A method for manufacturing a large split type rotary bearing ring
By forging bar stock into square billets and extruding them into straight strips, and combining this with a three-point tooling to adjust the curvature, the problem of mismatched cross-sections in the billet-making process of circular arc billets was solved, improving material utilization and billet strength, and reducing production costs and processing difficulty.
Patent Information
- Application Number
- CN202611467779.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-10
AI Technical Summary
The existing circular arc blanks are difficult to form a cross-sectional profile that matches the ring during the blanking process, resulting in low material utilization, large subsequent processing volume, insufficient blank strength and wear resistance, and high processing difficulty and cost.
The bar stock is heated and forged into a square billet, which is then extruded and stretched to form a straight billet. During the extrusion and stretching process, the billet is rolled into a predetermined cross-sectional profile. The curvature is gradually adjusted using a three-point tooling to finally form a circular arc billet.
It improves material utilization, reduces subsequent machining allowance, enhances the structural strength and wear resistance of the billet, and reduces production costs and processing difficulty.
Smart Images

Figure CN123060033A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of slewing bearing ring manufacturing technology, specifically relating to a method for preparing ultra-large split slewing bearing rings. Background Technology
[0002] A slewing bearing is a large bearing capable of simultaneously bearing axial loads, radial loads, and overturning moments. It typically consists of an inner ring, an outer ring, and rolling elements positioned between them. With the increasing size of wind power generation, port machinery, mining machinery, and large-scale engineering equipment, the diameter of slewing bearings is also increasing. For ultra-large slewing bearings with diameters reaching tens of meters or even larger, due to limitations in forging equipment, machining equipment, and transportation conditions, the rings usually employ a split structure. This involves dividing the ring circumferentially into multiple arc-shaped segments, manufacturing each segment separately, and then sequentially assembling these segments circumferentially to form a complete ring. Because the rings typically incorporate raceways, steps, and other structures, the arc-shaped blank not only needs to have a corresponding curvature, but its cross-section also needs to match the cross-sectional shape of the ring. Therefore, the forming quality of the arc-shaped blank is subject to high requirements.
[0003] However, in the current process of blanking, the overall size and curvature of the blank are usually controlled, resulting in a rectangular or other relatively simple cross-section. This fails to create a cross-sectional profile that matches the raceway during blanking. To ensure the subsequent machining of the raceway, steps, and other structures required for the raceway, a large machining allowance needs to be reserved in the width and thickness directions of the blank, and a large amount of material needs to be removed through subsequent machining. This not only wastes raw materials and increases machining workload and time, but also easily cuts or damages the original metal flow lines inside the blank. At the same time, the current blanking method does not provide sufficient extrusion at different parts of the blank cross-section, resulting in a low degree of material densification. It is difficult to form a favorable compressive stress state inside and on the surface of the blank, which affects the structural strength and wear resistance of the resulting raceway. In addition, the large volume and weight of ultra-large circular arc blanks make clamping, positioning, and transportation difficult during machining, further increasing the processing difficulty and production cost of circular arc blanks. Summary of the Invention
[0004] This invention provides a method for preparing a blank for an ultra-large split slewing bearing ring, which solves the problem mentioned in the background art that existing circular arc blanks are difficult to form the required cross-sectional profile during the blanking process, resulting in low material utilization, large subsequent processing volume, and insufficient blank strength and wear resistance.
[0005] The technical solution adopted in this invention is: a method for manufacturing a blank of an ultra-large split-type turntable bearing ring, comprising the following steps:
[0006] The bar stock is heated and then forged to initially form a square billet.
[0007] The square billet is extruded and stretched to extend it along its length, and the cross-section of the square billet is rolled and shaped during the extrusion and stretching process to form a straight strip billet with a predetermined cross-sectional profile.
[0008] The above-mentioned straight strip blank is processed into a circular arc blank with a predetermined curvature using a three-point tooling.
[0009] Preferably, when extruding and stretching the square blank, extrusion is performed sequentially at different locations along the length of the square blank, and the areas of two adjacent extrusions at least partially overlap.
[0010] Preferably, after completing one round of extrusion and extension along the length of the square billet, the placement direction of the square billet is adjusted, and extrusion and extension are performed again along the length of the square billet.
[0011] Preferably, the cross-sectional profile of the square billet is gradually formed by multiple rolling processes, and the cross-sectional dimensions of the square billet are checked between two adjacent rolling processes until the predetermined cross-sectional profile is formed.
[0012] Preferably, during the extrusion and stretching process of the square billet, the square billet needs to be heated once or multiple times.
[0013] Preferably, the length of the straight strip blank is greater than the theoretical unfolded length of the arc blank, so as to form process allowances at both ends of the straight strip blank for subsequent removal.
[0014] Preferably, the three-point fixture includes two support wheels located on one side of the straight billet and a rolling wheel located on the other side of the straight billet. The two support wheels are spaced apart along the length of the straight billet, and the rolling wheel is correspondingly positioned between the two support wheels.
[0015] Preferably, a three-point tooling is used to perform multiple bending processes on the straight blank, and the pressing amount of the rolling wheel on the straight blank is increased between two adjacent bending processes to change the curvature of the blank until the predetermined curvature is achieved.
[0016] Preferably, after the straight strip blank is formed into an arc blank, the portions at both ends of the arc blank that do not reach the predetermined arc length are cut off, and the two end faces of the arc blank are shaped to make the arc blank reach the predetermined arc length.
[0017] The beneficial effects of this invention are as follows:
[0018] 1. The present invention first forges the bar stock into a square billet, and then forms a straight billet through extrusion and extension. During the extrusion and extension process, the billet is simultaneously rolled to form a predetermined cross-sectional profile. This allows the cross-section of the straight billet to be close to the cross-sectional shape required for the ring beforehand, reducing subsequent machining allowance and material removal, improving material utilization, shortening the processing cycle and reducing production costs.
[0019] 2. This invention continuously extrudes, extends, and rolls square billets, making the internal structure of the billets more compact and ensuring that the metal flow lines are continuously distributed along the length of the straight billets, reducing the damage to the metal flow lines caused by subsequent extensive cutting. At the same time, the rolling action helps to form a favorable compressive stress state inside and on the surface of the billets, thereby improving the structural strength and wear resistance of the arc billets and providing a good billet foundation for improving the load-bearing capacity and service life of the rings.
[0020] 3. This invention uses a three-point tooling to gradually process straight strip blanks into arc blanks. By adjusting the pressing amount of the rolling roller on the straight strip blank, the curvature of the arc blank can be gradually adjusted, avoiding excessive bending in a single operation that could cause the blank to crack or deform its cross-section. This makes the curvature of the arc blank more uniform and can meet the blanking requirements of ultra-large turntable bearing rings of different diameters. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the blank forming process of the present invention;
[0022] Figure 2 This is a schematic diagram of the circular arc blank forming process using a three-point tooling according to the present invention.
[0023] in:
[0024] 1. Support wheel; 2. Compactor wheel. Detailed Implementation
[0025] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0026] like Figure 1-2 As shown, a method for manufacturing an ultra-large split slewing bearing ring includes steps such as heating bar stock and forging square billets, forming straight bar billets, forming arc-shaped billets, and end processing. Specifically, the bar stock is sequentially processed to form square billets, straight bar billets with predetermined cross-sectional profiles, and arc-shaped billets. Multiple arc-shaped billets, after subsequent machining, can be sequentially joined circumferentially to form the ultra-large slewing bearing ring.
[0027] Before blanking, the curvature, theoretical arc length, and cross-sectional dimensions of each arc blank are determined based on the diameter, cross-sectional shape, and number of circumferentially arranged arc blanks of the slewing bearing rings to be manufactured. The cross-sectional dimensions of the arc blanks should be based on the finished ring dimensions, allowing for machining allowances required for subsequent machining. The length of the straight blank is determined based on the theoretical unfolded length of the arc blank, and machining allowances are added at both ends of the straight blank to ensure that the actual length of the straight blank is greater than the theoretical unfolded length of the arc blank. This allows for the removal of any portions at both ends that do not reach the predetermined curvature after bending.
[0028] The blanking method for the ultra-large split slewing bearing ring is as follows.
[0029] The first step is to heat the bar stock and forge the square billet.
[0030] Select bar stock that meets the material and weight requirements of the ring and send it into the heating furnace for heating. The heating temperature and holding time of the bar stock can be determined according to the material grade, diameter and subsequent forging requirements of the bar stock, so that the bar stock is heated evenly from the surface to the inside and reaches a suitable temperature for forging, avoiding problems such as cracks or uneven local deformation during the forging process due to large temperature differences between the inside and outside of the bar stock.
[0031] After the bar stock is heated, it is transferred to a forging machine, where it is forged to initially form a square billet. In practice, two opposite sides of the bar stock can be forged first, then the orientation of the bar stock can be adjusted to forge the other two opposite sides. By repeatedly forging different sides of the bar stock, the originally round or near-round bar stock is gradually transformed into a square billet with four sides.
[0032] In this step, the bar stock is pre-forged into a square billet, which helps to determine the placement direction and stress position during subsequent extrusion, so that the billet maintains a relatively stable posture during the subsequent elongation process, and also helps to improve the deformation uniformity of various parts of the billet.
[0033] The second step involves extruding, stretching, and shaping the cross-sectional profile of the square blank.
[0034] A square billet is placed in the working position of a forging or rolling equipment, and the billet is extruded and extended to extend along its length. During the extrusion and extension process, the cross-section of the billet is rolled and shaped to form a straight strip billet with a predetermined cross-sectional profile.
[0035] Specifically, when extruding and stretching a square billet, extrusion begins from one end along the length of the billet and proceeds sequentially to different locations. Each extrusion reduces the cross-sectional dimension at the corresponding location and causes the material at that location to flow primarily along the length of the billet, thus gradually elongating the billet. After extruding one location, the billet is moved a predetermined distance relative to the extrusion location before extruding the adjacent location.
[0036] The areas of two adjacent extrusions overlap at least partially, meaning that a portion of the area of the later extrusion is located within the area of the previous extrusion. This avoids leaving insufficiently deformed portions between adjacent extrusion areas and reduces the occurrence of local bulges, depressions, or abrupt changes in cross-sectional dimensions along the length of the straight billet. By extruding the square billet step by step from one end to the other in the manner described above, one round of extrusion and extension along the length of the square billet is completed.
[0037] After one round of extrusion and stretching, the placement orientation of the square billet is adjusted so that the other surface to be processed faces the extrusion position, and extrusion and stretching are performed again along the length of the square billet. The adjustment of the placement orientation of the square billet can be determined based on its current cross-sectional shape and predetermined cross-sectional profile, so that different parts of the billet's cross-section can be extruded to the appropriate degree. Through multiple rounds of extrusion and stretching, the length of the square billet gradually increases, and its straightness, cross-sectional dimensions, and the degree of deformation in each part gradually reach the predetermined requirements.
[0038] While the square billet is being extruded and stretched, its cross-section is rolled into shape. In practice, the amount of reduction at different parts of the square billet's cross-section can be controlled according to a predetermined cross-sectional profile; alternatively, an anvil or rolling mill with corresponding forming surfaces can be used to roll corresponding parts of the square billet's cross-section, causing the material to redistribute along the cross-sectional direction after compression. After multiple rolling operations, the cross-section of the square billet gradually changes from its initial square shape to a predetermined cross-sectional profile that matches the cross-section of the ring to be manufactured.
[0039] The cross-sectional profile of a square billet is gradually shaped through multiple rolling processes. The initial rolling is mainly used to quickly adjust the overall cross-sectional dimensions of the billet, while the later rolling is mainly used to refine the profile and dimensions of various parts of the cross-section. By adopting a gradual rolling method, it is possible to avoid localized cracking, folding, or distortion of the cross-sectional profile of the billet caused by excessive single-stage pressing.
[0040] Between two adjacent rolling passes, the cross-sectional dimensions of the square billet are inspected. During inspection, calipers, gauges, or a test template adapted to the predetermined cross-sectional profile can be used to measure the width, height, and relative position of different parts of the billet's cross-section. If the dimensions of a certain part do not meet the requirements, the rolling amount for that part is increased or adjusted during the next rolling pass. Once all parts of the cross-section have reached the predetermined dimensions, the rolling process completes the shaping of the cross-sectional profile, resulting in a straight strip-shaped billet with the predetermined cross-sectional profile.
[0041] By simultaneously forming a predetermined cross-sectional profile during the extrusion and stretching of the square billet, the cross-section of the straight billet is made close to the required cross-sectional shape of the ring beforehand. This reduces the amount of material that needs to be removed during subsequent machining, improving material utilization. At the same time, continuous extrusion and rolling increase the density of the billet's internal structure, ensuring a continuous distribution of metal flow lines along the length of the straight billet. This also helps create a favorable stress state within and on the surface of the billet, providing a solid foundation for improving the ring's structural strength, wear resistance, and load-bearing capacity.
[0042] Because square billets have large lengths and cross-sectional dimensions, their temperature gradually decreases during multiple rounds of extrusion, stretching, and rolling. When the billet temperature drops to a level unsuitable for continued plastic deformation, or when the deformation resistance of the billet increases significantly, extrusion and stretching are stopped, and the square billet is returned to the heating furnace for supplementary heating. The number of supplementary heating cycles can be determined based on the billet material, billet size, and actual processing time; it can be performed once or multiple times. After supplementary heating, the remaining extrusion, stretching, and cross-sectional rolling are resumed. This prevents the billet from continuing to deform and crack at excessively low temperatures, while also reducing the load on the extrusion equipment.
[0043] Once the length of the straight billet reaches the predetermined requirement and its cross-sectional profile and dimensions pass inspection, a smaller reduction amount can be used to trim the billet as a whole to improve its straightness and surface flatness. The trimmed billet retains a predetermined length of machining allowance at both ends, which is not removed in this step.
[0044] The third step is to use a three-point tooling to form the arc blank.
[0045] The straight billet, after being extruded, stretched, and rolled into cross-section, is transferred to a three-point tooling. Depending on the material, cross-sectional dimensions, and bending properties of the straight billet, bending can be performed while maintaining a certain temperature, or the straight billet can be reheated before bending to reduce its bending deformation resistance.
[0046] The three-point fixture includes two support wheels 1 located on one side of the straight billet and a rolling wheel 2 located on the other side of the straight billet. The two support wheels 1 are spaced apart along the length of the straight billet, and the rolling wheel 2 is correspondingly positioned between the two support wheels 1. The two support wheels 1 are used to form two spaced-apart support points on the straight billet from one side, and the rolling wheel 2 is used to apply rolling pressure to the straight billet from the other side, thereby creating three mutually cooperating force-bearing positions on the straight billet.
[0047] A straight strip-shaped blank is placed between two support rollers 1 and a pressing roller 2, and the cross-section of the blank is kept in a predetermined orientation to prevent it from tipping over or bending in the wrong direction during the bending process. Pressure is applied to the straight strip-shaped blank by the pressing roller 2, and the blank is moved along its length relative to the two support rollers 1 and the pressing roller 2, causing the blank to bend continuously along its length.
[0048] During the initial bending process, the pressing amount of the rolling roller 2 on the straight blank is relatively small, causing the blank to initially form a small curvature. After completing one bending process, the curvature of the straight blank is detected, and based on the detection results, the pressing amount of the rolling roller 2 is increased, allowing the straight blank to pass between the two support rollers 1 and the rolling roller 2 again. As the pressing amount of the rolling roller 2 gradually increases, the curvature of the straight blank gradually increases.
[0049] A three-point tooling is used to bend the straight billet multiple times. Between each adjacent bending operation, the pressure of the two rollers on the straight billet is increased to alter its curvature until the desired curvature is achieved. Compared to bending the straight billet to the target curvature in one go, gradually increasing the bending amount in multiple stages allows for a more uniform distribution of plastic deformation along the length of the straight billet. This reduces cracking, cross-sectional deformation, or abrupt changes in curvature caused by excessive local deformation, thus improving the forming quality of the curved billet.
[0050] After each bending process, the curvature of different positions on the blank can be checked using a curvature detection template or other curvature detection tools. When the local curvature is less than the predetermined curvature, the corresponding position can be bent and adjusted again using a three-point fixture. When the curvature of the main part of the arc blank reaches the predetermined requirement, the bending process is stopped, and an arc blank with the predetermined curvature is obtained.
[0051] The fourth step is to process the ends of the arc-shaped blank.
[0052] Because the three-point tooling requires two support rollers 1 and one rolling roller 2 to achieve the bending effect, the portion of the straight blank near both ends cannot simultaneously form a complete three-point force relationship with the three rollers. Therefore, after bending, the ends of the arc blank may have a curvature smaller than the predetermined curvature or retain some straight sections. To avoid this affecting the effective arc length of the arc blank and the subsequent splicing accuracy, process allowances are pre-set at both ends when determining the initial length of the straight blank.
[0053] After the straight blank is formed into an arc blank, the cutting positions at both ends are determined according to the predetermined arc and arc length of the arc blank, and the portions at both ends that do not reach the predetermined arc are cut off. After cutting, the two end faces of the arc blank are shaped to remove protrusions, burrs, and cutting allowances, so that the arc blank reaches the predetermined arc length and that the two end faces of the arc blank can mate with the corresponding end faces of adjacent arc blanks. By leaving process allowances at both ends of the straight blank and cutting off the ends with insufficient arc after bending, the impact of the straight ends produced by the three-point bending process on the forming accuracy of the arc blank can be reduced, so that the main body of the arc blank has a more uniform arc and the dimensional accuracy when multiple arc blanks are spliced together circumferentially.
[0054] This completes the preparation of one arc-shaped blank. After processing multiple arc-shaped blanks using the same method, these blanks can be placed on an assembly platform for pre-assembly to check the curvature, length, and end-face fit of each blank. Qualified arc-shaped blanks can then undergo heat treatment, machining, and surface treatment to ultimately produce corresponding arc-shaped ring segments. These segments are then sequentially assembled circumferentially to form an ultra-large split-type slewing bearing ring.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for manufacturing a blank of an ultra-large split-type slewing bearing ring, characterized in that, Includes the following steps: The bar stock is heated and then forged to initially form a square billet. The square billet is extruded and stretched to extend it along its length, and the cross-section of the square billet is rolled and shaped during the extrusion and stretching process to form a straight strip billet with a predetermined cross-sectional profile. The above-mentioned straight strip blank is processed into a circular arc blank with a predetermined curvature using a three-point tooling.
2. The method for preparing a blank of an ultra-large split-type turntable bearing ring according to claim 1, characterized in that: When extruding and stretching a square billet, extrusion is performed sequentially at different locations along the length of the square billet, and the areas of two adjacent extrusions at least partially overlap.
3. The method for preparing a blank of an ultra-large split-type turntable bearing ring according to claim 2, characterized in that: After completing one round of extrusion and extension along the length of the square billet, adjust the placement direction of the square billet and extrude and extend it again along the length of the square billet.
4. The method for preparing a blank of an ultra-large split-type turntable bearing ring according to claim 1, characterized in that: The cross-sectional profile of the square billet is gradually formed through multiple rolling processes, and the cross-sectional dimensions of the square billet are checked between adjacent rolling processes until the predetermined cross-sectional profile is formed.
5. The method for preparing a blank of an ultra-large split-type slewing bearing ring according to claim 1, characterized in that: During the extrusion and stretching process of square billets, the square billets need to be heated once or multiple times.
6. The method for preparing a blank of an ultra-large split-type turntable bearing ring according to claim 1, characterized in that: The length of the straight blank is greater than the theoretical unfolded length of the circular blank, so as to form process allowances at both ends of the straight blank for subsequent removal.
7. The method for preparing a blank of an ultra-large split-type turntable bearing ring according to claim 1, characterized in that: The three-point fixture includes two support wheels (1) located on one side of the straight billet and a rolling wheel (2) located on the other side of the straight billet. The two support wheels (1) are spaced apart along the length of the straight billet, and the rolling wheel (2) is correspondingly located between the two support wheels (1).
8. The method for preparing a blank of an ultra-large split-type slewing bearing ring according to claim 7, characterized in that: The straight blank is bent multiple times using a three-point tooling, and the pressing amount of the rolling wheel (2) on the straight blank is increased between two adjacent bending processes to change the curvature of the blank until the predetermined curvature is reached.
9. The method for preparing a blank of an ultra-large split-type slewing bearing ring according to claim 6, characterized in that: After the straight strip blank is formed into an arc blank, the portions at both ends of the arc blank that do not reach the predetermined arc are cut off, and the two end faces of the arc blank are shaped to make the arc blank reach the predetermined arc length.