By combining Ba ion-doped TiO2 with graphene, a multi-level conductive pathway and interface bridging structure are constructed, which solves the shortcomings of existing coating materials in terms of conductivity, hydrophobicity and radiative cooling performance. This achieves a synergistic improvement in conductive stability and radiative cooling performance, and is applicable to fields such as electronic devices and building energy conservation.
Patent Information
- Application Number
- CN202611376829.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-10
AI Technical Summary
Existing coating materials cannot simultaneously guarantee conductivity and high hydrophobicity and radiative cooling performance. Furthermore, traditional carbon-based fillers tend to agglomerate in polymer matrices, resulting in discontinuous conductive pathways, insufficient mechanical stability, and degraded surface functions in the coating.
By combining Ba ion-doped TiO2 with graphene, a Ti-O-C and Ba-O-C interface bridging structure is formed, constructing a multi-level conductive pathway. Utilizing the infrared emission capability of the PVDF substrate, a composite coating that combines conductivity, superhydrophobicity, and radiation cooling is prepared.
It significantly enhances the electrical conductivity and hydrophobicity of the coating, achieving a synergistic improvement in electrical conductivity and radiative cooling performance, making it suitable for multifunctional applications in complex service environments.
Smart Images

Figure CN123063010A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional coating materials technology, specifically relating to a barium ion-doped titanium dioxide / graphene / PVDF multifunctional composite coating and its preparation method and application. In particular, it relates to a multifunctional composite coating material with conductive, superhydrophobic and radiative cooling properties, which can be used in building exterior surfaces, heat dissipation of electronic devices, antistatic surfaces, antifouling and self-cleaning surfaces, and outdoor thermal management materials. Background Technology
[0002] With the development of electronic devices, building energy conservation, outdoor equipment, and functional protective materials, single-function coatings are no longer sufficient to meet the demand for synergistic performance in complex service environments, including conductivity, waterproofing, antifouling, and thermal management. Traditional conductive coatings typically rely on carbon black, graphene, carbon nanotubes, or metal fillers to construct a conductive network. However, while these materials improve conductivity, they often enhance solar absorption, which is detrimental to radiative cooling. At the same time, some carbon-based fillers tend to agglomerate in the polymer matrix, resulting in discontinuous conductive pathways, insufficient mechanical stability, and degraded surface functions in the coating.
[0003] Titanium dioxide possesses high chemical stability, good weather resistance, high refractive index, and good infrared emission capabilities, making it a promising candidate for applications in radiation refrigeration and functional coatings. However, ordinary titanium dioxide is a wide-bandgap semiconductor with poor intrinsic conductivity, making it difficult to meet the requirements for antistatic or conductive applications when used alone as a coating. Furthermore, while single TiO2 / PVDF coatings exhibit some infrared emission and hydrophobicity, their conductivity is insufficient, and their rough surface structure and interfacial charge transport capabilities are limited.
[0004] Graphene possesses excellent electrical conductivity and mechanical strengthening properties, which can be used to improve the electron transport capability of coatings. However, when using the graphene / PVDF system alone, graphene is prone to sheet stacking, and its strong light absorption characteristics may reduce the coating's solar reflectivity and radiative cooling effect. Furthermore, the interfacial bonding between graphene and PVDF is limited, and there is still room for improvement in the coating's surface structure and stability. Therefore, there is an urgent need to develop a multifunctional composite coating material that can ensure the coating's electrical conductivity while also possessing high hydrophobicity and radiative cooling properties. Summary of the Invention
[0005] The present invention aims to provide a multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF, its preparation method, and its application. This coating introduces lattice distortion and oxygen vacancies into TiO2 through Ba ion doping, reducing the band gap of TiO2 and improving its intrinsic conductivity. Simultaneously, it utilizes graphene to construct a continuous conductive network and forms multi-level conductive pathways through Ti-O-C and Ba-O-C interface bridging structures, thereby significantly enhancing the coating's conductivity.
[0006] Another objective of this invention is to provide an application of a functional coating that combines conductivity, superhydrophobicity, and radiation cooling, prepared by mixing the above-mentioned powder material with PVDF, in building energy conservation.
[0007] To solve the above-mentioned technical problems, the present invention is implemented as follows:
[0008] In a first aspect, the present invention provides a multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF, the composite coating comprising a PVDF matrix and Ba ion-doped TiO2 / graphene composite functional powder dispersed in the PVDF matrix; the Ba ion-doped TiO2 / graphene composite functional powder comprising Ba ion-doped TiO2 nanoparticles and graphene sheets. The Ba ion-doped TiO2 nanoparticles contain oxygen vacancies induced by Ba ion doping, and a Ti-O-C and / or Ba-O-C interfacial connection structure is formed between the Ba ion-doped TiO2 nanoparticles and the graphene sheets, giving the composite coating conductive, hydrophobic, and radiative cooling functions.
[0009] Preferably, the Ba / Ti molar ratio in the Ba ion-doped TiO2 is 1% to 10%, more preferably 3% to 7%.
[0010] Preferably, the graphene content is 0.5% to 20% of the mass of Ba ion-doped TiO2, more preferably 3% to 12%, and even more preferably 5% to 10%.
[0011] Preferably, the average particle size of the Ba ion-doped TiO2 nanoparticles is 10–300 nm, and more preferably 20–150 nm.
[0012] Preferably, based on the mass of the coating solid components, the content of the Ba ion-doped TiO2 / graphene composite functional powder is 10%–80%, the PVDF content is 20%–90%, and the balance is additives; the content of the additives is 0–5%, and the sum of the three is 100%; the additives are selected from one or more of dispersants, film-forming aids, defoamers, and leveling agents.
[0013] Preferably, the coating has infrared emission properties in the 8–13 μm atmospheric window band, and the water contact angle is not less than 130° and the sliding angle is not more than 10°.
[0014] Secondly, the present invention provides a method for preparing a multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF. The method involves doping titanium dioxide with barium ions, then combining it with graphene, stirring and sonicating until uniformly mixed, followed by hydrothermal reaction, calcination, centrifugation, washing, drying, and grinding to finally obtain the product.
[0015] As a preferred embodiment, the method for preparing the barium-doped titanium dioxide / graphene / PVDF multifunctional composite coating includes the following steps:
[0016] (1) Graphene material is dispersed in a solvent to obtain a graphene dispersion;
[0017] (2) Add the titanium source and barium source to the graphene dispersion and stir to mix, so that the titanium source is hydrolyzed, condensed or deposited in situ on the graphene surface;
[0018] (3) The mixture obtained in step (2) was subjected to a hydrothermal reaction. After the reaction was completed, it was cooled to room temperature, centrifuged, washed and dried to obtain the Ba ion-doped TiO2 / graphene precursor.
[0019] (4) The precursor is heat-treated to obtain Ba ion-doped TiO2 / graphene composite functional powder;
[0020] (5) The Ba ion-doped TiO2 / graphene composite functional powder is added to PVDF slurry and dispersed by stirring, ultrasonication, ball milling or sand milling to obtain composite coating slurry;
[0021] (6) The composite coating slurry is coated on the substrate surface, leveled at room temperature, and then dried and cured to obtain a barium ion doped titanium dioxide / graphene / PVDF multifunctional composite coating.
[0022] Preferably, in step (1), the graphene material includes graphene, graphene oxide, reduced graphene oxide, few-layer graphene, or any combination thereof.
[0023] Preferably, in step (1), the solvent includes N,N-dimethylformamide, N-methylpyrrolidone, dimethylacetamide, acetone, ethanol, water, or a mixture thereof.
[0024] Preferably, in step (1), the graphene material is added to a solvent and ultrasonically dispersed for 30–120 min to obtain a graphene dispersion. The mass concentration of the graphene material in the graphene dispersion is 0.1–5.0 mg·mL. -1 More preferably, it is 0.5–2.0 mg·mL. -1 More preferably, 1.0–1.5 mg·mL -1 .
[0025] Preferably, in step (2), the barium source includes barium acetate, barium nitrate, barium chloride, barium hydroxide, or any combination thereof.
[0026] Preferably, in step (2), the titanium source includes tetrabutyl titanate, isopropyl titanate, titanium tetrachloride, titanium sulfate, titanate, or any combination thereof.
[0027] Preferably, in step (2), the Ba / Ti molar ratio is 0.1% to 15%, more preferably 1% to 10%, and even more preferably 3% to 7%; based on the theoretical product mass of the titanium source calculated as TiO2, the amount of graphene material added is 0.5% to 20% of the theoretical product mass of TiO2, more preferably 3% to 12%, and even more preferably 5% to 10%.
[0028] Preferably, in step (2), the mixture is stirred for 1-6 hours.
[0029] Preferably, in step (3), the hydrothermal reaction temperature is 100–220 °C and the reaction time is 4–48 h. More preferably, the hydrothermal reaction temperature is 150–200 °C and the reaction time is 16–32 h.
[0030] Preferably, in step (4), the heat treatment temperature is 250–600 °C, the heat treatment time is 0.5–6 h, and the heat treatment atmosphere is air, nitrogen, argon, or an inert atmosphere. More preferably, the heat treatment temperature is 400–500 °C, and the heat treatment time is 1–3 h.
[0031] Preferably, in step (5), the PVDF matrix is polyvinylidene fluoride; the mass concentration of PVDF in the PVDF slurry is 5% to 25%, more preferably 8% to 15%, and even more preferably 10% to 12%. The solvent used in the PVDF slurry includes N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, acetone, tetrahydrofuran, ethyl acetate or mixtures thereof, preferably N,N-dimethylformamide, or a mixture of N,N-dimethylformamide and acetone.
[0032] The PVDF slurry also contains additives selected from one or more of dispersants, film-forming aids, defoamers, and leveling agents. The dispersants include one or more of polyvinylpyrrolidone, polyacrylate dispersants, phosphate dispersants, polyester dispersants, polyurethane dispersants, and polyether-modified polysiloxanes, with an addition amount of 0.1% to 3% of the mass of the composite functional powder, more preferably 0.5% to 2%.
[0033] The film-forming aid includes one or more of triethyl citrate, acetylated tributyl citrate, tributyl citrate, propylene carbonate, propylene glycol methyl ether acetate, and ethylene glycol butyl ether, and the amount added is 0.5% to 5% of the mass of PVDF, more preferably 1% to 3%.
[0034] The defoamer includes one or more of dimethyl silicone oil, polyether-modified polysiloxane, organosilicon defoamer, and non-silicone polymer defoamer, and its addition amount is 0.05% to 0.5% of the total mass of the composite coating slurry.
[0035] The leveling agent includes one or more of polyacrylate leveling agents, polyether-modified polysiloxane leveling agents, polyester-modified polysiloxane leveling agents, or fluorinated surfactants, and its addition amount is 0.05% to 0.5% of the total mass of the composite coating slurry.
[0036] Preferably, in step (5), the content of the Ba ion-doped TiO2 / graphene composite functional powder is 10% to 80%, and the PVDF content is 20% to 90%.
[0037] Preferably, in step (6), the coating method includes scraping, spraying, spin coating, dip coating, roller coating, or brush coating.
[0038] Preferably, in step (6), the leveling process is carried out at room temperature for 10 to 60 minutes; the drying temperature is 60 to 120 °C and the drying time is 2 to 24 hours; the curing temperature is 80 to 140 °C and the curing heat treatment time is 0.5 to 4 hours.
[0039] Preferably, in step (6), the substrate includes glass, metal, ceramic, cement-based material, wood, plastic, fabric, polyester film, polyimide film, or building exterior wall material.
[0040] Preferably, the thickness of the composite coating is 10–1000 μm, and more preferably 30–500 μm.
[0041] Thirdly, the present invention provides the application of the above-mentioned barium-doped titanium dioxide / graphene / PVDF multifunctional composite coating in building energy conservation, heat dissipation of electronic devices, antistatic materials, outdoor thermal management materials, antifouling and self-cleaning materials, metal protective materials or flexible functional films.
[0042] Compared with the prior art, the present invention has the following characteristics:
[0043] 1. This invention introduces oxygen vacancies and lattice defects by doping TiO2 with Ba ions, thereby reducing the band gap of TiO2 and improving the intrinsic conductivity of TiO2, thus solving the problem of poor conductivity of a single TiO2 / PVDF coating.
[0044] 2. This invention combines graphene with Ba-doped TiO2 to form Ti-O-C and Ba-O-C interfacial bridging structures between TiO2 particles and graphene, thereby constructing a multi-level conductive pathway composed of oxygen vacancies, interfacial chemical bonds, and graphene sheets, which improves the electron transport efficiency and conductivity stability of the coating.
[0045] 3. In this invention, Ba ions regulate the growth of TiO2 crystals, reduce the particle size of TiO2 nanoparticles, improve particle dispersibility, and form a micro-nano rough structure on the coating surface. This, combined with the low surface energy characteristics of PVDF, significantly enhances the hydrophobic or superhydrophobic properties of the coating.
[0046] 4. In this invention, the PVDF matrix has strong mid-infrared emission capability, and the Ba-doped TiO2 nanoparticles can enhance the infrared emission of the coating in the 8-13 μm atmospheric window range. At the same time, the TiO2 particles have a scattering effect on sunlight, which improves the solar reflectivity of the coating and alleviates the problem of sunlight absorption caused by graphene fillers, thus achieving a balance between electrical conductivity and radiative cooling performance.
[0047] 5. This invention can be widely applied in fields such as electronic devices, building energy conservation, and outdoor equipment. It is especially suitable for complex service environments with strict requirements for conductivity, corrosion resistance, self-cleaning, radiation cooling, and multi-functional integration. It has significant engineering application value and market promotion prospects.
[0048] It should be noted that the technical contribution of this invention does not lie in pursuing optimal single radiative cooling performance. While graphene-free TiO2 / PVDF coatings can achieve superior cooling effects, their conductivity is severely insufficient, failing to meet the requirements for antistatic and conductive applications. This invention, through Ba ion doping modification within a system that incorporates graphene to construct a conductive network, achieves a synergistic balance among conductivity, solar reflectivity, and 8~13μm infrared emissivity. This results in an integrated composite coating that simultaneously possesses conductivity, antistatic properties, superhydrophobic self-cleaning capabilities, and radiative thermal management, adapting to the multifunctional requirements of complex outdoor service scenarios. Attached Figure Description
[0049] Figure 1 This is a scanning electron microscope (SEM) image of the Ba ion-doped TiO2 / graphene composite functional powder obtained in this invention.
[0050] Figure 2 This is a transmission electron microscope (TEM) image of the Ba ion-doped TiO2 / graphene composite functional powder obtained in this invention.
[0051] Figure 3 This is a schematic diagram of the conductive pathway formation mechanism in the multifunctional composite coating of the present invention;
[0052] Figure 4 For TiO2 / G samples and Ba 2+ Comparison of O1s high-resolution X-ray photoelectron spectroscopy (XPS) spectra of TiO2 / G samples;
[0053] Figure 5 For TiO2 / G samples and Ba 2+Comparison of C1s high-resolution X-ray photoelectron spectroscopy (XPS) spectra of TiO2 / G samples;
[0054] Figure 6 TiO2, Ba 2+ -TiO2, TiO2 / G, Ba 2+ - Comparison of Raman spectra of TiO2 / G samples;
[0055] Figure 7 For TiO2 / G samples and Ba 2+ Comparison of electron paramagnetic resonance (EPR) spectra of TiO2 / G samples;
[0056] Figure 8 This is a schematic diagram of the radiation cooling and superhydrophobic mechanism of the multifunctional composite coating of the present invention;
[0057] Figure 9 The bar chart shows the electrical conductivity comparison of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3; where a: volume resistivity; b: electrical conductivity.
[0058] Figure 10 The graph shows a comparison of the water contact angle and sliding angle of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3.
[0059] Figure 11 Mid-infrared reflectance curves for Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0060] Figure 12 Emissivity curves for Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0061] Figure 13 The graphs show the temperature-time variation curves of the back side of Examples 1, 1, 2 and 3 under outdoor sunlight conditions. Detailed Implementation
[0062] The present invention will now be described in detail through specific embodiments. These embodiments are provided to enable a more thorough understanding of the invention and to fully convey the scope of the invention to those skilled in the art. As used throughout the specification and claims, the terms "comprising" or "including" are open-ended and are interpreted as "comprising but not limited to". The following description is a preferred embodiment for carrying out the invention; however, this description is intended to illustrate the general principles of the specification and is not intended to limit the scope of the invention. The scope of protection of the invention is determined by the appended claims. Unless otherwise specified, all reagents and materials used in the present invention are commercially available.
[0063] Example 1
[0064] A method for preparing a barium-doped titanium dioxide / graphene / PVDF multifunctional composite coating includes the following steps:
[0065] (1) Measure 50 mL of anhydrous ethanol and 50 mL of deionized water to prepare a mixed solvent with an ethanol / water volume ratio of 1:1. Weigh 0.14 g of graphene oxide and add it to the above 100 mL mixed solvent. First, stir at 600 r·min -1 Mechanical stirring for 30 min, followed by ultrasonic dispersion using a 300 W ultrasonic power device for 60 min. During ultrasonication, intermittent operation was used, and the temperature of the dispersion was controlled below 30 °C using a water bath or ice bath, yielding a mass concentration of 1.4 mg·mL⁻¹. -1 Graphene oxide dispersion.
[0066] (2) Weigh 8.52 g of tetrabutyl titanate, which is approximately 0.025 mol. Heat at 800 r·min -1 Under stirring conditions, tetrabutyl titanate was added at a rate of 1.0 mL / min. -1 The solution is slowly added dropwise to the graphene oxide dispersion obtained in step (1).
[0067] Weigh out 0.320 g of anhydrous barium acetate, approximately 0.00125 mol, according to a Ba / Ti molar ratio of 5%. Dissolve the barium acetate in a small amount of deionized water beforehand, then slowly add it to the above mixture. After the addition is complete, accelerate at 600 r·min⁻¹. -1 Continue stirring for 4 hours to allow the titanium and barium sources to fully hydrolyze and condense, forming a uniform precursor on the surface of the graphene oxide sheets.
[0068] (3) Transfer the mixture obtained in step (2) to a 150 mL polytetrafluoroethylene-lined hydrothermal reactor, ensuring the reaction volume does not exceed 80% of the reactor's effective volume. Place the reactor in an oven and maintain the temperature at 180 °C for 24 h. After the reaction is complete, allow it to cool naturally to room temperature and then reheat it at 8000 r·min. -1 Centrifuge for 10 min and collect the solid product. Wash three times with deionized water and anhydrous ethanol, and then vacuum dry at 60 °C for 12 h to obtain the Ba-doped TiO2 / graphene precursor.
[0069] (4) The precursor obtained in step (3) is placed in a tube furnace and heat-treated under a nitrogen atmosphere. The nitrogen flow rate is controlled at 150 mL / min. -1 , at 2 ℃·min -1The temperature was increased to 450 °C at a heating rate, held for 2 h, and then naturally cooled to room temperature under nitrogen protection. The heat-treated product was ground and passed through a 200-mesh sieve to obtain Ba ion-doped TiO2 / graphene composite functional powder.
[0070] (5) Weigh 1.40 g of PVDF and add it to 12.60 g of N,N-dimethylformamide, and incubate at 60 °C with a flow rate of 500 r·min. -1 Stir for 4 hours to fully dissolve the PVDF, obtaining a PVDF slurry with a PVDF mass concentration of 10%. Weigh 2.10 g of the Ba ion-doped TiO2 / graphene composite functional powder obtained in step (4) and slowly add it to the above PVDF slurry. In this embodiment, the mass ratio of the composite functional powder to PVDF is:
[0071]
[0072] Based on the mass of the solid components in the coating, the composite functional powder accounts for 60% and PVDF accounts for 40%.
[0073] The mixing system was first subjected to 800 r·min -1 Mechanical stirring for 30 min, followed by ultrasonic dispersion at 300 W for 30 min, with the slurry temperature controlled to not exceed 35 ℃ during ultrasonication. Subsequently, ball milling was performed using a planetary ball mill at a speed of 300 r·min. -1 The ball milling time was 2 hours, and the ball-to-material mass ratio was 5:1. Intermittent ball milling was used, with a 5-minute pause after every 15 minutes of milling to avoid excessively high slurry temperature, ultimately resulting in a uniformly dispersed composite coating slurry.
[0074] (6) The composite coating slurry obtained in step (5) was degassed under vacuum for 15 min, and then coated onto a clean glass, aluminum plate, or polyester film substrate using a scraping method. The wet film thickness was controlled to be 300 μm. After coating, the coating was leveled at room temperature for 30 min, then pre-dried at 60 ℃ for 2 h, and then vacuum dried at 80 ℃ for 8 h to fully remove N,N-dimethylformamide. Finally, the coating was heat-treated at 100 ℃ for 2 h and cooled to room temperature to obtain a Ba ion-doped TiO2 / graphene / PVDF multifunctional composite coating.
[0075] Comparative Example 1
[0076] A method for preparing a graphene / PVDF composite coating includes the following steps:
[0077] (1) Measure 50 mL of anhydrous ethanol and 50 mL of deionized water to prepare a mixed solvent with an ethanol / water volume ratio of 1:1. Weigh 0.20 g of graphene oxide and add it to the above 100 mL mixed solvent. First, stir at 600 r·min-1 Mechanical stirring for 30 min, followed by ultrasonic dispersion using a 300 W ultrasonic power device for 60 min. During ultrasonication, the temperature of the dispersion was controlled below 30 ℃ using a water bath or ice bath to obtain a uniform graphene oxide dispersion.
[0078] (2) The graphene oxide dispersion obtained in step (1) was transferred to a 150 mL polytetrafluoroethylene-lined hydrothermal reactor and reacted at 180 °C for 24 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature and then reacted at 8000 r·min. -1 Centrifuge for 10 min and collect the solid product. Wash three times with deionized water and anhydrous ethanol, respectively, and then vacuum dry at 60 °C for 12 h to obtain the hydrothermally treated graphene precursor.
[0079] (3) The graphene precursor obtained in step (2) was placed in a tube furnace and heat-treated under a nitrogen atmosphere. The nitrogen flow rate was controlled at 150 mL / min. -1 , at 2 ℃·min -1 The temperature was increased to 450 °C at a heating rate, held for 2 h, and then naturally cooled to room temperature under nitrogen protection. The resulting product was ground and passed through a 200-mesh sieve to obtain heat-treated graphene powder.
[0080] This step uses the same hydrothermal and heat treatment conditions as in Example 1 to reduce the impact of different heat treatment histories on the graphene structure and conductivity.
[0081] (4) Weigh 1.40 g of PVDF and add it to 12.60 g of N,N-dimethylformamide, and incubate at 60 °C with a flow rate of 500 r·min. -1 Stir for 4 hours to fully dissolve PVDF, resulting in a PVDF slurry with a PVDF mass concentration of 10%.
[0082] (5) Weigh 0.14 g of the heat-treated graphene powder obtained in step (3) and add it to the PVDF slurry obtained in step (4). In this comparative example, the mass ratio of graphene to PVDF is:
[0083]
[0084] The mixing system was first subjected to 800 r·min -1 Mechanical stirring for 30 min, followed by ultrasonic dispersion at 300 W for 30 min, with the slurry temperature controlled to not exceed 35 ℃ during ultrasonication. Subsequently, ball milling was performed using a planetary ball mill at a speed of 300 r·min. -1The ball milling time was 2 hours, and the ball-to-material mass ratio was 5:1. Intermittent ball milling was used, with a 5-minute pause after every 15 minutes of milling, to obtain a uniformly dispersed graphene / PVDF composite coating slurry.
[0085] (6) The composite coating slurry obtained in step (5) is degassed under vacuum for 15 min, and then coated onto a clean glass, aluminum plate or polyester film substrate by scraping. The wet film thickness is controlled to be 300 μm. After coating, it is leveled at room temperature for 30 min, then pre-dried at 60 ℃ for 2 h, and then vacuum dried at 80 ℃ for 8 h to fully remove N,N-dimethylformamide. Finally, it is heat-treated at 100 ℃ for 2 h and cooled to room temperature to obtain a graphene / PVDF composite coating.
[0086] Comparative Example 2
[0087] A method for preparing a titanium dioxide / PVDF composite coating includes the following steps:
[0088] (1) Measure 50 mL of anhydrous ethanol and 50 mL of deionized water. Weigh 8.95 g of tetrabutyl titanate, about 0.0263 mol, and dissolve it in 50 mL of anhydrous ethanol to obtain a tetrabutyl titanate ethanol solution.
[0089] At 800 r·min -1 Under mechanical stirring conditions, the tetrabutyl titanate ethanol solution was stirred at a rate of 1.0 mL / min. -1 Slowly add the solution dropwise to 50 mL of deionized water at a rate of 600 r·min. After the addition is complete, accelerate the reaction at 600 r·min. -1 Continue stirring for 4 hours, then treat with an ultrasonic dispersion device with an ultrasonic power of 300 W for 60 minutes. During the ultrasonication process, use a water bath or ice bath to control the system temperature below 30 °C to obtain a homogeneous TiO2 precursor mixture. Theoretically, 8.95 g of tetrabutyl titanate can generate approximately 2.10 g of TiO2.
[0090] (2) Transfer the mixture obtained in step (1) to a 150 mL polytetrafluoroethylene-lined hydrothermal reactor, with the volume of the reaction liquid not exceeding 80% of the effective volume of the reactor. Place the reactor in an oven and keep it at 180 °C for 24 h.
[0091] After the reaction is complete, allow it to cool naturally to room temperature, then spray at 8000 r·min -1 Centrifuge for 10 min and collect the solid product. Wash three times with deionized water and anhydrous ethanol, respectively, and then dry under vacuum at 60 °C for 12 h to obtain the TiO2 precursor.
[0092] (3) The TiO2 precursor obtained in step (2) is placed in a tube furnace and heat-treated under a nitrogen atmosphere. The nitrogen flow rate is controlled at 150 mL·min. -1 , at 2 ℃·min -1 The temperature was increased to 450 °C at a heating rate, held for 2 h, and then naturally cooled to room temperature under nitrogen protection.
[0093] The heat-treated product was ground and passed through a 200-mesh sieve to obtain TiO2 functional powder.
[0094] (4) Weigh 1.40 g of PVDF and add it to 12.60 g of N,N-dimethylformamide, and incubate at 60 °C with a flow rate of 500 r·min. -1 Stir for 4 hours to fully dissolve PVDF, resulting in a PVDF slurry with a PVDF mass concentration of 10%.
[0095] (5) Weigh 2.10 g of the TiO2 functional powder obtained in step (3) and slowly add it to the PVDF slurry obtained in step (4). In this comparative example, the mass ratio of TiO2 functional powder to PVDF is:
[0096]
[0097] Based on the mass of the solid components in the coating, the content of TiO2 functional powder is 60%, and the content of PVDF is 40%. The mixture was first subjected to a flow rate of 800 r·min⁻¹. -1 Mechanical stirring for 30 min, followed by ultrasonic dispersion at 300 W for 30 min, with the slurry temperature controlled to not exceed 35 ℃ during ultrasonication. Subsequently, ball milling was performed using a planetary ball mill at a speed of 300 r·min. -1 The ball milling time was 2 hours, and the ball-to-material mass ratio was 5:1. Intermittent ball milling was used, with a 5-minute pause after every 15 minutes of milling, to obtain a uniformly dispersed TiO2 / PVDF composite coating slurry.
[0098] (6) The composite coating slurry obtained in step (5) is degassed under vacuum for 15 min, and then coated onto a clean glass, aluminum plate or polyester film substrate by scraping. The wet film thickness is controlled to be 300 μm. After coating, it is leveled at room temperature for 30 min, then pre-dried at 60 ℃ for 2 h, and then vacuum dried at 80 ℃ for 8 h to fully remove N,N-dimethylformamide; finally, it is heat-treated at 100 ℃ for 2 h and cooled to room temperature to obtain TiO2 / PVDF composite coating.
[0099] Comparative Example 3
[0100] A method for preparing a titanium dioxide / graphene / PVDF composite coating includes the following steps:
[0101] (1) Measure 50 mL of anhydrous ethanol and 50 mL of deionized water to prepare a mixed solvent with an ethanol / water volume ratio of 1:1. Weigh 0.14 g of graphene oxide and add it to the above 100 mL mixed solvent. First, stir at 600 r·min -1 Mechanical stirring for 30 min, followed by ultrasonic dispersion using a 300 W ultrasonic power device for 60 min. During ultrasonication, the dispersion temperature was maintained below 30 °C using a water bath or ice bath, yielding a concentration of 1.4 mg / mL. -1 Graphene oxide dispersion.
[0102] (2) Weigh 8.52 g of tetrabutyl titanate, which is approximately 0.025 mol. Heat at 800 r·min -1 Under stirring conditions, tetrabutyl titanate was added at a rate of 1.0 mL / min. -1 The solution was slowly added dropwise to the graphene oxide dispersion obtained in step (1). After the addition was complete, the solution was accelerated at 600 r·min. -1 Continue stirring for 4 hours to allow tetrabutyl titanate to fully hydrolyze and condense, forming a TiO2 precursor on the surface of the graphene oxide sheets, thus obtaining a TiO2 / graphene oxide precursor mixture.
[0103] In this comparative example, the mass ratio of graphene oxide to tetrabutyl titanate is:
[0104]
[0105] Theoretically, 8.52 g of tetrabutyl titanate can generate about 2.00 g of TiO2. Therefore, the amount of graphene oxide added is 7% of the theoretical product mass of TiO2.
[0106] (3) Transfer the mixture obtained in step (2) to a 150 mL polytetrafluoroethylene-lined hydrothermal reactor, with the volume of the reaction liquid not exceeding 80% of the effective volume of the reactor. Place the reactor in an oven and keep it at 180 °C for 24 h.
[0107] After the reaction is complete, allow it to cool naturally to room temperature, then spray at 8000 r·min -1 Centrifuge for 10 min and collect the solid product. Wash three times with deionized water and anhydrous ethanol, respectively, and then vacuum dry at 60 °C for 12 h to obtain the TiO2 / graphene precursor.
[0108] (4) The TiO2 / graphene precursor obtained in step (3) was placed in a tube furnace and heat-treated under a nitrogen atmosphere. The nitrogen flow rate was controlled at 150 mL·min. -1 , at 2 ℃·min -1The temperature was increased to 450 °C at a heating rate, held for 2 h, and then naturally cooled to room temperature under nitrogen protection. The heat-treated product was ground and passed through a 200-mesh sieve to obtain TiO2 / graphene composite functional powder.
[0109] (5) Weigh 1.40 g of PVDF and add it to 12.60 g of N,N-dimethylformamide, and incubate at 60 °C with a flow rate of 500 r·min. -1 Stir for 4 hours to fully dissolve PVDF, resulting in a PVDF slurry with a PVDF mass concentration of 10%.
[0110] (6) Weigh 2.10 g of the TiO2 / graphene composite functional powder obtained in step (4) and slowly add it to the PVDF slurry obtained in step (5). In this comparative example, the mass ratio of TiO2 / graphene composite functional powder to PVDF is:
[0111]
[0112] Based on the mass of the solid components in the coating, the TiO2 / graphene composite functional powder content is 60%, and the PVDF content is 40%. The mixture was first subjected to a flow rate of 800 r·min⁻¹. -1 Mechanical stirring for 30 min, followed by ultrasonic dispersion at 300 W for 30 min, with the slurry temperature controlled to not exceed 35 ℃ during ultrasonication. Subsequently, ball milling was performed using a planetary ball mill at a speed of 300 r·min. -1 The ball milling time was 2 hours, and the ball-to-material mass ratio was 5:1. Intermittent ball milling was used, with a 5-minute pause after every 15 minutes of milling, to obtain a uniformly dispersed TiO2 / graphene / PVDF composite coating slurry.
[0113] (7) The composite coating slurry obtained in step (6) is degassed under vacuum for 15 min, and then coated onto a clean glass, aluminum plate or polyester film substrate by scraping. The wet film thickness is controlled to be 300 μm. After coating, it is leveled at room temperature for 30 min, then pre-dried at 60 ℃ for 2 h, and then vacuum dried at 80 ℃ for 8 h to fully remove N,N-dimethylformamide; finally, it is heat-treated at 100 ℃ for 2 h and cooled to room temperature to obtain TiO2 / graphene / PVDF composite coating.
[0114] The Ba ion-doped TiO2 / graphene composite functional powder prepared in Example 1 of this invention was observed using a scanning electron microscope. It can be seen that the Ba ion-doped TiO2 is dispersed in particulate form on the sheets of two-dimensional graphene. Figure 1 As shown in the image. This structure is more conducive to the creation of superhydrophobic structures. Its transmission scanning electron microscope (SEM) image is shown below. Figure 2As shown, Ba ions doped TiO2 are distributed in a spherical shape, while graphene is in a sheet-like shape, corresponding to the scanning microscope.
[0115] The product prepared in this invention introduces lattice distortion and oxygen vacancies into TiO2 through Ba ion doping, reducing the band gap of TiO2 and improving its intrinsic conductivity. Simultaneously, it utilizes graphene to construct a continuous conductive network and forms multi-level conductive pathways through Ti-O-C and Ba-O-C interface bridging structures, thereby significantly enhancing the coating's conductivity. The mechanism is as follows: Figure 3 As shown.
[0116] To further analyze the interfacial chemical structure, lattice changes, and oxygen vacancy states in Ba-doped TiO2 / graphene composite functional powders, the interfacial chemical structure, lattice changes, and oxygen vacancy states of TiO2 / G and Ba were analyzed respectively. 2+ -TiO2 / G samples were tested using XPS, Raman, and EPR methods, and the results are as follows: Figure 4-7 As shown.
[0117] Depend on Figure 4 The high-resolution XPS spectrum of O 1s shown indicates that the O 1s spectrum of the sample can be decomposed into components such as Ti—O—Ti lattice oxygen, oxygen vacancy-related defect oxygen, Ti—O—C interface oxygen, and surface Ti—OH. Compared with undoped TiO2 / G, Ba 2+ The presence of oxygen vacancy-related components in the TiO2 / G sample indicates that Ba ion doping alters the local coordination environment of TiO2 and promotes the formation of lattice defects and oxygen vacancies. Simultaneously, the presence of Ti-O-C related components suggests that the contact between TiO2 nanoparticles and graphene sheets is not a simple physical one, but rather an oxygen-containing interfacial connection structure.
[0118] Depend on Figure 5 The C 1s high-resolution XPS spectrum shown indicates the presence of C—C / C=C bonds, oxygen-containing carbon bonds, and carbon components related to the TiO2 / graphene interface in the sample. Compared to the TiO2 / G sample, Ba... 2+ The changes in the peak shape and relative intensity of the interface-related peaks in the TiO2 / G sample further indicate that Ba doping has a regulatory effect on the electronic environment of the TiO2 / graphene interface. Combined with the Ti-O-C related components in the O 1s spectrum, it can be proved that a relatively tight interfacial connection is formed between the TiO2 nanoparticles and the graphene sheets.
[0119] like Figure 6 As shown, TiO2's The characteristic vibration peak is located at approximately 144.85 cm. -1 After Ba doping, this characteristic peak shifted to approximately 145.51 cm⁻¹. -1 The characteristic peak of the composite TiO2 and graphene is located at approximately 145.26 cm⁻¹. -1 Ba2+ The TiO2 / G sample further shifted to approximately 146.42 cm⁻¹. -1 The continuous shift of the characteristic peaks indicates that Ba ion doping and the graphene interface altered the local vibrational environment of the TiO2 lattice, reflecting the lattice distortion caused by Ba doping and the interfacial coupling between TiO2 and graphene.
[0120] like Figure 7 As shown, TiO2 / G and Ba 2+ -TiO2 / G samples were all in An EPR characteristic signal was observed nearby, which can be attributed to a defect center formed by electron trapping from an oxygen vacancy. Ba 2+ The EPR signal intensity of the -TiO2 / G sample was significantly higher than that of the TiO2 / G sample, indicating that Ba ion doping increased the oxygen vacancy concentration in TiO2. Oxygen vacancies can form defect energy levels and provide electron migration sites, which is beneficial for reducing the electron transport resistance between TiO2 particles.
[0121] The combined XPS, Raman, and EPR results show that Ba doping induces lattice distortion and increases oxygen vacancy concentration in TiO2, while also modulating the local electronic structure at the TiO2 / graphene interface. The Ti-O-C interface connections, oxygen vacancy defect transport pathways, and the conductive network of the graphene sheets work together to provide multi-scale channels for electron transport in the composite functional powder. The cassie structure constructed on the coating surface further enhances the coating's hydrophobicity. Simultaneously, the large number of CF bonds within PVDF also improves the coating's hydrophobicity, as illustrated in the following diagram: Figure 8 As shown.
[0122] Performance Testing and Comparison
[0123] (1) Conductivity test: Coated samples of Examples 1, Comparative Examples 1-3, and pure PVDF were prepared with basically the same size and thickness. The sheet resistance of each sample was tested using a four-probe resistance meter, and the actual dry film thickness of the sample was measured using a thickness gauge. At least 5 different locations were randomly selected for testing each sample, and the average value was taken as the test result. The volume resistivity was calculated based on the sheet resistance and coating thickness:
[0124]
[0125] In the formula, The volume resistivity of the coating is expressed in Ω·cm. The sheet resistance is expressed in Ω / □. The dry film thickness of the coating is given in cm. The coating conductivity is calculated using the following formula:
[0126]
[0127] In the formula, Electrical conductivity, measured in S·cm -1 For high-resistivity samples whose resistivity exceeds the effective testing range of the four-probe instrument, a high-resistivity meter is used for auxiliary measurement.
[0128] Test results are as follows Figure 9 As shown in Table 1, the volume resistivity of pure PVDF is 8.85 × 10⁻⁶. 8 Ω·cm, corresponding to a conductivity of only 1.13×10 -9 S·cm -1 This indicates that pure PVDF is essentially an electrically insulating material. After introducing TiO2, the volume resistivity of Comparative Example 2 decreased to 2.89 × 10⁻⁶. 6 The conductivity increased to 3.46 × 10⁻⁶ Ω·cm. -7 S·cm -1 However, an effective continuous electronic transmission network has not yet been formed.
[0129] After the addition of graphene, the volume resistivity of Comparative Example 3 decreased significantly to 6.46 × 10⁻⁶. -1 The conductivity increased to 1.55 S·cm. -1 This result demonstrates that the graphene sheets form interconnected electron transport channels within the PVDF matrix, resulting in an order-of-magnitude improvement in the coating's conductivity.
[0130] The volume resistivity of Example 1 further decreased to 3.14 × 10⁻⁶. -1 The electrical conductivity reaches 3.18 S·cm (Ω·cm). -1 Compared to Comparative Example 3, the conductivity increased to approximately 2.05 times (while the volume resistivity decreased to approximately 1 / 2.06). Combined with XPS, Raman, and EPR results, it can be seen that Ba doping-induced lattice distortion and oxygen vacancies increased the defect electron migration sites in TiO2; simultaneously, the Ti-O-C interface improved the Ba... 2+ - Interfacial charge transport between TiO2 nanoparticles and graphene sheets. Therefore, the oxygen vacancy transport pathway, the TiO2 / graphene interface, and the conductive network of the graphene sheets collectively reduce the resistivity of the composite coating.
[0131] Comparative Example 1 shows a graphene / PVDF coating with low filler content, whose volume resistivity is 1.12 × 10⁻⁶. -1 Ω·cm, corresponding to a conductivity of 8.93 S·cm -1Comparative Example 1 contains only graphene as a functional filler, achieving a high level of conductivity. However, its total filler mass and filler composition differ from Example 1. Therefore, this application does not conduct a quantitative comparison of its conductivity performance with Example 1. The purpose of Comparative Example 1 is solely to qualitatively reveal the inherent defects of the pure graphene / PVDF system: relying solely on graphene to achieve high conductivity leads to a strong solar absorption effect, which is detrimental to radiative cooling applications. This invention evaluates the performance gain brought about by Ba ion doping modification, with the comparison between Example 1 and Comparative Example 3 as the core basis. The conductivity of Example 1 reaches 3.18 S·cm. -1 It has good conductivity and antistatic properties, meeting the practical application requirements for conductivity and antistatic properties.
[0132] Table 1. Resistivity and conductivity of the samples
[0133]
[0134] Preparation method of pure PVDF: The same glass as in Example 1 was selected as the substrate. The substrate surface was cleaned sequentially with deionized water and anhydrous ethanol to remove surface dust and oil, and then dried at 60 °C for 30 min for later use. 1.40 g of polyvinylidene fluoride was weighed and added to 12.60 g of N,N-dimethylformamide, and the mixture was heated at 60 °C at 500 r·min. -1 Mechanical stirring for 4 hours was performed to fully dissolve the PVDF, resulting in a transparent and uniform PVDF slurry. The remaining steps were the same as in Example 1.
[0135] (2) Contact angle test
[0136] The surface wetting properties of Examples 1, Comparative Examples 1-3, and the pure PVDF coating were tested using an optical contact angle meter. The contact angle meter was an OCA 25 model (DataPhysics Instruments, Germany), equipped with an automatic sample introduction system, a side-view imaging system, and a programmable tilting sample stage. Before testing, each coating sample was cut into identical specimens and equilibrated in an environment with a temperature of 23±2 °C and a relative humidity of 50%±5% for at least 2 hours.
[0137] For the water contact angle test, 5 μL of deionized water was slowly dropped onto the coating surface using a microsyringe. After the droplet had been in contact with the coating surface and stabilized for 3 seconds, a side view image of the droplet was acquired. The Young-Laplace method was used to fit the droplet profile, obtaining the contact angles on the left and right sides of the droplet. The average of the two contact angles was taken as the water contact angle at that test location. For each sample, at least five non-overlapping locations were randomly selected for testing, with a minimum distance of 5 mm between adjacent test locations. The final result was expressed as the arithmetic mean of the five test results.
[0138]
[0139] In the formula, is the average water contact angle of the sample, is the th water contact angle measured at the position, is the number of test positions, which in this embodiment .
[0140] The sliding angle test is carried out using a programmable tilting sample stage matched with a contact angle measuring instrument. 10 μL of deionized water is dropped onto the horizontally placed coating surface, and after standing for 5 s, the sample stage is tilted at a constant speed of 1°·s -1 . When the water droplet starts to move continuously and the moving distance exceeds 2 mm, the included angle between the sample stage and the horizontal plane at this time is recorded, and is taken as the water droplet sliding angle. Each sample is tested at no less than 5 different positions, and the arithmetic mean value is taken:
[0141]
[0142] In the formula, is the average sliding angle, is the th sliding angle measured at the position.
[0143] The test results are shown in Figure 10 . The average water contact angle of the pure PVDF coating is 111.15°, and the sliding angle is 45.3°. The C—F bonds in PVDF endow it with low surface energy, thus showing certain hydrophobicity; however, the surface of the pure PVDF coating is relatively flat, the actual contact area between the water droplet and the coating is large, and the interfacial pinning effect on the water droplet is strong, resulting in a high sliding angle.
[0144] The TiO₂ / PVDF coating of Comparative Example 2 has a water contact angle of 116.62° and a sliding angle of 38.2°. The addition of TiO₂ particles increases the surface roughness of the coating, slightly increasing the water contact angle compared with pure PVDF. However, the single TiO₂ particles have not formed a sufficient micro-nano composite rough structure, and the oxygen-containing groups on the TiO₂ surface have a certain interfacial effect on water droplets, so its sliding angle is still relatively high.
[0145] The water contact angle of the graphene / PVDF coating of Comparative Example 1 is increased to 130.22°, and the sliding angle is reduced to 27.1°. The low-polarity surface of the graphene sheets and the layered undulating structure formed in the PVDF matrix reduce the effective contact area between the water droplet and the coating, thereby improving the hydrophobicity of the coating and reducing the adhesion of water droplets.
[0146] In Comparative Example 3, the water contact angle of the TiO2 / graphene / PVDF coating was further increased to 141.02°, while the sliding angle was reduced to 16.2°. These results demonstrate that TiO2 nanoparticles and graphene sheets can synergistically construct a rough structure combining particle protrusions and sheet undulations, trapping some air between the water droplet and the coating, reducing the solid-liquid contact ratio, and thus giving the coating higher hydrophobicity.
[0147] Ba in Example 1 2+ The TiO2 / graphene / PVDF composite coating exhibits the highest water contact angle and the lowest sliding angle, with an average water contact angle of 154.33° and an average sliding angle of only 6.3°. The water contact angle is greater than 150° and the sliding angle is less than 10°, indicating that Example 1 possesses typical low-adhesion superhydrophobic characteristics.
[0148] This performance is mainly attributed to the regulation of TiO2 crystal growth and particle dispersion state by Ba doping, enabling Ba... 2+ -TiO2 nanoparticles can be more uniformly loaded onto graphene sheets, forming a multi-level rough structure composed of nanoparticles, sheet undulations, and micron-sized particle clusters within the PVDF matrix. This structure can trap air beneath the water droplet, keeping the droplet primarily in a Cassie-Baxter composite contact state, significantly reducing the actual contact area between the water droplet and the solid surface. Simultaneously, the low surface energy of PVDF further weakens the interfacial interaction between the water droplet and the coating. Therefore, Example 1 not only exhibits a large static water contact angle but also low droplet sliding resistance, demonstrating excellent water repellency, low adhesion, and potential self-cleaning properties.
[0149] (3) Reflectivity test
[0150] The spectral reflectance of Example 1, Comparative Examples 1-3, and the pure PVDF coating was measured using a UV-Vis-NIR spectrophotometer. The testing instrument was a LAMBDA 1050+ UV-Vis-NIR spectrophotometer (PerkinElmer, USA), equipped with a diffuse reflectance integrating sphere accessory with a diameter of 150 mm.
[0151] The test wavelength range is 300–2500 nm, the spectral sampling interval is 2 nm, the spectral bandwidth is 5 nm, and the scan rate is 600 nm·min. -1 The test employed a near-normal incident integrating sphere reflectance measurement mode with an incident angle of approximately 8°. The specular reflection port remained closed, meaning the SCI mode, which includes specular reflection, was used to measure the total hemispherical reflectance of the coating, comprising both specular and diffuse reflection. Prior to testing, a calibrated Spectralon standard white board was used for 100% reflectance baseline correction.
[0152] All coating samples used the same substrate material, and the dry film thickness was controlled within the same range. At least three different locations were randomly selected for testing each sample, and the test was repeated three times at each location. The average spectrum was taken as the final reflectance spectrum of the sample.
[0153] Spectral reflectance was tested according to the method specified in ASTM E903-20, and the spectral reflectance in the range of 300–2500 nm was weighted using the AM1.5G standard solar spectral irradiance specified in ASTM G173-23. ASTM E903-20 is applicable to determining the spectral reflectance of materials and calculating solar weighted optical parameters using an integrating sphere, while ASTM G173-23 provides the corresponding standard solar spectral weights.
[0154] The solar spectral weighted reflectance is calculated according to the following formula:
[0155]
[0156] In the formula:
[0157] The solar spectral weighted reflectance is in the range of 300–2500 nm.
[0158] For coating at wavelength Spectral reflectance at;
[0159] The standard solar spectral irradiance is AM1.5G as specified in ASTM G173-23.
[0160] Wavelength, in nm.
[0161] Test results are as follows Figure 11As shown, none of the samples exhibited obvious sharp reflection peaks in the 300–2500 nm range, showing a relatively smooth broad-band reflection characteristic overall. However, significant differences in reflectivity were observed among the different coating compositions. The TiO2 / PVDF coating of Comparative Example 2 exhibited the highest solar spectral reflectivity, maintaining approximately 90%–93% across most of the tested wavelengths. TiO2 has a high refractive index, creating a large refractive index difference with the PVDF matrix, resulting in strong interfacial scattering. Furthermore, this coating does not contain graphene, which has broad-band absorption characteristics, thus exhibiting the highest solar reflectivity. The pure PVDF coating showed a reflectivity of approximately 77%–84% in the tested wavelength range. PVDF itself has relatively weak absorption of visible and near-infrared light; its semi-crystalline structure, internal pores, and polymer-air interface can generate some light scattering, resulting in a moderate level of solar reflectivity. The graphene / PVDF coating of Comparative Example 1 had the lowest reflectivity, approximately 32%–37% in the 300–2500 nm range. This is because graphene has strong absorption capabilities in the visible and near-infrared broadband bands, and its sheets form a continuous light-absorbing structure in the PVDF matrix, significantly increasing the coating's absorption of solar radiation. This result indicates that although graphene can significantly improve the conductivity of the coating, using graphene alone will significantly reduce its solar reflectivity, which is detrimental to passive radiative cooling during the day. The reflectivity of the TiO2 / graphene / PVDF coating in Comparative Example 3 increased to approximately 70%–77%. The introduction of TiO2 nanoparticles increased the refractive index mismatch interface within the coating, causing multiple scatterings of sunlight between the TiO2 particles, graphene sheets, and the PVDF matrix, which to some extent weakened the light absorption caused by graphene. However, due to limitations in the dispersion and interface structure of undoped TiO2 particles in the graphene sheets and PVDF matrix, its reflectivity is still lower than that of pure PVDF and Comparative Example 2. Example 1's Ba... 2+ The TiO2 / graphene / PVDF coating maintains a reflectivity of approximately 88%–91% in the 300–2500 nm range, only slightly lower than the TiO2 / PVDF coating without graphene, and significantly higher than the TiO2 / graphene / PVDF coating. Ba doping alters the crystal growth and particle aggregation state of TiO2, making Ba… 2+ -TiO2 particles can be more uniformly loaded onto graphene sheets and dispersed in the PVDF matrix, increasing the number of optical interfaces and multiple scattering paths within the coating. 2+ - The coverage of graphene sheets by TiO2 particles can also reduce the broadband absorption effect of graphene to a certain extent.
[0162] Therefore, although Example 1 has a slightly lower reflectivity than the TiO2 / PVDF coating due to the presence of graphene, it still maintains a high level of solar reflectivity. Combined with its 3.18 S·cm...-1 As can be seen from the conductivity, Example 1 achieves a good balance between solar reflectivity and electrical conductivity, overcoming the inherent technical contradiction of pure graphene-based composite coatings that "if high conductivity is pursued, strong solar absorption will occur, which is not conducive to radiative cooling".
[0163] (4) Emissivity test
[0164] Fourier transform infrared (FTIR) spectrometry with a gold-plated integrating sphere was used to measure the mid-infrared reflectance spectra of Example 1, Comparative Examples 1-3, and the pure PVDF coating in the wavelength range of 5–22 μm. Before testing, the samples were equilibrated in an environment with a temperature of (23±2)℃ and a relative humidity of (50±5)% for at least 24 h. The test employed a near-normal incidence method with an incident angle of 8°, and the integrating sphere collected the specular and diffuse reflectance signals of the samples; the spectral resolution was 4 cm⁻¹. -1 Each sample was scanned 32 or 64 times and the average value was taken. At least three different locations were selected for testing for each sample, and the average value of the test results at each location was taken as the spectral reflectance of the sample.
[0165] Prior to testing, a calibrated gold-plated mirror was used for background and 100% reflectance baseline calibration. Since each coating is prepared on an infrared-blocking substrate surface, and the transmittance of the coating within the test wavelength band can be approximated as zero, that is:
[0166]
[0167] According to the law of conservation of energy and Kirchhoff's law of thermal radiation, the spectral emissivity of the sample is calculated using the following formula:
[0168]
[0169] In the formula, wavelength Spectral emissivity at that location For spectral absorbance, The total reflectance measured by the integrating sphere. denoted as spectral transmittance.
[0170] The average infrared emissivity of the coating in the 8–13 μm atmospheric window was calculated using a weighted average of the 300 K Planck blackbody radiation spectrum.
[0171]
[0172] in, , For temperature The spectral radiance of the Planck blackbody under the given conditions.
[0173] Test results are as follows Figure 12As shown, all coatings exhibited strong infrared emission capabilities within the 8–13 μm atmospheric window range, with TiO2 / PVDF, graphene / PVDF, TiO2 / graphene / PVDF, and Ba... 2+ The average infrared emissivity of the TiO2 / graphene / PVDF coatings were 0.88, 0.82, 0.90, and 0.94, respectively. The pure PVDF coating also exhibited high infrared emissivity in this band.
[0174] Depend on Figure 12 As can be seen, the graphene / PVDF coating of Comparative Example 1 exhibits relatively low emissivity in the 8–13 μm range, with an average value of 0.82. This may be due to the strong broadband light absorption characteristics of the graphene sheets, but their stacking in the PVDF matrix reduces the effective exposure of some infrared vibrational groups, thus limiting their spectral emission capability within the atmospheric window.
[0175] The TiO2 / PVDF coating in Comparative Example 2 showed an average infrared emissivity of 0.88, indicating that the infrared vibrational response of the TiO2 particles and the PVDF matrix can improve the coating's absorption of mid-infrared radiation. The TiO2 / graphene / PVDF coating in Comparative Example 3 further increased its average infrared emissivity to 0.90, demonstrating that the composite structure formed by the TiO2 nanoparticles and graphene sheets can increase the propagation path of infrared radiation within the coating and improve the effective absorption rate of the coating in the 8–13 μm range.
[0176] Ba in Example 1 2+ The TiO2 / graphene / PVDF coating exhibited the highest spectral emissivity in the 8–13 μm range, with an average emissivity of 0.94, and was generally higher than other samples in the approximately 9–13 μm band. This indicates a good synergistic effect between Ba-doped TiO2, graphene, and PVDF. Ba doping can regulate the crystal growth, particle size, and dispersion state of TiO2 particles, making Ba... 2+ - TiO2 nanoparticles are more uniformly loaded onto graphene sheets, forming a multi-scale rough structure. This structure can extend the propagation path of infrared radiation within the coating, enhancing multiple reflections and absorptions; according to Kirchhoff's law of thermal radiation, the increase in absorptivity corresponds to an increase in emissivity. Simultaneously, the C-F, CF2, and C-C chemical bonds in PVDF exhibit strong vibrational responses in the mid-infrared band, further enhancing the coating's infrared radiation capability within the 8–13 μm atmospheric window.
[0177] Therefore, while maintaining conductivity and superhydrophobicity, Example 1 also has a high atmospheric window infrared emissivity, which is beneficial for releasing the heat absorbed by the coating to the outside world through mid-infrared radiation, thereby improving its passive radiative cooling performance.
[0178] (5) Outdoor temperature test
[0179] Test samples of 5 cm × 5 cm were prepared from Examples 1, Comparative Examples 1-3, and the blank substrate. The substrate material, coating area, coating thickness, and surface orientation of each coating were kept consistent. The samples were horizontally fixed on polystyrene insulation foam boards with a thickness of not less than 20 mm, and the spacing between adjacent samples was kept consistent to reduce the influence of substrate thermal conductivity and heat exchange between samples on the test results.
[0180] Place a T-type or K-type thermocouple firmly against the center of the back of each sample and secure it with thermally conductive tape to ensure full contact between the thermocouple and the sample. All thermocouples and connecting wires should be positioned on the back of the sample to avoid direct sunlight. A separate thermocouple with a ventilated radiation shield should be placed at the same height as the sample to measure the air temperature. Before testing, calibrate each thermocouple using a constant-temperature water bath or a standard thermometer to ensure that the temperature deviation between different channels does not exceed ±0.2 ℃.
[0181] The outdoor test was conducted on a clear day with no significant cloud cover, from 9:00 AM to 5:00 PM. A multi-channel temperature recorder was used to record the temperature every minute, and the average of every five consecutive data points was plotted as a temperature-time curve. During the test, a total radiation meter, a thermo-hygrometer, and an anemometer were used to simultaneously record the horizontal solar irradiance, ambient temperature, relative humidity, and wind speed.
[0182] Test results are as follows Figure 13 As shown, as solar irradiance gradually increases, the temperature of each sample begins to rise from the morning and reaches its highest value around 12:30 to 14:00; subsequently, as solar irradiance decreases, the temperature of each sample gradually decreases, and the overall trend is basically consistent with the change in outdoor solar irradiance.
[0183] according to Figure 13 The estimated maximum air temperature near noon is approximately 30.2 ℃. The highest temperature of the graphene / PVDF coating in Comparative Example 1 is approximately 50.0 ℃, significantly higher than other samples, indicating that graphene has a strong ability to absorb sunlight and easily generates significant photothermal heating under solar irradiation. This directly demonstrates the shortcomings of the pure graphene / PVDF system when applied to radiative cooling. The highest temperature of the TiO2 / graphene / PVDF coating in Comparative Example 3 is approximately 40.8 ℃, indicating that the introduction of TiO2 improves the coating's sunlight scattering ability and reduces the photothermal accumulation caused by graphene.
[0184] Ba in Example 1 2+The highest temperature of the TiO2 / graphene / PVDF coating was approximately 35.0 °C, which is about 5.8 °C lower than that of Comparative Example 3. This indicates that Ba-doped TiO2 can further improve the particle dispersion and light scattering ability, and, together with the coating's high 8–13 μm infrared emissivity, reduce heat accumulation caused by solar radiation. Therefore, Example 1 exhibits a significant relative cooling effect.
[0185] However, the highest temperature of the TiO2 / PVDF coating in Comparative Example 2 was approximately 31.8 °C, about 3.2 °C lower than that in Example 1, making it the coating sample with the lowest temperature shown in the figure. This may be because Comparative Example 2 does not contain strongly light-absorbing graphene, resulting in higher solar reflectivity and lower solar energy absorption. Although Example 1 improved solar scattering and mid-infrared emission capabilities through Ba-doped TiO2, the graphene in it still absorbs some solar radiation, thus its outdoor temperature is higher than that of the TiO2 / PVDF coating.
[0186] The outdoor tests were conducted under clear weather conditions from 9:00 AM to 5:00 PM. During the tests, the horizontal solar irradiance ranged from 180 to 950 W·m⁻¹. -2 The maximum solar irradiance at noon is approximately 950 W·m. -2 The air temperature was 25.5–30.2 ℃, the relative humidity was 42%–58%, and the wind speed was 0.4–1.8 m·s. -1 During the test, there was no significant cloud cover, and the solar irradiance first increased and then decreased over time. There were no obstructions around the test platform, and all samples were under the same solar irradiance and environmental heat exchange conditions.
[0187] This invention includes multiple comparative examples to illustrate the technical effects. Comparative Examples 2 and 3 maintain the same total solid content of the functional filler as Example 1 and serve as the core control experimental group for evaluating the technical effects of Ba ion doping. Comparative Example 1 is a graphene / PVDF sample with a low graphene filler content. The total mass and composition of the filler in this group differ from Example 1 and are only used to qualitatively illustrate the inherent technical defect of pure graphene / PVDF materials—"high conductivity but strong solar absorption"—and are not used for quantitative performance comparison with Example 1. The demonstration of the inventive technical effect of this invention uses the performance improvement of Example 1 compared to Comparative Example 3 under the same filler load conditions as core evidence.
[0188] It is understood that the above specific description of the present invention is only for illustrating the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that modifications or equivalent substitutions can still be made to the present invention to achieve the same technical effect; as long as the use needs are met, they are all within the protection scope of the present invention.
Claims
1. A multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF, characterized in that, The composite coating comprises a PVDF matrix and Ba ion-doped TiO2 / graphene composite functional powder dispersed in the PVDF matrix; the Ba ion-doped TiO2 / graphene composite functional powder comprises Ba ion-doped TiO2 nanoparticles and graphene sheets; the Ba ion-doped TiO2 nanoparticles contain oxygen vacancies induced by Ba ion doping, and a Ti-O-C and / or Ba-O-C interface connection structure is formed between the Ba ion-doped TiO2 nanoparticles and the graphene sheets, giving the composite coating conductive, hydrophobic, and radiative cooling functions.
2. The multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF according to claim 1, characterized in that, The molar ratio of Ba / Ti in the Ba ion-doped TiO2 is 1% to 10%.
3. The multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF according to claim 2, characterized in that, The Ba / Ti molar ratio in the Ba ion-doped TiO2 is 3% to 7%.
4. The multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF according to claim 1, characterized in that, The graphene content is 0.5% to 20% of the mass of Ba ion-doped TiO2.
5. The multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF according to claim 1, characterized in that, The average particle size of the Ba ion-doped TiO2 nanoparticles is 10–300 nm.
6. The multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF according to claim 1, characterized in that, Based on the mass of the solid components in the coating, the content of the Ba ion-doped TiO2 / graphene composite functional powder is 10%–80%, the PVDF content is 20%–90%, and the balance is additives; the content of the additives is 0–5%, and the sum of the three is 100%; the additives are selected from one or more of dispersants, film-forming aids, defoamers, and leveling agents.
7. The multifunctional composite coating of barium-doped titanium dioxide / graphene / PVDF according to claim 1, characterized in that, The coating exhibits infrared emission performance in the 8–13 μm atmospheric window band, with a water contact angle of not less than 130° and a sliding angle of not more than 10°.
8. The method for preparing the barium-doped titanium dioxide / graphene / PVDF multifunctional composite coating according to any one of claims 1-7, characterized in that, Includes the following steps: (1) Graphene material is dispersed in a solvent to obtain a graphene dispersion; (2) Add titanium source and barium source to the graphene dispersion, stir and mix, so that titanium source and barium source are hydrolyzed, condensed or deposited on graphene surface; (3) The mixture obtained in step (2) was subjected to a hydrothermal reaction. After the reaction was completed, it was cooled to room temperature, centrifuged, washed and dried to obtain the Ba ion-doped TiO2 / graphene precursor. (4) The precursor is heat-treated to obtain Ba ion-doped TiO2 / graphene composite functional powder; (5) The Ba ion-doped TiO2 / graphene composite functional powder is added to PVDF slurry and dispersed evenly to obtain composite coating slurry; (6) The composite coating slurry is applied to the substrate surface, leveled at room temperature, dried and cured to obtain the multifunctional composite coating.
9. The preparation method according to claim 8, characterized in that, In step (1), the graphene material includes one or more of graphene, graphene oxide, reduced graphene oxide, and few-layer graphene. In step (2), the titanium source includes one or more of tetrabutyl titanate, isopropyl titanate, titanium tetrachloride, titanium sulfate, or titanate; the barium source includes one or more of barium acetate, barium nitrate, barium chloride, and barium hydroxide. In step (3), the hydrothermal reaction temperature is 100–220 °C, and the reaction time is 4–48 h; In step (4), the heat treatment temperature is 250–600 °C and the heat treatment time is 0.5–6 h; In step (6), the coating method includes scraping, spraying, spin coating, dip coating, roller coating, or brush coating.
10. The application of the barium-doped titanium dioxide / graphene / PVDF multifunctional composite coating according to any one of claims 1 to 7 in building energy conservation, heat dissipation of electronic devices, antistatic materials, outdoor thermal management materials, antifouling and self-cleaning materials, metal protective materials or flexible functional films.