A sling assembly frame and its manufacturing method
By using chromium-aluminum co-infiltration technology to form an anti-corrosion composite infiltration layer on the surface of the sling rack, the corrosion problem of the rack in high humidity and high salt spray environment is solved, achieving corrosion resistance and convenient maintenance, which is suitable for the management of slings in shipbuilding and repair workshops.
Patent Information
- Application Number
- CN202611444066.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
Existing sling racks are prone to corrosion in the high humidity and high salt spray environment of shipbuilding and repair workshops, and are inconvenient to maintain. They cannot effectively prevent tool damage from impacts, and it is inconvenient to adjust the configuration time during navigation and docking.
The chromium-aluminum co-diffusion surface treatment technology forms an anti-corrosion composite infiltration layer on the surface of the rack. Through reasonable structural design, the slings are classified and placed for management. The chromium-aluminum co-diffusion layer is metallurgically bonded to the base material, and has the ability to be repassivated, making it suitable for high humidity and high salt spray environments.
It improves the corrosion resistance of the rack, extends its service life, avoids the risk of coating peeling, and has the ability to be repassivated, making it suitable for the high humidity and high salt spray environment of shipbuilding and repair workshops.
Smart Images

Figure CN123061850A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of tooling technology, specifically to a sling assembly rack, and more particularly to a sling assembly rack for on-site sling placement management in shipbuilding and repair workshops and its manufacturing method. Background Technology
[0002] In shipbuilding and repair workshops, docks, and on ships, maintenance tools typically include wire ropes, nylon slings, shackles, and rust removal equipment such as electric grinders, drills, and brushes. Ships operating on polar routes may also have icebreaking equipment. The variety and quantity of tools are vast. To improve on-site management and standardize the placement of these tools, preventing haphazard and disorganized storage, standardized tooling is needed for tool management.
[0003] In existing technologies, simple shelves or racks are typically used to store slings and rigging in workshops and ship warehouses. These racks are mostly composed of ordinary carbon steel square tubing and steel plates, with a rust-preventive paint coating for protection. Shipbuilding and repair workshops are usually located in coastal areas with high salt spray content in the air, and tools are frequently exposed to seawater or salty, humid environments during use. Ordinary rust-preventive paint is prone to blistering and peeling in salt spray environments. Once the paint film is damaged, the base material of the rack will rust, seriously affecting the structural strength and service life of the rack.
[0004] Considering that tools often become contaminated with dirt, including seawater and rust, placing them directly on ordinary racks can easily cause them to be bumped and damaged, resulting in paint damage and making maintenance particularly inconvenient. Electrostatic powder coating of racks is often more effective, but it still cannot avoid bumps and damage. Damage to electrostatic powder coating requires specialized equipment, which is often not convenient to place in valuable ship space. In addition, considering that the configuration time during voyages and docking is inconvenient to adjust, it is generally not suitable to purchase low-value items such as racks that may require customization during port calls.
[0005] To meet the needs of ship navigation, an ideal pylon needs to have a long service life, low maintenance requirements, be as corrosion-resistant as possible, and have the capacity to support necessary tools. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a sling assembly bracket and its manufacturing method. Through reasonable structural design, the slings can be classified and placed for management. The corrosion resistance of the bracket can be improved through chromium-aluminum co-infiltration surface treatment technology, making it suitable for the high humidity and high salt spray environment of shipbuilding and repair workshops.
[0007] To achieve the above objectives, the technical solution provided by the present invention is as follows: A lifting sling assembly includes a frame, a panel, and a hook assembly. The frame is composed of multiple square tubes and includes a bottom frame and a support frame vertically positioned above the bottom frame. The panel is laid on at least a portion of the outer surface of the frame. The hook assembly is mounted on the support frame and includes a central hook and side hooks. Support legs are located below the bottom frame, lifting the bottom frame off the ground to create a transfer space for forklifts. The outer surfaces of the frame, panel, and hook assembly are covered with an anti-corrosion composite coating.
[0008] Preferably, the base material of the frame, panel and hook assembly is carbon structural steel or low alloy steel.
[0009] Preferably, the anti-corrosion composite infiltration layer is a chromium-aluminum co-infiltration layer, the thickness of the anti-corrosion composite infiltration layer is 50μm to 300μm, the mass fraction of chromium in the infiltration layer is 15% to 30%, and the mass fraction of aluminum is 5% to 15%.
[0010] The present invention also provides a method for manufacturing a sling assembly bracket, comprising the following steps: S1. Provide multiple square tubes, combine the multiple square tubes to form a skeleton, the skeleton includes a bottom frame and a support frame vertically set above the bottom frame; provide steel plates, lay the steel plates on at least part of the outer surface of the skeleton to form a panel; provide round steel, bend the round steel into hooks, combine the hooks on the support frame to form a hook assembly; set support legs below the bottom frame to form a transfer space between the bottom frame and the ground.
[0011] S2. Clean the surface of the square tube before assembly to remove surface oxide scale and oil stains.
[0012] S3. A solid powder diffusion infiltration method is used to form an anti-corrosion composite infiltration layer on the surface of the bracket. The square tube is placed in a sealed box containing solid infiltration agent and buried in the solid infiltration agent. It is kept at a temperature of 1000℃ to 1150℃ for 4 to 12 hours, so that chromium and aluminum elements can diffuse into the surface of the bracket through thermal diffusion.
[0013] S4. The square tube after the diffusion layer is subjected to diffusion annealing treatment, so that the diffused chromium and aluminum elements react with the iron elements in the bracket matrix to generate chromium and aluminum ferrite solid solution and intermetallic compounds, forming an anti-corrosion composite diffusion layer.
[0014] S5. Perform final heat treatment on the square tube to transform the matrix structure into tempered sorbite or tempered troostite.
[0015] Preferably, in step S1, the surface cleaning is carried out by sandblasting or shot blasting, and the surface roughness Ra of the cleaned bracket is not greater than 6.3 μm.
[0016] Preferably, in step S3, the solid infiltrator comprises, by mass percentage: 25% to 40% chromium powder, 15% to 25% aluminum powder, 30% to 55% alumina filler, and 1% to 3% ammonium chloride activator.
[0017] Preferably, in step S3, the solid infiltrator also contains silicon powder, and the mass percentage of silicon powder in the solid infiltrator is 3% to 8%. Chromium, aluminum and silicon elements are simultaneously infiltrated into the surface of the square tube to form a chromium-aluminum-silicon ternary co-infiltration layer.
[0018] Preferably, in step S3, the solid penetrant also contains rare earth element powder, which is cerium powder or lanthanum powder, and the mass percentage of the rare earth element powder in the solid penetrant is 0.5% to 2%.
[0019] Preferably, in step S3, the solid powder diffusion treatment is carried out under a protective atmosphere or vacuum conditions; in step S4, the diffusion annealing treatment is carried out at a temperature of 1000°C to 1100°C for a holding time of 2 hours to 6 hours, and then cooled to room temperature by furnace cooling.
[0020] Preferably, in step S5, the final heat treatment includes quenching and tempering, with the quenching temperature being 850°C to 900°C and the holding time being 1 hour to 3 hours, and the tempering temperature being 550°C to 650°C and the holding time being 2 hours to 5 hours, so that the matrix structure is transformed into tempered sorbite.
[0021] The advantages and beneficial effects of this invention are as follows: A chromium-aluminum co-infiltration technology is used to form an anti-corrosion composite infiltration layer on the surface of the square tube. The infiltration layer and the substrate are metallurgically bonded, eliminating the risk of coating peeling. The aluminum element in the infiltration layer has re-passivation capability; when the surface is scratched, the exposed aluminum element preferentially oxidizes to form a dense oxide film, resealing the damaged area. This is particularly suitable for the harsh environment of high humidity and high salt spray in shipbuilding and repair workshops. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the overall structure of the sling assembly frame of the present invention.
[0023] Figure 2 This is a schematic diagram of the hook structure of the present invention.
[0024] The annotations in the attached figures are explained as follows: 1-Frame; 11-Bottom frame; 12-Support frame; 13-Vertical square tube; 14-Horizontal square tube; 2-Panel; 3-Hook assembly; 31-Middle hook; 32-Side hook; 4-Support leg; 5-Transfer space. Detailed Implementation
[0025] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings. It is to be understood that the specific embodiments described herein are merely illustrative of this application and not intended to limit it. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application.
[0026] The terms “comprising” and “having”, and any variations thereof, used in this application are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not limited to the steps or units listed, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to such process, method, product, or apparatus.
[0027] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly or implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0028] Please see Figure 1 and Figure 2 The present invention provides a sling assembly bracket, comprising a frame 1, a panel 2, and a hook assembly 3.
[0029] The frame 1 is the main load-bearing structure of the hanger, composed of multiple square tubes. The frame 1 includes a bottom frame 11 and a support frame 12 vertically positioned above the bottom frame 11. The bottom frame 11, composed of multiple square tubes forming a rectangular planar structure, bears the overall weight of the hanger and transfers the load to the ground. The support frame 12 includes vertical square tubes 13 and horizontal square tubes 14. The vertical square tubes 13 are located at the rear edge of the bottom frame 11 and extend vertically upwards; the horizontal square tubes 14 connect adjacent vertical square tubes 13, reinforcing the support frame 12 and providing installation positions for the hook assembly 3.
[0030] In this embodiment, the front edge of the bottom frame 11 does not have a vertical square tube 13, forming an open access port. Operators can directly access the slings from the front of the rack without having to go around to the side or back of the rack, making it convenient to use.
[0031] Panel 2 is laid on the rear side and top surface of frame 1, surrounding and covering the square tube frame. Panel 2 is made of steel plates of different specifications, which are fixed to the square tubes of frame 1 by combination or bolt connection. Panel 2 serves two purposes: firstly, it acts as a seal to prevent small tools from falling from behind the hanger; secondly, the surface of panel 2 forms a flat marking area, which can be used to affix or spray-paint signs to classify and label lifting slings of different specifications and tonnages.
[0032] Support legs 4 are provided below the bottom frame 11. The support legs 4 are made of square tubing or steel plate and are vertically installed at the four corners of the bottom frame 11, raising the bottom frame 11 a certain height off the ground. The distance between the bottom frame 11 and the ground is sufficient to accommodate the insertion of a forklift fork, forming a transfer space 5 for forklift insertion, facilitating the overall transfer of the rack. A pallet structure is formed below the bottom frame 11, ensuring that the slings do not contact the ground when suspended, preventing them from getting damp or contaminated with ground oil.
[0033] Hook assembly 3 is mounted on support frame 12 and includes intermediate hooks 31 and side hooks 32. Multiple intermediate hooks 31 are arranged at intervals along the horizontal direction of support frame 12, used for suspending long slings such as wire ropes and nylon slings. Intermediate hooks 31 are made of round steel through bending, forming a U-shape or J-shape, with their openings facing upwards or forwards. Side hooks 32 are located on the left and right sides of support frame 12, used for suspending ring-shaped tools such as shackles. Side hooks 32 are also made of round steel through bending, with their opening directions being the same as or different from the opening directions of the intermediate hooks 31.
[0034] The middle hook and side hooks are formed in one piece and are fastened to the frame as needed. They are not directly welded to the panel. The outer hook panel has mounting holes and grooves. The panel and the support frame are formed in one piece. The support frame is welded and fixed after the joint is installed. It should be noted that the welding and fixing here should be done after the composite seepage layer is completed.
[0035] The outer surfaces of the frame 1, panel 2, and hook assembly 3 are covered with an anti-corrosion composite diffusion layer. This layer is a chromium-aluminum co-diffusion layer, formed through a solid powder diffusion diffusion method. The thickness of the anti-corrosion composite diffusion layer ranges from 50 μm to 300 μm, with a chromium mass fraction of 15% to 30% and an aluminum mass fraction of 5% to 15%. Chromium primarily contributes to corrosion resistance and oxidation resistance, while aluminum preferentially oxidizes to form a dense oxide film, providing a sealing and protective effect on the diffusion layer. When scratches occur on the hanger surface, the aluminum exposed to air preferentially reacts with oxygen, forming a dense oxide film in situ on the damaged surface, resealing the damaged area and achieving re-passivation.
[0036] The manufacturing method of the lifting sling assembly bracket of the present invention will be described in detail below.
[0037] In step S1, multiple square tubes are provided and cut to size according to the design. The specifications of the square tubes are determined based on the load-bearing requirements of the rack; square tubes in different parts can use the same or different specifications. The cut square tubes are assembled and positioned according to the structural design of the frame 1 to form the frame 1. Steel plates are provided and cut to size according to the design. The cut steel plates are laid on the rear side and top surface of the frame 1 and fixed by combination or bolt connection to form the panel 2. Round steel is provided and bent into shape according to the design shape of the hooks. The bent hooks are assembled on the support frame 12 according to the design position to form the hook group 3. Support legs 4 are assembled below the bottom frame 11 to form a transfer space 5 between the bottom frame 11 and the ground. The height of the support legs 4 is determined according to the size of the forklift fork arm, usually 80mm to 150mm.
[0038] Before assembly, the surfaces of the various frame components of the hanger contain contaminants such as oxide scale, welding slag, and oil. These contaminants hinder the contact between alloying elements and the substrate surface during the subsequent co-diffusion process, leading to discontinuous diffusion layers and localized leakage. Therefore, step S2 involves cleaning the surface of the square tube. Surface cleaning is performed using sandblasting or shot blasting with white or brown fused alumina as the abrasive. The surface roughness Ra of the cleaned hanger should not exceed 6.3 μm. Appropriate surface roughness is beneficial for the contact and adsorption of the solid diffusion agent with the substrate surface, but excessive roughness will result in uneven diffusion layer thickness, while insufficient roughness will hinder agent adhesion. After cleaning, residual dust on the surface is blown away with compressed air.
[0039] Chromium-aluminum co-diffusion is the process of forming an alloy diffusion layer rich in chromium and aluminum on the surface of the mounting bracket. The solid diffusion agent, by mass percentage, comprises: 25% to 40% chromium powder to provide the chromium source; 15% to 25% aluminum powder to provide the aluminum source; 30% to 55% alumina filler to prevent sintering and ensure the diffusion agent's looseness; and 1% to 3% ammonium chloride activator, which decomposes at high temperatures to produce hydrogen chloride gas, cleaning the substrate surface and promoting the diffusion of active atomic states of the alloying elements. The cleaned mounting bracket is then placed in a sealed enclosure, and the square tube is completely submerged in the solid diffusion agent. The sealed enclosure must have excellent high-temperature sealing properties to prevent air from entering and causing oxidation of the diffusion layer surface.
[0040] The sealed enclosure is typically constructed with a heat-resistant lining, mimicking the shape of a square tube to minimize the loss of the diffusion agent. The enclosure is placed in a heating furnace and heated to 1000°C to 1150°C, held for 4 to 12 hours. Within this temperature range, chromium and aluminum have sufficient diffusion rates to form an effective diffusion layer. Below 1000°C, the diffusion rate of chromium is too low to form a sufficient thickness for corrosion resistance within a reasonable time; above 1150°C, the matrix grains coarsen, and excessive growth of intermetallic compounds in the diffusion layer increases its brittleness. The diffusion treatment is performed under a protective atmosphere such as argon or vacuum to prevent oxidation of the diffusion layer surface at high temperatures.
[0041] In a preferred embodiment of the present invention, silicon powder is also added to the solid infiltration agent. The addition of silicon allows chromium, aluminum, and silicon to infiltrate simultaneously, forming a chromium-aluminum-silicon ternary co-infiltration layer. Silicon has an atomic radius similar to that of iron and can partially dissolve in ferrite, reducing the difference in thermal expansion coefficients between the infiltration layer and the substrate, decreasing thermal stress during cooling, and improving the bonding strength between the infiltration layer and the substrate. The mass percentage of silicon powder in the infiltration agent is 3% to 8%.
[0042] In another preferred embodiment of the present invention, rare earth element powder, specifically cerium powder or lanthanum powder, is added to the solid infiltration agent, and the mass percentage of the rare earth element powder in the solid infiltration agent is 0.5% to 2%. The infiltration-promoting effect of rare earth elements stems from their larger atomic radii. The segregation of rare earth atoms at grain boundaries causes lattice distortion, providing more grain boundary diffusion channels for chromium and aluminum atoms, thus significantly improving the diffusion rate. For the same infiltration layer thickness, the addition of rare earth elements can reduce the co-infiltration temperature by approximately 50°C or shorten the holding time by approximately 30%.
[0043] Traditional organic coatings or thermally sprayed metal coatings rely on physical isolation to block corrosive media. Once the coating is damaged, the corrosive media directly contact the substrate, forming a large cathodic-small anodic galvanic corrosion pattern at the damaged area. Corrosion concentrates in the damaged area, accelerating local penetration. In contrast, the chromium-aluminum co-diffusion layer of this invention is a diffusion layer, with a metallurgical bond between the layer and the substrate, eliminating the risk of interface delamination. The aluminum element in the layer endows it with re-passivation capability. When the surface of the layer suffers localized damage due to scratches, impacts, or long-term service, the aluminum element exposed to air preferentially reacts with oxygen, forming a dense oxide film in situ on the damaged surface. This oxide film forms at an extremely fast rate and has extremely high density, effectively resealing the damaged area and preventing further penetration of corrosive media into the substrate. This mechanism is similar to the passivation behavior of chromium in stainless steel, but aluminum oxide has higher thermodynamic stability and density than chromium oxide.
[0044] Alumina has a lower formation free energy, allowing it to form under lower oxygen partial pressures. Furthermore, its molar volume matches well with the aluminum matrix, making the oxide film less prone to cracking and peeling. Therefore, even if localized microscopic damage occurs on the surface of the diffusion layer in a corrosive environment, the diffusion layer can achieve re-passivation of the damaged area through preferential oxidation of aluminum, confining the corrosion process to a very shallow surface area and preventing corrosion from extending into the matrix. Simultaneously, chromium in the diffusion layer provides long-term corrosion resistance. Chromium is dissolved in the ferrite matrix, increasing the electrode potential of the matrix and reducing the corrosion current density. Chromium reduces the overall corrosion rate, while aluminum is responsible for the rapid repair of damaged areas; together, they ensure the diffusion layer maintains its complete protective function during long-term service.
[0045] After co-diffusion treatment, the diffused chromium and aluminum elements are mainly concentrated in a very shallow area on the surface of the square tube, with a large concentration gradient and no obvious diffusion transition layer between the diffused layer and the matrix. This makes the interface prone to stress concentration and cracking. Therefore, step S4 involves diffusion annealing. The diffusion annealing temperature is 1000℃ to 1100℃, and the holding time is 2 to 6 hours. At this temperature, the chromium and aluminum atoms enriched on the surface continue to diffuse inward, while iron atoms in the matrix diffuse outward, forming a diffusion transition zone with a gradual change in composition between the diffused layer and the matrix. This transition zone eliminates the abrupt interface jump between the diffused layer and the matrix, enabling a metallurgical bond between them. During diffusion annealing, chromium, aluminum, and iron undergo a solid-state reaction, generating a ferrite solid solution containing chromium and aluminum, as well as Fe-Al and Fe-Cr intermetallic compounds. After annealing, the tube is cooled to room temperature by furnace cooling to reduce thermal stress.
[0046] The matrix structure of the square tube after diffusion annealing exhibits coarse grains and decreased strength and toughness due to prolonged high-temperature holding. Step S5 involves readjusting the matrix structure through a final heat treatment. The final heat treatment includes quenching and tempering. The quenching temperature is 850℃ to 900℃, held for 1 to 3 hours, to re-austenite the matrix before quenching to obtain a martensitic structure. The tempering temperature is 550℃ to 650℃, held for 2 to 5 hours, to decompose the martensite into tempered sorbite.
[0047] The square tube of the sling assembly treated by this invention has a surface salt spray corrosion resistance time of not less than 1000 hours, meeting the usage requirements of high humidity and high salt spray environment in shipbuilding and repair workshops.
[0048] The technical solution of the present invention will be described in detail below with reference to specific embodiments.
[0049] Example 1 This embodiment provides a sling assembly bracket and its manufacturing method.
[0050] The frame 1 is composed of square tubes of different specifications. The bottom frame 11 is a rectangular structure composed of 50mm×50mm×3mm square tubes, with dimensions of 1500mm×800mm. The vertical square tubes 13 supporting the frame 12 are 40mm×40mm×3mm square tubes, located at the rear edge of the bottom frame 11, with a height of 1200mm. The horizontal square tubes 14 are 30mm×30mm×2.5mm square tubes, connecting adjacent vertical square tubes 13 at intervals of 300mm. Four supporting legs 4 are provided at the bottom of the bottom frame 11, with a height of 120mm.
[0051] Panel 2 is a 2mm thick steel plate, laid on the rear side and top surface of frame 1, and fixed by assembly. The surface of panel 2 has a marking area.
[0052] The hook assembly 3 includes five central hooks 31 and two side hooks 32. The central hooks 31 are made of round steel with a diameter of 10mm bent into a J shape and are arranged at 200mm intervals along the length of the horizontal square tube 14. The side hooks 32 are made of round steel with a diameter of 10mm bent into an L shape and are located on the left and right sides of the support frame 12.
[0053] The base material of the bracket is Q235B carbon structural steel.
[0054] After assembly, the bracket is sandblasted with 16-mesh white corundum as abrasive, resulting in a surface roughness Ra of 5.2μm. Compressed air is then used to blow away surface dust.
[0055] Prepare a solid infiltration agent by mass percentage: 35% chromium powder, 20% aluminum powder, 43% alumina filler, and 2% ammonium chloride activator, with the sum of the mass percentages of all components being 100%. Place the rack into a sealed enclosure and cover it with the infiltration agent. Heat to 1050℃ under an argon protective atmosphere and hold for 8 hours.
[0056] The bracket after diffusion annealing was held at 1050℃ for 4 hours for diffusion annealing, and then furnace cooled to room temperature at a cooling rate of 30℃ / h.
[0057] The rack was heated to 880℃ and held for 1.5 hours, then oil-quenched to room temperature. It was then tempered at 600℃ for 3 hours and furnace-cooled to room temperature.
[0058] According to the test, the thickness of the surface coating of the bracket in this embodiment is 180μm, and the time for red rust to appear in the neutral salt spray test is 1200 hours.
[0059] Example 2 The solid infiltrator, by mass percentage, consists of: 33% chromium powder, 18% aluminum powder, 6% silica powder, 41% alumina filler, and 2% ammonium chloride activator, with the sum of the mass percentages of all components being 100%. The co-infiltrating temperature is 1050℃, and the infiltration time is 8 hours. The remaining steps are the same as in Example 1.
[0060] Testing revealed that the thickness of the infiltration layer on the surface of the bracket in this embodiment is 165 μm, and the interface between the infiltration layer and the substrate is well bonded. The critical load in the scratch test is approximately 20% higher than that in Embodiment 1. The time to the appearance of red rust in the neutral salt spray test is 1150 hours.
[0061] Example 3 The solid infiltrator, by mass percentage, consists of: 34% chromium powder, 19% aluminum powder, 1.5% cerium powder, 44% alumina filler, and 1.5% ammonium chloride activator, with the sum of the mass percentages of all components being 100%. The co-infiltrating temperature is 1000℃, and the temperature is maintained for 6 hours. The remaining steps are the same as in Example 1.
[0062] Testing revealed that the thickness of the infiltration layer on the surface of the bracket in this embodiment is 155μm, which is comparable to the thickness of the infiltration layer obtained in Example 1 after heat preservation at 1050℃ for 8 hours. The time for red rust to appear in the neutral salt spray test is 1180 hours.
[0063] Example 4 The bracket base material in this embodiment is Q345B low alloy steel, and it adopts chromium-aluminum-silicon ternary co-infiltration.
[0064] The solid infiltration agent, by mass percentage, consists of: 34% chromium powder, 17% aluminum powder, 5% silicon powder, 42% alumina filler, and 2% ammonium chloride activator, with the sum of the mass percentages of all components being 100%. The co-infiltration temperature is 1000℃, and the holding time is 10 hours. The quenching temperature is 860℃, and the tempering temperature is 620℃.
[0065] According to the test, the thickness of the surface coating of the bracket in this embodiment is 200μm, and the time for red rust to appear in the neutral salt spray test is 1100 hours.
[0066] Comparative Example 1 is a Q235B bracket without surface treatment, which is only assembled without any anti-corrosion treatment. Extensive red rust appeared after 24 hours of neutral salt spray testing.
[0067] Comparative Example 2 is a Q235B rack coated with conventional anti-rust paint. The coating process is as follows: after sandblasting, two coats of epoxy zinc-rich primer and two coats of polyurethane topcoat are applied, with a total dry film thickness of 120μm. After 240 hours of neutral salt spray testing, blistering of the paint film and rust spread occurred.
[0068] Comparative Example 3 is a Q235B hanging rack treated with hot-dip galvanizing, with a zinc coating thickness of 85μm. White rust appeared after 500 hours of neutral salt spray testing.
[0069] The time for red rust to appear on the rack in the neutral salt spray test of Embodiment 1 of the present invention is 1200 hours, which is superior to 24 hours in Comparative Example 1, 240 hours in Comparative Example 2, and 500 hours in Comparative Example 3. Furthermore, the coating layer of the rack in Embodiment 1 of the present invention is metallurgically bonded to the substrate, eliminating the risk of coating peeling, and the coating layer has re-passivation capability, making it particularly suitable for the harsh environment of high humidity and high salt spray in shipbuilding and repair workshops.
[0070] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A sling assembly frame, characterized in that, include: The skeleton is composed of multiple square tubes, and the skeleton includes a bottom frame and a support frame vertically arranged above the bottom frame; A panel is laid on at least a portion of the outer surface of the skeleton; A hook assembly, disposed on the support frame, includes a middle hook and side hooks; The bottom frame is provided with support legs, which lift the bottom frame off the ground to form a transfer space for forklifts to insert. The outer surfaces of the frame, the panel, and the hook assembly are covered with an anti-corrosion composite impregnation layer.
2. The sling assembly frame according to claim 1, characterized in that: The base material of the frame, the panel, and the hook assembly is carbon structural steel or low alloy steel.
3. The sling assembly frame according to claim 1, characterized in that: The anti-corrosion composite infiltration layer is a chromium-aluminum co-infiltration layer with a thickness of 50μm to 300μm. The mass fraction of chromium in the infiltration layer is 15% to 30%, and the mass fraction of aluminum is 5% to 15%.
4. A method for manufacturing a sling assembly bracket, characterized in that, Includes the following steps: S1. Provide multiple square tubes, which can be combined to form a skeleton, the skeleton including a bottom frame and a support frame vertically arranged above the bottom frame; A steel plate is provided and laid on at least a portion of the outer surface of the frame to form a panel; round steel is provided and bent into hooks, which are then assembled on the support frame to form a hook assembly; support legs are provided below the bottom frame to create a transfer space between the bottom frame and the ground. S2. Clean the surface of the square tube to remove oxide scale and oil stains; S3. A solid powder diffusion infiltration method is used to form an anti-corrosion composite infiltration layer on the surface of the square tube. The square tube is placed in a sealed box containing a solid infiltration agent and buried in the solid infiltration agent. It is kept at a temperature of 1000℃ to 1150℃ for 4 to 12 hours to allow chromium and aluminum elements to diffuse into the surface of the square tube through thermal diffusion. S4. The square tube after the diffusion layer is subjected to diffusion annealing treatment, so that the diffused chromium and aluminum elements react with the iron elements in the square tube matrix to generate chromium and aluminum ferrite solid solution and intermetallic compounds, forming an anti-corrosion composite diffusion layer. S5. Perform final heat treatment on the square tube to transform the matrix structure into tempered sorbite or tempered troostite.
5. The manufacturing method of the sling assembly bracket according to claim 4, characterized in that: In step S1, the surface cleaning is carried out by sandblasting or shot blasting, and the surface roughness Ra of the cleaned bracket is no greater than 6.3μm.
6. The method for manufacturing the sling assembly bracket according to claim 4, characterized in that: In step S3, the solid infiltrator comprises, by mass percentage: 25% to 40% chromium powder, 15% to 25% aluminum powder, 30% to 55% alumina filler, and 1% to 3% ammonium chloride activator.
7. The method for manufacturing the sling assembly bracket according to claim 6, characterized in that: In step S3, the solid infiltration agent also contains silicon powder, and the silicon powder accounts for 3% to 8% of the mass of the solid infiltration agent. Chromium, aluminum and silicon elements are simultaneously infiltrated into the surface of the hanger to form a chromium-aluminum-silicon ternary co-infiltration layer.
8. The method for manufacturing the sling assembly bracket according to claim 7, characterized in that: In step S3, the solid penetrant also contains rare earth element powder, wherein the rare earth element is cerium powder or lanthanum powder, and the mass percentage of the rare earth element powder in the solid penetrant is 0.5% to 2%.
9. The method for manufacturing the sling assembly bracket according to claim 4, characterized in that: In step S3, the solid powder diffusion treatment is carried out under a protective atmosphere or vacuum conditions; in step S4, the diffusion annealing treatment is carried out at a temperature of 1000℃ to 1100℃, and the holding time is 2 hours to 6 hours. After annealing, the powder is cooled to room temperature by furnace cooling.
10. The method for manufacturing the sling assembly bracket according to claim 4, characterized in that: In step S5, the final heat treatment includes quenching and tempering. The quenching temperature is 850°C to 900°C and the holding time is 1 hour to 3 hours. The tempering temperature is 550°C to 650°C and the holding time is 2 hours to 5 hours, so that the matrix structure is transformed into tempered sorbite.