Composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions and its preparation method

The preparation of composite materials by co-pyrolysis of biomass and mineral tailings solves the problem of insufficient resource utilization of mineral tailings and biomass waste, and achieves simultaneous and efficient removal of phosphate, ammonia nitrogen and fluoride, simplifying the process and reducing costs.

CN123059614APending Publication Date: 2026-11-10WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611526366.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies do not fully utilize the resources of mineral tailings and agricultural and forestry biomass waste. Traditional water treatment materials are unable to remove phosphates, ammonia nitrogen and fluorides simultaneously. Furthermore, existing biochar-based composite material treatment processes are complex and costly, making it difficult to achieve direct and simultaneous adsorption and removal of multiple pollutants.

Method used

By mixing biomass with mineral tailings at least twice its mass and pyrolyzing it under anaerobic or hypoxic conditions, a composite material is prepared. Utilizing the activation of the mineral tailings and the synergistic effect of the biomass carbon skeleton during the co-pyrolysis process, a composite material with high specific surface area and mesoporous structure is formed, achieving the simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions.

Benefits of technology

It achieves a high simultaneous removal rate of phosphate, ammonia nitrogen, and fluoride ions in water, reaching over 85%, reducing treatment costs and simplifying the process, and has good prospects for engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123059614A_ABST
    Figure CN123059614A_ABST
Patent Text Reader

Abstract

This invention relates to a composite material for the simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions, and its preparation method. The preparation method includes mixing biomass with mineral tailings at least twice the mass of the biomass, followed by pyrolysis under anaerobic or anoxic conditions to obtain the composite material for the simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions. This invention eliminates the need for additional chemical modifiers such as metal salts; the composite material is obtained through the co-pyrolysis of mineral tailings and biomass. Co-pyrolysis induces the transformation of the carbonate mineral phase in the mineral tailings into the active oxide phase, simultaneously forming a well-developed mesoporous structure. This provides conditions for the precipitation, fixation, and solution mass transfer of anionic pollutants, enabling the composite material to simultaneously remove phosphate, ammonia nitrogen, and fluoride ions from water bodies with a removal rate of at least 85%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid adsorbent composition technology, specifically to a composite material and preparation method for simultaneously removing phosphate, ammonia nitrogen and fluoride ions. Background Technology

[0002] Mineral tailings are typically mineral residues discharged during mining, beneficiation, or flotation processes. They are characterized by fine particles, complex composition, and difficulty in comprehensive utilization. Due to their low level of resource utilization, long-term stockpiling not only occupies a large amount of land resources but also may cause dust pollution and leachate release under the influence of wind erosion and rain, posing certain ecological and environmental risks. Meanwhile, agricultural and forestry biomass waste (such as bamboo powder, straw, rice husks, and sawdust) is produced in large quantities and comes from a wide range of sources. Improper disposal can easily further increase environmental hazards. Therefore, achieving high-value utilization of mineral tailings and biomass waste is of practical significance.

[0003] Industrial wastewater containing phosphorus, fluoride, and ammonia nitrogen is characterized by complex composition and high pollutant concentrations. Existing technologies often employ chemical precipitation and adsorption methods, but these technologies are typically optimized for single pollutants. Simultaneous deep removal of multiple pollutants often requires various reagents or multi-stage treatment units, increasing operating costs and sludge disposal pressure.

[0004] Existing technologies for preparing water treatment materials using biochar and mineral solid waste include schemes that improve phosphorus removal performance by loading active components such as magnesium and iron onto the surface of biochar, and composite resource utilization schemes that use minerals and biomass for other applications. However, there is still room for optimization in technologies that start from the activation of calcium-containing minerals in mineral tailings, and use the simultaneous co-pyrolysis of mineral tailings and biomass to form mineral phase reconstruction and synergistic pore structure, and then apply it to the simultaneous treatment of high-concentration, multi-pollutant wastewater. Therefore, it is necessary to provide a composite material preparation method that does not require complex chemical modification, can fully utilize the active mineral components in mineral tailings and synergistically interact with the carbon structure of biomass, in order to reduce the pressure of solid waste disposal and improve the simultaneous treatment capacity of complex industrial wastewater. Summary of the Invention

[0005] The purpose of this invention is to address the insufficient utilization of existing mineral tailings and agricultural and forestry biomass waste resources, as well as the difficulty of traditional water treatment materials in simultaneously removing phosphates, ammonia nitrogen, and fluorides.

[0006] To achieve the above-mentioned technical objectives, this invention provides a method for preparing a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions, comprising: Biomass is mixed with mineral tailings at least twice the mass of the biomass, and then pyrolyzed under anaerobic or hypoxic conditions to obtain a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions.

[0007] Furthermore, the mass ratio of the biomass to the mineral tailings is 1:3-6.

[0008] Furthermore, the pyrolysis is performed by heating to 800-1000℃ at a heating rate of 8-12℃ / min and holding at that temperature for 0.5-2h.

[0009] Furthermore, the mineral tailings have a particle size of less than 100 mesh, and the biomass has a particle size of less than 40 mesh.

[0010] Furthermore, after the pyrolysis is completed, the resulting solid is pulverized and passed through an 80-150 mesh sieve.

[0011] Furthermore, the mineral tailings include at least one of phosphorus tailings, iron tailings, and magnesite tailings, preferably phosphorus tailings.

[0012] Furthermore, the biomass is agricultural and forestry waste.

[0013] The present invention also provides a composite material for simultaneously removing phosphate, ammonia nitrogen and fluoride ions, obtained by the above preparation method.

[0014] Furthermore, the surface area of ​​the composite material is 6-12m². 2 / g, with an average pore size of 26-30nm.

[0015] This invention also provides the application of the above-mentioned composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions in water treatment, characterized in that it includes, The composite material for simultaneously removing phosphate, ammonia nitrogen, and fluoride ions is applied to the water to be treated at a dosage of 5-100 g / L to simultaneously remove phosphate, ammonia nitrogen, and fluoride ions from the water.

[0016] The present invention also provides a wastewater treatment reagent, comprising the above-mentioned composite material for simultaneously removing phosphate, ammonia nitrogen and fluoride ions.

[0017] Compared with the prior art, the beneficial effects of the present invention include: This invention eliminates the need for additional chemical modifiers such as metal salts. A composite material is obtained through the co-pyrolysis of mineral tailings and biomass. Co-pyrolysis induces the transformation of the carbonate mineral phase in the tailings into the active oxide phase, simultaneously forming a well-developed mesoporous structure. This provides conditions for the precipitation, fixation, and mass transfer of anionic pollutants, enabling the composite material to simultaneously remove phosphate, ammonia nitrogen, and fluoride ions from water, with a removal rate of at least 85%.

[0018] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0020] Figure 1 This is a schematic diagram of the preparation method of the composite material for simultaneous removal of phosphate, ammonia nitrogen and fluoride ions according to the present invention; Figure 2 This is a flowchart of the preparation method of the composite material for simultaneous removal of phosphate, ammonia nitrogen and fluoride ions according to the present invention; Figure 3 The XRD patterns are of the phosphate tailings powder and the resulting composite material that simultaneously removes phosphate, ammonia nitrogen and fluoride ions in Example 1 of this invention. Figure 4(a) and Figure 4(b) are the nitrogen adsorption-desorption isotherms and pore size distribution diagrams of the phosphorus tailings powder used in Example 1, respectively. Figure 4(c) and Figure 4(d) are the nitrogen adsorption-desorption isotherms and pore size distribution diagrams of the composite material obtained in Example 1, respectively. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the invention, are intended to cover non-exclusive inclusion.

[0023] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0024] In recent years, the use of biochar prepared from biomass pyrolysis as an adsorbent for wastewater treatment has become a research hotspot. Biochar has advantages such as wide availability of raw materials, low cost, large specific surface area, and abundant surface functional groups. However, the surface of raw biochar is usually negatively charged, resulting in poor adsorption performance for phosphate and fluoride ions existing in anionic form. To overcome this deficiency, researchers have proposed a technical route of modifying biochar with metal oxides or mineral materials. Among these, the use of mineral processing waste as a modifier to prepare biochar-based composite materials through calcination or co-pyrolysis processes has attracted attention due to its combination of environmental benefits ("waste-to-waste treatment") and improved adsorption performance.

[0025] However, current biochar-mineral composite materials have the following shortcomings in use: 1. Existing biochar-based composite materials mostly adopt a step-by-step treatment mode of "precipitation to remove fluoride first, followed by adsorption of nitrogen and phosphorus" when treating wastewater containing phosphorus, fluoride, and ammonia nitrogen, or only target the adsorption and removal of one or two types of pollutants. They have not yet achieved the direct and simultaneous adsorption and removal of phosphorus, fluoride, and ammonia nitrogen pollutants through a single composite material.

[0026] 2. In existing biomass and mineral processing waste composite material preparation technologies, the biomass ratio is usually high, with the mass ratio of biomass to mineral processing waste mostly between 1:1 and 9:1. The proportion of mineral processing waste is relatively low, resulting in a limited content of active metal components in the material, making it difficult to provide sufficient adsorption active sites to meet the needs of simultaneous removal of multiple pollutants.

[0027] 3. In existing technologies, the composite of biomass and mineral processing waste often adopts a multi-step process of impregnation followed by calcination, which is relatively complex and has high preparation costs, making it unsuitable for large-scale application.

[0028] In view of this, the present invention provides a method for preparing a composite material for simultaneously removing phosphate, ammonia nitrogen, and fluoride ions, comprising, Biomass is mixed with mineral tailings at least twice the mass of the biomass, and then pyrolyzed under anaerobic or hypoxic conditions to obtain a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions.

[0029] In some preferred embodiments, the mass ratio of the biomass to the mineral tailings is 1:3-6.

[0030] Mineral tailings are rich in metallic elements such as Mg, Ca, Fe, and Al. When tailings are added at a ratio more than twice that of biomass, the loading of metal oxides in the composite material is significantly increased, and the density of adsorption active sites per unit mass of material is greatly increased. This invention employs a high proportion of mineral tailings, while the carbon skeleton generated by biomass pyrolysis still plays a crucial role in dispersion and stabilization. The porous structure of biochar uniformly disperses the metal oxide nanoparticles, preventing their aggregation and thus exposing more active surfaces. During co-pyrolysis, the addition of biomass effectively reduces the pyrolysis activation energy of the mineral components, and the dispersion of biochar promotes the reaction activation of nano-metal oxides. Simultaneously, the presence of the carbon skeleton ensures that the material retains a certain porosity after high-temperature calcination, which is beneficial for the mass transfer and diffusion of pollutants.

[0031] In some preferred embodiments, the pyrolysis is performed by heating to 750-1050°C at a rate of 8-12°C / min and holding at that temperature for 0.5-2 hours. Under the high-temperature calcination conditions of 750-1050°C, the carbonate minerals in the tailings undergo significant decomposition. Taking calcium-based and magnesium-based minerals as examples, calcium carbonate decomposes into CaO in the 600-800°C range, and magnesium salts decompose to form MgO. When the temperature is further increased to above 750°C, the mineral decomposition is more complete, the crystallinity of CaO and MgO increases, and the active sites are more fully exposed. These phases have higher thermal stability and unique surface chemical properties, providing more stable chemisorption sites for phosphate, ammonia nitrogen, and fluoride ions. However, excessively high temperatures may cause the carbon framework pore structure to collapse, so the pyrolysis temperature should not be too high.

[0032] Optimizing the particle size distribution of the raw materials is beneficial for a more complete pyrolysis reaction. In some preferred embodiments, the particle size of the mineral tailings is less than 100 mesh, and the particle size of the biomass is less than 40 mesh.

[0033] Fine particle size facilitates the dispersion of the composite material in water. In some preferred embodiments, after the pyrolysis is completed, the resulting solid is pulverized and passed through an 80-150 mesh sieve.

[0034] In some preferred embodiments, the biomass is agricultural and forestry waste. The agricultural and forestry waste is not strictly limited and can, for example, be at least one of bamboo powder, straw, sawdust, rice husks, etc. The mineral tailings include at least one of phosphorus tailings, iron tailings, and magnesite tailings.

[0035] The present invention will be further described in detail below through specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0036] Example 1 A method for preparing a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions, such as... Figure 1 and Figure 2 As shown, it includes the following steps: S1. Weigh 50.00g of phosphorus tailings powder with a particle size <150μm; weigh 10.00g of waste bamboo powder with a particle size <420μm, with a mass ratio of 5:1; place the phosphorus tailings powder and waste bamboo powder in a mortar and grind and mix for 30min until the mixture is evenly distributed by visual inspection, thus obtaining the mixed precursor.

[0037] S2. Transfer the mixed precursor to a 50mL covered corundum crucible, compact it, and then cover the crucible with the lid to create an oxygen-limited pyrolysis environment.

[0038] S3. Place the crucible in a box-type muffle furnace and heat it from room temperature to 900℃ at a heating rate of 10℃ / min. After reaching the target temperature, hold it at that temperature for 60 minutes.

[0039] S4. Turn off the power to the muffle furnace and allow it to cool naturally to room temperature. Grind the obtained product and pass it through a 100-mesh sieve to obtain a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions.

[0040] Examples 2-4 Compared with Example 1, the difference is that the amount of phosphorus tailings powder used in step S1 is 30.00g, 40.00g and 60.00g respectively, that is, the mass ratio of phosphorus tailings powder to waste bamboo powder is 3:1, 4:1 and 6:1 respectively.

[0041] Example 5 The difference compared to Example 1 is that the temperature is raised to 1000°C in step S3.

[0042] Examples 6-8 Compared with Example 1, the difference is that waste bamboo powder was replaced with sawdust, rice husks and corn stalks of the same mass and particle size.

[0043] Examples 9-10 Compared with Example 1, the difference is that iron tailings and magnesite tailings of the same mass and particle size are used to replace phosphorus tailings powder.

[0044] Comparative Example 1 The difference compared to Example 1 is that the temperature is raised to 700°C in step S3. Comparative Example 2 Phosphate tailings powder with a particle size of <150μm.

[0045] Comparative Example 3 A method for preparing pyrolytic phosphate tailings includes the following steps: Phosphate tailings powder with a particle size <150μm was transferred to a 50mL covered corundum crucible, compacted, and then covered with the crucible lid to create an oxygen-limited pyrolysis environment. The crucible was then placed in a box-type muffle furnace and heated from room temperature to 900℃ at a heating rate of 10℃ / min. After reaching the target temperature, the temperature was held for 60min. The power to the muffle furnace was turned off, and the furnace was allowed to cool naturally to room temperature. The resulting product was then ground and passed through a 100-mesh sieve to obtain pyrolytic phosphate tailings.

[0046] Comparative Example 4 A method for preparing pyrolytic phosphate tailings includes the following steps: Waste bamboo powder with a particle size <420μm was transferred to a 50mL covered corundum crucible, compacted, and then covered with the crucible lid to create an oxygen-limited pyrolysis environment. The crucible was then placed in a box-type muffle furnace and heated from room temperature to 900℃ at a heating rate of 10℃ / min. After reaching the target temperature, the temperature was held for 60min. The power to the muffle furnace was turned off, and the furnace was allowed to cool naturally to room temperature. The resulting product was then ground and passed through a 100-mesh sieve.

[0047] Comparative Example 5 A method for preparing a mixture of pyrolytic phosphate tailings and biomass includes the following steps: (1) Transfer the phosphorus tailings powder with a particle size <150μm to a 50mL corundum crucible with a lid, compact it, and then cover the crucible with a lid to form an oxygen-limited pyrolysis environment. Then place the crucible in a box-type muffle furnace and heat it from room temperature to 900℃ at a heating rate of 10℃ / min. After reaching the target temperature, hold it for 60min. Turn off the power of the muffle furnace and let it cool naturally to room temperature. Grind the obtained product and pass it through a 100-mesh sieve to obtain pyrolytic phosphorus tailings.

[0048] (2) Pyrolytic phosphate tailings and waste bamboo powder with a particle size of <420μm are mixed at a mass ratio of 5:1 to obtain a mixture of pyrolytic phosphate tailings and biomass.

[0049] The crystal forms of the phosphate tailings powder and the composite material obtained from pyrolysis in Example 1 were observed using X-ray diffraction. Figure 3As can be seen, the phosphate tailings powder exhibits multiple characteristic diffraction peaks within a diffraction angle range of 10°-80°, with phases including MgO, CaCO3, Ca(OH)2, CaO, SiO2, and Ca5(PO4)3F, mainly corresponding to calcite (CaCO3), MgO, Ca(OH)2, and CaO. The resulting composite material shows enhanced CaO characteristic peaks, while MgO and other mineral peaks are still retained. This phase change indicates that the reducing atmosphere generated during biomass pyrolysis promotes the phase transformation and activation of calcium and magnesium minerals in the phosphate tailings, thus providing more active sites for the removal of phosphates and fluorides.

[0050] The specific surface area and pore characteristics of the phosphorus tailings powder and the composite material obtained by pyrolysis in Example 1 were tested using nitrogen adsorption-desorption. As can be seen from Figures 4(a) and 4(b), and Figures 4(c) and 4(d), the specific surface area and average pore size of the composite material are significantly increased. Table 1 summarizes the specific surface area and pore characteristics of the phosphorus tailings powder and the composite material obtained by pyrolysis.

[0051] Table 1

[0052] As shown in Table 1, compared with phosphate tailings, the composite material exhibits superior pore structure characteristics at 900℃, with its BET specific surface area increasing from 4.661 m². 2 / g increased to 9.481m 2 / g, the micropore area increased from 0.983m² 2 / g increased to 2.278m 2 / g, both the total pore volume and average pore size increased. The pore size distribution results showed that the pore size of both materials was mainly concentrated in the mesoporous range of 2-50 nm, with the composite material showing a more significant pore volume distribution in the 2-10 nm range. This indicates that the co-pyrolysis process promoted pore formation and pore structure optimization, resulting in a porous structure that is more conducive to pollutant mass transfer and adsorption reactions.

[0053] To evaluate the performance of the materials obtained in the examples and comparative examples in removing phosphate, ammonia nitrogen, and fluoride ions from water, leachate from a phosphogypsum stockpile in Hubei Province was used as the test water sample. The concentrations of phosphate, ammonia nitrogen, and fluoride ions were 5860 mg / L, 407 mg / L, and 2643 mg / L, respectively. The dosage of each material was 50 g / L, and adsorption was performed at room temperature with magnetic stirring for 4 h. After adsorption, centrifugation was performed, and the residual concentration of the supernatant was determined. Phosphate was removed using the molybdenum-antimony spectrophotometric method, ammonia nitrogen was removed using the Nessler's reagent method, and fluoride ions were removed using the ion-selective electrode method.

[0054] Table 2 shows the removal performance of phosphate, ammonia nitrogen, and fluoride ions in phosphogypsum leachate of different ratios of phosphate tailings powder and waste bamboo powder in Examples 1-4.

[0055] Table 2

[0056] Table 2 shows that the mass ratio of phosphate tailings powder to biomass powder has a significant impact on the pollutant removal performance of the composite material. When the mass ratio is 3:1-6:1, the resulting composite material exhibits high removal rates for both phosphate and fluoride ions, and good removal effect for ammonia nitrogen. Among these, the ammonia nitrogen removal rate reaches 86.3% when the mass ratio is 5:1, showing the best overall removal effect. When the mass ratio is further increased to 6:1, the ammonia nitrogen removal rate decreases to 73.8%, indicating that a low biomass ratio is not conducive to ammonia nitrogen removal. Therefore, a mass ratio of 3:1-6:1 is a suitable range, with 5:1 being the preferred ratio.

[0057] Table 3 shows the removal performance of phosphate, ammonia nitrogen, and fluoride ions in phosphogypsum leachate at different pyrolysis temperatures in Examples 1, 5, and Comparative Example 5.

[0058] Table 3

[0059] Table 3 shows that the co-pyrolysis temperature significantly affects the performance of the composite material in removing phosphate, ammonia nitrogen, and fluoride ions from phosphogypsum leachate. When the co-pyrolysis temperature is 900℃, the removal rates of phosphate, ammonia nitrogen, and fluoride ions reach 99.9%, 86.3%, and 98.6%, respectively, exhibiting the best overall removal performance. This is because at higher pyrolysis temperatures, mineral decomposition is more thorough, the crystallinity of CaO and MgO increases, and the active sites are more fully exposed. These phases possess higher thermal stability and unique surface chemical properties, providing more stable chemisorption sites for phosphate, ammonia nitrogen, and fluoride ions. However, excessively high temperatures may lead to the collapse of the carbon framework pore structure, and the pyrolysis temperature should not be too high.

[0060] Table 4 shows the removal performance of phosphate, ammonia nitrogen, and fluoride ions in phosphogypsum leachate from different mineral tailings in Examples 1, 9, and 10.

[0061] Table 4

[0062] Table 4 shows that the composite materials of Examples 1, 9, and 10 can simultaneously remove phosphate, ammonia nitrogen, and fluoride ions, with good removal rates. Under the same bamboo powder pyrolysis biochar conditions, the composite material prepared using phosphate tailings achieved removal rates of 99.9%, 86.3%, and 98.6% for phosphate, ammonia nitrogen, and fluoride ions, respectively, all higher than those using iron tailings and magnesite tailings. Therefore, phosphate tailings are a superior mineral tailings raw material, and the phosphate tailings / bamboo powder pyrolysis biochar composite material exhibits the best comprehensive pollutant removal performance.

[0063] Table 5 shows the removal performance of different materials on phosphate, ammonia nitrogen, and fluoride ions in phosphogypsum leachate.

[0064] Table 5

[0065] Table 5 shows that after heat treatment at 900℃, the removal rates of phosphate, ammonia nitrogen, and fluoride ions in the phosphate tailings increased from 8.6%, 12.3%, and 5.1% in Comparative Example 2 to 94.3%, 79.5%, and 78.8% in Comparative Example 3, respectively. These results indicate that heat treatment can significantly improve the removal capacity of phosphate tailings for these pollutants. Combined with changes in material composition, it can be inferred that at higher temperatures, some calcium components in the phosphate tailings may be activated or undergo phase transformation, thereby forming reaction sites more conducive to pollutant removal.

[0066] Based on this, under the same phosphate tailings heat treatment conditions, the introduction of bamboo powder carbonization components further increased the phosphate removal rate from 94.3% to 99.9%, the ammonia nitrogen removal rate from 79.5% to 86.3%, and the fluorine removal rate from 78.8% to 98.6%. This indicates that the introduction of bamboo powder carbonization components has a relatively positive promoting effect on the removal of ammonia nitrogen and fluorine. At the same time, the phosphate removal effect is further improved on the basis of the original activated phosphate tailings, indicating that the composite system has a certain synergistic effect.

[0067] Comparative Example 4 demonstrates that biochar has a poor removal effect on phosphate, ammonia nitrogen, and fluoride ions. Comparative Example 5 shows that, under the same phosphate tailings treatment conditions, the composite material obtained by physically mixing bamboo powder and phosphate tailings has a very limited removal effect on phosphate, ammonia nitrogen, and fluoride ions, even worse than Comparative Example 3. These results indicate that bamboo powder, during co-pyrolysis, not only acts as a pore-forming agent to optimize the pore structure of the material, but also promotes the activation and transformation of calcium components in the phosphate tailings through the reducing atmosphere generated by its pyrolysis. This synergistic effect cannot be replaced by simple physical mixing.

[0068] Examples 6 to 8 show that agricultural and forestry biomass such as sawdust, rice husks, and corn stalks can be co-pyrolyzed with phosphate tailings to prepare composite materials with similar multi-pollutant removal capabilities, indicating that the present invention has good universality for different biomass raw materials.

[0069] In summary, this invention, by separately calcining mineral tailings and biomass at high temperatures and then combining them, prepares a mineral tailings / biochar composite material. This material fully utilizes the high-calcium active components of activated mineral tailings and the porous adsorption structure of biochar, achieving synergistic and efficient removal of phosphates, ammonia nitrogen, and fluorides from wastewater simultaneously. The preparation method of this invention requires no chemical reagents, uses solid waste as raw material, and features a simple and controllable process, demonstrating promising engineering application prospects.

[0070] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions, characterized in that, include, Biomass is mixed with mineral tailings at least twice the mass of the biomass, and then pyrolyzed under anaerobic or hypoxic conditions to obtain a composite material that simultaneously removes phosphate, ammonia nitrogen, and fluoride ions.

2. The method for preparing the composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions according to claim 1, characterized in that, The mass ratio of the biomass to the mineral tailings is 1:3-6.

3. The method for preparing the composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions according to claim 1, characterized in that, The pyrolysis is performed by heating the temperature to 750-1050℃ at a rate of 8-12℃ / min and holding it at that temperature for 0.5-2h.

4. The method for preparing the composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions according to claim 1, characterized in that, The mineral tailings have a particle size of less than 100 mesh, and the biomass has a particle size of less than 40 mesh.

5. The method for preparing the composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions according to claim 1, characterized in that, After the pyrolysis is completed, the resulting solid is pulverized and passed through an 80-150 mesh sieve.

6. The method for preparing the composite material for simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions according to claim 1, characterized in that, The biomass in question is agricultural and forestry waste; The mineral tailings include at least one of phosphorus tailings, iron tailings, and magnesite tailings.

7. A composite material for simultaneously removing phosphate, ammonia nitrogen, and fluoride ions, characterized in that, It is obtained by the preparation method according to any one of claims 1-6.

8. The composite material for simultaneously removing phosphate, ammonia nitrogen, and fluoride ions according to claim 7, characterized in that, Its surface area is 6-12m² 2 / g, with an average pore size of 26-30nm.

9. The application of a composite material for simultaneously removing phosphate, ammonia nitrogen, and fluoride ions as described in claim 7 or 8 in water treatment, characterized in that, include, The composite material for simultaneously removing phosphate, ammonia nitrogen, and fluoride ions is applied to the water to be treated at a dosage of 5-100 g / L to simultaneously remove phosphate, ammonia nitrogen, and fluoride ions from the water.

10. A wastewater treatment reagent, characterized in that, The composite material for the simultaneous removal of phosphate, ammonia nitrogen, and fluoride ions as described in claim 7 or 8.