A dual-scale low-shrinkage alkali-activated mortar for graphite tailings and its preparation method

By combining graphite tailings powder and granulated blast furnace slag powder to form a composite cementitious material, and basalt manufactured sand and graphite tailings sand to form a composite fine aggregate, and by combining graded treatment and segmented water addition and mixing, the problem of fragmented utilization of graphite tailings in powder and sand grades has been solved, and the high strength and stability of low-shrinkage alkali-activated mortar has been achieved.

CN123062230APending Publication Date: 2026-11-10NORTHEAST AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611483695.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively address the synergistic utilization of graphite tailings at both the powder and sand scales. This results in excessive drying shrinkage of high-slag alkali-activated mortar, reduced workability of basalt manufactured sand due to its sharp edges and rough surfaces, unstable effective water-cement ratio due to fluctuations in the water absorption state of graphite tailings sand, and fragmented utilization of graphite tailings.

Method used

A composite cementitious material composed of graphite tailings powder and granulated blast furnace slag powder, and a composite fine aggregate composed of basalt manufactured sand and graphite tailings sand are formed. Through graded treatment and segmented water addition and mixing, combined with sodium silicate nonahydrate and polycarboxylate-based high-performance water-reducing agent, a dual-scale low-shrinkage alkali-activated mortar is formed.

Benefits of technology

It enables dual-scale utilization of graphite tailings, improves the shrinkage performance and workability of mortar, stabilizes the water-cement ratio, enhances 28-day compressive strength, and reduces drying shrinkage strain.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062230A_ABST
    Figure CN123062230A_ABST
Patent Text Reader

Abstract

This invention discloses a dual-scale low-shrinkage alkali-activated mortar made from graphite tailings and its preparation method, belonging to the field of solid waste resource utilization technology. The mortar comprises graphite tailings powder, granulated blast furnace slag powder, sodium silicate nonahydrate, water, and a composite fine aggregate composed of basalt manufactured sand and graphite tailings sand. The graphite tailings powder and graphite tailings sand are obtained from the same graphite tailings raw material through drying, grading, and separation. One portion is ground and sieved to obtain graphite tailings powder, and the other portion is sieved to obtain graphite tailings sand. Mortar shrinkage is controlled by the proportion of graphite tailings powder, the gradation of the composite fine aggregate, the moisture content of the aggregate, and the correction of sodium silicate nonahydrate crystal water. In the embodiments, when the mass ratio of basalt manufactured sand to graphite tailings sand is 80:20, the 28-day compressive strength is 37.6 MPa, and the 28-day drying shrinkage strain is 525 microstrain.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid waste resource utilization technology, specifically relating to a dual-scale low-shrinkage alkali-activated mortar for graphite tailings and its preparation method. Background Technology

[0002] Graphite beneficiation processes generate large quantities of graphite tailings, whose mineral composition typically includes quartz, feldspar, mica, iron-bearing minerals, carbonate minerals, and a small amount of residual graphite. The mineral composition, particle size, water absorption rate, and residual sulfide content of graphite tailings vary across different mining areas. Existing resource utilization methods include using them as road or backfill materials, as fine aggregate to replace natural sand, and as a powder component in cement-based or alkali-activated materials after grinding or activation.

[0003] Granulated blast furnace slag possesses potential hydraulic activity and can form cementitious products and provide strength under silicate-based alkaline activation conditions. However, the alkaline activation system for high-activity slag reacts rapidly, often accompanied by significant autogenous shrinkage and drying shrinkage. Blending milled graphite tailings powder with slag can reduce the proportion of highly reactive slag while simultaneously providing fine particle filling, thus balancing the mechanical and shrinkage properties of the mortar.

[0004] On the other hand, research has been conducted on the use of graphite tailings as a fine aggregate to replace natural sand, basalt manufactured sand as a fine aggregate for mortar or concrete, and graphite tailings sand for alkali-activated mortar. However, simply adding basalt manufactured sand or graphite tailings sand to existing alkali-activated systems easily results in single-material substitution or parallel combinations, making it difficult to solve the problem of synergistic utilization of the same graphite tailings at both the powder and sand scales. Furthermore, the sharp edges and rough surfaces of basalt manufactured sand may affect workability, and fluctuations in the particle size and water absorption state of graphite tailings sand can cause changes in the effective water-cement ratio.

[0005] Therefore, it is necessary to combine the functional division of the same graphite tailings at different particle size scales, the particle size complementarity of composite fine aggregates, the shrinkage control of alkali-activated cementitious phase and aggregate phase, and the correction of aggregate moisture content to form a low-shrinkage alkali-activated mortar with a clear composition and preparation process. Summary of the Invention

[0006] In order to overcome the shortcomings of the prior art, this invention provides a graphite tailings dual-scale low-shrinkage alkali-activated mortar and its preparation method, which effectively solves the problems of excessive drying shrinkage of high slag alkali-activated mortar, decreased workability due to the sharp edges and rough surfaces of basalt manufactured sand, unstable effective water-cement ratio due to fluctuations in the water absorption state of graphite tailings sand, and the disconnect between the utilization of graphite tailings powder and the utilization of sand grades.

[0007] The technical solution adopted in this invention is as follows: This invention proposes a dual-scale low-shrinkage alkali-activated mortar for graphite tailings and its preparation method, comprising a composite cementitious material, sodium silicate nonahydrate, water, and composite fine aggregate; the composite cementitious material is composed of graphite tailings powder and granulated blast furnace slag powder; the composite fine aggregate is composed of basalt manufactured sand and graphite tailings sand. The same graphite tailings raw material is dried, graded, and then split; one portion is ground and screened to obtain graphite tailings powder, and the other portion is screened to obtain graphite tailings sand.

[0008] In this invention, graphite tailings powder is used for component adjustment and fine particle filling of composite cementitious materials, graphite tailings sand is used for fine particle supplementation of composite fine aggregates, and basalt manufactured sand is used to form the main gradation of composite fine aggregates; the dual scale refers to the micron-scale of graphite tailings powder and the sand-scale of graphite tailings sand.

[0009] Based on a total mass of 100 parts, the composite cementitious material consists of graphite tailings powder and granulated blast furnace slag powder, with graphite tailings powder comprising 10–50 parts and granulated blast furnace slag powder comprising 50–90 parts, and the sum of their mass parts being 100 parts; sodium silicate nonahydrate, in sodium oxide equivalent, comprises 3%–11% of the composite cementitious material mass; the water-cement ratio is 0.42–0.52; the mass ratio of composite fine aggregate to composite cementitious material is 1.5–2.8; the composite fine aggregate consists of basalt manufactured sand and graphite tailings sand, with the mass fractions of basalt manufactured sand and graphite tailings sand in the composite fine aggregate being 70%–90% and 10%–30%, respectively, and the sum of their mass fractions being 100%.

[0010] Furthermore, based on a total mass of 100 parts of composite cementitious materials, graphite tailings powder accounts for 20-40 parts, and granulated blast furnace slag powder accounts for 60-80 parts; the median particle size of graphite tailings powder is 4-8 micrometers, and the D50 of granulated blast furnace slag powder is 8-40 micrometers.

[0011] Furthermore, sodium silicate nonahydrate comprises 5% to 7% of the composite cementitious material by weight of sodium oxide equivalent, and the water-cement ratio is 0.46 to 0.50.

[0012] Furthermore, the basalt manufactured sand has a particle size of less than 4.75 mm, a fineness modulus of 2.6–3.0, an apparent density of 2600–2800 kg / m³, a bulk density of 1500–1850 kg / m³, a 24-hour water absorption rate of no more than 1.5%, a stone powder mass fraction of 3%–10%, a methylene blue value of no more than 1.4, a crushing index of no more than 25%, and an irregular particle mass fraction of no more than 30%.

[0013] Furthermore, the mass fraction of particles with a diameter of 0.075–1.18 mm in the graphite tailings sand is not less than 80%, the fineness modulus is 0.8–1.8, the apparent density is 2700–2950 kg / m³, and the bulk density is 1300–1650 kg / m³.

[0014] Furthermore, the mass ratio of basalt manufactured sand to graphite tailings sand is 75:25 to 85:15, and the mass ratio of composite fine aggregate to composite cementitious material is 1.8 to 2.4.

[0015] Furthermore, the mortar also includes a polycarboxylate-based high-performance water-reducing agent, the dosage of which is 0.2% to 0.8% of the mass of the composite cementitious material by solid weight.

[0016] In this invention, the water-cement ratio is calculated as the ratio of the nominal total water mass to the total mass of graphite tailings powder and granulated blast furnace slag powder. The nominal total water mass includes the crystal water contained in sodium silicate nonahydrate and the theoretically added mixing water before correction; the actual added mixing water is based on the theoretically added mixing water before correction, and is corrected according to the measured moisture content and 24-hour water absorption rate of basalt manufactured sand and graphite tailings sand.

[0017] The above-mentioned mortar preparation method includes the following steps:

[0018] Step S1: Dry and classify the graphite tailings raw material, further grind and screen a portion of it to obtain graphite tailings powder, and screen the other portion to obtain graphite tailings sand.

[0019] Step S2: Weigh graphite tailings powder, granulated blast furnace slag powder and sodium silicate nonahydrate according to the set ratio, dry mix for 2-5 minutes to obtain composite cementitious dry material;

[0020] Step S3: Screen and shape the basalt manufactured sand as needed, control the particle size, fineness modulus, stone powder content and the proportion of irregular particles, and determine the apparent density, bulk density, moisture content and 24-hour water absorption rate of the basalt manufactured sand and graphite tailings sand; weigh the basalt manufactured sand and graphite tailings sand according to the set ratio, premix for 1 to 3 minutes to obtain composite fine aggregate;

[0021] Step S4: Calculate the nominal total water volume of the system according to the set water-cement ratio, deduct the sodium silicate crystal water nonahydrate, and obtain the theoretical additional mixing water volume before correction. Then, correct the actual additional mixing water volume according to the moisture content and 24-hour water absorption rate of the basalt manufactured sand and graphite tailings sand.

[0022] Step S5: First, add 70% to 85% of the actual added mixing water to the composite gel dry material and stir at low speed for 1 to 3 minutes to form a uniform slurry; after adding the premixed composite fine aggregate, stir at low speed for 1 to 2 minutes, then add the remaining actual added mixing water, and add polycarboxylate-based high-performance water-reducing agent when it is necessary to improve workability, and stir at high speed for 1 to 3 minutes.

[0023] Step S6: Pour the mixture into a mold and vibrate it or mold it according to the mortar standard. Cover it to prevent early water loss. Remove the mold after about 24 hours and continue curing after removing the mold.

[0024] By adopting the above technical solution, the beneficial effects achieved by the present invention are as follows:

[0025] (i) The same graphite tailings are diverted to prepare graphite tailings powder and graphite tailings sand, which are used for composite cementitious materials and composite fine aggregates, respectively. The graphite tailings powder is compounded with granulated blast furnace slag powder, which helps to achieve dual-scale utilization and regulate mortar shrinkage.

[0026] (ii) The complementary gradation of basalt manufactured sand and graphite tailings sand helps to improve the filling properties and mortar workability of composite fine aggregate;

[0027] (iii) The amount of water added for mixing is adjusted according to the moisture content of the aggregate and the water absorption rate in 24 hours, and water is added in stages and mixed step by step, which helps to stabilize the actual water-cement ratio and improve the uniformity of the mixture.

[0028] In three embodiments with the same cementitious material composition, sodium oxide equivalent, water-cement ratio, and sand-cement ratio, when the mass ratio of basalt manufactured sand to graphite tailings sand was 80:20, the 28-day compressive strength was 37.6 MPa and the drying shrinkage strain was 525 microstrain. Attached Figure Description

[0029] Figure 1 This is a flowchart of the preparation method of the present invention;

[0030] Figure 2 Bar charts showing the 28-day compressive strength of Examples 1-3;

[0031] Figure 3 The bar chart shows the 28-day drying shrinkage strain of Examples 1-3.

[0032] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof. Detailed Implementation

[0033] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0034] Detailed implementation examples are provided below:

[0035] Example 1:

[0036] Based on 1000 grams of composite cementitious material, the mass ratio of graphite tailings powder to granulated blast furnace slag powder was 30:70, the sodium oxide equivalent was 5%, the water-cement ratio was 0.48, the sand-cement ratio was 2.0, and the mass ratio of basalt manufactured sand to graphite tailings sand was 90:10. 300 grams of graphite tailings powder, 700 grams of granulated blast furnace slag powder, and 229.3 grams of sodium silicate nonahydrate (converted to 5% sodium oxide equivalent) were weighed and dry-mixed for 3 minutes to obtain the composite cementitious dry material. 1800 grams of basalt manufactured sand and 200 grams of graphite tailings sand were weighed and pre-mixed for 2 minutes to obtain the composite fine aggregate.

[0037] Based on a water-cement ratio of 0.48, the nominal total water in the system is 480 grams, of which approximately 130.8 grams are sodium silicate nonahydrate crystal water. Without considering aggregate moisture content correction, the theoretical value of the added mixing water is approximately 349.2 grams. Taking the theoretical feed without considering aggregate moisture content correction as an example, approximately 280 grams of added mixing water is first added to the composite cementitious dry material and stirred at low speed for 2 minutes to form a slurry. After adding the composite fine aggregate, stirring at low speed continues for 1 minute. The remaining added mixing water is mixed with a polycarboxylate-based high-performance water-reducing agent (measured at 0.4% of the composite cementitious material mass) and added, then stirred at high speed for 2 minutes to obtain the mixture. In actual preparation, the added mixing water is corrected according to the measured aggregate moisture content and 24-hour water absorption rate, and the initial and remaining added mixing water are allocated according to the corrected total amount.

[0038] The mixture was poured into molds, vibrated to compact, and covered to prevent early water loss. After approximately 24 hours, the molds were removed, and the mortar was cured according to the same curing regime. Testing showed that the mortar had a 28-day compressive strength of 36.8 MPa and a 28-day drying shrinkage strain of 610 microstrains.

[0039] Example 2:

[0040] Based on 1000 grams of composite cementitious material, the mass ratio of graphite tailings powder to granulated blast furnace slag powder was 30:70, the sodium oxide equivalent was 5%, the water-cement ratio was 0.48, the sand-cement ratio was 2.0, and the mass ratio of basalt manufactured sand to graphite tailings sand was 80:20. 300 grams of graphite tailings powder, 700 grams of granulated blast furnace slag powder, and 229.3 grams of sodium silicate nonahydrate (converted to 5% sodium oxide equivalent) were weighed and dry-mixed for 3 minutes to obtain the composite cementitious dry material. 1600 grams of basalt manufactured sand and 400 grams of graphite tailings sand were weighed and pre-mixed for 2 minutes to obtain the composite fine aggregate.

[0041] Based on a water-cement ratio of 0.48, the nominal total water in the system is 480 grams, of which approximately 130.8 grams are sodium silicate nonahydrate crystal water. Without considering aggregate moisture content correction, the theoretical value of the added mixing water is approximately 349.2 grams. Taking the theoretical feed without considering aggregate moisture content correction as an example, approximately 280 grams of added mixing water is first added to the composite cementitious dry material and stirred at low speed for 2 minutes to form a slurry. After adding the composite fine aggregate, stirring at low speed continues for 1 minute. The remaining added mixing water is mixed with a polycarboxylate-based high-performance water-reducing agent (measured at 0.4% of the composite cementitious material mass) and added, then stirred at high speed for 2 minutes to obtain the mixture. In actual preparation, the added mixing water is corrected according to the measured aggregate moisture content and 24-hour water absorption rate, and the initial and remaining added mixing water are allocated according to the corrected total amount.

[0042] The mixture was poured into molds, vibrated to compact, and covered to prevent early water loss. After approximately 24 hours, the molds were removed, and the mortar was cured according to the same curing regime. Testing showed that the mortar had a 28-day compressive strength of 37.6 MPa and a 28-day drying shrinkage strain of 525 microstrain.

[0043] Example 3:

[0044] Based on 1000 grams of composite cementitious material, the mass ratio of graphite tailings powder to granulated blast furnace slag powder was 30:70, the sodium oxide equivalent was 5%, the water-cement ratio was 0.48, the sand-cement ratio was 2.0, and the mass ratio of basalt manufactured sand to graphite tailings sand was 70:30. 300 grams of graphite tailings powder, 700 grams of granulated blast furnace slag powder, and 229.3 grams of sodium silicate nonahydrate (converted to 5% sodium oxide equivalent) were weighed and dry-mixed for 3 minutes to obtain the composite cementitious dry material. 1400 grams of basalt manufactured sand and 600 grams of graphite tailings sand were weighed and pre-mixed for 2 minutes to obtain the composite fine aggregate.

[0045] Based on a water-cement ratio of 0.48, the nominal total water in the system is 480 grams, of which approximately 130.8 grams are sodium silicate nonahydrate crystal water. Without considering aggregate moisture content correction, the theoretical value of the added mixing water is approximately 349.2 grams. Taking the theoretical feed without considering aggregate moisture content correction as an example, approximately 280 grams of added mixing water is first added to the composite cementitious dry material and stirred at low speed for 2 minutes to form a slurry. After adding the composite fine aggregate, stirring at low speed continues for 1 minute. The remaining added mixing water is mixed with a polycarboxylate-based high-performance water-reducing agent (measured at 0.4% of the composite cementitious material mass) and added, then stirred at high speed for 2 minutes to obtain the mixture. In actual preparation, the added mixing water is corrected according to the measured aggregate moisture content and 24-hour water absorption rate, and the initial and remaining added mixing water are allocated according to the corrected total amount.

[0046] The mixture was poured into molds, vibrated to compact, and covered to prevent early water loss. After approximately 24 hours, the molds were removed, and the mortar was cured according to the same curing regime. Testing showed that the mortar had a 28-day compressive strength of 36.4 MPa and a 28-day drying shrinkage strain of 565 microstrain.

[0047] Experimental Example: Performance Testing Methods and Results

[0048] The mortar fluidity can be determined using the method specified in GB / T 2419; the flexural strength and compressive strength can be determined according to GB / T17671-2021, ensuring consistency in specimen size, molding, and curing regime for each group; drying shrinkage can be tested using the same mortar shrinkage test method. After reaching the specified reference age, the drying shrinkage specimens are transferred to a uniform drying environment for length change testing, and the length change is measured at 7 days, 14 days, 28 days, 56 days, and 90 days under the same temperature and humidity regime. The performance results listed in the embodiments of this invention are the 28-day compressive strength and 28-day drying shrinkage strain; data from other ages not listed are not included in the embodiment results.

[0049] Table 1. Implementation ratios and 28-day performance of the experimental examples.

[0050] Example Cementitious material ratio Fine aggregate ratio 28-day compressive strength of neat pulp (MPa) 28-day compressive strength of mortar (MPa) 28-day drying shrinkage strain / micro-strain Example 1 30 / 70 90 / 10 42.0 36.8 610 Example 2 30 / 70 80 / 20 42.0 37.6 525 Example 3 30 / 70 70 / 30 42.0 36.4 565

[0051] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

[0052] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention; the actual structure is not limited thereto. In conclusion, if those skilled in the art are inspired by this description and design similar structures and embodiments without departing from the spirit of the invention, such designs should fall within the protection scope of the present invention.

Claims

1. A dual-scale low-shrinkage alkali-activated mortar for graphite tailings, characterized in that: The mixture includes a composite cementitious material, sodium silicate nonahydrate, water, and composite fine aggregate; based on a total mass of 100 parts, the composite cementitious material consists of 10-50 parts graphite tailings powder and 50-90 parts granulated blast furnace slag powder, with the sum of their mass parts being 100 parts; the sodium silicate nonahydrate, in sodium oxide equivalent, constitutes 3%-11% of the mass of the composite cementitious material; The water-cement ratio is 0.42–0.52; the mass ratio of the composite fine aggregate to the composite cementitious material is 1.5–2.8; the composite fine aggregate is composed of basalt manufactured sand and graphite tailings sand, wherein the basalt manufactured sand accounts for 70%–90% of the mass of the composite fine aggregate, and the graphite tailings sand accounts for 10%–30%, and the sum of their mass fractions is 100%; the graphite tailings powder and the graphite tailings sand are obtained by drying and classifying the same graphite tailings raw material, wherein a portion is ground and screened to obtain the graphite tailings powder, and the other portion is screened to obtain the graphite tailings sand; the median particle size of the graphite tailings powder is 2–12 micrometers, and the graphite tailings sand is sand-grade graphite tailings particles retained after screening.

2. The graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 1, characterized in that: Based on a total mass of 100 parts of the composite cementitious material, the graphite tailings powder comprises 20-40 parts, and the granulated blast furnace slag powder comprises 60-80 parts; the median particle size of the graphite tailings powder is 4-8 micrometers, and the D50 of the granulated blast furnace slag powder is 8-40 micrometers.

3. The graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 1, characterized in that: The sodium silicate nonahydrate is 5% to 7% of the mass of the composite cementitious material based on sodium oxide equivalent, and the water-cement ratio is 0.46 to 0.

50.

4. The graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 1, characterized in that: The manufactured basalt sand has a particle size of less than 4.75 mm, a fineness modulus of 2.6–3.0, an apparent density of 2600–2800 kg / m³, a bulk density of 1500–1850 kg / m³, a 24-hour water absorption rate of no more than 1.5%, a stone powder mass fraction of 3%–10%, a methylene blue value of no more than 1.4, a crushing index of no more than 25%, and an irregular particle mass fraction of no more than 30%.

5. The graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 1, characterized in that: The graphite tailings sand contains at least 80% particles with a diameter of 0.075–1.18 mm, a fineness modulus of 0.8–1.8, an apparent density of 2700–2950 kg / m³, and a bulk density of 1300–1650 kg / m³. When using the graphite tailings sand and basalt manufactured sand, the amount of additional mixing water should be adjusted based on the measured moisture content and 24-hour water absorption rate.

6. The graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 1, characterized in that: The mass ratio of the basalt manufactured sand to the graphite tailings sand is 75:25 to 85:15, and the mass ratio of the composite fine aggregate to the composite cementitious material is 1.8 to 2.

4.

7. The graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 1, characterized in that: It also includes a polycarboxylate-based high-performance water-reducing agent, wherein the dosage of the polycarboxylate-based high-performance water-reducing agent is 0.2% to 0.8% of the mass of the composite cementitious material based on solid mass.

8. A method for preparing a graphite tailings dual-scale low-shrinkage alkali-activated mortar according to any one of claims 1 to 7, characterized in that: Includes the following steps: Step S1: Dry and classify the graphite tailings raw material, grind and screen a portion of it to obtain graphite tailings powder, and screen the other portion to obtain graphite tailings sand. Step S2: Dry mix graphite tailings powder, granulated blast furnace slag powder and sodium silicate nonahydrate in a set ratio to obtain composite cementitious dry material; Step S3: Screen the basalt manufactured sand and perform necessary shaping. Measure the moisture content and 24-hour water absorption rate of the basalt manufactured sand and graphite tailings sand. Premix the basalt manufactured sand and graphite tailings sand according to the set ratio to obtain composite fine aggregate. Step S4: Calculate the nominal total water volume of the system according to the set water-cement ratio, include the crystal water contained in sodium silicate nonahydrate in the nominal total water volume of the system, obtain the theoretical additional mixing water volume before correction, and correct the actual additional mixing water volume according to the moisture content and 24-hour water absorption rate of basalt manufactured sand and graphite tailings sand. Step S5: Mix the composite gel dry material with a portion of the actual external mixing water to form a slurry, add the composite fine aggregate and continue stirring, then add the remaining actual external mixing water, and add polycarboxylate-based high-performance water-reducing agent when it is necessary to improve workability, and continue stirring to obtain the mixture. Step S6: Shape and cure the mixture.

9. The method for preparing a graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 8, characterized in that: In step S1, the drying temperature is 60–105 degrees Celsius; in step S2, the dry mixing time is 2–5 minutes; in step S3, the premixing time is 1–3 minutes; in step S5, 70%–85% of the actual added mixing water is added first, and the mixture is stirred at low speed for 1–3 minutes to form a slurry. After adding the composite fine aggregate, the mixture is stirred at low speed for 1–2 minutes, and then the remaining actual added mixing water is added. When using a polycarboxylate-based high-performance water-reducing agent, the polycarboxylate-based high-performance water-reducing agent is added simultaneously, and the mixture is stirred at high speed for 1–3 minutes.

10. The method for preparing a graphite tailings dual-scale low-shrinkage alkali-activated mortar according to claim 8, characterized in that: After molding, the product is first cured in an environment with a temperature of 20±2 degrees Celsius and a relative humidity of not less than 90%. After about 24 hours, the mold is removed and the product continues to be cured.