Rubber composition

By adding specific lubricants and crosslinking agents to the EBENB rubber composition, the adhesion problem of uncured rubber blanks is solved, productivity is improved and low-temperature sealing performance is maintained, making it suitable for low-temperature high-pressure gas sealing components.

CN123062818APending Publication Date: 2026-11-10NOK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611458154.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-03-28
Filing Date
2019-03-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing ethylene-propylene-diene copolymer rubber (EPDM) exhibits conflicting sealing properties at high and low temperatures, and the adhesion of uncured rubber blanks leads to low productivity.

Method used

Add 0.1 to 2.5 parts by weight of a lubricant with a flow temperature of 50°C to 100°C to an appropriate amount of crosslinking agent and other additives to an ethylene-butene-5-ethylidene-2-norbornene terpolymer (EBENB) rubber composition.

Benefits of technology

It improves the adhesion problem of uncured rubber blanks, increases productivity, and maintains good sealing performance in low-temperature environments, making it particularly suitable for low-temperature high-pressure gas sealing components below -39℃.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a rubber composition in which 1.0 to 2.0 parts by weight of a fatty acid amide-based lubricant having a flow temperature of 60 to 95°C is compounded per 100 parts by weight of an ethylene-butene-5-ethylidene-2-norbornene terpolymer. The flow temperature of the lubricant refers to the lowest temperature at which the lubricant can maintain a flow state. The rubber composition, by compounding the specified lubricant, achieves the following effects: preventing the adhesion of uncured rubber blanks to each other, improving the productivity in the rubber blank preparation process and the vulcanization molding process of crosslinked molded products such as sealing members, and not compromising the low-temperature properties of the crosslinked molded products. The rubber composition can be effectively used as a crosslinked molded material for sealing members that require high-pressure gas sealing functionality in low-temperature environments of -39°C or lower.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Case Analysis This application is a divisional application of patent application No. 201980017202.8 (PCT International Patent Application PCT / JP2019 / 010521), filed on March 14, 2019, entitled "Rubber Composition". Technical Field

[0002] This invention relates to a rubber composition. More specifically, it relates to an ethylene-butene-5-ethylidene-2-norbornene terpolymer rubber composition. Background Technology

[0003] For ethylene-propylene-diene copolymer rubber (EPDM) that exhibits sealing properties at both high and low temperatures, the lack of unsaturated bonds in the main chain leads to a conflicting relationship between rubber strength and low-temperature performance and the increase in ethylene content. Therefore, EPDM compositions struggle to achieve sealing properties at temperatures exceeding certain limits.

[0004] In order to obtain rubber molded articles that can maintain the same level of hardness as existing EPDM rubber molded articles, especially with excellent low-temperature rubber properties, the applicant previously proposed a rubber composition comprising an ethylene-butene-ethylidene norbornene terpolymer [EBENB], carbon black, a hardness modifier and a crosslinking agent (Patent Document 1).

[0005] This rubber composition can produce rubber molded products with the same level of hardness as rubber molded products using existing EPDM, especially with excellent low-temperature rubber properties. However, the polymer copolymer of EBENB has very high adhesion, especially the adhesion between uncured rubber blanks. Therefore, there is a problem of very poor productivity in the rubber blank preparation process and the vulcanization molding process of cross-linked molded products such as sealing components.

[0006] Existing technical documents Patent documents Patent Document 1: WO 2017 / 170190 A1 Summary of the Invention The technical problem that the invention aims to solve The object of the present invention is to provide an EBENB rubber composition that improves productivity in the vulcanization process of cross-linked molded articles, such as rubber blank preparation and sealing components, due to the adhesion between unvulcanized rubber blanks, without compromising the low-temperature properties of the cross-linked molded articles.

[0007] Means for solving technical problems The above-mentioned object of the present invention is achieved by the following rubber composition, wherein every 100 parts by weight of the ethylene-butene-5-ethylidene-2-norbornene terpolymer contains 0.1 to 2.5 parts by weight of a lubricant with a flow temperature of 50°C to 100°C.

[0008] Invention Effects The rubber composition of the present invention, when combined with a specific lubricant, can achieve the following effects: prevent difficulties caused by the adhesion of uncured rubber blanks to each other, improve productivity in the rubber blank preparation process and the vulcanization molding process of cross-linked molded products such as sealing components, and without impairing the low-temperature properties of the cross-linked molded product.

[0009] This rubber composition can be effectively used as a cross-linked molding material for sealing components that require high-pressure gas sealing in low-temperature environments below -39°C. Detailed Implementation

[0010] In rubber compositions, the properties of rubber materials such as EBENB and EPDM have a significant impact on the overall material cost and production efficiency of the rubber composition. Because EBENB has better cold resistance than EPDM, a rubber composition with the desired low-temperature rubber properties can be achieved by using less EPDM, thus reducing the overall material cost of the rubber composition.

[0011] In addition, because EBENB is more flexible than EPDM, it has excellent processability such as mixing, dispersibility, and molding properties, which greatly improves production efficiency and reduces production costs.

[0012] The rubber composition of the present invention, which uses EBENB in ​​this way, can reduce the production cost of rubber molded articles from the viewpoint of material cost and production efficiency compared with existing rubber compositions using EPDM.

[0013] As an EBENB, any EBENB can be used that copolymerizes ethylene and butene with a small amount (about 0.1% to 20% by weight, preferably about 3% to 15% by weight) of 5-ethylidene-2-norbornene. In fact, commercially available products such as Mitsui Chemicals' Metallocene EBT can be used directly.

[0014] The iodine value of EBENB is preferably about 3g / 100g to 20g / 100g, more preferably about 5g / 100g to 18g / 100g. Within this range, its excellent heat aging resistance and weather resistance prevent aging of rubber molded products, and it can maintain a stable molecular state even at low temperatures, thereby improving low-temperature sealing performance.

[0015] Mooney viscosity ML of EBENB 1+4 (100°C) Preferably, the Mooney viscosity is about 10 to 45, more preferably about 15 to 35. If the Mooney viscosity is too low, the compression set may increase and the tensile strength may decrease. On the other hand, if the Mooney viscosity is too high, although the physical properties are improved, the processability may be poor. It should be noted that the Mooney viscosity ML 1+4 (100℃) can be calculated according to the provisions of JISK6300-1:2013.

[0016] Furthermore, the ethylene content in EBENB is preferably about 60% to 80% by weight, more preferably about 65% to 75% by weight. Within this range, EBENB exhibits a minimum glass transition temperature (Tg), thus improving its cold resistance.

[0017] In EBENB, every 100 parts by weight of EBENB contains 0.1 to 2.5 parts by weight, preferably 0.5 to 2.2 parts by weight, of a lubricant with a flow temperature (according to JIS K5601-2-2 corresponding to ISO 4625) of about 50°C to 100°C, preferably about 60°C to 95°C. Here, the flow temperature of the lubricant refers to the lowest temperature at which it can maintain a flow state.

[0018] When the flow temperature is below the above range, adhesion between uncured rubber blanks may sometimes occur. On the other hand, when the flow temperature is above the above range, adhesion with the mixer during mixing cannot be prevented.

[0019] In addition, when the mixing ratio is less than the above range, it cannot prevent the uncured rubber blanks from adhering to each other. On the other hand, when the mixing ratio is more than the above range, it will impair the low-temperature sealing performance.

[0020] As a lubricant with a flow temperature of about 50°C to 100°C, preferably about 60°C to 95°C, fatty acid metal salt-based lubricants, fatty acid amide-based lubricants, fatty acid ester-based lubricants, or organosilicon-based lubricants can be used.

[0021] As a lubricant for fatty acid metal salt systems, zinc salts of high-grade saturated or unsaturated fatty acids with more than 12 carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid, can be used.

[0022] As a fatty acid amide-based lubricant, monoamides, substituted monoamides, diamides, hydroxymethylamides, etc. of the above-mentioned higher fatty acids can be used.

[0023] As a fatty acid ester lubricant, lower alkyl esters with fewer than 5 carbon atoms, such as methyl ester, ethyl ester, and butyl ester of the aforementioned higher fatty acids, can be used.

[0024] In addition, as an organosilicon-based lubricant, compounds with siloxane bonds on the main chain, mixtures thereof with inorganic carriers, etc., can be used.

[0025] As a crosslinking agent, organic peroxides are preferred. Examples of organic peroxides include: tert-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, 2,5-dimethyl-2,5-di-tert-butylperoxy-3-hexyne, tert-butylcumyl peroxide, 1,3-di-tert-butylperoxyisopropylbenzene, 2,5-dimethyl-2,5-di(benzoyl peroxide)hexane, tert-butylperoxybenzoate, tert-butylperoxyisopropyl carbonate, n-butyl-4,4-di-tert-butylperoxyvalerate, etc.

[0026] The amount of crosslinking agent incorporated relative to 100 parts by weight of EBENB is preferably about 0.5 parts by weight to 10 parts by weight, more preferably about 1 part by weight to 5 parts by weight. By being within the above range, foaming during vulcanization that prevents molding can be prevented, and since the crosslinking density becomes good, it becomes easy to obtain a rubber composition with sufficient physical properties.

[0027] Alternatively, masterbatches containing the organic peroxides described above can be used, such as the Japanese Zeon product DCP30ZP03K (30% by weight of dicumyl peroxide, 30% by weight of Zetpol 2010L, and 40% by weight of SRF carbon black). These masterbatches are preferred in terms of improving the mixing and dispersibility when preparing rubber compositions.

[0028] Furthermore, crosslinking accelerators can be included as needed. Common crosslinking accelerators include triallyl isocyanurate, triallyl cyanate, liquid polybutadiene, N,N'-m-phenylenebismaleimide, and trimethylolpropane trimethacrylate. By adding appropriate amounts of crosslinking accelerators, crosslinking efficiency can be improved, thereby enhancing heat resistance and mechanical properties, and ultimately improving the stability of the sealing component.

[0029] In addition to the components mentioned above, fillers, acid acceptors, antioxidants, and other commonly used compounding agents in the rubber industry may be added and used as appropriate as needed in the rubber composition. The amount of the compounding agent relative to 100 parts by weight of EBENB is preferably about 300 parts by weight or less.

[0030] Examples of fillers include: inorganic fillers such as carbon black, silica, silicates, calcium carbonate, magnesium carbonate, clay, talc, bentonite, sericite, mica, hydrated alumina, and barium sulfate; and resin fillers such as polyethylene, polypropylene, polystyrene, coumarone-indene resin, melamine resin, and phenolic resin.

[0031] When using carbon black, the oil absorption of DBP is preferably 100 ml / 100 g or more. In addition, when using silica, it is preferable to use a silane coupling agent at the same time.

[0032] Rubber compositions can be prepared by mixing various materials using mixers such as single-screw extruders, twin-screw extruders, rollers, Banbury mixers, kneaders, and high-shear mixers.

[0033] Alternatively, the rubber composition can be cross-linked by using an injection molding machine, compression molding machine, or similar equipment, typically under pressure vulcanization at approximately 150°C to 230°C for about 0.5 to 30 minutes. Furthermore, after the primary vulcanization described above, a secondary vulcanization can be performed as needed to ensure vulcanization reaches the interior of the vulcanizate. This secondary vulcanization can typically be performed by heating in an oven at approximately 150°C to 250°C for about 0.5 to 24 hours.

[0034] Rubber molded articles obtained by vulcanizing the rubber composition of the present invention have excellent low-temperature rubber properties, particularly at -50°C, and can be used in low-temperature environments (e.g., about -40°C to -60°C), making them suitable for use as rubber molded articles. For such rubber molded articles, the TR70 value, determined by the low-temperature elastic recovery test specified in JIS K6261:2006 corresponding to ISO 2921, is preferably below -39°C.

[0035] Furthermore, the rubber molded article of the present invention preferably has a moderate hardness. For example, if the rubber molded article is an O-ring, the type A hardness (durometer hardness) specified in JIS K6253-1:2012 is preferably 65 to 95.

[0036] Examples of such rubber molded products include: sealing components, insulators, vibration dampers, and sound insulators used for sealing cryogenic and high-pressure gases. Among these, sealing components suitable for use in cryogenic environments and exhibiting excellent cryogenic sealing performance are particularly suitable for sealing equipment containing high-pressure gases (e.g., high-pressure hydrogen).

[0037] The shape of the rubber molded article of the present invention is not particularly limited, and it can be made into various shapes depending on the application. For example, the shapes that can be used as sealing members include O-rings, gaskets, sheets, etc.

[0038] Example The present invention will now be described with reference to embodiments.

[0039] Example 1 EBENB (Mitsui Chemicals Metallocene EBT) 100 parts by weight HAF CB (Asahi Carbon product Asahi 70#, 70〃) DBP oil absorption capacity: 101ml / 100g Zinc oxide 5" Stearic acid 1 〃 Fatty acid amide lubricant (Nippon Chemicals' Diamide O-200, 2") Refined oleamide (flow temperature 73℃) Plasticizer (Idemitsu Kosan product Diana Process Oil PW380) 5 〃 Antioxidant (BASF Japan product Irganox 1010) 1 〃 Organic peroxides (Japanese oil and fat products: Percumyl D, dicumyl peroxide) 3 〃 Vulcanization accelerator (Taic, Nippon Chemical Products) 0.5 μm In the above-mentioned components with a target JIS A hardness of 75 for the crosslinked compound, the components other than the organic peroxide and the vulcanization accelerator are kneaded in a kneader, and then the organic peroxide and the vulcanization accelerator are added and kneaded in an open roller.

[0040] For the obtained open roll compound, the adhesion force on the surface of the uncured rubber blank was measured using a viscosity tester (Toyo Seiki HTC-1). The adhesion force of 0 to less than 8 N was rated as ○, and the adhesion force of 8 to 20 N was rated as ×.

[0041] In addition, for crosslinked products obtained by a single crosslinking at 180°C for 8 minutes and a second crosslinking at 180°C for 24 hours, the TR10 and TR70 values ​​were measured according to JIS K6261 when the deformation in the low-temperature region recovered 10% and 70% respectively.

[0042] Example 2 In Example 1, the amount of fatty acid amide lubricant was changed to 1 part by weight.

[0043] Example 3 In Example 1, instead of fatty acid amide lubricant, the same amount (2 parts by weight) of fatty acid ester lubricant (Schill + Seilacher “Struktol” AG product Struktol WB222, flow temperature 65°C) was used.

[0044] Example 4 In Example 1, instead of fatty acid amide lubricant, the same amount (2 parts by weight) of silicone lubricant (Schill + Seilacher “Struktol” AG product Struktol WS180, flow temperature 90°C) was used.

[0045] Comparative Example 1 In Example 1, fatty acid amide lubricant was not used.

[0046] Comparative Example 2 In Example 1, the amount of fatty acid amide lubricant was changed to 3 parts by weight.

[0047] Comparative Example 3 In Example 1, instead of a fatty acid amide lubricant, the same amount (2 parts by weight) of a fatty acid derivative with a flow temperature of 102°C (Struktol WB 16, a product of Schill + Seilacher “Struktol” AG) was used.

[0048] Comparative Example 4 In Example 1, instead of fatty acid amide lubricant, the same amount (2 parts by weight) of a fatty acid derivative with a flow temperature of 105°C (Schill+Seilacher “Struktol” AG product Struktol HT204) was used.

[0049] The results obtained through the above embodiments and comparative examples are shown in the table below.

[0050] surface Example: Adhesion between uncured rubber blanks TR10 (°C) TR70 (°C) Example 1 ○ -57 -40 Example 2 ○ -57 -41 Example 3 ○ -57 -39 Example 4 ○ -57 -40 Comparative Example 1 × -57 -42 Comparative Example 2 ○ -57 -37 Comparative Example 3 × -57 -40 Comparative Example 4 × -57 -40 The results above show that in Comparative Example 2, which uses 3 parts by weight of fatty acid amide lubricant, although the adhesion between the uncured rubber blanks was rated as ○, the TR70 value increased by 5°C compared to Comparative Example 1, which did not contain fatty acid amide lubricant, raising concerns about its potential impact on low-temperature sealing.

Claims

1. A rubber composition, characterized in that, The rubber composition contains 1.0 to 2.0 parts by weight of a fatty acid amide lubricant with a flow temperature of 60°C to 95°C per 100 parts by weight of ethylene-butene-5-ethylidene-2-norbornene terpolymer. The flow temperature of a lubricant refers to the lowest temperature at which it can maintain its flow state.

2. The rubber composition according to claim 1, wherein, It also contains 0.5 to 10 parts by weight of organic peroxide.

3. A cross-linked molded article, characterized in that, The cross-linked molded article is obtained by cross-linking the rubber composition according to claim 2.

4. The cross-linked molded article according to claim 3, characterized in that, The TR70 value of the cross-linked molded article, corresponding to JIS K6261 of ISO 2921, is below -39°C.

Citation Information