A kitchen waste bag and its preparation method

By using a three-layer co-extrusion blown film structure and organically modified montmorillonite, the problems of oil seepage and insufficient mechanical strength of garbage bags in greasy environments have been solved, achieving the effects of oil resistance, impermeability, and puncture resistance.

CN123061673APending Publication Date: 2026-11-10ZHUHAI ZHENGTAI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611586979.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing garbage bags are prone to oil seepage and reduced heat-sealing strength after prolonged contact with grease, and their mechanical strength is insufficient, making it difficult to meet the needs of processing kitchen waste.

Method used

The film adopts a three-layer co-extrusion blown film structure. The surface and inner layers contain POE elastomer, and the core layer contains organic modified montmorillonite. A labyrinth barrier network is formed by expanding the montmorillonite layer with specific quaternary ammonium salts to improve oil penetration resistance and mechanical strength.

Benefits of technology

It significantly extends the penetration path of oil molecules, improves the oil resistance and impermeability of garbage bags and their mechanical strength, and meets the usage requirements of kitchen waste bags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061673A_ABST
    Figure CN123061673A_ABST
Patent Text Reader

Abstract

This invention discloses a kitchen waste bag and its preparation method, relating to the technical field of polymer packaging materials. A kitchen waste bag includes a bag body made of a film formed by multi-layer co-extrusion blown film. The film, from the outside to the inside, consists of a surface layer, a core layer, and an inner layer. The surface layer and inner layer comprise composite metallocene polyethylene I, linear low-density polyethylene, low-density polyethylene, and POE elastomer. The core layer comprises composite metallocene polyethylene II, linear low-density polyethylene, low-density polyethylene, organically modified montmorillonite, and maleic anhydride-grafted polyethylene. The organically modified montmorillonite is obtained by co-intercalating montmorillonite with a dual long-chain alkyl quaternary ammonium salt and a vinyl quaternary ammonium salt. The technical solution of this application endows the garbage bag with excellent oil resistance, impermeability, mechanical strength, and heat-sealing performance, meeting the requirements for the use of kitchen waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of polymer packaging materials, and in particular to a kitchen waste bag and its preparation method. Background Technology

[0002] Because kitchen waste is generally complex in composition, it usually contains a lot of water, oil, or hard and sharp objects such as fish bones, bone fragments, and fruit pits. Therefore, higher requirements are placed on the oil resistance, heat sealing and mechanical strength of garbage bags.

[0003] Most commercially available garbage bags are made of low-density polyethylene, linear low-density polyethylene, or a blend of both, using single or double-layer blown film, with a thickness generally around 0.01-0.02 mm. Because polyethylene is a non-polar material, its ability to block grease is limited. Therefore, after prolonged contact with grease, the outer surface of these garbage bags is prone to oil seepage, especially at the bottom heat seal and pleats. Contact with grease reduces the heat seal strength, further increasing the risk of leakage and bag breakage. Simultaneously, garbage bags have relatively low mechanical strength. Sharp objects inside the bag can create concentrated loads during disposal or handling, easily puncturing the bag. The puncture site will then tear quickly under tensile stress, causing the bag to break. Furthermore, a single bag of kitchen waste can weigh several kilograms wet, and the bottom heat seal is prone to cracking and leaking due to prolonged immersion in oil and concentrated loads during subsequent lifting. This makes them unsuitable for long-term loading or transportation of kitchen waste containing high levels of grease and sharp objects. Summary of the Invention

[0004] In order to improve the oil resistance, seepage prevention, mechanical strength and heat sealing performance of garbage bags, so that they can be used for the treatment of daily kitchen waste, this application provides a kitchen waste bag and a method for preparing the same.

[0005] Firstly, the kitchen waste bag provided in this application adopts the following technical solution: A kitchen waste bag includes a bag body made of a three-layer film formed by multi-layer co-extrusion blown film, wherein the film consists of a surface layer, a core layer and an inner layer from the outside to the inside. The outer layer and the inner layer comprise the following parts by weight of raw materials: The composition includes 30-36 parts of composite metallocene polyethylene, 35-40 parts of linear low-density polyethylene, 10-15 parts of low-density polyethylene, 10-16 parts of POE elastomer, 3.5-4.5 parts of processing auxiliaries, and 0-3 parts of color masterbatch. The core layer comprises the following parts by weight of raw materials: Composite metallocene polyethylene II 40-50 parts, linear low-density polyethylene 20-30 parts, low-density polyethylene 15-20 parts, organic modified montmorillonite 3-6 parts, maleic anhydride grafted polyethylene 5-10 parts, processing auxiliary material II 0.6-2 parts. The organically modified montmorillonite is prepared by co-intercalation of montmorillonite with a dual long-chain alkyl quaternary ammonium salt and a vinyl quaternary ammonium salt.

[0006] By adopting the above technical solution, a three-layer co-extrusion blown film structure consisting of a surface layer, a core layer, and an inner layer is used. POE elastomer is introduced into the surface and inner layers, while organically modified montmorillonite, modified by specific quaternary ammonium salts, is introduced into the core layer. Simultaneously, the raw material components and proportions of each layer are specifically adjusted. This approach endows the bag with excellent heat-sealing toughness, puncture resistance, and tear resistance, as well as good oil permeability resistance and mechanical strength. Specifically, the organically modified montmorillonite is prepared by co-intercalating montmorillonite with dual long-chain alkyl quaternary ammonium salts and vinyl quaternary ammonium salts. The dual long-chain alkyl quaternary ammonium salts effectively expand the layers and improve hydrophobicity, while the vinyl quaternary ammonium salts provide reactive groups. These groups synergistically interact with maleic anhydride-grafted polyethylene and the polyethylene matrix, promoting the intercalation, exfoliation, and uniform dispersion of montmorillonite within the polyethylene matrix, forming a labyrinthine barrier network that significantly extends the oil molecule penetration path. In addition, organically modified montmorillonite can also be used as a heterogeneous nucleating agent to appropriately increase the crystallinity of the core layer. This is beneficial for reducing the permeable area of ​​the amorphous region, improving the oil permeability resistance of the core layer, and also for improving the mechanical strength of the core layer. This allows the garbage bag to have comprehensive properties such as oil resistance, puncture resistance, tear resistance, and reliable load-bearing capacity, thus meeting the requirements of kitchen waste bags for oil permeability resistance and mechanical strength.

[0007] Optionally, the dual long-chain alkyl quaternary ammonium salt is a dual long-chain alkyl quaternary ammonium salt containing C16-C18.

[0008] Optionally, the dual long-chain alkyl quaternary ammonium salt is one of dihexadecyl dimethyl ammonium chloride, dioctadecyl dimethyl ammonium chloride, and dihydrogenated tallow dimethyl ammonium chloride; Optionally, the vinyl quaternary ammonium salt is one of vinyltrimethylammonium chloride or vinylbenzyltrimethylammonium chloride.

[0009] By adopting the above technical solution, the C16-C18 double long-chain alkyl quaternary ammonium salt has sufficient chain length and hydrophobicity. After being effectively inserted into the interlayer of montmorillonite, it can effectively weaken the interlayer interaction and expand the interlayer spacing of montmorillonite to a degree that is conducive to the insertion of polyethylene molecular chains. This promotes the intercalation and delamination of organically modified montmorillonite during core layer processing, which is conducive to the formation of a more uniform dispersion and a more complete barrier network, thereby improving the oil penetration resistance of garbage bags.

[0010] Optionally, the method for preparing the organically modified montmorillonite includes the following steps: Montmorillonite was dispersed in water and heated to 40-550-60℃. Then, a dual long-chain alkyl quaternary ammonium salt and a vinyl quaternary ammonium salt were added. The mixture was heated to 80-90℃ and stirred to react. After the reaction was completed, the mixture was cooled, filtered, washed with water, dried, ground, and sieved to obtain the organically modified montmorillonite.

[0011] By adopting the above technical solution, it is possible to ensure that the double long-chain alkyl quaternary ammonium salt and vinyl quaternary ammonium salt can fully undergo ion exchange and intercalation reaction with montmorillonite. Moreover, water washing can effectively remove incompletely intercalated free quaternary ammonium salt, which helps to prevent excessive free quaternary ammonium salt from causing problems such as plasticization and decreased thermal stability during subsequent core layer processing. This helps to improve the subsequent processing stability of organically modified montmorillonite and ensure the processing performance of the core layer.

[0012] Optionally, the molar amount of cations in the added dual long-chain alkyl quaternary ammonium salt is controlled to be 0.5-0.8 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinyl quaternary ammonium salt is controlled to be 0.4-0.6 times the cation exchange capacity of montmorillonite.

[0013] By adopting the above technical solution, it can be ensured that both the dual long-chain alkyl quaternary ammonium salt and the vinyl quaternary ammonium salt can exchange with montmorillonite cations and form a reasonable co-intercalation structure between montmorillonite layers. This prevents the exchange failure of one intercalation ion due to the activity or volume of a single intercalation ion. Specifically, the dual long-chain alkyl quaternary ammonium salt provides sufficient layer expansion and hydrophobic modification for organic modification, while the vinyl quaternary ammonium salt provides some reaction sites. By controlling the amount of the two intercalation ions, sufficient layer expansion and improved compatibility can be achieved without the problems of plasticization, decreased thermal stability, and increased cost caused by excessive free quaternary ammonium salt. This ensures that the organically modified montmorillonite is uniformly dispersed in the core layer and forms an effective barrier network.

[0014] Optionally, based on the total mass of the composite metallocene polyethylene I, the composite metallocene polyethylene I is composed of the following raw materials in the following mass percentages: Octyl metallocene polyethylene with a melt index of 0.8-1.2 g / 10 min is 60-75%; Hexyl metallocene polyethylene I with a melt index of 1.0-1.5 g / 10 min is 10-15%; and Hexyl metallocene polyethylene II with a melt index of 1.8-2.4 g / 10 min is 15-25%. Based on the total mass of the composite metallocene polyethylene II, the composite metallocene polyethylene II is composed of the following raw materials in the following mass percentages: The melt flow index (MFI) of the following raw materials was 30-40% for octyl metallocene polyethylene (MCPE) with a melt flow index of 0.8-1.2 g / 10 min, 40-50% for hexyl metallocene polyethylene I with a melt flow index of 1.0-1.5 g / 10 min, and 10-20% for hexyl metallocene polyethylene II with a melt flow index of 1.8-2.4 g / 10 min. The MFI test conditions for all the above raw materials were 190℃ and 2.16 kg.

[0015] By adopting the above technical solutions, octyl metallocene polyethylene (MCPE) accounts for 60-75% in composite metallocene polyethylene I, providing excellent long side chain entanglement and puncture and tear resistance. The addition of hexyl metallocene polyethylene I and hexyl metallocene polyethylene II adjusts the overall strength and processing fluidity, giving both the surface and inner layers good heat-sealing toughness and tear propagation resistance. In composite metallocene polyethylene II, octyl metallocene polyethylene accounts for 30-40%, hexyl metallocene polyethylene I for 40-50%, and hexyl metallocene polyethylene II for 10-20%. Combined with organically modified montmorillonite, the core layer achieves high rigidity and barrier properties at a lower cost. Simultaneously, it ensures that the melt flowability of the core layer, surface layer, and inner layers is matched, allowing the core layer melt to be extruded synchronously and uniformly with the melts on both sides during the blown film process. This avoids problems such as poor interlayer bonding or uneven film thickness caused by differences in melt flowability.

[0016] Optionally, the melt index of the linear low-density polyethylene is 1.5-2 g / 10 min; the melt index of the low-density polyethylene is 2-3 g / 10 min; the melt index of the POE elastomer is 2-3 g / 10 min; and the melt index test conditions for all the above raw materials are 190℃ and 2.16 kg.

[0017] By adopting the above technical solution, the melt flow index range is conducive to the formation of appropriate crystallization and orientation of linear low-density polyethylene and low-density polyethylene, and promotes the uniform dispersion of POE elastomer in the surface layer and inner layer and plays a toughening role. This allows for the synergistic regulation of the melt flow and mechanical strength of each layer, enabling the film to obtain excellent puncture resistance, tear resistance and heat sealing performance while maintaining good processing stability.

[0018] At the same time, the composite metallocene polyethylene with specific melt index combinations between each layer can regulate the melt flow of each layer system, which helps to prevent interface fluctuations or uneven thickness between the core layer and the surface layer and inner layer due to differences in melt viscosity.

[0019] To ensure uniform and stable film formation of the melt at the die during the blown film process, and to match the mechanical performance requirements of each layer, the surface layer and inner layer should have good processing performance as well as tear resistance and tensile strength. Ultimately, this ensures the smooth progress of the three-layer co-extrusion blown film process and the production of a finished film with uniform thickness and stable performance.

[0020] Optionally, the processing aid I includes processing aid I, antistatic agent, opening agent and slip agent, and the mass ratio of processing aid I, antistatic agent, opening agent and slip agent is 1:2:(2-3):(2-3); The processing aid II includes processing aid II, antioxidant and calcium stearate, and the mass ratio of processing aid II, antioxidant and calcium stearate is 1:(1-2.5):(0.6-1).

[0021] By adopting the above technical solutions, processing aid I can effectively reduce adhesion and surface defects between films while ensuring heat sealing effect; while the antioxidant and calcium stearate in processing aid II can inhibit the thermal decomposition and volatilization of intercalated modified quaternary ammonium salts during high-temperature extrusion, which is beneficial to reduce the generation of odors during processing. Combined with processing aids, it can effectively improve the processing stability of the core layer.

[0022] Optionally, based on the total thickness of the film, the thickness ratio of the surface layer, the core layer, and the inner layer is (1-1.5):(2-3):(1-1.5), and the thickness ratio of the surface layer to the inner layer is 1:1.

[0023] By adopting the above technical solution, the symmetrical thickness ratio can balance the stress of the garbage bag, preventing warping and delamination caused by uneven thickness of each layer. This helps ensure that the formed garbage bag has good flatness, is not prone to self-curling and wrinkling, and is easy to fold and roll on the production line. In addition, at this film thickness ratio, the core layer accounts for the main part of the total thickness, which can provide sufficient oil penetration resistance and mechanical support for the garbage bag, while the appropriate thickness of the surface layer and inner layer can provide sufficient heat-sealing toughness, puncture resistance and tear expansion resistance. By controlling the thickness of each layer of the film, it is beneficial to achieve a good balance between oil penetration resistance, mechanical strength, puncture resistance and heat-sealing effect in the kitchen waste bag.

[0024] Secondly, the method for preparing a kitchen waste bag provided in this application adopts the following technical solution: A method for preparing a kitchen waste bag includes the following steps: S1. Mix the raw materials evenly according to the proportion, extrude and granulate, and dry them thoroughly to obtain surface layer masterbatch, core layer masterbatch and inner layer masterbatch respectively. S2. The surface layer masterbatch, the core layer masterbatch, and the inner layer masterbatch are respectively fed into independent extruders. The masterbatch is melted and plasticized by the extruder. The melt of each masterbatch is distributed to the flow channel of each layer by the layer distributor. The three melts are combined and the blank is extruded from the die head and die orifice under high pressure. The blank is blown into a film by the top blowing method. After being cooled by the air ring, blown, and pulled and wound, a semi-finished film is obtained. S3. The semi-finished film is welded and sealed using a bag-making machine, then cut, folded, and rolled up to obtain the kitchen waste bag.

[0025] By adopting the above technical solution, the thickness ratio of each layer of the film can be accurately controlled. Furthermore, the top-blowing method combined with air ring cooling for longitudinal and transverse stretching of the extruded preform promotes the orientation and grain refinement of polyethylene molecules in both directions, forming an interpenetrating network structure to enhance the oil permeability resistance and mechanical properties of the garbage bag. In addition, the preparation method is simple, and the equipment used can directly utilize traditional extrusion blow molding equipment without large-scale equipment upgrades, facilitating rapid factory deployment and large-scale production.

[0026] Optionally, step S2 may also include a step of forming a ribbon: S201. The surface masterbatch containing the colored masterbatch is fed into an independent extruder. The masterbatch is melted and plasticized by the extruder. The surface masterbatch melt containing the colored masterbatch is distributed to the surface flow channel by the layer distributor. It is combined with the surface melt and the blank is extruded from the die head and die orifice under high pressure. The blank is blown into a film by the top blowing method. It is cooled and inflated by the air ring and several colored stripes extending longitudinally along the film are formed on the surface layer.

[0027] By adopting the above technical solution, the ribbon and the surface layer can be integrally formed during the blown film process, and are firmly bonded to the surface layer, making them less likely to fall off. This eliminates the need for additional printing or lamination processes and does not affect the oil penetration resistance and mechanical properties of the garbage bag. As a result, the ribbon can provide identification and classification functions throughout the entire life cycle of the garbage bag, and achieve effective identification throughout the entire process of garbage classification.

[0028] In summary, the technical solution of this application has at least one of the following beneficial effects: 1. By adopting a three-layer structure, each layer is compounded with polyethylene raw materials in different proportions. At the same time, POE elastomer is introduced into the surface and inner layers, and organic modified montmorillonite with specific quaternary ammonium salt to expand the interlayer spacing is introduced into the core layer. This can ensure the oil penetration resistance of the garbage bag while maintaining good comprehensive mechanical properties, meeting the requirements of kitchen waste bags for oil penetration resistance, puncture resistance, and damage resistance.

[0029] 2. By introducing organically modified montmorillonite, which is made by co-intercalating montmorillonite with dual long-chain alkyl quaternary ammonium salt and vinyl quaternary ammonium salt, into the core layer, it is beneficial to promote the intercalation, peeling and uniform dispersion of montmorillonite in the polyethylene matrix, and to form a labyrinthine barrier network in the core layer, which can significantly extend the oil molecule penetration path and improve the oil penetration resistance of the garbage bag.

[0030] 3. By introducing organically modified montmorillonite into the core layer, the organically modified montmorillonite can also act as a heterogeneous nucleating agent to appropriately increase the crystallinity of the core layer and reduce the permeable area of ​​the amorphous region, which is beneficial to improving the oil permeability resistance and mechanical strength of the core layer. Attached Figure Description

[0031] Figure 1This is a cross-sectional view of a kitchen waste bag according to Embodiment 1 of this application.

[0032] Explanation of reference numerals in the attached figures: 1. Top layer; 2. Core layer; 3. Inner layer. Detailed Implementation

[0033] The following is in conjunction with the appendix Figure 1 The preparation examples, embodiments, and comparative examples further illustrate this application in detail.

[0034] Some of the raw materials used in the following examples and comparative examples can be commercially available products. The specific selection is as follows. Those skilled in the art can select other equivalent commercially available products as needed.

[0035] Octyl metallocene polyethylene was selected from Saudi Aramco COHERE 8102, with a melt index of 1 g / 10 min (190℃, 2.16 kg).

[0036] Hexyl metallocene polyethylene I was selected from ExxonMobil Exceed 1023CA, with a melt index of 1 g / 10 min (190℃, 2.16 kg).

[0037] Hexyl metallocene polyethylene II was selected from ExxonMobil Exceed 2227ED, with a melt index of 2.2 g / 10 min (190℃, 2.16 kg).

[0038] The linear low-density polyethylene used is LG Chem FC1500, with a melt index of 1.5 g / 10 min (190℃, 2.16 kg).

[0039] The low-density polyethylene used is ExxonMobil LD136.MN, with a melt index of 2 g / 10 min (190℃, 2.16 kg).

[0040] The POE elastomer used is LG Chem Lucene LC370, with a melt index of 3 g / 10 min (190℃, 2.16 kg).

[0041] The fluoroelastomer PPA selected is Luju Chemical's PPA9000P.

[0042] The high molecular weight silicone used is Dow Corning MB50-002.

[0043] Preparation Example

[0044]

Preparation Example 1

[0045] A method for preparing organically modified montmorillonite includes the following steps: 10 kg of sodium montmorillonite was dispersed in 100 L of water, heated to 50 °C, and then dihydrogenated tallow dimethyl ammonium chloride and vinylbenzyltrimethyl ammonium chloride were added. The mixture was heated to 85 °C and stirred for 2 h. After the reaction was completed, the mixture was cooled, filtered, washed with water, dried, ground and sieved to obtain the organic modified montmorillonite.

[0046] In this preparation example, the molar amount of cations in the added dihydrogenated tallow-based dimethyl ammonium chloride was controlled to be 0.8 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinylbenzyltrimethyl ammonium chloride was controlled to be 0.4 times the cation exchange capacity of montmorillonite. Specifically, the sodium-based montmorillonite used was PGW sodium-based montmorillonite from Xianfeng Nano, with a CEC of 145 meq / 100g. Calculations showed that the pure mass of the added dihydrogenated tallow-based dimethyl ammonium chloride was 6.79 kg, and the pure mass of the added vinylbenzyltrimethyl ammonium chloride was 1.23 kg.

[0047]

Preparation Example 2

[0048] A method for preparing organically modified montmorillonite includes the following steps: 10 kg of sodium montmorillonite was dispersed in 100 L of water, heated to 60 °C, and then dioctadecyl dimethyl ammonium chloride and vinylbenzyl trimethyl ammonium chloride were added. The mixture was heated to 90 °C and stirred for 2 h. After the reaction was completed, the mixture was cooled, filtered, washed with water, dried, ground and sieved to obtain the organic modified montmorillonite.

[0049] In this preparation example, the molar amount of cations in the added dioctadecyl dimethyl ammonium chloride was controlled to be 0.5 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinylbenzyltrimethyl ammonium chloride was controlled to be 0.6 times the cation exchange capacity of montmorillonite. Specifically, the sodium-based montmorillonite used was PGW sodium-based montmorillonite from Xianfeng Nano, with a CEC of 145 meq / 100g. Calculations showed that the pure mass of the added dioctadecyl dimethyl ammonium chloride was 4.25 kg, and the pure mass of the added vinylbenzyltrimethyl ammonium chloride was 1.84 kg.

[0050]

Preparation Example 3

[0051] In the preparation method of this example, the molar amount of cations in the added hexadecyl dimethyl ammonium chloride is controlled to be 0.8 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinylbenzyltrimethyl ammonium chloride is controlled to be 0.4 times the cation exchange capacity of montmorillonite. Calculations show that the pure mass of added hexadecyl dimethyl ammonium chloride is 6.15 kg, and the pure mass of added vinylbenzyltrimethyl ammonium chloride is 1.23 kg.

[0052] All other process parameters are the same as in [Preparation Example 1].

[0053]

Preparation Example 4

[0054] In the preparation method of this example, the molar amount of cations in the added didodecyl dimethyl ammonium chloride is controlled to be 0.8 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinylbenzyltrimethyl ammonium chloride is controlled to be 0.4 times the cation exchange capacity of montmorillonite. Calculations show that the mass of pure didodecyl dimethyl ammonium chloride added is 4.85 kg, and the mass of pure vinylbenzyltrimethyl ammonium chloride added is 1.23 kg.

[0055]

Preparation Example 5

[0056] A method for preparing organically modified montmorillonite includes the following steps: 10 kg of sodium-based montmorillonite was dispersed in 100 L of water, heated to 50 °C, and then dihydrogenated tallow dimethyl ammonium chloride was added. The mixture was heated to 85 °C and stirred for 2 h. After the reaction was completed, the mixture was cooled, filtered, washed with water, dried, ground, and sieved to obtain the organically modified montmorillonite.

[0057] In this preparation example, the molar amount of cations in the added dihydrogenated tallow dimethyl ammonium chloride was controlled to be 1.2 times the cation exchange capacity of montmorillonite. The calculated mass of the added pure dihydrogenated tallow dimethyl ammonium chloride was 10.21 kg.

[0058]

Preparation Example 6

[0059] A method for preparing organically modified montmorillonite includes the following steps: 10 kg of sodium montmorillonite was dispersed in 100 L of water, heated to 50 °C, and then vinylbenzyltrimethylammonium chloride was added. The mixture was heated to 85 °C and stirred for 2 h. After the reaction was completed, the mixture was cooled, filtered, washed with water, dried, ground, and sieved to obtain the organically modified montmorillonite.

[0060] In this preparation example, the molar amount of cations in the added vinylbenzyltrimethylammonium chloride was controlled to be 1.2 times the cation exchange capacity of montmorillonite. The calculated mass of pure vinylbenzyltrimethylammonium chloride added was 3.68 kg.

[0061]

Preparation Example 7

[0062] In the preparation method of this example, the molar amount of cations in the added monohydrogenated tallow trimethylammonium chloride was controlled to be 0.8 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinylbenzyltrimethylammonium chloride was controlled to be 0.4 times the cation exchange capacity of montmorillonite. Calculations showed that the pure product mass of the added monohydrogenated tallow trimethylammonium chloride was 4.03 kg, and the pure product mass of the added vinylbenzyltrimethylammonium chloride was 1.23 kg.

[0063] Example

[0064]

Example 1

[0065] In this embodiment, both the outer layer 1 and the inner layer 3 of the film comprise the following raw materials: 30kg composite metallocene polyethylene I, 40kg linear low-density polyethylene, 15kg low-density polyethylene, 10.5kg POE elastomer and 4.5kg processing auxiliary material I.

[0066] Among them, the composite metallocene polyethylene I includes 18 kg of octyl metallocene polyethylene, 4.5 kg of hexyl metallocene polyethylene I and 7.5 kg of hexyl metallocene polyethylene II.

[0067] The processing aid I includes 0.5 kg of processing aid I, 1 kg of antistatic agent, 1.5 kg of opening agent, and 1.5 kg of slip agent. Specifically, processing aid I is a composition of 0.2 kg of fluoroelastomer PPA and 0.3 kg of high molecular weight silicone; the antistatic agent is octadecyl diethanolamine; the opening agent is 1500 mesh hydrophobic silica; and the slip agent is erucamide.

[0068] The film's surface layer 1 also features four color strips, evenly distributed along the circumference of the bag. Specifically, the color strips differ from surface layer 1 in that the color strip raw material also includes 3 kg of color masterbatch.

[0069] In this embodiment, the core layer 2 of the thin film comprises the following raw materials: 50kg composite metallocene polyethylene II, 20kg linear low-density polyethylene, 15kg low-density polyethylene, 5kg organic modified montmorillonite, 8kg maleic anhydride grafted polyethylene and 2kg processing auxiliary material II.

[0070] Among them, the composite metallocene polyethylene II includes 20 kg of octyl metallocene polyethylene, 20 kg of hexyl metallocene polyethylene I and 10 kg of hexyl metallocene polyethylene II.

[0071] The organically modified montmorillonite was prepared according to [Preparation Example 1].

[0072] Processing aid II includes 0.5 kg of processing aid II, 0.4 kg of antioxidant 1010, 0.6 kg of antioxidant 168, and 0.5 kg of calcium stearate. Specifically, processing aid II is a composition of 0.2 kg of fluoroelastomer PPA and 0.3 kg of high molecular weight silicone.

[0073] A method for preparing a kitchen waste bag includes the following steps: S1. Mix the raw materials evenly according to the proportion, extrude and granulate, and dry them thoroughly to obtain surface layer masterbatch, core layer masterbatch and inner layer masterbatch respectively. S2. The surface layer masterbatch, core layer masterbatch and inner layer masterbatch are fed into independent extruders. The masterbatch is melted and plasticized by the extruder. The melt of each masterbatch is distributed to the flow channel of each layer by the layer distributor. The three melts are combined and the blank is extruded from the die head and die orifice under high pressure. The blank is blown into a film by the top blowing method. After being cooled by the air ring, blown, and pulled and wound, a semi-finished film is obtained. S3. The semi-finished film is welded and sealed using a bag-making machine, then cut, folded, and rolled up to obtain the kitchen waste bag.

[0074] S2 also includes the step of forming a color band: S201. The surface masterbatch containing the colored masterbatch is fed into an independent extruder. The masterbatch is melted and plasticized by the extruder. The surface masterbatch melt containing the colored masterbatch is distributed to the surface flow channel by the layer distributor. It is combined with the surface melt and the blank is extruded from the die head and die orifice under high pressure. The blank is blown into a film by the top blowing method. It is cooled and inflated by the air ring and several colored stripes extending longitudinally along the film are formed on the surface layer 1.

[0075]

Example 2

[0076] In this embodiment, the thickness ratio of the surface layer 1, the core layer 2, and the inner layer 3 of the film is 1.5:2:1.5.

[0077] In this embodiment, both the outer layer 1 and the inner layer 3 of the film comprise the following raw materials: 36kg composite metallocene polyethylene I, 35kg linear low-density polyethylene, 10kg low-density polyethylene, 15.5kg POE elastomer and 3.5kg processing auxiliary material I.

[0078] Among them, the composite metallocene polyethylene I includes 27 kg of octyl metallocene polyethylene, 3.6 kg of hexyl metallocene polyethylene I and 5.4 kg of hexyl metallocene polyethylene II.

[0079] Among them, processing aid I includes 0.5 kg processing aid I, 1 kg antistatic agent, 1 kg opening agent and 1 kg slip agent.

[0080] The film's surface layer 1 also features four color strips, evenly distributed along the circumference of the bag. Specifically, the color strips differ from surface layer 1 in that the color strip raw material also includes 3 kg of color masterbatch.

[0081] In this embodiment, the core layer 2 of the thin film comprises the following raw materials: 40kg composite metallocene polyethylene II, 30kg linear low-density polyethylene, 20kg low-density polyethylene, 3kg organic modified montmorillonite, 5kg maleic anhydride grafted polyethylene and 2kg processing auxiliary material II.

[0082] Among them, the composite metallocene polyethylene II includes 16 kg of octyl metallocene polyethylene, 20 kg of hexyl metallocene polyethylene I and 4 kg of hexyl metallocene polyethylene II.

[0083] The organically modified montmorillonite was prepared according to [Preparation Example 2].

[0084] Processing aid II includes 0.5 kg of processing aid II, 0.4 kg of antioxidant 1010, 0.8 kg of antioxidant 168, and 0.3 kg of calcium stearate. Specifically, processing aid II is a composition of 0.2 kg of fluoroelastomer PPA and 0.3 kg of high molecular weight silicone.

[0085]

Example 3

[0086] In this embodiment, the organically modified montmorillonite was prepared according to [Preparation Example 3].

[0087]

Example 4

[0088] In this embodiment, the organically modified montmorillonite was prepared according to [Preparation Example 4].

[0089]

Example 5

[0090] In this embodiment, neither the outer layer 1 nor the inner layer 3 contains octyl metallocene polyethylene (OMPE), and instead, an equal amount of hexyl metallocene polyethylene (HME) replaces the octyl MPE. Specifically, the composite MPE comprises 22.5 kg of hexyl MPE and 7.5 kg of hexyl MPE.

[0091] Comparative Example

[0092] Comparative Example 1 A garbage bag, which differs from [Example 1] in that it has a single-layer structure, specifically a bag made of a single-layer film formed by extrusion blown film.

[0093] In this comparative example, the raw material of the single-layer film is the same as that of the surface layer in [Example 1].

[0094] A method for preparing a garbage bag includes the following steps: S1. Mix the raw materials evenly according to the proportion, extrude and granulate, and dry them thoroughly to obtain film masterbatch; S2. The film masterbatch is fed into an independent extruder, where it is melted and plasticized. The preform is then extruded under high pressure from the die head and die orifice. The preform is blown into a film using an upward blowing method. After being cooled by an air ring, inflated, and pulled and wound up, a semi-finished film is obtained. S3. The semi-finished film is welded and sealed using a bag-making machine, then cut, folded, and rolled up to obtain the kitchen waste bag.

[0095] Comparative Example 2 One type of garbage bag differs from [Comparative Example 1] in that the raw material of its single-layer film is different.

[0096] In this comparative example, the raw material of the single-layer film is the same as that of the core layer in [Example 1].

[0097] Comparative Example 3 A garbage bag that differs from [Example 1] in that its core layer 2 is different, specifically, the core layer 2 does not contain organically modified montmorillonite.

[0098] In this comparative example, an equal amount of sodium-based montmorillonite was used to replace the organically modified montmorillonite.

[0099] Comparative Example 4 A garbage bag that differs from [Example 1] in that its core layer 2 is different, specifically the organically modified montmorillonite in the core layer 2.

[0100] In this comparative example, the organically modified montmorillonite was prepared from [Preparation Example 5].

[0101] Comparative Example 5 A garbage bag that differs from [Example 1] in that its core layer 2 is different, specifically the organically modified montmorillonite in the core layer 2.

[0102] In this comparative example, the organically modified montmorillonite was prepared from [Preparation Example 6].

[0103] Comparative Example 6 A garbage bag that differs from [Example 1] in that its core layer 2 is different, specifically the organically modified montmorillonite in the core layer 2.

[0104] In this comparative example, the organically modified montmorillonite was prepared from [Preparation Example 7].

[0105] Performance testing

[0106] Sample preparation: Garbage bag samples were prepared according to the formulations and processes of the various embodiments and comparative examples, with a finished thickness of 0.02 mm. If it is necessary to test certain mechanical properties of the bag, it can be cut into corresponding test samples according to the standard test dimensions, and the area without color bands should be used for testing.

[0107] 1. Oil permeability resistance: The test is conducted in accordance with GB / T 16929-2025 Packaging Materials Test Method Oil Permeability. A mixture of lard and peanut oil in a 1:1 mass ratio is used as the test oil. The inner layer is used as the contact surface to contact the test oil. The oven temperature is controlled at 40℃. The test time interval is 0.5 hours. The interval between the first oil permeation and the last test time is recorded, for example, "0-0.5". If the test time exceeds 12 hours, "≥12" is recorded directly.

[0108] 2. Puncture resistance: The test was conducted in accordance with section 6.6.13 of GB / T 10004-2008 Plastic composite films, bags and tapes for packaging - dry lamination and extrusion lamination. Five samples were tested. After the test, the average puncture force (N) of each sample was recorded and the results were retained to two decimal places.

[0109] 3. Drop resistance: The test shall be conducted in accordance with section 6.7 of GB / T 24454-2009 Plastic garbage bags, with a test load of 3000g. After the test, a steel ball with a diameter of 38mm shall be used to determine whether the garbage bag is broken. 30 samples shall be tested. If ≥27 samples are unbroken, the sample shall be recorded as "qualified"; otherwise, the sample shall be recorded as "unqualified".

[0110] 4. Right-angle tear strength test: The test shall be conducted in accordance with GB / T 10004-2008 Dry lamination and extrusion lamination of plastic composite films, bags and tapes for packaging and QB / T 1130-91 Test method for right-angle tear performance of plastics, and the longitudinal and transverse right-angle tear strength (kN / m) of each sample shall be recorded.

[0111] Table 1. Partial performance test data of garbage bags

[0112] Based on the data from Example 1, Comparative Examples 1-3, and Table 1, it can be seen that by adopting a three-layer structure, with each layer being compounded with polyethylene raw materials in different proportions, and by introducing POE elastomer into the surface layer 1 and inner layer 3, and introducing organically modified montmorillonite with a specific quaternary ammonium salt to expand the interlayer spacing into the core layer 2, the oil penetration resistance of the garbage bag can be improved while maintaining good comprehensive mechanical properties, thereby meeting the requirements of kitchen waste bags for oil penetration resistance, puncture resistance, and damage resistance.

[0113] As can be seen from the comparative examples 1-3 and their data comparison, when a single-layer garbage bag is prepared using only the raw material formulation of the outer layer 1 of this application, although the mechanical strength and toughness of the bag can meet the requirements of a kitchen waste bag, its oil penetration resistance is far inferior to that of Example 1, which has a three-layer structure. When a single-layer garbage bag is prepared using only the raw material formulation of the core layer 2 of this application, its oil penetration resistance is significantly improved compared to Comparative Example 1, but it is generally harder and more brittle, resulting in its drop resistance failing to meet the usage requirements. When the core layer 2 is directly replaced with unmodified sodium-based montmorillonite instead of organically modified montmorillonite, the oil penetration resistance, puncture resistance, and tear strength of the garbage bag are far lower than those of Example 1 due to the poor dispersion of unmodified montmorillonite in the polyethylene matrix, failing to meet the usage requirements. Therefore, the three-layer structure designed in this application and the introduction of specific organically modified montmorillonite into the core layer 2 are necessary conditions for achieving excellent oil penetration resistance and mechanical properties in kitchen waste bags.

[0114] Based on the data from Example 1, Comparative Examples 3-5, and Table 1, it is evident that montmorillonite modified with a two-component quaternary ammonium salt co-intercalation containing dual long-chain alkyl and vinyl groups exhibits superior oil permeability resistance, puncture resistance, and tear strength compared to unmodified montmorillonite or montmorillonite prepared with a single component modification. This is likely because the introduction of dual long-chain alkyl quaternary ammonium salts effectively expands the interlayer spacing of montmorillonite, weakening the interaction between layers. Conversely, the introduction of vinyl quaternary ammonium salts reacts with the introduced maleic anhydride-grafted polyethylene, synergistically enhancing the compatibility of montmorillonite with the matrix resin while simultaneously expanding the montmorillonite layers. This achieves uniform dispersion and allows the core layer 2 to fully form a peelable structure. On one hand, peeling dispersion reduces the permeable area of ​​the core layer 2, lowering the penetration rate of oil molecules. On the other hand, it acts as a heterogeneous nucleating agent for the core layer 2, increasing the PE crystallinity of the core layer 2, thus simultaneously improving the overall barrier performance and mechanical properties of the garbage bag.

[0115] Based on the data from Examples 1, 3-4, Comparative Example 6, and Table 1, it can be seen that as the alkyl chain length of the introduced dual-long-chain alkyl quaternary ammonium salt shortens, its layer-expansion effect on montmorillonite weakens, leading to a certain degree of reduction in the oil penetration resistance and mechanical strength of the garbage bag. Replacing the dual-long-chain alkyl quaternary ammonium salt with a single-long-chain alkyl quaternary ammonium salt of the same group results in a significant decrease in the oil penetration resistance of the garbage bag, and its mechanical properties are also inferior to those of Example 1. This may be because, under the same molar amount of cations, the layer-expansion effect of the single-long-chain alkyl quaternary ammonium salt on montmorillonite is far less than that of the dual-long-chain alkyl quaternary ammonium salt, and the layer-expansion effect of the shorter-chain dual-long-chain alkyl quaternary ammonium salt is also poor. Consequently, strong interactions still exist between the layers of montmorillonite modified by these two intercalation methods, which is detrimental to its uniform dispersion in the polyethylene matrix and prevents it from fully exerting its barrier-enhancing and crystallization nucleation functions, ultimately leading to a decline in the overall performance of the garbage bag.

[0116] Based on the data from Examples 1 and 5 and Table 1, it can be seen that when octyl metallocene polyethylene is removed from the outer layer 1 and the inner layer 3 and replaced with an equal amount of hexyl metallocene polyethylene I, although the tear strength and puncture resistance of the resulting garbage bag decrease significantly, its oil penetration resistance and drop resistance still meet the usage requirements. Moreover, the cost of hexyl metallocene polyethylene is lower than that of octyl metallocene polyethylene. Therefore, this formulation can also be applied to usage scenarios with lower strength requirements. The formulation components of the outer layer 1 and the inner layer 3 can be adjusted according to actual usage needs.

[0117] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this specific embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A kitchen waste bag, characterized in that: The bag body is made of a three-layer film formed by multi-layer co-extrusion blown film, wherein the film consists of a surface layer (1), a core layer (2) and an inner layer (3) from the outside to the inside; The outer layer (1) and the inner layer (3) comprise the following parts by weight of raw materials: The composition includes 30-36 parts of composite metallocene polyethylene, 35-40 parts of linear low-density polyethylene, 10-15 parts of low-density polyethylene, 10-16 parts of POE elastomer, 3.5-4.5 parts of processing auxiliaries, and 0-3 parts of color masterbatch. The core layer (2) comprises the following parts by weight of raw materials: Composite metallocene polyethylene II 40-50 parts, linear low-density polyethylene 20-30 parts, low-density polyethylene 15-20 parts, organic modified montmorillonite 3-6 parts, maleic anhydride grafted polyethylene 5-10 parts, processing auxiliary material II 0.6-2 parts. The organically modified montmorillonite is prepared by co-intercalation of montmorillonite with a dual long-chain alkyl quaternary ammonium salt and a vinyl quaternary ammonium salt.

2. The kitchen waste bag according to claim 1, characterized in that: The dual long-chain alkyl quaternary ammonium salt is a dual long-chain alkyl quaternary ammonium salt containing C16-C18.

3. A kitchen waste bag according to claim 1, characterized in that: The method for preparing the organically modified montmorillonite includes the following steps: Montmorillonite was dispersed in water and heated to 450-560°C. Then, a dual long-chain alkyl quaternary ammonium salt and a vinyl quaternary ammonium salt were added. The mixture was heated to 80-90°C and stirred to react. After the reaction was completed, the mixture was cooled, filtered, washed with water, dried, ground, and sieved to obtain the organically modified montmorillonite.

4. A kitchen waste bag according to claim 3, characterized in that: The molar amount of cations in the added dual-chain alkyl quaternary ammonium salt is controlled to be 0.5-0.8 times the cation exchange capacity of montmorillonite, and the molar amount of cations in the added vinyl quaternary ammonium salt is controlled to be 0.4-0.6 times the cation exchange capacity of montmorillonite.

5. A kitchen waste bag according to claim 1, characterized in that: Based on the total mass of the composite metallocene polyethylene I, the composite metallocene polyethylene I is composed of the following raw materials in the following mass percentages: Octyl metallocene polyethylene with a melt index of 0.8-1.2 g / 10 min is 60-75%; Hexyl metallocene polyethylene I with a melt index of 1.0-1.5 g / 10 min is 10-15%; and Hexyl metallocene polyethylene II with a melt index of 1.8-2.4 g / 10 min is 15-25%. Based on the total mass of the composite metallocene polyethylene II, the composite metallocene polyethylene II is composed of the following raw materials in the following mass percentages: The melt flow index (MFI) of the following raw materials was 30-40% for octyl metallocene polyethylene (MCPE) with a melt flow index of 0.8-1.2 g / 10 min, 40-50% for hexyl metallocene polyethylene I with a melt flow index of 1.0-1.5 g / 10 min, and 10-20% for hexyl metallocene polyethylene II with a melt flow index of 1.8-2.4 g / 10 min. The MFI test conditions for all the above raw materials were 190℃ and 2.16 kg.

6. A kitchen waste bag according to claim 5, characterized in that: The melt index of the linear low-density polyethylene is 1.5-2 g / 10 min; the melt index of the low-density polyethylene is 2-3 g / 10 min; the melt index of the POE elastomer is 2-3 g / 10 min; the melt index test conditions for all the above raw materials are 190℃ and 2.16 kg.

7. A kitchen waste bag according to claim 1, characterized in that: The processing aid I includes processing aid I, antistatic agent, opening agent and slip agent, and the mass ratio of processing aid I, antistatic agent, opening agent and slip agent is 1:2:(2-3):(2-3); The processing aid II includes processing aid II, antioxidant and calcium stearate, and the mass ratio of processing aid II, antioxidant and calcium stearate is 1:(1-2.5):(0.6-1).

8. A kitchen waste bag according to claim 1, characterized in that: Based on the total thickness of the film, the thickness ratio of the surface layer (1), the core layer (2) and the inner layer (3) is (1-1.5):(2-3):(1-1.5), and the thickness ratio of the surface layer (1) and the inner layer (3) is 1:

1.

9. A method for preparing a kitchen waste bag, used to prepare a kitchen waste bag as described in any one of claims 1-8, characterized in that, Includes the following steps: S1. Mix the raw materials evenly according to the proportion, extrude and granulate, and dry them thoroughly to obtain surface layer masterbatch, core layer masterbatch and inner layer masterbatch respectively. S2. The surface layer masterbatch, the core layer masterbatch, and the inner layer masterbatch are respectively fed into independent extruders. The masterbatch is melted and plasticized by the extruder. The melt of each masterbatch is distributed to the flow channel of each layer by the layer distributor. The three melts are combined and the blank is extruded from the die head and die orifice under high pressure. The blank is blown into a film by the top blowing method. After being cooled by the air ring, blown, and pulled and wound, a semi-finished film is obtained. S3. The semi-finished film is welded and sealed using a bag-making machine, then cut, folded, and rolled up to obtain the kitchen waste bag.

10. A method for preparing a kitchen waste bag according to claim 9, characterized in that, S2 also includes the step of forming the color band: S201. The surface masterbatch containing the colored masterbatch is put into an independent extruder. The masterbatch is melted and plasticized by the extruder. The surface masterbatch melt containing the colored masterbatch is distributed to the surface flow channel by the layer distributor. It is combined with the surface melt and the blank is extruded from the die head and die orifice under high pressure. The blank is blown into a film by the top blowing method. It is cooled and blown by the air ring and formed into several colored strips extending longitudinally along the film in the surface layer (1).