A high-temperature fire-resistant cable material, its preparation method, and its application.
By modifying ammonium polyphosphate to form hydrogen bonds with polyvinyl chloride, the problem of poor compatibility between ammonium polyphosphate and polyvinyl chloride is solved, thereby improving the mechanical properties and flame retardant effect of the cable material.
Patent Information
- Application Number
- CN202611154622.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-10
AI Technical Summary
The flame retardant and fireproof properties of flexible PVC cable materials are poor, and the compatibility between ammonium polyphosphate and PVC is poor, which affects the mechanical properties.
Modified ammonium polyphosphate flame retardant is prepared by generating P-OH groups and forming electrostatic interactions with amino flame retardants. It then forms hydrogen bonds with polyvinyl chloride and adds plasticizers and other components to prepare high-temperature fireproof cable material.
It significantly improves the compatibility between ammonium polyphosphate and polyvinyl chloride, enhances the tensile strength and elongation at break of the cable material, and improves the limiting oxygen index and flame retardant properties.
Smart Images

Figure SMS_5 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable technology, specifically to a high-temperature resistant fireproof cable material, its preparation method, and its application. Background Technology
[0002] Flexible polyvinyl chloride (PVC) with added plasticizers such as DOP possesses excellent mechanical strength, flexibility, and impact resistance, making it widely used in cable sheathing materials, hoses, and films. However, adding excessive plasticizers to PVC can affect its flame-retardant properties, limiting its practical application in flame-retardant and fire-resistant cables. Flame retardants such as ammonium polyphosphate, aluminum hydroxide, and antimony trioxide are typically added.
[0003] Ammonium polyphosphate is inexpensive and readily available, has good flame retardant properties, is halogen-free and heavy metal-free, and is environmentally friendly, making it widely used in cables, coatings, adhesives, and other fields. However, ammonium polyphosphate has poor compatibility with polyvinyl chloride (PVC), and excessive addition can affect the mechanical properties of PVC. Modification of ammonium polyphosphate, such as silane coupling agent grafting and shell coating, can improve its compatibility with polymers, reduce its hygroscopicity, and improve the mechanical properties of the material. Summary of the Invention
[0004] This invention solves the problem of poor flame retardant and fireproof performance of flexible polyvinyl chloride cable materials.
[0005] The technical solution of the present invention is: a high-temperature fireproof cable material, comprising 100 parts by weight of polyvinyl chloride, 40-50 parts by weight of plasticizer, 3-4 parts by weight of stabilizer, 0.8-1.3 parts by weight of lubricant, and 20-35 parts by weight of modified ammonium polyphosphate flame retardant.
[0006] Preferably, the plasticizer includes di(2-ethylhexyl) phthalate.
[0007] Preferably, the stabilizer includes a calcium-zinc stabilizer.
[0008] Preferably, the lubricant includes polyethylene wax and stearic acid.
[0009] Preferably, the amino flame retardant is prepared by the following method: In an ice bath, dichloromethane, triethylamine in a molar ratio of (1-1.1):1:(1-1.4), Boc-serine methyl ester, and 5,5-dimethyl-2-chloro-1,3,2-dioxophosphoryl caprolactone phosphate are added to a flask. The mixture is then stirred at room temperature for 10-14 h, filtered, and trifluoroacetic acid is added to the filtrate. The mixture is stirred at room temperature for 2-3 h, and sodium bicarbonate solution is added to the solution. The mixture is poured into a separatory funnel and shaken for extraction. After standing and separating the layers, the organic layer is collected, dried with anhydrous sodium sulfate, filtered, and the filtrate is concentrated by rotary evaporation. The product is recrystallized in ethyl acetate to obtain the amino flame retardant. The reaction formula is as follows: .
[0010] Preferably, the modified ammonium polyphosphate flame retardant is prepared by the following method: 100 parts by weight of ammonium polyphosphate are added to a flask, placed in an oil bath, heated to 260-265°C, and stirred. The generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During stirring, a small amount of product is transferred from the flask and added to water. When the pH of the aqueous solution (1% by mass) reaches 3.2-4, it is cooled. Water, ethanol, and 9-24 parts by weight of amino flame retardant are added to the flask, and the mixture is rapidly stirred for 6-10 hours. The mixture is then heated to evaporate, cooled in an ice-water bath, filtered, and the precipitate is dried to obtain the modified ammonium polyphosphate flame retardant. The reaction formula is as follows: .
[0011] The preferred method for preparing high-temperature fireproof cable material is as follows: polyvinyl chloride, plasticizer, stabilizer, lubricant, and modified ammonium polyphosphate flame retardant are added to a mixer and mixed at 80-90℃ for 10-15 minutes. Then, the mixture is plasticized in a two-roll plasticizer at 160-165℃ for 7-10 minutes and discharged to obtain high-temperature fireproof cable material.
[0012] Preferably, the high-temperature fireproof cable material is used in the high-temperature fireproof cable, and the cable consists of, from the inside out, a copper conductor, a magnesium oxide insulation layer, a copper sheath layer, a ceramicized silicone rubber fireproof strip, and the high-temperature fireproof cable material.
[0013] The beneficial technical effects of this invention are as follows: Ammonium polyphosphate is activated at high temperature to remove some NH3, generating P-OH groups. These groups then form electrostatic interactions with the amino groups of an amino flame retardant, thus modifying the ammonium polyphosphate and obtaining a modified ammonium polyphosphate flame retardant. Finally, this modified ammonium polyphosphate is mixed with polyvinyl chloride (PVC), plasticizers, etc., to obtain a high-temperature resistant fire-resistant cable material. The modified ammonium polyphosphate flame retardant introduces ester groups, which form hydrogen bonds with PVC, significantly improving the compatibility between ammonium polyphosphate and PVC, allowing the PVC cable material to maintain good tensile strength and elongation at break. Furthermore, the introduction of a dioxophosphate caprolactone phosphate flame-retardant structure into the ammonium polyphosphate further enhances its flame-retardant effect, giving the PVC sheath material a higher limiting oxygen index and flame-retardant performance. Detailed Implementation
[0014] The present invention will be further described in detail below through specific implementation examples. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention. After reading the present invention, any modifications of the present invention in various equivalent forms by those skilled in the art fall within the scope of the appended claims.
[0015] Example 1: A method for preparing a high-temperature resistant fireproof cable material: (1) In an ice bath, add 300 mL of dichloromethane, 0.1 mol of triethylamine, 0.1 mol of Boc-serine methyl ester (CAS No. 2766-43-0), and 0.12 mol of 5,5-dimethyl-2-chloro-1,3,2-dioxophosphorylcaprolactone phosphate (CAS No. 4090-55-5) to a flask. Then stir the mixture at room temperature for 12 h, filter, add 180 mL of trifluoroacetic acid to the filtrate, stir the mixture at room temperature for 2 h, add sodium bicarbonate solution to the solution, pour the mixture into a separatory funnel and shake to extract, allow it to stand to separate the layers, take the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate by rotary evaporation. The product is recrystallized in ethyl acetate to obtain an amino flame retardant.
[0016] (2) Add 200g of ammonium polyphosphate to the flask, place it in an oil bath, heat it to 260°C, stir it, and the generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During the stirring process, a small amount of product in the flask is removed and added to water. When the pH of the aqueous solution (mass fraction of 1%) reaches 4, it is cooled to room temperature. 1.5L of water, 200mL of ethanol, and 18g of amino flame retardant are added to the flask. The mixture is stirred rapidly for 6 hours, heated to evaporate and remove the ethanol, cooled in an ice-water bath, filtered, and the precipitate is dried to obtain the modified ammonium polyphosphate flame retardant.
[0017] (3) Add 1 kg of polyvinyl chloride (model Qilu S-700, Kunshan Chaoheng Plastics, the same below), 400 g of di(2-ethylhexyl) phthalate, 33 g of calcium zinc stabilizer (model WWP-D08A, Guangdong Weilinna New Material Technology, the same below), 4.5 g of lubricant polyethylene wax (model TS-5204, Wuhan Lingfan Technology, the same below), 6 g of stearic acid, and 200 g of modified ammonium polyphosphate flame retardant to a mixer, mix at 80°C for 15 min, and then plasticize the mixture in a two-roll plasticizer at 165°C for 8 min, and discharge the material to obtain high temperature fireproof cable material.
[0018] Example 2, a method for preparing a high-temperature resistant fireproof cable material: (1) In an ice bath, add 850 mL of dichloromethane, 0.33 mol of triethylamine, 0.3 mol of Boc-serine methyl ester, and 0.39 mol of 5,5-dimethyl-2-chloro-1,3,2-dioxophosphoryl caprolactone phosphate to a flask. Then stir the mixture at room temperature for 14 h, filter, add 500 mL of trifluoroacetic acid to the filtrate, stir the mixture at room temperature for 3 h, add sodium bicarbonate solution to the solution, pour the mixture into a separatory funnel and shake to extract, allow it to stand to separate the layers, take the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate by rotary evaporation. The product is recrystallized in ethyl acetate to obtain an amino flame retardant.
[0019] (2) Add 250g of ammonium polyphosphate to the flask, place it in an oil bath, heat it to 260°C, stir it, and the generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During the stirring process, a small amount of product in the flask is removed and added to water. When the pH of the aqueous solution (mass fraction of 1%) reaches 3.5, it is cooled to room temperature. 2L of water, 500mL of ethanol, and 47.5g of amino flame retardant are added to the flask. The mixture is stirred rapidly for 8 hours, heated to evaporate and remove the ethanol, cooled in an ice-water bath, filtered and dried to obtain modified ammonium polyphosphate flame retardant.
[0020] (3) Add 1 kg of polyvinyl chloride, 430 g of di(2-ethylhexyl) phthalate, 30 g of calcium zinc stabilizer, 6 g of lubricant polyethylene wax, 7 g of stearic acid, and 250 g of modified ammonium polyphosphate flame retardant to a mixer and mix at 80°C for 15 min. Then, put the mixture into a two-roll plasticizer and plasticize at 160°C for 10 min. Discharge the material to obtain high-temperature fireproof cable material.
[0021] Example 3, a method for preparing a high-temperature resistant fireproof cable material: (1) In an ice bath, add 900 mL of dichloromethane, 0.3 mol of triethylamine, 0.3 mol of Boc-serine methyl ester, and 0.3 mol of 5,5-dimethyl-2-chloro-1,3,2-dioxophosphoryl caprolactone phosphate to a flask. Then stir the mixture at room temperature for 12 h, filter, add 550 mL of trifluoroacetic acid to the filtrate, stir the mixture at room temperature for 2 h, add sodium bicarbonate solution to the solution, pour the mixture into a separatory funnel and shake to extract, allow it to stand to separate the layers, take the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate by rotary evaporation. The product is recrystallized in ethyl acetate to obtain an amino flame retardant.
[0022] (2) Add 300g of ammonium polyphosphate to the flask, place it in an oil bath, heat it to 265°C, stir it, and the generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During the stirring process, a small amount of product in the flask is removed and added to water. When the pH of the aqueous solution (mass fraction of 1%) reaches 3.5, it is cooled to room temperature. 2.5L of water, 600mL of ethanol, and 52g of amino flame retardant are added to the flask. The mixture is stirred rapidly for 10h, heated to evaporate and remove the ethanol, cooled in an ice-water bath, filtered, and the precipitate is dried to obtain the modified ammonium polyphosphate flame retardant.
[0023] (3) Add 1 kg of polyvinyl chloride, 470 g of di(2-ethylhexyl) phthalate, 40 g of calcium zinc stabilizer, 3 g of lubricant polyethylene wax, 5 g of stearic acid, and 300 g of modified ammonium polyphosphate flame retardant to a mixer and mix at 90°C for 10 min. Then, put the mixture into a two-roll plasticizer and plasticize at 160°C for 10 min. Discharge the material to obtain high-temperature fireproof cable material.
[0024] Example 4: A method for preparing a high-temperature resistant fireproof cable material: (1) In an ice bath, add 1.5 L of dichloromethane, 0.5 mol of triethylamine, 0.5 mol of Boc-serine methyl ester, and 0.6 mol of 5,5-dimethyl-2-chloro-1,3,2-dioxophosphorylcaprolactone phosphate to a flask. Then stir the mixture at room temperature for 10 h, filter, add 1 L of trifluoroacetic acid to the filtrate, stir the mixture at room temperature for 3 h, add sodium bicarbonate solution to the solution, pour the mixture into a separatory funnel and shake to extract, let it stand to separate the layers, take the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate by rotary evaporation. The product is recrystallized in ethyl acetate to obtain an amino flame retardant.
[0025] (2) Add 350g of ammonium polyphosphate to the flask, place it in an oil bath, heat it to 260°C, stir it, and the generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During the stirring process, a small amount of product in the flask is removed and added to water. When the pH of the aqueous solution (mass fraction of 1%) reaches 3.2, it is cooled to room temperature. Add 3L of water, 900mL of ethanol, and 84g of amino flame retardant to the flask, stir and mix rapidly for 10h, heat to evaporate and remove ethanol, cool in an ice water bath, filter and dry the precipitate to obtain modified ammonium polyphosphate flame retardant.
[0026] (3) Add 1 kg of polyvinyl chloride, 500 g of di(2-ethylhexyl) phthalate, 38 g of calcium zinc stabilizer, 4 g of lubricant polyethylene wax, 6 g of stearic acid, and 350 g of modified ammonium polyphosphate flame retardant to a mixer and mix at 85°C for 15 min. Then, put the mixture into a two-roll plasticizer and plasticize at 160°C for 10 min. Discharge the material to obtain high-temperature fireproof cable material.
[0027] Comparative Example 1: A method for preparing a cable material: (1) Add 1kg of polyvinyl chloride, 400g of di(2-ethylhexyl) phthalate, 33g of calcium zinc stabilizer, 4.5g of lubricant polyethylene wax, 6g of stearic acid and 200g of ammonium polyphosphate to a mixer and mix at 80°C for 15min. Then, put the mixture into a two-roll plasticizer and plasticize at 165°C for 8min. Discharge the material to obtain cable material.
[0028] Comparative Example 2, a method for preparing a cable material: (1) In an ice bath, add 300 mL of dichloromethane, 0.1 mol of triethylamine, and 0.1 mol of methyl 3-hydroxypropionate (CAS No. 6149-41-3) to a flask, then add 0.12 mol of 5,5-dimethyl-2-chloro-1,3,2-dioxophosphorylcaprolactone phosphate. Stir the mixture at room temperature for 12 h, filter, concentrate the filtrate by rotary evaporation, and recrystallize the product in ethyl acetate to obtain a flame retardant with the following structural formula: .
[0029] (2) Add 200g of ammonium polyphosphate to the flask, place it in an oil bath, heat it to 260°C, stir it, and the generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During the stirring process, a small amount of product in the flask is removed and added to water. When the pH of the aqueous solution (mass fraction of 1%) reaches 4, it is cooled to room temperature. 1.5L of water, 200mL of ethanol, and 18g of amino flame retardant are added to the flask. The mixture is stirred rapidly for 6 hours, heated to evaporate and remove the ethanol, cooled in an ice-water bath, filtered and dried to obtain ammonium polyphosphate flame retardant.
[0030] (3) Add 1 kg of polyvinyl chloride, 400 g of di(2-ethylhexyl) phthalate, 33 g of calcium zinc stabilizer, 4.5 g of lubricant polyethylene wax, 6 g of stearic acid, and 200 g of ammonium polyphosphate flame retardant to a mixer and mix at 80°C for 15 min. Then, put the mixture into a two-roll plasticizer and plasticize at 165°C for 8 min. Discharge the material to obtain cable material.
[0031] Comparative Example 3: A method for preparing a cable material: (1) In an ice bath, add 300 mL of dichloromethane, 0.1 mol of triethylamine, and 0.1 mol of N-Boc-ethanolamine (CAS No. 26690-80-2) to a flask, then add 0.12 mol of 5,5-dimethyl-2-chloro-1,3,2-dioxophosphorylcaprolactone phosphate. Stir the mixture at room temperature for 12 h, filter, add 180 mL of trifluoroacetic acid to the filtrate, stir at room temperature for 2 h, add sodium bicarbonate solution to the solution, pour into a separatory funnel, shake to extract, allow to stand for separation, take the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate by rotary evaporation. Recrystallize the product in dichloromethane to obtain an amino flame retardant with the following structural formula: .
[0032] (2) Add 200g of ammonium polyphosphate to the flask, place it in an oil bath, heat it to 260°C, stir it, and the generated ammonia gas is recovered into a receiving bottle containing water through an inclined condenser. During the stirring process, a small amount of product in the flask is removed and added to water. When the pH of the aqueous solution (mass fraction of 1%) reaches 4, it is cooled to room temperature. 1.5L of water, 200mL of ethanol, and 18g of amino flame retardant are added to the flask. The mixture is stirred rapidly for 6 hours, heated to evaporate and remove the ethanol, cooled in an ice-water bath, filtered, and the precipitate is dried to obtain the modified ammonium polyphosphate flame retardant.
[0033] (3) Add 1 kg of polyvinyl chloride, 400 g of di(2-ethylhexyl) phthalate, 33 g of calcium zinc stabilizer, 4.5 g of lubricant polyethylene wax, 6 g of stearic acid, and 200 g of modified ammonium polyphosphate flame retardant to a mixer and mix at 80°C for 15 min. Then, put the mixture into a two-roll plasticizer and plasticize at 165°C for 8 min. Discharge the material to obtain cable material.
[0034] The cable material was hot-pressed at 165℃ for 8 minutes and 10MPa in a flat vulcanizing machine, and then cold-pressed for 5 minutes to make test pieces. The performance was tested according to GB / T 8815-2008 standard.
[0035] Table 1 In Comparative Example 1, the added ammonium polyphosphate showed poor compatibility with polyvinyl chloride (PVC), severely affecting the mechanical properties of PVC and resulting in low tensile strength and elongation at break of the PVC cable material. The modified ammonium polyphosphate flame retardants in each embodiment introduced ester groups, forming hydrogen bonds with PVC, significantly improving the compatibility between ammonium polyphosphate and PVC, and maintaining good tensile strength and elongation at break for the PVC cable material. Furthermore, the ammonium polyphosphate incorporated dioxane-caprolactone phosphate (DAP). The flame-retardant structure further improves the flame-retardant effect of ammonium polyphosphate, giving the PVC sheath material a higher limiting oxygen index and flame-retardant performance.
[0036] The flame retardant in Comparative Example 2 does not contain amino groups and cannot electrostatically interact with the P-OH groups of ammonium polyphosphate. It does not introduce ester groups into the ammonium polyphosphate, resulting in poor compatibility between ammonium polyphosphate and polyvinyl chloride. The tensile strength and elongation at break of the polyvinyl chloride cable material are lower than those in Example 1.
[0037] The amino flame retardant in Comparative Example 3 does not contain ester groups, resulting in poor compatibility between the modified ammonium polyphosphate flame retardant and polyvinyl chloride. The tensile strength and elongation at break of the polyvinyl chloride cable material are lower than those in Example 1.
Claims
1. A high-temperature resistant fireproof cable material, characterized in that, The high-temperature fireproof cable material comprises 100 parts by weight of polyvinyl chloride, 40-50 parts by weight of plasticizer, 3-4 parts by weight of stabilizer, 0.8-1.3 parts by weight of lubricant, and 20-35 parts by weight of modified ammonium polyphosphate flame retardant. The modified ammonium polyphosphate flame retardant is prepared by the following method: ammonium polyphosphate is added to a flask, placed in an oil bath, heated and stirred, cooled, and then water, ethanol, and amino flame retardant are added, stirred and mixed, heated and evaporated, cooled in an ice-water bath, filtered, and the precipitate is dried to obtain the modified ammonium polyphosphate flame retardant. The structural formula of the amino flame retardant is as follows: .
2. The high-temperature resistant fireproof cable material according to claim 1, characterized in that, The plasticizer includes di(2-ethylhexyl) phthalate, and the stabilizer includes calcium zinc stabilizer.
3. The high-temperature resistant fireproof cable material according to claim 1, characterized in that, The lubricant includes any one or a combination of polyethylene wax and stearic acid.
4. The high-temperature resistant fireproof cable material according to claim 1, characterized in that, During the heating and stirring process, the product in the flask is transferred and added to water. When the pH of the aqueous solution reaches 3.2-4, an amino flame retardant is added.
5. The high-temperature resistant fireproof cable material according to claim 1, characterized in that, The temperature during heating and stirring is 260-265℃; the stirring and mixing time is 6-10 hours.
6. The high-temperature resistant fireproof cable material according to claim 1, characterized in that, The amount of ammonium polyphosphate is 100 parts by weight, and the amount of amino flame retardant is 9-24 parts by weight.
7. The high-temperature resistant fireproof cable material according to claim 1, characterized in that, The amino flame retardant was prepared by the following method: In an ice bath, dichloromethane, triethylamine, Boc-serine methyl ester, and 5,5-dimethyl-2-chloro-1,3,2-dioxophosphorylcaprolactone phosphate were added to a flask. The mixture was then stirred and reacted at room temperature for 10-14 hours. After filtration, trifluoroacetic acid was added to the filtrate, and the mixture was stirred and reacted at room temperature for 2-3 hours. Sodium bicarbonate solution was added to the solution, and the mixture was poured into a separatory funnel and shaken for extraction. After standing and separating the layers, the organic layer was collected, dried with anhydrous sodium sulfate, filtered, and the filtrate was concentrated by rotary evaporation. The product was recrystallized in ethyl acetate to obtain the amino flame retardant.
8. The high-temperature resistant fireproof cable material according to claim 7, characterized in that, The molar ratio of triethylamine, Boc-serine methyl ester, and 5,5-dimethyl-2-chloro-1,3,2-dioxophosphorylcaprolactone phosphate is (1-1.1):1:(1-1.4).
9. A method for preparing a high-temperature resistant fireproof cable material as described in any one of claims 1-8, characterized in that, The preparation method is as follows: polyvinyl chloride, plasticizer, stabilizer, lubricant, and modified ammonium polyphosphate flame retardant are added to a mixer and mixed at 80-90℃ for 10-15 minutes. Then, the mixture is plasticized in a two-roll plasticizer at 160-165℃ for 7-10 minutes and discharged to obtain high-temperature fireproof cable material.
10. The application of a high-temperature fire-resistant cable material obtained by the preparation method as described in claim 9 in high-temperature fire-resistant cables, characterized in that, The cable is composed of a copper conductor, a magnesium oxide insulation layer, a copper sheath layer, a ceramicized silicone rubber fireproof strip, and high-temperature fireproof cable material.