A long-afterglow foamed polypropylene bead, its preparation method, and its molded part
By preparing phosphorescent powder masterbatch, nucleating agent masterbatch, lubricant masterbatch and antioxidant masterbatch in foamed polypropylene beads, and combining it with carbon dioxide physical foaming, the problems of uneven cell size and poor molding fusion performance in long-afterglow foamed polypropylene beads were solved, and the combination of long-afterglow luminescence and high-efficiency molding performance was achieved.
Patent Information
- Application Number
- CN202611294334.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to coordinate long afterglow properties, cell size uniformity, and molding fusion properties in foamed polypropylene beads. In particular, uneven dispersion of rare earth aluminate long afterglow powder leads to poor cell nucleation and molding fusion properties.
Using random copolymer polypropylene as a carrier, phosphorescent powder masterbatch, nucleating agent masterbatch, lubricant masterbatch and antioxidant masterbatch are prepared by melt blending. Combined with carbon dioxide physical foaming agent, long afterglow foamed polypropylene beads are prepared to improve the uniformity of cell size and the bead fusion performance of molded parts.
While achieving long afterglow performance, it improves the uniformity of bead cell size and the bead fusion performance of molded parts, and can obtain long afterglow luminescence effect without additional surface luminescent coating, thus improving the overall performance of molded parts.
Smart Images

Figure CN123062771A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of foamed polypropylene technology, and in particular to a long-afterglow foamed polypropylene bead, its preparation method, and a molded part thereof. Background Technology
[0002] Expanded polypropylene (EPP) is lightweight, provides cushioning and energy absorption, is impact-resistant, heat-resistant, weather-resistant, and recyclable. It can be used in automotive parts, packaging, toys, building decoration, outdoor components, and safety equipment. Applications such as nighttime warnings, low-light visual signage, and decoration require EPP molded parts to have a long afterglow emission function without relying on an external power source.
[0003] One existing approach is to apply a glow-in-the-dark coating to the surface of the finished EPP molded part. This method facilitates altering the surface appearance of the part, but the coating is located in an area susceptible to friction and impact, and may wear down or peel off in some areas over long-term use; the coating process and coating system also add to the manufacturing steps.
[0004] JP2000336201A discloses a method for adding phosphorescent pigments to polyolefin resin and then heating and foaming to produce phosphorescent polyolefin foam; CN109486020B discloses a method for preparing PP phosphorescent masterbatch from polypropylene, surface-modified phosphorescent powder, superdispersant, antioxidant, and heat stabilizer; CN115895117A discloses foamed polypropylene beads containing inorganic functional materials, maleic anhydride-grafted modified polypropylene, and functional masterbatch. The above methods relate to phosphorescent polyolefin foam, PP phosphorescent masterbatch, and functional foamed polypropylene beads, respectively.
[0005] EPP beads require sequential processes including high-temperature, high-pressure medium infiltration, depressurization foaming, air pre-compression, and steam molding. Rare-earth aluminate long-afterglow powder has high hardness and density, and its direct addition to polypropylene can easily lead to uneven dispersion, potentially affecting cell nucleation, growth, and steam molding fusion between beads. Therefore, when introducing long-afterglow powder into EPP beads, it is necessary to coordinate long-afterglow performance, cell size uniformity, and molding fusion performance. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a long-afterglow foamed polypropylene bead, its preparation method and molding part, which improves the uniformity of bead cell size and the bead fusion performance of the molding part while obtaining long-afterglow performance.
[0007] To solve the above-mentioned technical problems, the present invention provides a method for preparing long-afterglow foamed polypropylene beads, comprising the following steps.
[0008] S1, random copolymer polypropylene carrier, rare earth aluminate long afterglow powder and maleic anhydride grafted modified polypropylene wax are melt-blended and granulated to obtain luminescent powder masterbatch.
[0009] S2, using random copolymer polypropylene as a carrier, melt-blends and granulates a cell nucleating agent to obtain a nucleating agent masterbatch.
[0010] S3 uses random copolymer polypropylene as a carrier to melt-blend and granulate the lubricant to obtain lubricant masterbatch.
[0011] S4 uses random copolymer polypropylene as a carrier to melt-blend and granulate antioxidants to obtain antioxidant masterbatch.
[0012] S5 is prepared by mixing random copolymer polypropylene, polypropylene base color masterbatch, phosphorescent powder masterbatch, nucleating agent masterbatch, lubricant masterbatch and antioxidant masterbatch, and then melting and extruding and pelletizing to obtain long afterglow polypropylene microparticles.
[0013] S6 disperses long-afterglow polypropylene microparticles in an aqueous dispersion system containing water, inorganic dispersant, and organic dispersant.
[0014] S7. Carbon dioxide physical foaming agent is introduced into the reactor to allow carbon dioxide to penetrate into the long-afterglow polypropylene microparticles. After maintaining the set temperature and pressure, the material is depressurized and discharged into the atmospheric pressure foaming pipe to foam the long-afterglow polypropylene microparticles, thus obtaining long-afterglow foamed polypropylene beads.
[0015] By weight, the luminescent powder masterbatch comprises 40 parts random copolymer polypropylene carrier, 50 parts rare earth aluminate long afterglow powder, and 10 parts maleic anhydride grafted modified polypropylene wax. The mass ratio of rare earth aluminate long afterglow powder to maleic anhydride grafted modified polypropylene wax is 5:1.
[0016] In one embodiment, the rare earth aluminate long afterglow powder is an untreated powder with a particle size of 8-13 μm and a specification of 1500 mesh; the maleic anhydride grafted modified polypropylene wax has a grafting rate of 7% and a number average molecular weight of 8000.
[0017] By weight, the nucleating agent masterbatch may include 10 parts of cell nucleating agent and 90 parts of random copolymer polypropylene carrier. The cell nucleating agent may be selected from at least one of polytetrafluoroethylene powder, zinc borate, talc, barium sulfate, calcium carbonate, calcium stearate, and silica, and the average particle size may be 3 to 10 μm.
[0018] By weight, the lubricant masterbatch may comprise 10 parts lubricant and 90 parts random copolymer polypropylene carrier. The lubricant may be selected from at least one of erucamide and glyceryl monostearate.
[0019] Based on parts by weight, the antioxidant masterbatch may include 10 parts antioxidant 1010, 10 parts antioxidant 168 and 80 parts random copolymer polypropylene carrier.
[0020] Polypropylene base color masterbatch is an optional component, which is a homogeneous mixture of polypropylene carrier and colorant, and can be selected according to the color requirements of the molded parts; the example uses fluorescent green polypropylene base color masterbatch.
[0021] Based on a total of 100 parts by weight of all components, the long-afterglow polypropylene microparticles may include, optionally, 1-10 parts of polypropylene base color masterbatch, 10-20 parts of phosphorescent powder masterbatch, 1-3 parts of nucleating agent masterbatch, 1-5 parts of lubricant masterbatch, 1-5 parts of antioxidant masterbatch, and the balance being random copolymer polypropylene. Examples 1-3 show that when the phosphorescent powder masterbatch is 10-15 parts, the resulting molded parts also possess long-afterglow properties, and the proportion of beads with destroyed pores in the fracture surface is not less than 94%.
[0022] The melt flow rate of random copolymer polypropylene at 230℃ and 2.16 kg load can be 6 to 9 g / 10 min, and the melting point can be 130 to 150℃, and further 138 to 148℃.
[0023] In step S6, by weight, water can be 1000-2000 parts, kaolin can be 0.3-20 parts, and organic dispersant can be 0.3-16 parts. The organic dispersant is an aqueous solution of sodium dodecylbenzenesulfonate with an effective ingredient content of 30%. In step S7, long-afterglow polypropylene microparticles can be 100-1000 parts.
[0024] In step S7, the temperature inside the reactor can be 140–155℃, the pressure inside the reactor can be 1.6–4.0 MPa gauge pressure, and the holding time can be 5–30 min. The material is depressurized to a foaming pipe at atmospheric pressure and an atmosphere temperature of 80–101℃, and remains in the foaming pipe for 4–15 s. Carbon dioxide is used as a physical foaming agent under the above conditions.
[0025] The resulting long afterglow foamed polypropylene beads can be characterized by the first DSC temperature rise curve to aid in the characterization of their foaming thermal history. During the test, the high-temperature melting peak and its endothermic enthalpy, which are higher than the inherent melting point of random copolymer polypropylene, are recorded.
[0026] The present invention also provides long-afterglow foamed polypropylene beads, the beads comprising a random copolymer polypropylene matrix having a closed-cell structure, and rare earth aluminate long-afterglow powder and maleic anhydride grafted modified polypropylene wax dispersed in the matrix.
[0027] The present invention also provides a long-afterglow foamed polypropylene molded part, which is obtained by air pre-compression and steam molding of the long-afterglow foamed polypropylene beads.
[0028] Compared with Comparative Example 1, which did not add maleic anhydride-grafted modified polypropylene wax to the phosphorescent powder masterbatch, and Comparative Example 2, which directly added long afterglow powder and maleic anhydride-grafted modified polypropylene wax, Example 1, after using a phosphorescent powder masterbatch of 40:50:10, showed a narrower observation and statistical range for cell size and an increased proportion of beads with destroyed cells in the fracture surface of the molded part.
[0029] Rare earth aluminate long afterglow powder is dispersed in the polypropylene matrix of beads and molded parts, so that the molded parts can obtain long afterglow luminescence performance without the need for a separate surface luminescent coating. Attached Figure Description
[0030] Figure 1 SEM comparison images of the cross sections of long afterglow foamed polypropylene beads obtained in Example 1, Comparative Example 1, and Comparative Example 2. Figure 1 In the figures, (a), (b), and (c) are Example 1, Comparative Example 1, and Comparative Example 2, respectively. Detailed Implementation
[0031] The technical solution of the present invention is further illustrated below through examples. Unless otherwise specified, all raw materials are commercially available industrial-grade raw materials.
[0032] Long afterglow performance test: The molded part was made into a circular disc with a diameter of 50 mm and a thickness of 5 mm, and placed in a black sample dish with an inner diameter of 50 mm and a depth of 5 mm. The test was conducted in a dark room with a background illuminance of no more than 0.01 lx. A D65 standard light source with a color temperature of 6500 K was used, and the sample was excited at 1000 lx for 10 min. The afterglow brightness was read 1 s after the excitation stopped, and the afterglow brightness decayed to 0.32 mcd / m². 2 The testing instrument was an SSP9511 afterglow meter, and the testing method was in accordance with GB / T 24981.2-2020 "Test Methods for Rare Earth Long Afterglow Phosphors - Part 2: Determination of Afterglow Brightness".
[0033] Cell morphology testing: Cross-sections were prepared by cutting the beads and observed using a Hitachi S-4800 scanning electron microscope at an accelerating voltage of 3.0 kV. Five fields of view were randomly selected from each group, and at least 100 complete cells were measured using ImageJ 1.52a; incomplete cells at the boundaries were not counted. The equivalent diameter D of the cell was determined. eq according to Calculate, where A is the projected area of the bubble. Record the minimum and maximum equivalent diameters of all measured complete bubbles as the observation and statistical range.
[0034] DSC testing: Using a DSC 3500 Sirius differential scanning calorimeter, approximately 1.1 mg of sample was weighed and heated from 60 °C to 180 °C at a heating rate of 10 °C / min under a nitrogen atmosphere with a flow rate of 50 mL / min. The endothermic enthalpy was obtained by integrating the high-temperature melting peak above the intrinsic melting point of random copolymer polypropylene under a unified integral baseline.
[0035] Molding weld bond evaluation: Break the molded part and count at least 200 foam beads on the fracture surface. Beads that separate only along the surface and whose internal cells are not torn are considered undamaged beads; beads whose surface or internal cells are torn are considered damaged beads. The percentage of damaged beads is calculated as n / N × 100%, where n is the number of damaged beads and N is the total number of beads counted.
[0036] Example 1
[0037] The random copolymer polypropylene A has a melt flow rate of 7 g / 10 min at 230℃ and a load of 2.16 kg, and a melting point of 142℃. The rare earth aluminate long afterglow powder is based on SrAl₂O₄ and contains Eu. 2+ and Dy 3+ The powder is an untreated powder with activated ions, a particle size of 8–13 μm, and a mesh size of 1500. The maleic anhydride-grafted modified polypropylene wax has a grafting rate of 7% and a number-average molecular weight of 8000. The cell nucleating agent is silica with an average particle size of 5 μm; the lubricant is erucamide; the antioxidants are antioxidant 1010 and antioxidant 168; and the masterbatch is a fluorescent green PP-based masterbatch. The aqueous dispersion system uses deionized water, a 30% sodium dodecylbenzenesulfonate aqueous solution, and kaolin.
[0038] Preparation of luminescent powder masterbatch: By weight, 40 parts of random copolymer polypropylene A, 50 parts of rare earth aluminate long afterglow powder and 10 parts of maleic anhydride grafted modified polypropylene wax were premixed for 5 min, fed into a twin-screw extruder, and extruded at 170-190℃ and screw speed of 300 r / min. After water cooling and pelletizing, luminescent powder masterbatch was obtained.
[0039] Preparation of nucleating agent masterbatch: 90 parts of random copolymer polypropylene A and 10 parts of silica were premixed at high speed for 5 min, and then extruded by twin screw extrusion at 170-190℃ and screw speed of 300 r / min, followed by water cooling and pelletizing to obtain nucleating agent masterbatch.
[0040] Lubricant masterbatch preparation: 90 parts of random copolymer polypropylene A and 10 parts of erucamide were premixed at high speed for 5 min, and then extruded by twin screw extrusion at 170-190℃ and screw speed of 300 r / min, followed by water cooling and pelletizing to obtain lubricant masterbatch.
[0041] Preparation of antioxidant masterbatch: 80 parts of random copolymer polypropylene A, 10 parts of antioxidant 1010 and 10 parts of antioxidant 168 were premixed at high speed for 5 min, and then extruded in a twin-screw extruder at 170-190℃ and 300 r / min. The mixture was then water-cooled and pelletized to obtain antioxidant masterbatch.
[0042] Preparation of long-afterglow polypropylene microparticles: 72 parts of random copolymer polypropylene A, 5 parts of fluorescent green PP base color masterbatch, 15 parts of phosphorescent powder masterbatch, 2 parts of nucleating agent masterbatch, 3 parts of lubricant masterbatch and 3 parts of antioxidant masterbatch were mixed in a high-speed mixer for 5 min, and then extruded by twin screw at 180-200℃ and screw speed of 350 r / min, and water-cooled and pelletized to obtain long-afterglow polypropylene microparticles with a single particle weight of 1.1 mg and an average length of 1.5 mm.
[0043] Preparation of aqueous dispersion system in reactor: Add 1500 parts of deionized water, 8 parts of the organic dispersion aid and 10 parts of kaolin to the high-pressure reactor and stir at 60 r / min for 10 min until uniform.
[0044] Kettle foaming: 500 parts of long-afterglow polypropylene microparticles were added to a high-pressure reactor. After sealing, carbon dioxide was introduced, and the temperature was raised to 145℃ after 60 min with stirring at 60 r / min. The pressure inside the reactor was adjusted to 2.4 MPa gauge pressure and maintained at 145℃ and 2.4 MPa gauge pressure for 10 min. The pressure relief valve was opened, and the material was discharged into the atmospheric pressure foaming pipeline. The temperature inside the foaming pipeline was 101℃, and the material residence time was approximately 8 s. Long-afterglow foamed polypropylene beads with a bulk density of 45 g / L were collected.
[0045] Tests showed that the equivalent diameter of the bubbles in the obtained beads ranged from 50 to 100 μm.
[0046] Molding: The beads were pre-pressed under an air pressure of 0.2 MPa gauge pressure for 10 hours and then placed into a metal mold with an inner cavity size of 460 mm long, 350 mm wide, and 50 mm thick. Saturated steam was introduced into the mold to bring the steam pressure in the mold cavity to 0.24 MPa gauge pressure and maintained until the beads melted. The steam supply was then stopped, and the molded part was cooled until it could be demolded, resulting in a fluorescent green and glossy long-afterglow foamed polypropylene molded part. The afterglow brightness 1 s after excitation was stopped was 510 mcd / m². 2 The afterglow brightness decreased to 0.32 mcd / m 2 The time was 7 hours; 258 beads were counted from the fracture surface, of which 245 were beads with damaged cells, accounting for 95.0%.
[0047] Example 2
[0048] Example 2 uses the same random copolymer polypropylene A, rare earth aluminate long afterglow powder, maleic anhydride grafted modified polypropylene wax, silica, erucamide, antioxidant, color masterbatch, and aqueous dispersion system as Example 1. The preparation methods of the phosphorescent powder masterbatch, nucleating agent masterbatch, lubricant masterbatch, and antioxidant masterbatch are the same as in Example 1.
[0049] The long-afterglow polypropylene microparticles were made from 67 parts of random copolymer polypropylene A, 5 parts of fluorescent green PP base color masterbatch, 20 parts of phosphorescent powder masterbatch, 2 parts of nucleating agent masterbatch, 3 parts of lubricant masterbatch and 3 parts of antioxidant masterbatch. The mixing, extrusion and pelletizing conditions were the same as in Example 1. The resulting microparticles had a single particle weight of 1.1 mg and an average length of 1.5 mm.
[0050] The aqueous dispersion system, autoclave foaming, and molding processes were the same as in Example 1, yielding beads with a bulk density of 45 g / L. The observed statistical range of the equivalent diameter of the bead pores was 60–120 μm. The afterglow brightness of the molded part 1 s after excitation was stopped was 740 mcd / m². 2 The afterglow brightness decreased to 0.32 mcd / m 2 The time was 9 hours; 235 beads were analyzed from the fracture surface, of which 188 were beads with damaged cells, accounting for 80.0%.
[0051] Example 3
[0052] Example 3 uses the same raw materials, preparation methods for each functional masterbatch, aqueous dispersion system, autoclave foaming and molding conditions as Example 1.
[0053] The long-afterglow polypropylene microparticles are made from 77 parts of random copolymer polypropylene A, 5 parts of fluorescent green PP base color masterbatch, 10 parts of phosphorescent powder masterbatch, 2 parts of nucleating agent masterbatch, 3 parts of lubricant masterbatch and 3 parts of antioxidant masterbatch. The resulting microparticles have a single particle weight of 1.1 mg and an average length of 1.5 mm.
[0054] The bulk density of the obtained beads was 45 g / L, and the observed statistical range of the equivalent diameter of the bubbles was 40–80 μm. The afterglow brightness of the molded part 1 s after excitation was stopped was 300 mcd / m². 2 The afterglow brightness decreased to 0.32 mcd / m 2 The time was 6 hours; 247 beads were counted from the fracture surface, of which 244 were beads with damaged cells, accounting for 98.8%.
[0055] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that maleic anhydride-grafted modified polypropylene wax is not added to the luminescent powder masterbatch. Specifically, 50 parts of random copolymer polypropylene A and 50 parts of rare earth aluminate long afterglow powder are premixed for 5 min, and then extruded by twin screw extrusion at 170-190°C and a screw speed of 300 r / min, followed by water cooling and pelletizing to obtain the luminescent powder masterbatch.
[0056] The remaining steps were the same as in Example 1, resulting in beads with a bulk density of 45 g / L. The observed statistical range of the equivalent diameter of the bead pores was 30–200 μm. The afterglow brightness of the molded part 1 s after excitation was stopped was 500 mcd / m². 2 The afterglow brightness decreased to 0.32 mcd / m 2 The time was 7 hours; 251 beads were counted from the fracture surface, of which 175 were beads with damaged cells, accounting for 69.7%.
[0057] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that, instead of preparing the phosphorescent powder masterbatch separately, rare earth aluminate long-afterglow powder and maleic anhydride grafted modified polypropylene wax were directly added during the preparation of long-afterglow polypropylene microparticles. The preparation methods of the nucleating agent masterbatch, lubricant masterbatch, and antioxidant masterbatch were the same as in Example 1.
[0058] 78 parts of random copolymer polypropylene A, 5 parts of fluorescent green PP base color masterbatch, 7.5 parts of rare earth aluminate long afterglow powder, 2 parts of nucleating agent masterbatch, 3 parts of lubricant masterbatch, 3 parts of antioxidant masterbatch and 1.5 parts of maleic anhydride grafted modified polypropylene wax were mixed for 5 min. The mixture was then extruded by twin screw extrusion at 180-200℃ and screw speed of 350 r / min, and water-cooled and pelletized to obtain long afterglow polypropylene microparticles with a single particle weight of 1.1 mg and an average length of 1.5 mm.
[0059] The remaining steps were the same as in Example 1, yielding beads with a bulk density of 45 g / L. The observed statistical range of the equivalent diameter of the bead pores was 80–500 μm, and larger pores and broken pores were observed. The afterglow brightness of the molded part 1 s after excitation was stopped was 490 mcd / m². 2 The afterglow brightness decreased to 0.32 mcd / m 2 The time was 7 hours; 220 beads were counted from the fracture surface, of which 109 were beads with damaged cells, accounting for 49.5%.
[0060] Performance Comparison The performance of Examples 1-3 and Comparative Examples 1-2 is shown in Table 1.
[0061] Table 1 Performance comparison of Examples 1-3 and Comparative Examples 1-2
[0062] The afterglow brightness and afterglow time of Example 1 and Comparative Example 1 are similar, but the observation statistical range of the equivalent diameter of the bubbles in Example 1 is narrower, and the proportion of beads with destroyed bubbles in the fracture surface increases from 69.7% to 95.0%. Compared with Comparative Example 2, with the same amount of rare earth aluminate long afterglow powder and maleic anhydride grafted modified polypropylene wax, the pre-prepared phosphorescent powder masterbatch reduces the upper limit of the observation statistical range of the equivalent diameter of the bubbles from 500 μm to 100 μm, and increases the proportion of beads with destroyed bubbles in the fracture surface from 49.5% to 95.0%.
[0063] Examples 1-3 show that when the amount of phosphorescent powder masterbatch added is increased from 10 parts to 20 parts, the afterglow brightness and afterglow time are improved, but the proportion of beads with destroyed cells on the fracture surface decreases to 80.0% at an addition amount of 20 parts. Under the existing experimental conditions, an addition amount of 10-15 parts balances long afterglow performance and molding fusion.
[0064] Figure 1 (a) Figure 1 (b) and Figure 1 (c) Representative SEM views of the bead cross sections obtained in Example 1, Comparative Example 1 and Comparative Example 2 are shown respectively. Figure 1 (c) Larger bubbles and broken bubbles can be observed; the precise observation and statistical range of the equivalent diameter of bubbles in each group shall be based on the measurement results of 5 fields of view and no less than 100 complete bubbles in each group as listed in Table 1.
[0065] Examples 1 and Comparative Examples 1 and 2 show that pre-preparing a phosphorescent powder masterbatch by mixing a random copolymer polypropylene carrier, rare earth aluminate long afterglow powder, and maleic anhydride graft-modified polypropylene wax in a weight ratio of 40:50:10, and then using 10-15 parts of the phosphorescent powder masterbatch to prepare EPP microparticles, can improve the uniformity of bead pore size and the bead fusion performance of the molded parts while maintaining the long afterglow performance.
[0066] The above embodiments are used to illustrate the technical solution of the present invention, and the specific scope of protection is subject to the claims.
Claims
1. A method for preparing long-afterglow foamed polypropylene beads, characterized in that, Includes the following steps: (1) According to the weight, 40 parts of random copolymer polypropylene carrier, 50 parts of untreated rare earth aluminate long afterglow powder and 10 parts of maleic anhydride grafted modified polypropylene wax are melt-blended and granulated to obtain luminous powder masterbatch. (2) Based on a total of 100 parts by weight of each component, 1 to 10 parts of the selected polypropylene base color masterbatch, 10 to 15 parts of the phosphorescent powder masterbatch, 1 to 3 parts of the nucleating agent masterbatch, 1 to 5 parts of the lubricant masterbatch, 1 to 5 parts of the antioxidant masterbatch and the remainder of random copolymer polypropylene are melt-blended, extruded and pelletized to obtain long afterglow polypropylene microparticles. (3) Disperse the long-afterglow polypropylene microparticles in an aqueous dispersion system, introduce carbon dioxide physical foaming agent, and keep it at 140-155℃ and 1.6-4.0 MPa gauge pressure for 5-30 min. Then depressurize the material to atmospheric pressure and a foaming pipe with an atmosphere temperature of 80-101℃ and keep it for 4-15 s to obtain long-afterglow foamed polypropylene beads.
2. The preparation method according to claim 1, characterized in that, The particle size of the rare earth aluminate long afterglow powder is 8-13 μm; the grafting rate of the maleic anhydride grafted modified polypropylene wax is 7%, and the number average molecular weight is 8000.
3. The preparation method according to claim 1, characterized in that, In step (1), the random copolymer polypropylene carrier, the rare earth aluminate long afterglow powder and the maleic anhydride grafted modified polypropylene wax are premixed for 5 min and then extruded and granulated at 170-190℃ and screw speed of 300 r / min using a twin-screw extrusion.
4. The preparation method according to claim 1, characterized in that, The nucleating agent masterbatch consists of 10 parts silica and 90 parts random copolymer polypropylene carrier; the lubricant masterbatch consists of 10 parts erucamide and 90 parts random copolymer polypropylene carrier; the antioxidant masterbatch consists of 10 parts antioxidant 1010, 10 parts antioxidant 168 and 80 parts random copolymer polypropylene carrier.
5. The preparation method according to claim 1, characterized in that, The random copolymer polypropylene has a melt flow rate of 6–9 g / 10 min at 230°C and 2.16 kg load, and a melting point of 130–150°C.
6. The preparation method according to claim 1, characterized in that, The aqueous dispersion system comprises, by weight, 1000-2000 parts water, 0.3-20 parts kaolin and 0.3-16 parts organic dispersing agent; the organic dispersing agent is an aqueous solution of sodium dodecylbenzenesulfonate with an active ingredient content of 30%.
7. A long-afterglow foamed polypropylene bead, characterized in that, The long-afterglow foamed polypropylene beads are prepared by the preparation method described in claim 2. The beads have a closed-cell structure. Rare earth aluminate long-afterglow powder and maleic anhydride grafted modified polypropylene wax are dispersed in a random copolymer polypropylene matrix, and the mass ratio of the two is 5:
1. The statistical aperture of no less than 100 complete cells is measured by randomly selecting 5 fields of view in each group. The observation and statistical range of the equivalent diameter of the cells is 40 to 100 μm.
8. The long afterglow foamed polypropylene beads according to claim 7, characterized in that, The bulk density of the long afterglow foamed polypropylene beads is 45 g / L.
9. A long-afterglow foamed polypropylene molded part, characterized in that, The long-afterglow foamed polypropylene beads as described in claim 7 are obtained by air pre-compression and steam molding; the afterglow brightness read at 1000 lx illuminance for 10 min and 1 s after excitation stops is not less than 300 mcd / m². 2 The afterglow brightness decreased to 0.32 mcd / m 2 The time is not less than 6 hours; when counting at least 200 foam beads in the cross-section of the molded part, the proportion of beads with destroyed cells is not less than 94%.
10. The long afterglow foamed polypropylene molded part according to claim 9, characterized in that, After the long-afterglow foamed polypropylene beads are pre-pressed in air at a gauge pressure of 0.2 MPa for 10 hours, saturated steam is introduced to bring the steam pressure in the mold cavity to a gauge pressure of 0.24 MPa and maintain it until the beads melt and solidify. After cooling and shaping, the long-afterglow foamed polypropylene molded part is obtained.
Citation Information
Patent Citations
A PP phosphorescent masterbatch and its preparation method
CN109486020B
Antibacterial foamed polypropylene bead and preparation method thereof
CN115895117A
Luminescent polyolefin foam and its preparation
JP2000336201A