis, foaming agents are needed to control the internal pore structure of the material. Traditional foaming agents are usually chlorofluorocarbons (CFCs), which are highly harmful to the environment, especially depleting the ozone layer, and have therefore been gradually phased out in recent years. Newer foaming agents, such as cyclopentane and n-pentane, are organic compounds with high saturated vapor pressures and are easily volatilized into the environment, posing significant harm to human health and the environment, and failing to meet environmental protection requirements. Benzene, toluene, and acetone are commonly used as organic solvents or diluents in the synthesis of compounds and are widely used in industrial and agricultural production. If discharged into the environment without treatment, they will cause serious harm. Therefore, the efficient and thorough treatment of conventional hydrocarbons such as pentane, benzene, toluene, xylene, and acetone, as well as halogenated organic waste gas pollutants such as CFCs, dichloromethane, chlorobenzene, and p-chlorotoluene, is particularly urgent.
[0004] Currently, for high-concentration, high-value-added organic waste gases, activated carbon and other materials are typically used for adsorption, or ultra-low temperature condensation is used for recycling and reuse, achieving gas purification and compliance with emission standards. For low-concentration, low-value-added organic pollutants, a common treatment method is room-temperature activated carbon adsorption followed by high-temperature incineration (operating temperature above 850℃, and the equipment needs to operate continuously for extended periods), completely converting the pollutants into carbon dioxide and water. However, activated carbon after adsorbing organic matter is classified as hazardous waste, posing a high safety risk during storage, transportation, and treatment due to its flammability and explosiveness, requiring strict adherence to safety operating procedures. Therefore, there is an urgent need to develop a high-performance, low-cost, and long-term usable integrated catalyst for "adsorption concentration-catalytic degradation," utilizing acid centers to break the benzene ring structure and C-Cl bonds, and oxidation centers to achieve deep mineralization of organic byproducts, thus meeting the requirements of catalytic combustion technology and ensuring efficient treatment and compliance with emission standards for organic waste gases. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing and applying composite functional catalytic materials.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A method for preparing a composite functional catalytic material includes the following steps:
[0008] (a) Palladium nitrate aqueous solution, ferric nitrate nonahydrate, ammonium metatungstate hydrate, HZSM-5 molecular sieve and citric acid monohydrate were ground at room temperature to obtain a mixture;
[0009] (b) The mixture is dried and then calcined and cooled to room temperature to obtain a composite functional catalytic material.
[0010] Furthermore, in step (a), ferric nitrate nonahydrate, ammonium metatungstate hydrate, HZSM-5 molecular sieve, and palladium nitrate aqueous solution are added according to the following proportions: Fe / W molar ratio of 1 / 1, FeWO4 to HZSM-5 mass ratio of 1 / 1, and Pd content of 0.1-0.7% of the total mass of the target final product. The mass ratio of HZSM-5 molecular sieve to citric acid monohydrate is 1:9.6-9.9.
[0011] Furthermore, in step (b), the roasting is carried out in an air atmosphere.
[0012] Furthermore, in step (b), the calcination temperature is 500-800℃ and the calcination time is 100-150min.
[0013] An application of a composite functional catalytic material prepared according to the above method, wherein the catalytic material is used for adsorption and catalytic degradation of organic waste gas.
[0014] Furthermore, the organic waste gas is a gas containing at least one of chlorobenzene, toluene, and p-chlorotoluene.
[0015] Furthermore, the reaction temperature for catalytic degradation of organic waste gas is 160-400℃.
[0016] In summary, the present invention has the following beneficial effects:
[0017] (1) The preparation method of the composite functional catalytic material of the present invention has significant advantages such as safe operation, simple route and low cost.
[0018] (2) The composite functional catalytic material of the present invention has a special pore structure, solid acid properties and deep oxidation ability.
[0019] (3) The composite functional catalytic material developed in this invention has good treatment effects on room temperature adsorption concentration and heated catalytic purification of typical organic pollutants such as toluene, chlorobenzene and p-chlorotoluene. It can eliminate environmental pollutants efficiently and at low cost. Its saturated adsorption performance and catalytic degradation performance are significantly better than those of catalytic materials prepared by conventional impregnation method and sol-gel method. Attached Figure Description
[0020] Figure 1 The graph shows the adsorption performance test results of FeWO4 on toluene and chlorobenzene in a mixture of toluene and chlorobenzene and HZSM-5 molecular sieve on toluene and chlorobenzene in a mixture of toluene and chlorobenzene.
[0021] Figure 2 The graph shows the adsorption performance test results of the catalytic materials prepared in Example 3, Comparative Example 2, and Comparative Example 4 on toluene in a mixture of toluene and chlorobenzene.
[0022] Figure 3 The graph shows the adsorption performance test results of the catalytic materials prepared in Example 3, Comparative Example 2, and Comparative Example 4 on chlorobenzene in a mixture of toluene and chlorobenzene.
[0023] Figure 4 The graph shows the toluene conversion rate test results of the catalytic materials prepared in Comparative Example 1 and Examples 1-4 at different reaction temperatures for the catalytic degradation of a toluene-chlorobenzene mixture.
[0024] Figure 5 The graph shows the chlorobenzene conversion rate test results of the catalytic materials prepared in Comparative Example 1 and Examples 1-4 at different reaction temperatures for the catalytic degradation of a mixture of toluene and chlorobenzene.
[0025] Figure 6 The graph shows the test results of the total conversion of toluene and chlorobenzene in the catalytic degradation of a mixture of toluene and chlorobenzene by the catalytic materials prepared in Comparative Example 1 and Examples 1-4 at different reaction temperatures;
[0026] Figure 7 The graph shows the toluene conversion rate test results of the catalytic materials prepared in Example 3, Comparative Examples 2 and 4 at different reaction temperatures for catalytic degradation of a toluene-chlorobenzene mixture.
[0027] Figure 8 The graph shows the chlorobenzene conversion rate test results of the catalytic materials prepared in Example 3, Comparative Examples 2 and 4 at different reaction temperatures for catalytic degradation of a mixture of toluene and chlorobenzene.
[0028] Figure 9 The graph shows the test results of the total conversion of toluene and chlorobenzene in the catalytic degradation of a mixture of toluene and chlorobenzene by the catalytic materials prepared in Example 3, Comparative Examples 2 and 4 at different reaction temperatures;
[0029] Figure 10 The graph shows the toluene conversion rate test results of the catalytic materials prepared in Example 5, Comparative Example 3 and Comparative Example 5 at different reaction temperatures for catalytic degradation of a toluene-chlorobenzene mixture.
[0030] Figure 11 The graph shows the chlorobenzene conversion rate test results of the catalytic materials prepared in Example 5, Comparative Example 3 and Comparative Example 5 at different reaction temperatures for catalytic degradation of a mixture of toluene and chlorobenzene.
[0031] Figure 12 The graph shows the test results of the total conversion of toluene and chlorobenzene in the catalytic degradation of a mixture of toluene and chlorobenzene at different reaction temperatures using the catalytic materials prepared in Example 5, Comparative Example 3, and Comparative Example 5.
[0032] Figure 13 The graph shows the H2-TPR test results of the catalytic materials prepared in Example 3, Comparative Example 2 and Comparative Example 4, and FeWO4 and HZSM-5 molecular sieve.
[0033] Figure 14 Transmission electron microscopy (TEM) images of the catalytic materials prepared in Examples 3, 2, and 4, and of FeWO4 and HZSM-5 molecular sieves. Figure 14 (a) Partial to Figure 14 (d) consists of transmission electron microscopy images of the catalytic materials and FeWO4 prepared in Example 3, Comparative Example 2, and Comparative Example 4, respectively. Figure 14 (e) Part to Figure 14 (f) shows transmission electron microscopy images of HZSM-5 molecular sieve at different magnifications.
[0034] Figure 15 The N2 adsorption-desorption curves of the catalytic materials and FeWO4 prepared in Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 4 are shown.
[0035] Figure 16The pore size distribution curves of the catalytic materials and FeWO4 prepared in Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 4 are shown.
[0036] Figure 17 The XRD patterns of the catalysts and FeWO4 prepared in Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 4 are shown.
[0037] Figure 18 The images show the laser confocal Raman spectra of the catalytic materials and FeWO4 prepared in Examples 3, 1, 2 and 4. Detailed Implementation
[0038] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0039] The composite functional catalytic material of this invention can be used for adsorption and catalytic degradation of organic waste gas (gas containing at least one of chlorobenzene, toluene, and p-chlorotoluene). The preparation method is as follows:
[0040] (a) Palladium nitrate aqueous solution, ferric nitrate nonahydrate, ammonium metatungstate hydrate, HZSM-5 molecular sieve, and citric acid monohydrate are mechanically ground at room temperature to obtain a mixture; ferric nitrate nonahydrate, ammonium metatungstate hydrate, HZSM-5 molecular sieve, and palladium nitrate aqueous solution are added according to the following proportions: Fe / W molar ratio of 1 / 1, FeWO4 to HZSM-5 mass ratio of 1 / 1, and Pd content of 0.1-0.7% of the total mass of the target final product; the mass ratio of HZSM-5 molecular sieve to citric acid monohydrate is 1:9.6-9.9.
[0041] (b) After drying the mixture, it is calcined in air (calcination temperature is 500-800℃, calcination time is 100-150min; during calcination, palladium nitrate decomposes into Pd, iron nitrate and ammonium metatungstate are converted into FeWO4, citric acid decomposes into CO2 and H2O, and HZSM-5 molecular sieve remains unchanged), and then cooled to room temperature to obtain composite functional catalytic material.
[0042] This invention enables the synthesis of a Pd-FeWO4-HZSM-5 three-component composite functional catalytic material through a one-step, concise preparation process. In contrast, catalytic materials prepared using traditional impregnation or sol-gel methods require large amounts of water, and the Pd species in the synthesized catalytic material tend to agglomerate into larger particles, thus reducing the catalytic material's performance. The composite functional catalytic material synthesized in this invention utilizes the abundant pore structure of HZSM-5 molecular sieves (containing only Si, Al, and O elements) to concentrate and enrich organic waste gases (containing toluene, chlorobenzene, p-chlorotoluene, etc.) and adsorb them onto the inner and outer surfaces of the catalytic material, ensuring that the gas treated by adsorption meets emission standards. Furthermore, it can catalytically decompose organic pollutants into carbon dioxide, water, and hydrogen chloride at a certain reaction temperature, achieving complete mineralization. The exhaust gas after catalytic decomposition can be passed into soda lime water for fixation, thereby completely eliminating the pollutants.
[0043] The catalytic material synthesized in this invention possesses the deep oxidation capability of the noble metal Pd, the high-temperature resistance and oxidation-promoting capacity of the transition metal composite oxide FeWO4, and the dispersing and adsorption capacity of the HZSM-5 molecular sieve, achieving a synergistic effect of the three components. Compared with the direct high-temperature incineration treatment of organic pollutants, the catalytic material of this invention has a lower reaction temperature (160-400℃) for the catalytic degradation of organic matter, exhibiting significant energy-saving advantages.
[0044] Example 1
[0045] Palladium nitrate aqueous solution, ferric nitrate nonahydrate, ammonium metatungstate hydrate (molecular weight 2956.26), HZSM-5 molecular sieve (Si / Al molar ratio = 25, purchased from Tianjin Nanhua Catalyst Co., Ltd.), and citric acid monohydrate were mechanically ground for 40 minutes at room temperature (palladium nitrate aqueous solution concentration 0.217 mol / L, HZSM-5 molecular sieve addition amount 2.0384 g, citric acid monohydrate addition amount 19.62 g, ferric nitrate nonahydrate, ammonium metatungstate hydrate, and palladium nitrate aqueous solution concentration...). The addition amount was based on the following proportions: Fe / W molar ratio of 1 / 1, FeWO4 to HZSM-5 mass ratio of 1 / 1, and Pd content of 0.1% of the total mass of the target final product. The ground mixture was transferred to a crucible, dried at 110°C, and then placed in a muffle furnace. The temperature was increased to 500°C at a rate of 10°C / min, and calcined at this temperature in an air atmosphere for 120 minutes. After calcination, the mixture was naturally cooled to room temperature to obtain the composite functional catalytic material (named 0.1Pd-FeWZ).
[0046] Example 2
[0047] The composite functional catalytic material (named 0.3Pd-FeWZ) was prepared according to the method of Example 1, but the raw materials were added in proportions such that the Fe / W molar ratio in the target final product was 1 / 1, the mass ratio of FeWO4 to HZSM-5 was 1 / 1, and the Pd content was 0.3% of the total mass of the target final product.
[0048] Example 3
[0049] The composite functional catalytic material (named 0.5Pd-FeWZ) was prepared according to the method of Example 1, but the raw materials were added in proportions such that the Fe / W molar ratio in the target final product was 1 / 1, the mass ratio of FeWO4 to HZSM-5 was 1 / 1, and the Pd content was 0.5% of the total mass of the target final product.
[0050] Example 4
[0051] The composite functional catalytic material (named 0.7Pd-FeWZ) was prepared according to the method of Example 1, but the raw materials were added in proportions such that the Fe / W molar ratio in the target final product was 1 / 1, the mass ratio of FeWO4 to HZSM-5 was 1 / 1, and the Pd content was 0.7% of the total mass of the target final product.
[0052] Example 5
[0053] The composite functional catalytic material (named Pd-FeWZ-800) was prepared according to the method in Example 3. The Fe / W molar ratio in the target final product was 1 / 1, the mass ratio of FeWO4 to HZSM-5 was 1 / 1, and the Pd content was 0.5% of the total mass of the target final product. The difference was that the calcination temperature was changed to 800℃.
[0054] Comparative Example 1
[0055] The catalytic material (named FeW-Z) was prepared according to the method in Example 1, except that palladium nitrate was not added.
[0056] Comparative Example 2
[0057] The catalytic material (named Pd / FeWZ) was prepared by impregnation method, namely: ferric nitrate nonahydrate, ammonium metatungstate hydrate (molecular weight 2956.26), HZSM-5 molecular sieve, and citric acid monohydrate were mechanically ground at room temperature for 40 minutes. The ground mixture was then transferred to a crucible and placed in a muffle furnace. The temperature was increased from room temperature to 500°C at a rate of 10°C / min, and then calcined at this temperature in an air atmosphere for 120 minutes. After cooling, the obtained product was added to a 0.217 mol / L palladium nitrate aqueous solution and impregnated at room temperature for 12 hours. After evaporation at 80°C and drying at 110°C, it was calcined at 450°C for 120 minutes and then naturally cooled to room temperature to obtain the catalyst material (during the preparation process, the amount of HZSM-5 molecular sieve added was 2.0384 g, the amount of citric acid monohydrate added was 19.62 g, and the amounts of ferric nitrate nonahydrate, ammonium metatungstate hydrate, and palladium nitrate aqueous solution were added according to the following proportions: Fe / W molar ratio of 1 / 1, FeWO4 to HZSM-5 mass ratio of 1 / 1, and Pd content of 0.5% of the total mass of the target final product).
[0058] Comparative Example 3
[0059] The catalytic material (named Pd / FeWZ-800) was prepared according to the method of Comparative Example 2, except that it was impregnated with palladium nitrate aqueous solution at room temperature, heated and evaporated at 80°C, dried at 110°C, and then calcined at 800°C for 120 minutes.
[0060] Comparative Example 4
[0061] The catalytic material (named Pd / Z-FeW) was prepared using the sol-gel method, namely: HZSM-5 molecular sieve was added to an aqueous solution of palladium nitrate (0.217 mol / L), impregnated at room temperature for 12 hours, evaporated at 80℃, dried at 110℃, calcined at 450℃ for 120 minutes, and then naturally cooled to room temperature; the product was then added to an aqueous solution containing ferric nitrate nonahydrate, ammonium metatungstate hydrate (molecular weight 2956.26), and citric acid monohydrate, stirred at 80℃ for 4 hours, dried at 110℃, and then calcined at 500℃ for 120 minutes. After natural cooling to room temperature, the catalytic material was obtained (during the preparation process, the amount of HZSM-5 molecular sieve added was 0.998g, the amount of citric acid monohydrate added was 9.73g; the amount of water added to the aqueous solution containing ferric nitrate nonahydrate and ammonium metatungstate hydrate (molecular weight 2956.26) and citric acid monohydrate was 70g; the aqueous solutions of ferric nitrate nonahydrate, ammonium metatungstate hydrate, and palladium nitrate were added according to the following proportions: Fe / W molar ratio of 1 / 1, FeWO4 to HZSM-5 mass ratio of 1 / 1, and Pd content of 0.5% of the total mass of the target final product).
[0062] Comparative Example 5
[0063] The catalytic material (named Pd / Z-FeW-800) was prepared according to the method of Comparative Example 4, except that "calcination at 500℃ for 120 minutes" was changed to "calcination at 800℃ for 120 minutes".
[0064] Application examples
[0065] The catalytic materials obtained in the above examples and comparative examples are used to adsorb and catalytically degrade organic waste gas (containing at least one of organic pollutants such as toluene, chlorobenzene, and p-chlorotoluene).
[0066] (1) Test of the adsorption performance of catalytic materials for organic waste gas
[0067] The test method is as follows: The powder sample of the catalyst material to be tested is compressed into tablets using a tablet press, pulverized, and sieved to obtain particles of 40-60 mesh size; the particles (0.500g) are placed in a quartz glass tube (6mm×20cm) and heated to 400℃ for 30 minutes in an air flow (30mL / min) to remove physically adsorbed substances such as moisture and carbon dioxide. After cooling to 50℃, a mixture of toluene and chlorobenzene (i.e., a mixture of toluene, chlorobenzene, and air, with the concentrations of toluene and chlorobenzene both at 500ppm, and dry air as the equilibrium gas at a flow rate of 4.5L / h) is introduced to simulate the working conditions of industrial organic waste gas for adsorption experiments; the outlet exhaust gas is introduced into a gas chromatograph to detect the change in the concentration of escaping organic matter over time, and the adsorption performance data of the catalyst material are obtained.
[0068] The adsorption performance test results of FeWO4 on toluene and chlorobenzene in a mixture of toluene and chlorobenzene and the adsorption performance test results of HZSM-5 molecular sieve on toluene and chlorobenzene in a mixture of toluene and chlorobenzene are shown in the figure. Figure 1 The adsorption performance test results of the catalytic materials prepared in Examples 3, 2, and 4 for toluene and chlorobenzene in a mixture of toluene and chlorobenzene are shown in the figure. Figures 2-3 The results showed that the saturated adsorption performance of the catalytic material prepared by the method of the present invention for organic pollutants (toluene and chlorobenzene) was better than that of the catalytic materials synthesized by the conventional impregnation method and the sol-gel method (the time required for the catalytic material prepared in Example 3 to reach adsorption saturation for toluene and chlorobenzene was greater than 65 minutes). The time for the catalytic material prepared by the method of the present invention to maintain 100% adsorption rate of organic pollutants (toluene and chlorobenzene) was between that of the catalytic materials synthesized by the conventional impregnation method and the sol-gel method.
[0069] (2) Test of the catalytic degradation performance of catalytic materials on organic waste gas:
[0070] The test method was as follows: The powder sample of the catalytic material to be tested was compressed into tablets using a tablet press, pulverized, and sieved to obtain particles of 40-60 mesh size. 0.500 g of the particles were placed in a quartz glass tube (6 mm × 20 cm) and heated to 400°C for 30 minutes in an air flow (30 mL / min) to remove physically adsorbed moisture, carbon dioxide, and other substances. After cooling to 50°C, a mixture of toluene and chlorobenzene (i.e., a mixture of toluene, chlorobenzene, and air, with both toluene and chlorobenzene concentrations of 500 ppm, and dry air as the equilibrium gas at a flow rate of 4.5 L / h) was introduced. The apparatus was then heated to a specific temperature and maintained at this temperature for 30 minutes to test the catalytic performance. The outlet exhaust gas was passed into a gas chromatograph to detect the concentration of escaping organic matter over time, obtaining data on the catalytic degradation performance of the material. The catalytic degradation reaction temperatures in the experiment were 160°C, 200°C, 240°C, 280°C, 320°C, 360°C, and 400°C.
[0071] The test results of the toluene conversion, chlorobenzene conversion, and total toluene and chlorobenzene conversion of the catalytic materials prepared in Comparative Example 1 and Examples 1-4 at different reaction temperatures are shown in the figure. Figures 4-6 The test results of the toluene conversion rate, chlorobenzene conversion rate, and total toluene and chlorobenzene conversion rate of the catalytic materials prepared in Examples 3, 2, and 4 at different reaction temperatures are shown in the table below. Figures 7-9 The test results of the toluene conversion rate, chlorobenzene conversion rate, and total toluene and chlorobenzene conversion rate of the catalytic materials prepared in Examples 5, 3, and 5 at different reaction temperatures for catalytic degradation of a toluene-chlorobenzene mixture are shown in the figures. Figures 10-12 .
[0072] Table 1 shows the reaction temperatures at which the toluene conversion rate, chlorobenzene conversion rate, and total toluene and chlorobenzene conversion rate reached 90% in the catalytic degradation performance tests of different catalytic materials.
[0073] Table 1
[0074]
[0075] The catalytic degradation performance test results show that although only a very small amount of the noble metal Pd (content 0.1-0.7 wt%) is added to the catalytic material prepared by the method of the present invention, it can still eliminate pollutants at a relatively low reaction temperature during the catalytic degradation of toluene and chlorobenzene, which is significantly better than the sample without the addition of noble metal (prepared by Comparative Example 1). Compared with the conventional impregnation method (Comparative Example 2, Comparative Example 3) and sol-gel method (Comparative Example 4, Comparative Example 5) in the prior art, the catalytic material prepared by the method of the present invention has the lowest reaction temperature, the best catalyst performance, and the lowest energy consumption during the catalytic degradation of toluene and chlorobenzene, and has obvious environmental protection and energy saving advantages.
[0076] (3) Redox performance test of catalytic materials
[0077] The test method is as follows: The powder sample of the catalyst to be tested is compressed into tablets using a tablet press, pulverized and sieved to obtain particles of 40-60 mesh size. The particles (0.100g) are placed in a quartz glass tube (6mm×20cm) and heated to 400℃ for 30 minutes in an air flow (30mL / min) to remove physically adsorbed substances such as moisture and carbon dioxide. Then, N2 gas (30mL / min) is passed through to purge, and the temperature is cooled to 30℃. A mixture of H2 / N2 gas (5%H2+95%N2, flow rate 30mL / min) is then introduced. After the baseline of the gas chromatography stabilizes, the temperature is increased to 930℃ at a rate of 10℃ / min to conduct a hydrogen reduction test. The changes in gas composition are detected by a gas chromatograph equipped with a TCD detector.
[0078] The H2-TPR test results of the catalytic materials prepared in Examples 3, 2, and 4, and FeWO4 and HZSM-5 molecular sieves are shown in the figure. Figure 13 .
[0079] Furthermore, transmission electron microscopy (TEM) images of the catalytic materials prepared in Examples 3, 2, and 4, as well as FeWO4 and HZSM-5 molecular sieves, are shown below. Figure 14 The N2 adsorption-desorption curves and pore size distribution curves of the catalytic materials and FeWO4 prepared in Examples 3, 1, 2, and 4 are shown in the figures. Figure 15 , Figure 16 The XRD patterns and laser confocal Raman spectra of the catalytic materials and FeWO4 prepared in Examples 3, 1, 2, and 4 are shown below. Figure 17 , Figure 18 .
[0080] Depend on Figure 13 and Figure 14 It can be seen that although the Pd element content of the catalytic materials prepared in Example 3, Comparative Example 2 and Comparative Example 4 is the same, there are significant differences in the morphology and redox performance of the catalytic material samples obtained by different preparation methods. Compared with the comparative examples, the sample obtained by the preparation method of the present invention has a more uniform dispersion of metal components on the surface of molecular sieve and the best redox performance. Therefore, it exhibits the best pollutant removal ability and has significant application advantages.
[0081] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a composite functional catalytic material, characterized in that, Includes the following steps: (a) Palladium nitrate aqueous solution, ferric nitrate nonahydrate, ammonium metatungstate hydrate, HZSM-5 molecular sieve and citric acid monohydrate were ground at room temperature to obtain a mixture; (b) The mixture is dried and then calcined, and cooled to room temperature to obtain a composite functional catalytic material; In step (a), ferric nitrate nonahydrate, ammonium metatungstate hydrate, HZSM-5 molecular sieve, and palladium nitrate aqueous solution are added according to the following proportions: Fe / W molar ratio of 1 / 1, FeWO4 to HZSM-5 mass ratio of 1 / 1, and Pd content of 0.1-0.7% of the total mass of the target final product. The mass ratio of HZSM-5 molecular sieve to citric acid monohydrate is 1:9.6-9.
9. In step (b), the calcination is carried out in an air atmosphere at a temperature of 500-800℃ for 100-150 minutes.
2. An application of the composite functional catalytic material prepared according to claim 1, characterized in that, The catalytic material is used to adsorb and catalytically degrade organic waste gas, which is chlorobenzene and / or toluene.
3. The application of the composite functional catalytic material according to claim 2, characterized in that, The reaction temperature for catalytic degradation of organic waste gas is 160-400℃.
Citation Information
Patent Citations
Synthesis method and application of W-Fe-O composite metal oxide catalyst
CN112371133A
Diesel vehicle tail gas hydrocarbon substance catalytic oxidation adsorbent as well as preparation method and application thereof
CN121178122A