An ASA-CF-GF composite material, its preparation method and application
By using ASA-CF-GF composite materials, combined with specific additives and optimized processes, the performance shortcomings in ASA resin modification have been addressed, achieving a balance between high strength, toughness, and dimensional stability. This makes the material suitable for high-end industrial products and improves its overall performance and cost-effectiveness.
Patent Information
- Application Number
- CN202610952586.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-29
- Publication Date
- 2026-11-10
AI Technical Summary
Existing ASA resin modification methods suffer from insufficient rigidity, low tensile and flexural strength, and poor high-temperature dimensional stability. Furthermore, modifications using single carbon fibers or glass fibers can lead to problems such as poor filler dispersion, agglomeration, surface defects, and high costs, which limit their application in high-end industrial fields.
By using ASA-CF-GF composite material, the ratio of carbon fiber to glass fiber is optimized, and specific composite coupling agents, antioxidants, UV absorbers and lubricants are combined to achieve a balance between the material's mechanical strength, toughness, dimensional stability and cost. This solves the apparent defects such as filler agglomeration and fiber floating, and improves the overall performance of the material.
It achieves high strength, toughness, and dimensional stability in materials, improves processing fluidity and appearance quality, reduces costs, and is suitable for long-term use in high-end industrial products, extending their service life.
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, and more specifically, to an ASA-CF-GF composite material, its preparation method, and its application. Background Technology
[0002] ASA resin (acrylonitrile-styrene-acrylate copolymer) is a high-performance engineering plastic with excellent resistance to UV aging, weathering, yellowing, and surface gloss. Compared to ABS resin, it does not crack or fade during long-term outdoor use and is widely used in outdoor plastic products. However, pure ASA resin has drawbacks such as insufficient rigidity, low tensile and flexural strength, and poor dimensional stability at high temperatures, making it difficult to meet the requirements of heavy-duty and precision structural components.
[0003] Carbon fiber (CF) has advantages such as high strength, high modulus, low density, corrosion resistance, and high temperature resistance. It is a high-end reinforcing and modifying filler that can significantly improve the mechanical strength and lightweight properties of the resin matrix. However, carbon fiber is expensive, and when it is used to modify ASA resin alone, the filler has poor dispersibility and is prone to agglomeration, which leads to a decrease in the toughness of the composite material, rough surface of the product, and poor processing fluidity.
[0004] Glass fiber (GF) is inexpensive, has outstanding rigidity and excellent dimensional stability, and is a general-purpose reinforcing filler that can effectively improve the rigidity and deformation resistance of resin. However, glass fiber has average weather resistance, and filling it with ASA alone will significantly reduce the material's impact resistance. At the same time, the problem of surface fiber floating is serious, which affects the appearance quality and weather resistance of the product.
[0005] Currently, most methods of modifying ASA resin involve modifying it with a single carbon fiber or glass fiber, which has significant performance limitations and greatly restricts the large-scale application of ASA composite materials in high-end industrial fields.
[0006] In view of this, the present invention is proposed. Summary of the Invention
[0007] The purpose of this invention is to provide an ASA-CF-GF composite material, its preparation method, and its application. This ASA-CF-GF composite material improves weather resistance, mechanical strength, toughness, and dimensional stability. By improving the interfacial compatibility and dispersibility of the filler, it solves apparent defects such as fiber floating. While ensuring performance improvement, it achieves cost control, providing an economical and reliable solution for high-end applications.
[0008] This invention is implemented as follows: In a first aspect, the present invention provides an ASA-CF-GF composite material, comprising: ASA resin, carbon fiber, glass fiber, composite coupling agent, antioxidant, ultraviolet absorber and lubricant; wherein the mass ratio of ASA resin, carbon fiber and glass fiber is 65~85:3~10:8~20.
[0009] Secondly, the present invention provides a method for preparing the above-mentioned ASA-CF-GF composite material, which includes: mixing carbon fiber, glass fiber and coupling agent to obtain composite fiber filler; mixing ASA resin, antioxidant, ultraviolet absorber and lubricant to obtain resin premix; then feeding the resin premix into the main feed port of the extrusion equipment, and after the resin is completely melted, adding the composite fiber filler at a uniform speed through the side feed port, and continuously extruding after melting and mixing evenly; and then obtaining the ASA-CF-GF composite material after extrusion, pelletizing and drying.
[0010] Thirdly, the present invention provides the application of the above-mentioned ASA-CF-GF composite material in the preparation of outdoor building materials, housings of new energy equipment, automotive exterior parts or precision mechanical parts.
[0011] The present invention has the following beneficial effects: This invention synergistically modifies ASA resin by compounding it with carbon fiber and glass fiber, and then combines it with specific composite coupling agents, antioxidants, UV absorbers, and lubricants. The resulting ASA-CF-GF composite material retains the excellent weather resistance and anti-yellowing properties of the ASA matrix while significantly improving its overall performance. Mechanically, the tensile, flexural, and impact strengths are synergistically enhanced, achieving a good balance between strength and toughness. Dimensional shrinkage is effectively controlled, ensuring high precision and dimensional stability of the products. Furthermore, by optimizing the dispersion process, surface defects such as filler agglomeration, shedding, fiber floating, and surface roughness are fundamentally solved, giving the products excellent gloss and appearance quality, and significantly improving melt processing fluidity. Considering all these factors, the composite material exhibits significantly enhanced long-term reliability in harsh outdoor environments, with no fading, cracking, or other aging problems, and a significantly extended service life compared to traditional modified materials. Moreover, the composite material of this invention significantly reduces raw material costs, has a stable production process, and a high yield rate, making it suitable for various molding processes and suitable for large-scale application in the production of high-end industrial products, with broad application prospects. Detailed Implementation
[0012] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0013] Given that modifying ASA resin with a single carbon fiber or glass fiber results in decreased toughness, rough surface, poor processing fluidity, reduced impact resistance, and poor appearance and weather resistance, this invention proposes using both carbon fiber and glass fiber to modify ASA resin. However, this approach also suffers from problems such as unreasonable filler ratios, poor interfacial compatibility, and weak synergistic effects, making it impossible to simultaneously achieve the desired weather resistance, high strength, high toughness, low shrinkage, and good processing performance, and production costs are difficult to control. To improve these issues and obtain an ASA-CF-GF ternary synergistic modification scheme that balances product mechanical properties, processing performance, weather resistance, and production costs, this invention first screens and compares the types or models of ASA resin, carbon fiber, and glass fiber, then optimizes the compounding ratio of the three. Based on this, specific composite coupling agents, antioxidants, UV absorbers, and processing lubricants are screened for the ASA-CF-GF ternary synergistic modification scheme, resulting in a composite material with outstanding mechanical, processing, and weather resistance properties, and controllable costs.
[0014] In this invention, the raw materials of the ASA-CF-GF composite material include: ASA resin, carbon fiber, glass fiber, composite coupling agent, antioxidant, ultraviolet absorber and lubricant.
[0015] In some embodiments, the ASA composite material comprises, by weight, the following components: 65-85 parts of ASA resin, 3-10 parts of carbon fiber, 8-20 parts of glass fiber, 1.2-2.5 parts of coupling agent, 0.3-0.8 parts of antioxidant, 0.2-0.6 parts of ultraviolet absorber, and 0.4-1.0 parts of lubricant.
[0016] In some embodiments, the ASA resin is a high weather-resistant extrusion grade ASA resin; more preferably, the melt index of the ASA resin is 18~25g / 10min (220℃ / 10kg), and / or the tensile strength is ≥40MPa, which meets the above performance conditions and can ensure the basic weather resistance and processing fluidity of the matrix.
[0017] In some embodiments, the carbon fiber is carbon fiber with a lightly oxidized surface; more preferably, the carbon fiber is chopped carbon fiber; more preferably, the specifications of the chopped carbon fiber are: length 3~6mm, diameter 7~10μm.
[0018] In some embodiments, the glass fiber is alkali-free glass fiber; more preferably, the glass fiber is chopped alkali-free glass fiber; even more preferably, the specifications of the chopped alkali-free glass fiber are: length 4~7mm, diameter 10~13μm. This invention replaces part of the carbon fiber with glass fiber, which not only reduces production costs but also provides high-performance materials.
[0019] When carbon fiber and glass fiber are added to the composite system in the above proportions, carbon fiber provides advantages such as ultra-high strength, high modulus and lightweight, while glass fiber provides high rigidity and low shrinkage. The two interweave to form a three-dimensional support network, which makes up for the performance shortcomings of single filler modification. The resulting composite material has tensile strength, flexural strength and impact strength that are more than 20% higher than that of pure ASA resin, and the dimensional shrinkage rate is reduced to less than 0.3%. At the same time, it retains the excellent weather resistance and anti-yellowing properties of the ASA matrix, achieving a balance between strength and toughness, and rigidity and stability.
[0020] In some embodiments, the composite coupling agent includes silane coupling agent and titanate coupling agent. Combining these two types of coupling agents can effectively improve the interfacial bonding force between inorganic fibers and organic resins, eliminate filler agglomeration and shedding problems, significantly improve melt processing fluidity, and completely solve the defects of fiber floating and surface roughness in traditional glass fiber modified ASA. The product has high surface gloss and excellent appearance quality.
[0021] Preferably, the mass ratio of silane coupling agent to titanate coupling agent in the composite coupling agent is 2:1.
[0022] In some embodiments, the antioxidant includes antioxidant 1010 and antioxidant 168. By combining these two antioxidants, the thermo-oxidative aging of the composite material during high-temperature processing and long-term use can be effectively inhibited. More preferably, the mass ratio of antioxidant 1010 to antioxidant 168 is 1:1.
[0023] In some embodiments, the UV absorber includes benzotriazole UV absorbers, which are adapted to the outdoor weather resistance requirements of the ASA matrix. When combined with the antioxidants mentioned above, they can work with the weather resistance characteristics of the ASA matrix itself, so that the composite material can be used outdoors for a long time without fading, cracking, aging and failure. The service life is increased by more than 50% compared with traditional modified ASA materials.
[0024] In some embodiments, the processing lubricant includes zinc stearate and EBS lubricant. The processing lubricant of the present invention can reduce melt viscosity, improve filler dispersibility, and eliminate surface defects such as fiber floating and scratches.
[0025] To enable the large-scale production of the aforementioned ASA-CF-GF composite material, this invention has also optimized its extrusion processing. Therefore, this invention can also provide a method for preparing the aforementioned ASA-CF-GF composite material, comprising: S1. Mix carbon fiber, glass fiber and composite coupling agent to obtain composite fiber filler; S2. Mix ASA resin, antioxidant, UV absorber and lubricant to obtain resin premix; S3. Then, the resin premix is fed into the main feed port of the extrusion equipment. After the resin is completely melted, the composite fiber filler is added at a constant speed through the side feed port. After melting and mixing evenly, it is continuously extruded. S4. After extrusion, pelletizing, and drying, the ASA-CF-GF composite material is obtained.
[0026] In some embodiments, the extrusion conditions are as follows: temperature of each zone of the extrusion equipment: zone 1 190~200℃, zone 2 200~210℃, zone 3 225~zone 10 235℃; die head 225~235℃; screw speed 300~350r / min.
[0027] In some embodiments, the drying conditions are: drying at 80~90°C for 2~3 hours.
[0028] Using the above raw materials and preparation methods, composite materials with simultaneously improved weather resistance, mechanical strength, toughness, and dimensional stability can be obtained, balancing product performance and production costs. These composite materials are suitable for the current production needs of high-end industrial products.
[0029] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0030] Example 1 This embodiment is an ASA-CF-GF composite material, and the weight parts of its raw materials are as follows: The composition consists of 75 parts ASA resin, 6 parts chopped carbon fiber, 12 parts alkali-free glass fiber, 1.8 parts composite coupling agent, 0.5 parts antioxidant, 0.4 parts ultraviolet absorber, and 0.6 parts processing lubricant.
[0031] Among them, the ASA resin is a high weather-resistant extrusion grade ASA resin with a melt index of 18~25g / 10min (220℃ / 10kg) and a tensile strength ≥40MPa; the short-cut carbon fiber has a length of 3~6mm and a diameter of 7~10μm, and the surface is lightly oxidized; the alkali-free short-cut glass fiber has a length of 4~7mm and a diameter of 10~13μm; the composite coupling agent is a mixture of silane coupling agent and titanate coupling agent in a mass ratio of 2:1; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the ultraviolet absorber is a benzotriazole ultraviolet absorber; and the processing lubricant is a mixture of zinc stearate and EBS lubricant.
[0032] The preparation method of the above ASA-CF-GF composite material is as follows: (1) Filler pretreatment: Mix 6 parts of short carbon fiber and 12 parts of alkali-free glass fiber, add 1.8 parts of composite coupling agent, stir at low speed of 350r / min for 5min, and set aside. (2) Matrix premix: 75 parts ASA resin, 0.5 parts compound antioxidant, 0.4 parts UV absorber, and 0.6 parts processing lubricant were stirred at room temperature for 10 minutes to obtain a uniform premix. (3) Melt blending: The temperatures of each zone of the twin-screw extruder are 195℃, 215℃, 225℃~235℃ respectively, the screw speed is 300~350r / min, the resin premix is fed into the main feed, the pretreated fiber is fed into the side feed, and the melt blending is extruded. (4) Granulation and drying: water-cooled strip cutting and granulation, drying at 85℃ for 2.5h to obtain the finished composite material.
[0033] Example 2 This embodiment is an ASA-CF-GF composite material, which differs from Example 1 in the proportion of raw materials. The raw materials of this composite material are in the following weight parts: 70 parts ASA resin, 8 parts chopped carbon fiber, 15 parts alkali-free glass fiber, 2.0 parts composite coupling agent, 0.6 parts antioxidant, 0.5 parts ultraviolet absorber, and 0.8 parts processing lubricant.
[0034] Example 3 This embodiment is an ASA-CF-GF composite material, which differs from Example 1 in the proportion of raw materials. The raw materials of this composite material are in the following weight parts: 80 parts ASA resin, 4 parts chopped carbon fiber, 10 parts alkali-free glass fiber, 1.5 parts composite coupling agent, 0.4 parts antioxidant, 0.3 parts ultraviolet absorber, and 0.5 parts processing lubricant.
[0035] Comparative Example 1 This comparative example uses unmodified extrusion-grade ASA resin directly, without any fillers or additives.
[0036] Comparative Example 2 Compared with Example 1, this comparative example only added the same type of carbon fiber modified ASA resin. The raw material weight fractions of this composite material are: 75 parts ASA resin, 18 parts chopped carbon fiber, 1.8 parts composite coupling agent, 0.5 parts antioxidant, 0.4 parts ultraviolet absorber, and 0.6 parts processing lubricant. The preparation method is the same as that of Example 1.
[0037] Comparative Example 3 Compared with Example 1, this comparative example only added the same type of glass fiber modified ASA resin. The raw material weight fractions of this composite material are: 75 parts ASA resin, 18 parts alkali-free glass fiber, 1.8 parts composite coupling agent, 0.5 parts antioxidant, 0.4 parts ultraviolet absorber, and 0.6 parts processing lubricant. The preparation method is the same as that of Example 1.
[0038] Comparative Example 4 The difference from Example 1 is that the ratio of ASA resin, carbon fiber and glass fiber added exceeds the protection range, for example: 60:20:20.
[0039] Comparative Example 5 The difference from Example 1 is that the ratio of ASA resin, carbon fiber and glass fiber added exceeds the protection range, for example: 97:2:1.
[0040] Comparative Example 6 The difference from Example 1 is that the mass ratio of silane coupling agent to titanate coupling agent exceeds the protection range.
[0041] Comparative Example 7 The difference from Example 1 is that, in the combination of silane coupling agent and titanate coupling agent, the silane coupling agent or titanate coupling agent is replaced in equal amounts with a coupling agent of the same type in the art. Alternatively, a single coupling agent conventional in the art can be used directly for preparation.
[0042] Comparative Example 8 The difference from Example 1 is that the mass ratio of antioxidant 1010 to antioxidant 168 exceeds the protection range.
[0043] Comparative Example 9 The difference from Example 1 is that, in the combination of antioxidant 1010 and antioxidant 168, antioxidant 1010 or antioxidant 168 is replaced in equal amounts with an antioxidant of the same type in the art. Alternatively, it can be prepared directly using a single antioxidant conventional in the art.
[0044] Experimental Example 1 The composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were used to prepare standard test specimens. Mechanical properties and weather resistance were tested according to national standards GB / T1040, GB / T 9341, GB / T 1843, and GB / T 16422. The test results are as follows: Example 1: The composite material has a tensile strength of 60.5 MPa, a flexural strength of 85.3 MPa, and a simply supported beam impact strength of 10.6 kJ / m. 2 The dimensional shrinkage rate is 0.28%, and there is no obvious yellowing or cracking after 5000 hours of UV aging; Examples 2 and 3 demonstrate a balanced overall performance, combining high strength with good toughness; Comparative Example 1: The pure ASA resin had a tensile strength of 48.2 MPa and a flexural strength of 50.1 MPa, which were significantly lower than the required mechanical properties. Comparative Example 2 shows that the single carbon fiber modified material has poor toughness, poor melt flowability, and rough surface of the product. Comparative Example 3: The impact strength of the single glass fiber modified material is only 7.8 kJ / m. 2 Its impact resistance is obviously defective.
[0045] The above comparison results prove that the performance of the ternary compound modification scheme of the present invention is far superior to that of carbon fiber or glass fiber modification alone and pure resin system.
[0046] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. An ASA-CF-GF composite material, characterized in that, include: ASA resin, carbon fiber, glass fiber, composite coupling agent, antioxidant, ultraviolet absorber and lubricant; The mass ratio of ASA resin, carbon fiber and glass fiber is 65~85:3~10:8~20.
2. The ASA-CF-GF composite material according to claim 1, characterized in that, The ASA resin is a high weather-resistant extrusion-grade ASA resin; Preferably, the melt index of the ASA resin is 18~25g / 10min (220℃ / 10kg), and / or the tensile strength is ≥40MPa.
3. The ASA-CF-GF composite material according to claim 1, characterized in that, The carbon fiber is a carbon fiber with a lightly oxidized surface. Preferably, the carbon fiber is chopped carbon fiber; Preferably, the carbon fiber has the following specifications: length 3~6mm, diameter 7~10μm.
4. The ASA-CF-GF composite material according to claim 1, characterized in that, The glass fiber is alkali-free glass fiber; Preferably, the glass fiber is chopped glass fiber; Preferably, the glass fiber has the following specifications: length 4~7mm, diameter 10~13μm.
5. The ASA-CF-GF composite material according to claim 1, characterized in that, The composite coupling agent includes silane coupling agents and titanate coupling agents; Preferably, the mass ratio of silane coupling agent to titanate coupling agent in the composite coupling agent is 2:
1.
6. The ASA-CF-GF composite material according to claim 1, characterized in that, The ASA composite material comprises the following components by weight: 65-85 parts ASA resin, 3-10 parts carbon fiber, 8-20 parts glass fiber, 1.2-2.5 parts composite coupling agent, 0.3-0.8 parts antioxidant, 0.2-0.6 parts ultraviolet absorber, and 0.4-1.0 parts lubricant; Preferably, the antioxidant comprises antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; Preferably, the ultraviolet absorber includes benzotriazole ultraviolet absorbers; Preferably, the lubricant comprises zinc stearate and EBS lubricant.
7. The method for preparing the ASA-CF-GF composite material according to any one of claims 1 to 6, characterized in that, include: Carbon fiber, glass fiber and composite coupling agent are mixed to obtain composite fiber filler; ASA resin, antioxidant, UV absorber and lubricant are mixed to obtain resin premix; Then, the resin premix is fed into the main feed port of the extrusion equipment. After the resin is completely melted, the composite fiber filler is added at a constant speed through the side feed port. After being melted and mixed evenly, it is continuously extruded. After extrusion, pelletizing, and drying, the ASA-CF-GF composite material is obtained.
8. The preparation method according to claim 7, characterized in that, The extrusion conditions are: Temperatures in each zone of the extrusion equipment: Zone 1 190~200℃, Zone 2 200~210℃, Zone 3 225~Zone 10 235℃; Die head 225~235℃; Screw speed 300~350r / min.
9. The preparation method according to claim 7, characterized in that, The drying conditions are: drying at 80~90℃ for 2~3 hours.
10. The application of the ASA-CF-GF composite material as described in any one of claims 1 to 6 in the preparation of outdoor building materials, housings of new energy equipment, automotive exterior parts, or precision mechanical parts.