Aluminum ion-doped nickel-iron layered bimetallic hydroxides, their preparation methods and applications
By doping aluminum ions into nickel-iron layered bimetallic hydroxides, the electronic structure is optimized and catalytic active sites are increased, solving the problems of low conductivity and insufficient activity of NiFe LDH, achieving high-efficiency electrocatalytic performance, and making it suitable for cathode and anode applications in water electrolyzers.
Patent Information
- Application Number
- CN202611078918.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-10
AI Technical Summary
Nickel-iron base layer bimetallic hydroxide (NiFe LDH) has problems such as low intrinsic conductivity, insufficient active sites, poor hydrogen evolution reaction (HER) activity, and metal dissolution, which restrict its widespread application in the field of water electrolysis.
By doping aluminum ions into nickel-iron layered bimetallic hydroxides (NiFe LDHs), the electronic structure of NiFe LDHs was optimized, the number of catalytic active sites was increased, and the binding ability of reaction intermediates was adjusted. Aluminum-doped NiFe LDH nanosheet arrays were then grown on the substrate surface using a hydrothermal method.
It enhances the electrocatalytic activity of NiFe LDH for hydrogen evolution reaction (HER) and oxygen evolution reaction (OER), has low material cost, excellent electrocatalytic performance for hydrogen evolution and oxygen evolution reaction, and high stability, making it suitable as a cathode and anode material for water electrolyzers.
Smart Images

Figure CN123062014A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the fields of electrocatalysis and nanomaterials technology. Specifically, this application relates to an aluminum ion-doped nickel-iron layered bimetallic hydroxide, its preparation method, and its application. Background Technology
[0002] Electrochemical processes driven by renewable energy, utilizing electrocatalysts with special properties, can convert raw materials in the Earth's atmosphere (such as water, nitrogen, and carbon dioxide) into important fuels and chemicals. Among these electrochemical processes, water electrolysis for hydrogen production has received widespread attention due to the sustainability of hydrogen energy, as it can effectively address the issues of long-distance transportation and the volatility of renewable energy sources. However, the slow reaction kinetics at the cathode and anode have become a major bottleneck restricting the development of water electrolysis for hydrogen production. To improve the reaction rate of water electrolysis, designing highly active and stable electrocatalysts to reduce the overpotential of the reaction is of great significance.
[0003] Transition metal oxides and hydroxides have attracted widespread research interest due to their abundant reserves, low cost, and stability in electrolyte environments. Among them, nickel-iron layered bimetallic hydroxides (NiFe LDH) exhibit oxygen evolution reaction (OER) activity comparable to Ru-based and Ir-based noble metal catalysts in alkaline media, and their structure and composition are easily modulated, making them one of the most promising electrocatalysts. However, the low intrinsic conductivity, insufficient accessibility of active sites, poor hydrogen evolution reaction (HER) activity, and metal dissolution of NiFe LDH are key bottlenecks restricting its further application. Summary of the Invention
[0004] This application aims to at least partially address one of the technical problems in related technologies. Therefore, the purpose of this application is to provide an aluminum ion-doped nickel-iron layered bimetallic hydroxide, its preparation method, and its applications. By doping aluminum ions into the nickel-iron layered bimetallic hydroxide, this application optimizes the electronic structure of NiFe LDH, increases the number of catalytically active sites in the material, and adjusts the binding ability of reaction intermediates, thereby further enhancing the electrocatalytic HER and OER activities of NiFe LDH.
[0005] In a first aspect of this application, a method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxides is provided. According to embodiments of this application, the method includes: (1) Dissolve nickel salt, iron salt, aluminum salt, urea and ammonium fluoride in water to obtain a mixed solution; (2) Add the substrate to the mixed solution and carry out a hydrothermal reaction. After the reaction is completed, cool down and wash to obtain aluminum ion-doped nickel-iron layered bimetallic hydroxide.
[0006] The method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide according to the above embodiments of this application optimizes the electronic structure of NiFe LDH by doping it with aluminum ions, increases the number of catalytically active sites in the material, and adjusts the binding ability of reaction intermediates, thereby further enhancing the electrocatalytic HER and OER activities of NiFe LDH. Furthermore, the catalyst material of this application (i.e., aluminum ion-doped nickel-iron layered bimetallic hydroxide) has low cost, excellent electrocatalytic hydrogen evolution and oxygen evolution reaction performance, and high stability, and can be used as cathode and anode materials for water electrolyzers.
[0007] In addition, the method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the nickel salt includes at least one of nickel nitrate and nickel chloride; and / or, the iron salt includes at least one of ferric nitrate and ferric chloride; and / or, the aluminum salt includes at least one of aluminum nitrate and aluminum chloride.
[0008] In some embodiments of this application, the molar ratio of the nickel salt to the iron salt is (4~10):1; and / or, the molar ratio of the nickel salt to the aluminum salt is (8~10):1.
[0009] In some embodiments of this application, the total amount of the nickel salt, the iron salt and the aluminum salt is in a molar ratio of urea and ammonium fluoride to 1:(1~5):(4~10).
[0010] In some embodiments of this application, the substrate includes at least one of nickel foam, nickel felt, carbon cloth, and carbon paper.
[0011] In some embodiments of this application, the temperature of the hydrothermal reaction is 100°C to 150°C.
[0012] In some embodiments of this application, the hydrothermal reaction time is 4 to 8 hours.
[0013] In a second aspect of this application, an aluminum ion-doped nickel-iron layered bimetallic hydroxide (NiFe LDH) is proposed, which is prepared using the method described in the first aspect. Therefore, by doping the NiFe LDH with aluminum ions, this application optimizes the electronic structure of NiFe LDH, increases the number of catalytically active sites in the material, and adjusts the binding ability of reaction intermediates, thereby further enhancing the electrocatalytic HER and OER activities of NiFe LDH.
[0014] In addition, the aluminum ion-doped nickel-iron layered bimetallic hydroxide according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the total mass of the aluminum ion-doped nickel-iron layered bimetallic hydroxide is 100%, and the doping amount of the aluminum ions is 1% to 15%.
[0015] In a third aspect of this application, the application of aluminum ion-doped nickel-iron layered bimetallic hydroxide prepared by the method of the first aspect or the aluminum ion-doped nickel-iron layered bimetallic hydroxide of the second aspect in the electrolysis of water to produce hydrogen is proposed. The catalyst material of this application (i.e., aluminum ion-doped nickel-iron layered bimetallic hydroxide) has low cost, excellent electrocatalytic hydrogen evolution and oxygen evolution reaction performance, and high stability, and can be used as cathode and anode materials for water electrolyzers.
[0016] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0017] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic flowchart of a method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide according to some embodiments of this application; Figure 2 The images show the XRD patterns of the aluminum ion-doped nickel-iron layered bimetallic hydroxide prepared in Example 1 of this application and the nickel-iron layered bimetallic hydroxide prepared in Comparative Example 1. Figure 3 The LSV curves of OER for the aluminum ion-doped nickel-iron layered bimetallic hydroxide prepared in Example 1 of this application and the nickel-iron layered bimetallic hydroxide prepared in Comparative Example 1 are shown. Figure 4 The LSV curves of the aluminum ion-doped nickel-iron layered bimetallic hydroxide prepared in Example 1 of this application and the nickel-iron layered bimetallic hydroxide prepared in Comparative Example 1 are shown. Detailed Implementation
[0018] The embodiments of this application are described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application.
[0019] In a first aspect of this application, a method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxides is provided. According to embodiments of this application, refer to the appendix... Figure 1 The above method includes: S100: dissolving nickel salt, iron salt, aluminum salt, urea and ammonium fluoride in water to obtain a mixed solution; S200: adding a substrate to the mixed solution, carrying out a hydrothermal reaction, cooling after the reaction is completed, washing, and obtaining aluminum ion-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH).
[0020] The following details the beneficial effects achievable by the method proposed in this application for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH): Nickel-iron layered bimetallic hydroxides (NiFe LDH) offer advantages such as low cost and excellent OER activity. However, NiFe LDH suffers from low intrinsic conductivity, insufficient active sites, poor HER activity, and metal dissolution, severely hindering its widespread application in water electrolysis. This method, by doping NiFe LDH with aluminum ions, optimizes the electronic structure of NiFe LDH, increases the number of catalytic active sites, and adjusts the binding ability of reaction intermediates, thereby further enhancing the electrocatalytic HER and OER activity of NiFe LDH. Furthermore, the catalyst material of this application (i.e., aluminum ion-doped NiFe LDH) exhibits low cost, superior electrocatalytic hydrogen evolution and oxygen evolution reaction performance, and high stability, making it suitable as a cathode and anode material for water electrolyzers.
[0021] Simultaneously, this application utilizes a hydrothermal method to grow aluminum-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH) nanosheet arrays on the substrate surface. This process, conducted in a high-temperature, high-pressure, and closed environment, facilitates rapid reactant diffusion and high reactivity, promoting ordered atomic arrangement and resulting in Al-NiFe LDH crystals with high crystallinity and few lattice defects. High crystallinity signifies a more stable material structure, leading to higher electron transport efficiency and easier expression of intrinsic activity in electrocatalysis applications. Furthermore, the core advantage of this hydrothermal synthesis of Al-NiFe LDH lies in the precise control of the crystal growth process, enabling the production of materials with high crystallinity, regular morphology, and excellent performance. Uniform nanosheet arrays can be grown directly on a conductive substrate in one step, eliminating the need for subsequent coating processes, increasing the electrode's specific surface area, and improving electrode performance. Moreover, the reaction is carried out in a closed system, avoiding the introduction of external impurities, easily yielding a pure, single Al-NiFe LDH phase free of other nickel-iron oxide or hydroxide impurities, resulting in extremely high process repeatability. The synthesis process described in this application requires relatively mild reaction conditions and is simple to operate, requiring only 100℃~150℃ and a common oven. The equipment is simple, and the process is a one-step process, making it highly suitable for laboratory research and industrial applications.
[0022] Specifically, see the attached document. Figure 1 The above methods include: S100: Dissolve nickel salt, iron salt, aluminum salt, urea and ammonium fluoride in water to obtain a mixed solution; In this step, nickel salt, iron salt, aluminum salt, urea and ammonium fluoride are dissolved in water to obtain a mixed solution, which is then transferred to a reaction vessel.
[0023] In the embodiments of this application, the specific types of nickel salts are not particularly limited, and those skilled in the art can select them according to actual needs. As some specific embodiments, nickel salts include at least one of nickel nitrate and nickel chloride.
[0024] In the embodiments of this application, the specific types of iron salts are not particularly limited, and those skilled in the art can select them according to actual needs. As some specific embodiments, iron salts include at least one of ferric nitrate and ferric chloride.
[0025] In the embodiments of this application, the specific types of aluminum salts are not particularly limited, and those skilled in the art can choose according to actual needs. As some specific embodiments, aluminum salts include at least one of aluminum nitrate and aluminum chloride.
[0026] According to some specific embodiments of this application, the molar ratio of the nickel salt and the iron salt is (4~10):1, for example, it can be 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc., thereby further ensuring the effective synthesis of nickel-iron base layer bimetallic hydroxide (NiFe LDH).
[0027] According to some specific embodiments of this application, the molar ratio of the nickel salt and aluminum salt is (8~10):1, for example, it can be 8:1, 9:1, 10:1, etc., thereby further ensuring the effective synthesis of aluminum-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH).
[0028] According to some specific embodiments of this application, the total amount of the above-mentioned nickel salt, iron salt and aluminum salt and the molar ratio of urea and ammonium fluoride is 1:(1~5):(4~10), thereby further ensuring the effective synthesis of aluminum-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH).
[0029] S200: The substrate is added to the mixed solution, and a hydrothermal reaction is carried out. After the reaction is completed, the temperature is lowered and the solution is washed to obtain aluminum ion-doped nickel-iron layered bimetallic hydroxide.
[0030] In this step, the substrate can be added to the mixed solution and subjected to a hydrothermal reaction for a period of time. After the reaction is completed, the temperature is lowered and the sample is washed with pure water after the temperature drops to room temperature to obtain an aluminum ion-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH) sample.
[0031] During the hydrothermal process, urea decomposes upon heating, producing ammonia water, which further ionizes into ammonium ions (NH4+). + ) and hydroxide ions (OH) These slowly released OH It will react with Ni in the solution 2+ Fe 3+ And Al 3+ The reaction promotes the co-precipitation of various ions in a specific ratio, forming a layered Al-NiFe LDH crystal structure. The uniform decomposition of urea contributes to the formation of a uniform, nanostructured Al-NiFe LDH. This structure has a larger specific surface area than the dense structure obtained by direct precipitation with strong bases (such as NaOH), making it more advantageous for electrocatalytic applications. Although ammonium fluoride does not participate in the framework of Al-NiFe LDH, its presence directly determines the final microstructure of Al-NiFe LDH, thus affecting its performance. Fluoride ions (F...) In the reaction solution, specific crystal faces of the growing Al-NiFe LDH crystals can be selectively adsorbed or "etched" through coordination. This effect inhibits growth in certain directions and promotes the formation of nanosheet morphology. Furthermore, by controlling the amount of ammonium fluoride, the thickness, size, and arrangement of the Al-NiFe LDH nanosheets can be precisely controlled, ultimately obtaining a nanosheet array with a high specific surface area. This structure exposes more catalytically active sites, which is beneficial for improving its HER and OER performance.
[0032] In the embodiments of this application, the specific type of the substrate is not particularly limited, and those skilled in the art can choose according to actual needs. As some specific embodiments, the substrate includes at least one of nickel foam, nickel felt, carbon cloth, and carbon paper.
[0033] According to some specific embodiments of this application, the temperature of the above-mentioned hydrothermal reaction is 100℃~150℃, for example, it can be 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, etc., thereby further ensuring the smooth progress of the hydrothermal reaction, and thus further ensuring the effective synthesis of aluminum-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH).
[0034] According to some specific embodiments of this application, the hydrothermal reaction time is 4 to 8 hours, for example, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, etc., thereby further ensuring that the raw materials react fully, thereby further ensuring the effective synthesis of aluminum-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH).
[0035] In a second aspect of this application, an aluminum ion-doped nickel-iron layered bimetallic hydroxide (NiFe LDH) is proposed, which is prepared using the method described in the first aspect. Therefore, by doping the NiFe LDH with aluminum ions, this application optimizes the electronic structure of NiFe LDH, increases the number of catalytically active sites in the material, and adjusts the binding ability of reaction intermediates, thereby further enhancing the electrocatalytic HER and OER activities of NiFe LDH.
[0036] According to some specific embodiments of this application, the total mass of the aluminum ion-doped nickel-iron layered bimetallic hydroxide is 100%, and the doping amount of aluminum ions is 1% to 15%, for example, 1%, 3%, 5%, 7%, 10%, 12%, 15%, etc. This further ensures the optimization of the electronic structure of NiFe LDH, increases the number of catalytically active sites in the material, and adjusts the binding ability of reaction intermediates, thereby further enhancing the electrocatalytic activity of NiFe LDH.
[0037] In a third aspect of this application, the application of aluminum ion-doped nickel-iron layered bimetallic hydroxide prepared by the method of the first aspect or the aluminum ion-doped nickel-iron layered bimetallic hydroxide of the second aspect in the electrolysis of water to produce hydrogen is proposed. The catalyst material of this application (i.e., aluminum ion-doped nickel-iron layered bimetallic hydroxide) has low cost, excellent electrocatalytic hydrogen evolution and oxygen evolution reaction performance, and high stability, and can be used as cathode and anode materials for water electrolyzers.
[0038] The embodiments of this application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. In addition, unless otherwise specified, all reagents used in the following embodiments are commercially available or can be synthesized according to the methods described herein or known methods. For reaction conditions not listed, they are also readily available to those skilled in the art.
[0039] Example 1 This embodiment provides a method for preparing an aluminum ion-doped nickel-iron layered bimetallic hydroxide, including: 2 mmol of nickel nitrate, 0.25 mmol of ferric nitrate, 0.25 mmol of aluminum nitrate, 4 mmol of ammonium fluoride, and 10 mmol of urea were dissolved in 35 mL of purified water. After stirring evenly, the solution was transferred to a 50 mL reaction vessel. Two pieces of nickel foam (NF, 1 cm × 3 cm) were then added. The reaction was carried out at 120 °C for 6 hours. After cooling, the sample was washed several times with purified water and dried under vacuum at 60 °C for 8 hours to obtain an aluminum ion-doped nickel-iron layered bimetallic hydroxide (Al-NiFeLDH / NF) sample uniformly grown on the surface of the nickel foam.
[0040] X-ray diffraction, linear sweep voltammetry (LSW) tests for oxygen evolution reaction, and linear sweep voltammetry (LSW) tests for hydrogen evolution reaction were performed on the aluminum ion-doped nickel-iron layered bimetallic hydroxide (Al-NiFe LDH / NF) sample prepared in Example 1 and the nickel-iron layered bimetallic hydroxide (NiFe LDH / NF) sample prepared in Comparative Example 1, respectively. The results are as follows: Figure 2-4 As shown. Among them, the XRD pattern ( Figure 2 This indicates the successful synthesis of NiFe LDH / NF and Al-NiFe LDH / NF materials. As shown in the LSV curves of the OER (…),… Figure 3 The Al-NiFe LDH / NF prepared in Example 1, in 1.0 M KOH electrolyte at room temperature, achieved a speed of 500 mA / cm². 2 The required current density is only 293 mV overpotential, which is significantly better than the NiFe LDH / NF prepared in Comparative Example 1 (424 mV). (HER LSV curve) Figure 4 This indicates that the Al-NiFe LDH / NF prepared in Example 1 achieves a current density of 500 mA / cm². 2 The overpotential was only 326 mV, which is significantly better than that of NiFe LDH / NF prepared in Comparative Example 1 (458 mV).
[0041] Example 2 This embodiment provides a method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide, which is basically the same as the method in the previous embodiment, except that: The amount of ferric nitrate used is 0.2 mmol, which means the molar ratio of nickel nitrate to ferric nitrate is 10:1.
[0042] The same Al-NiFe LDH nanosheet array was obtained uniformly grown on the NF surface, but the nanosheet surface was smoother.
[0043] Example 3 This embodiment provides a method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide, which is basically the same as the method in the previous embodiment, except that: The amount of aluminum nitrate used is 0.2 mmol, which means the molar ratio of nickel nitrate to aluminum nitrate is 10:1.
[0044] The same Al-NiFe LDH nanosheet array was obtained uniformly grown on the NF surface, but the nanosheets were thicker.
[0045] Example 4 This embodiment provides a method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide, which is basically the same as the method in the previous embodiment, except that: The reaction temperature is 100℃.
[0046] The same Al-NiFe LDH nanosheet array was obtained uniformly grown on the NF surface, but the nanosheet size was smaller.
[0047] Comparative Example 1 This comparative example provides a method for preparing a nickel-iron layered bimetallic hydroxide, including: 2 mmol of nickel nitrate, 0.25 mmol of ferric nitrate, 4 mmol of ammonium fluoride, and 10 mmol of urea were dissolved in 35 mL of purified water and stirred until homogeneous. The mixture was then transferred to a 50 mL reactor. Two pieces of nickel foam (NF, 1 cm × 3 cm) were added, and the mixture was reacted at 120 °C for 6 hours. After cooling, the sample was washed several times with purified water and dried under vacuum at 60 °C for 8 hours to obtain a NiFe LDH (NiFe LDH / NF) sample uniformly grown on the surface of the nickel foam.
[0048] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0049] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A method for preparing aluminum ion-doped nickel-iron layered bimetallic hydroxide, characterized in that, include: (1) Dissolve nickel salt, iron salt, aluminum salt, urea and ammonium fluoride in water to obtain a mixed solution; (2) Add the substrate to the mixed solution and carry out a hydrothermal reaction. After the reaction is completed, cool down and wash to obtain aluminum ion-doped nickel-iron layered bimetallic hydroxide.
2. The method according to claim 1, characterized in that, The nickel salt includes at least one of nickel nitrate and nickel chloride; And / or, the iron salt includes at least one of ferric nitrate and ferric chloride; And / or, the aluminum salt includes at least one of aluminum nitrate and aluminum chloride.
3. The method according to claim 1, characterized in that, The molar ratio of the nickel salt to the iron salt is (4~10):1; And / or, the molar ratio of the nickel salt to the aluminum salt is (8~10):
1.
4. The method according to claim 1, characterized in that, The total metal content of the nickel salt, the iron salt, and the aluminum salt is in a molar ratio of 1:(1~5):(4~10) to the urea and the ammonium fluoride.
5. The method according to any one of claims 1 to 4, characterized in that, The substrate includes at least one of nickel foam, nickel felt, carbon cloth, and carbon paper.
6. The method according to any one of claims 1 to 4, characterized in that, The temperature of the hydrothermal reaction is 100℃~150℃.
7. The method according to claim 6, characterized in that, The hydrothermal reaction takes 4 to 8 hours.
8. An aluminum ion-doped nickel-iron layered bimetallic hydroxide, characterized in that, It is prepared by any one of claims 1 to 7.
9. The aluminum ion-doped nickel-iron layered bimetallic hydroxide according to claim 8, characterized in that, The total mass of the nickel-iron layered bimetallic hydroxide based on aluminum ion doping is 100%, and the doping amount of aluminum ions is 1% to 15%.
10. The application of an aluminum ion-doped nickel-iron layered bimetallic hydroxide prepared by any one of claims 1 to 7, or the aluminum ion-doped nickel-iron layered bimetallic hydroxide of claim 8 or 9, in the electrolysis of water to produce hydrogen, wherein the aluminum ion-doped nickel-iron layered bimetallic hydroxide is used as the cathode and anode of the electrolysis of water to produce hydrogen.