A metal multi-element anti-corrosion powder coating, its preparation method, and a coating method for hydraulic supports.
By using a combination of zinc phosphate, polyaniline, and modified kaolinite on the surface of the hydraulic support, a triple protection mechanism is formed, which solves the problems of corrosion resistance and adhesion on the surface of the hydraulic support, improves the anti-corrosion performance and impact resistance of the coating, and ensures the long-term stability of the hydraulic support.
Patent Information
- Application Number
- CN202611461403.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-10
AI Technical Summary
Existing powder coatings have weak corrosion resistance on the surface of hydraulic supports. They are prone to micro-cracks under dynamic loads and impacts, have poor adhesion and impact resistance, and corrosive media can easily spread at the damage point, leading to failure of the protective function.
Zinc phosphate is used as a fast-response component, polyaniline achieves electrochemical passivation, polyaniline-modified kaolinite constructs a dual physical anchoring structure, and combined with carboxyl polyester resin optimization, a triple active protection mechanism is formed to improve the coating's corrosion resistance and adhesion.
It significantly extends the coating's resistance to neutral salt spray tests, improves adhesion and impact resistance, reduces zinc usage, achieves stable corrosion protection and strong toughness throughout the entire lifecycle, and ensures the long-term safe operation of hydraulic supports.
Smart Images

Figure CN123063044A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion coatings, specifically to a metal multi-element anti-corrosion powder coating, its preparation method, and a coating method for hydraulic supports. Background Technology
[0002] Hydraulic supports in coal mines are core support equipment in underground fully mechanized mining faces. Their working environment is extremely harsh, with long-term exposure to high humidity, high chloride ion concentrations, and corrosive gases such as hydrogen sulfide. They endure cyclic high-pressure loads and frequently collide and scrape with coal walls and gangue during support relocation and installation. Therefore, the coating on the surface of coal mine hydraulic supports must possess excellent corrosion resistance, impact resistance, abrasion resistance, adhesion, and water resistance to ensure the long lifespan and safe operation of the equipment. Currently, coatings prepared using conventional powder coatings typically have a salt spray resistance time of only 300-500 hours, exhibiting weak corrosion resistance. Under dynamic loads and impacts, the coating is prone to micro-cracks or even localized peeling, losing its barrier function and exhibiting poor adhesion and impact resistance. Furthermore, once the coating suffers mechanical damage, corrosive media rapidly penetrates and spreads quickly from the damaged point to the surrounding areas and the bottom of the coating, leading to large-area blistering and peeling, and complete failure of the protective function. Therefore, the industry urgently needs an anti-corrosion powder coating that can simultaneously solve the three major problems of "long-lasting corrosion protection", "strong adhesion and impact resistance" and "inhibition of damage and corrosion spread" and can be applied to the surface of hydraulic supports.
[0003] Patent application CN117659758A discloses a method for preparing polyaniline nanocomposite materials for anti-corrosion coatings. The method includes uniformly dispersing a mixed powder containing graphene nanosheets, Al2O3 / ATO mixed nanoparticles, and a surfactant in an acidic solution to obtain a dispersion; adding aniline to the dispersion under an ice-water bath at 0-4°C and stirring to obtain a reaction solution; mixing and stirring the acidic solution and an initiator under an ice-water bath at 0-4°C to obtain an initiator solution; adding the initiator solution to the reaction solution to induce a polymerization reaction, obtaining a crude polyaniline nanocomposite material; and washing, drying, and grinding the crude polyaniline nanocomposite material to obtain the final polyaniline nanocomposite material. This polyaniline nanocomposite material, through in-situ polymerization of polyaniline on graphene nanosheets, effectively inhibits the agglomeration of graphene nanosheets and polyaniline. Furthermore, the layered structure of the polyaniline nanocomposite material within the coating forms a mesh structure in the base material, further effectively blocking the diffusion of oxygen, water, chloride ions, etc., thus providing excellent shielding against corrosive gases and significantly improving the corrosion resistance of metal surfaces. However, this polyaniline nanocomposite material only improves the inhibition of damage corrosion diffusion; it does not simultaneously achieve long-term corrosion protection and strong adhesion and impact resistance. Summary of the Invention
[0004] To provide a novel protective coating capable of forming on the surface of hydraulic supports that combines ultra-long lifespan, strong bonding, inhibition of corrosion spread, and active defense functions, thereby ensuring the long-term safe and stable operation of heavy equipment in coal mines, this invention utilizes zinc phosphate as a fast-response component to accelerate the formation of a passivation film on the metal surface during the initial stage of coating application; it leverages the conductive polymer properties of polyaniline to achieve electrochemical passivation, forming a non-consumable, long-lasting protection; and it uses polyaniline-modified kaolinite as a long-lasting, slow-release component to ensure continuous replenishment of chemical protection, achieving a triple active protection mechanism of "fast response, continuous non-consumable, and long-lasting replenishment," ensuring stable corrosion prevention throughout the entire lifecycle. Furthermore, the polyaniline-modified kaolinite in this invention can also construct a dual physical anchoring structure with montmorillonite nanoclay, ensuring that the interface bonding method changes from the physical encapsulation of existing technologies to physical interlocking, increasing the energy required for peeling by two orders of magnitude.
[0005] Specifically, the technical solution adopted in this invention is: a metal multi-element anti-corrosion powder coating, comprising the following raw materials in parts by weight: 500-700 parts of carboxylated polyester resin, 35-45 parts of polyaniline, 20-35 parts of polyaniline-modified kaolinite, 5-10 parts of zinc phosphate, 10-20 parts of montmorillonite nano-clay, and 24-30 parts of curing agent.
[0006] Furthermore, the polyaniline has a weight-average molecular weight (Mw) of 2000–10000, a molecular weight distribution (Mw / Mn) ≤4.5, a particle size ≤30μm, and a purity ≥99%. That is, if the molecular weight is too low, the molecular chains will be too short, the electronic conjugation length will be insufficient, and the electrochemical passivation ability will decrease. If the molecular weight is too high, the polyaniline molecular chains will be severely entangled and prone to aggregation. In this invention, the polyaniline needs to work synergistically with the polyaniline-modified kaolinite composite structure to exert a passivation effect. An excessively high molecular weight is not conducive to the uniform loading and dispersion of polyaniline on the surface of the kaolinite sheets. A suitable molecular weight distribution can ensure batch uniformity and conductivity; an excessively wide distribution may lead to premature failure of some low molecular weight components and difficulty in dispersing some high molecular weight components, affecting the long-term corrosion resistance.
[0007] Based on the above, the polyaniline-modified kaolinite is prepared by using kaolin and aniline monomers as raw materials, and generating nano-sized polyaniline on the surface of kaolin sheets through in-situ oxidative polymerization. Preferably, the mass of the aniline monomer is 0.05 to 0.5 times the mass of the kaolin. By precisely defining the preparation steps of the polyaniline-modified kaolinite, this process ensures that the aniline monomers are adsorbed onto the kaolin sheet surface and then polymerized in situ. The rigid sheet structure of kaolin effectively prevents the entanglement and aggregation of polyaniline molecular chains, allowing the polyaniline to be uniformly anchored on the sheet surface in the form of nanofibers, thereby significantly increasing its active specific surface area and improving electrochemical passivation efficiency. Simultaneously, the physical shielding function of the kaolin sheet and the active protection function of the polyaniline are integrated, giving the composite pigment dual anti-corrosion properties.
[0008] In one specific embodiment, the polyaniline-modified kaolinite is prepared by the following steps: Kaolin pretreatment: Commercially available kaolin is repeatedly washed with deionized water and separated by sedimentation to remove impurities. It is then dried at 105℃~110℃ to constant weight and pulverized through a 200~325 mesh sieve to obtain purified kaolin.
[0009] Aniline adsorption: Pretreated kaolin is dispersed in deionized water to prepare a suspension with a solid content of 5%–15%. The kaolin sheets are fully dispersed under high-speed stirring at 500 rpm–800 rpm. Aniline monomer at 0.05–0.5 times the mass of kaolin is slowly added dropwise to the suspension, and stirring is continued for 30–60 minutes to allow aniline to be uniformly adsorbed on the surface of the kaolin sheets.
[0010] In-situ oxidative polymerization: Add hydrochloric acid or dodecylbenzenesulfonic acid, which is 0.4 to 2.0 times the molar amount of aniline, as a dopant to the above suspension. Under acidic conditions (20℃ to 30℃) and pH ≤ 2, slowly add ammonium persulfate oxidant solution, which is 0.4 to 1.4 times the molar amount of aniline, over a period of 30 to 60 minutes. Control the polymerization temperature at room temperature and continue stirring for 6 to 24 hours to allow aniline to undergo in-situ oxidative polymerization on the surface of kaolinite flakes, generating nanofiber polyaniline that is tightly bonded to the surface of kaolinite flakes.
[0011] Washing and purification: The polymerization product is separated by vacuum filtration or centrifugation, and washed 2 to 4 times with deionized water and dilute hydrochloric acid alternately until the filtrate is colorless and transparent and pH≈6 to 7, to remove unreacted monomers, oligomers and excess acid.
[0012] Drying and pulverizing: The washed product is spray-dried with an inlet air temperature of 120℃~180℃ and an outlet temperature of ≤80℃ until the moisture content is ≤10%. After grinding through a 200-mesh sieve, the polyaniline-modified layered kaolinite is obtained.
[0013] Based on the above, the metal multi-component anti-corrosion powder coating also includes the following raw materials in parts by weight: 140-170 parts barium sulfate, 80-120 parts titanium dioxide, 0.3-1 part curing accelerator, 3-6 parts adhesion accelerator, 8-12 parts leveling agent, 4-6 parts defoamer, 6-20 parts anti-yellowing agent, and 1-3 parts wetting and dispersing agent. In this step, the addition of various additives promotes the formation of a cross-linked network structure, relaxes internal stress during curing, absorbs impact energy, interrupts the chain reaction leading to yellowing, and protects the molecular structure of polyester resin and polyaniline from damage.
[0014] Based on the above, the curing agent is triglycidyl isocyanurate, the curing accelerator is benzyltriphenylphosphine chloride, the adhesion accelerator is H-300 type adhesion accelerator, the leveling agent is polybutyl acrylate, the defoamer is benzoin, the anti-yellowing agent is hindered amine light stabilizer, and the wetting and dispersing agent is a polymeric wetting and dispersing agent.
[0015] Among these parameters, resin acid value is an indicator of the content of terminal carboxyl groups (-COOH) in polyester resin, directly determining the activity of the curing reaction and the crosslinking density of the coating. A high acid value significantly accelerates the reaction with the curing agent. This can lead to crosslinking before the resin has had time to level out during extrusion or melt mixing, causing gelation and hindering normal processing. Furthermore, a high acid value attracts more moisture, making resin particles more prone to absorbing moisture and clumping during storage and transportation, thus reducing storage stability. The glass transition temperature is the temperature at which the resin transitions from a hard, brittle glassy state to a soft, elastic state. An excessively high glass transition temperature also increases processing difficulty. Melt viscosity reflects the fluidity of the resin in the molten state. Too low a viscosity can cause sagging and dripping during high-temperature baking; while too high a viscosity results in poor melt flow, making it difficult to level the coating surface, affecting smoothness and gloss, and also reducing adhesion to the substrate.
[0016] Therefore, to ensure that the carboxylated polyester resin has good hydrolysis resistance and weather resistance, and to ensure that the obtained coating has high hardness, heat resistance and chemical resistance, the carboxylated polyester resin has an acid value of 32 mgKOH / g to 38 mgKOH / g, a glass transition temperature of 50℃ to 65℃, and a melt viscosity of 2000 mPa·s to 6000 mPa·s at 200℃.
[0017] In one specific embodiment, the specific preparation steps of the carboxylated polyester resin include: Esterification stage: Under nitrogen protection, neopentyl glycol and cyclohexanediol are first added to the reactor, along with 0.05%–0.15% dibutyltin oxide as a catalyst and 0.1%–0.3% triphenyl phosphite as a heat stabilizer. The temperature is raised to 160℃–180℃ to melt the polyols, and then terephthalic acid and isophthalic acid are gradually added. The temperature is gradually increased to 240℃–250℃ at a rate of 5℃ / h–10℃ / h, and the reaction is maintained at this temperature for 6h–10h under normal pressure until the acid value at the esterification endpoint drops to 10mgKOH / g–20mgKOH / g. The rigid benzene ring structure of terephthalic acid and the asymmetric molecular structure of isophthalic acid complete the initial block copolymerization in this stage, laying the foundation for the resin's rigid-flexible main chain structure.
[0018] Acid decomposition and end-capping stage: Cool the system to 230℃~240℃, add trimellitic anhydride (calculated according to the target acid value, accounting for about 6%~12% of the total feed), and carry out acid decomposition reaction at this temperature for 1h~3h, so that the anhydride group of trimellitic anhydride reacts with the hydroxyl group at the end of the polyester molecular chain, introducing carboxyl groups and branching structures onto the molecular chain. The acid value at the end of acid decomposition is controlled at 40mgKOH / g~50mgKOH / g.
[0019] Vacuum polycondensation stage: Vacuum is drawn to a system vacuum degree ≤100Pa using a gradient decompression method, and polycondensation is carried out at a temperature of 235℃~250℃ for 2h~4h. The reaction is driven towards higher molecular weight by removing the small molecule water generated by polycondensation, and finally a carboxylated polyester resin with an acid value of 32mgKOH / g~38mgKOH / g, a glass transition temperature of 50℃~65℃, and a melt viscosity of 2000 mPa·s~6000 mPa·s at 200℃ is obtained.
[0020] Post-processing: The reaction product is cooled to 170℃~200℃ and then melted and discharged. It is then cooled by steel belt and crushed into ≤5mm flakes or granules, and sealed in inner plastic and outer woven bags.
[0021] The present invention also provides a method for preparing a metal multi-component anti-corrosion powder coating for hydraulic supports, comprising: uniformly mixing the raw materials of the metal multi-component anti-corrosion powder coating described above to obtain a raw material mixture powder, and performing melt extrusion, rapid cooling, pulverization and sieving of the raw material mixture powder to obtain a metal multi-component anti-corrosion powder coating for hydraulic supports.
[0022] Based on the above, when performing melt extrusion and rapid cooling on the raw material mixture powder, a screw extruder is used for melt extrusion. The screw speed is controlled at 300 rpm to 600 rpm, the feeding zone temperature is 70℃ to 90℃, the melt mixing zone temperature is 100℃ to 120℃, and the melt homogenization zone temperature is 105℃ to 115℃. The molten material extruded from the screw extruder die is then rapidly cooled at 10℃ to 20℃ and pressed into continuous sheets with a thickness of 1 mm to 2 mm. In this step, by limiting the temperature of each zone, it is possible to prevent the material from sticking and bridging in the feeding zone, avoid substantial cross-linking and solidification in the melt mixing zone, and prevent localized gelation in the melt homogenization zone.
[0023] Based on the above, during the crushing and sieving process, the continuous thin sheets are first coarsely crushed using a pulverizer, and then finely ground and classified using an air classifier mill to obtain finely ground powder with a median particle size D50 of 30 μm to 60 μm. The finely ground powder is then sieved and separated sequentially using a cyclone separator and a rotary vibrating screen, controlling the content of fine particles smaller than 10 μm and coarse particles larger than 80 μm in the finely ground powder to be less than 10% each, thus obtaining the metal multi-element anti-corrosion powder coating. In this step, by controlling the proportion of this micro-powder to below 10%, the overall flowability of the powder system can be significantly optimized. During electrostatic spraying, it can effectively suppress dust flying, improve the uniformity of coating thickness and appearance quality, and reduce defects such as orange peel texture. Simultaneously, it can effectively prevent particle protrusions or foreign matter inclusions on the coating surface, thereby ensuring the smoothness and purity of the final coating film.
[0024] The present invention also provides a metal multi-element anti-corrosion powder coating for hydraulic supports prepared by the above preparation method.
[0025] The present invention also provides a coating method for a hydraulic support, comprising the following steps: Electrostatic spraying: The above-mentioned hydraulic support is electrostatically sprayed with metal multi-element anti-corrosion powder coating onto the mining hydraulic support using the electrostatic spraying method; Cross-linking and curing: The hydraulic support after electrostatic spraying is baked to cross-link and cure the metal multi-element anti-corrosion powder coating on the hydraulic support.
[0026] Based on the above, in the electrostatic spraying step, the electrostatic spraying voltage is controlled to be 60 KV to 90 KV, and the coating thickness on the mining hydraulic support is controlled to be 60 μm to 150 μm; in the crosslinking and curing step, the mining hydraulic support is baked at a temperature of 190℃ to 220℃ for 2 h to 4 h using infrared radiation and hot air convection.
[0027] Based on the above, the electrostatic spraying step further includes performing shot blasting to remove rust from the hydraulic support before spraying the multi-element anti-corrosion powder coating, and then preheating the hydraulic support in a preheating furnace. This step can reduce the temperature difference between the hydraulic support and the coating, thus avoiding affecting the performance of the coating.
[0028] The present invention also provides an anti-corrosion coating applied to the surface of a hydraulic support, the anti-corrosion coating being prepared by the above-described coating method.
[0029] This invention also provides an application of the above-mentioned metal multi-element anti-corrosion powder coating in the preparation of anti-corrosion coatings on the surface of metal materials. Preferably, the metal material is an iron or steel material with iron as its main component.
[0030] This invention has substantial features and advancements compared to existing technologies. Specifically, the metal multi-element anti-corrosion powder coating, its preparation method, and the coating method for hydraulic supports provided by this invention have the following advantages: (1) The corrosion resistance has been greatly improved. This invention retains 5-10 parts of zinc phosphate as a fast-response component, while introducing 20-35 parts of polyaniline-modified kaolinite as a long-lasting slow-release component, and coexists with 35-45 parts of polyaniline in the same coating system, forming a triple active protection mechanism of "fast response of zinc phosphate chemical passivation, continuous non-consumption of polyaniline electrochemical passivation, and long-lasting replenishment of polyaniline-modified kaolinite intelligent release", thus achieving stable corrosion protection throughout the entire cycle.
[0031] In existing technologies, the amount of zinc phosphate used is typically 30-50 parts, and the complete formation of its passivation film requires 48-72 hours, resulting in a protective "window period." Furthermore, as service time increases, the soluble salt is gradually consumed, leading to a decline in protective capability. More critically, existing technologies lack polyaniline as a core component, failing to achieve active electrochemical protection. Polyaniline, as a conductive polymer, possesses unique redox activity. Its doped and undoped states are reversible, enabling the transfer of the electrochemical corrosion reaction at the metal interface from the metal surface to the coating interior. Specifically, polyaniline induces the formation of a dense Fe2O3 / Fe3O4 passivation layer on the metal surface, while continuously supplying electrons to the metal interface through its conjugated conductive structure, maintaining the passivation potential of the metal and inhibiting corrosion reactions at their electrochemical source. Chemical passivation relies on the consumption of corrosion inhibitors, while electrochemical passivation is a sustainable, non-consumable protective method.
[0032] Meanwhile, this invention further addresses the inherent defect of polyaniline's tendency to agglomerate by modifying kaolinite with polyaniline. When polyaniline-modified kaolinite is selected, its layered structure provides an ideal loading substrate for polyaniline. Polyaniline nanofibers polymerize in situ on the surface of kaolinite sheets, effectively preventing the entanglement and agglomeration of polyaniline molecular chains, significantly increasing its active specific surface area and thus improving passivation efficiency. Simultaneously, the retained zinc phosphate rapidly releases phosphate ions in the early stages of coating application, accelerating passivation film formation and filling the initial window period of polyaniline passivation film formation. Polyaniline-modified kaolinite, utilizing its high specific surface area and nanoporous structure, achieves pH-responsive or ion-exchange-type intelligent release of the corrosion inhibitor during corrosive media penetration, ensuring continuous replenishment of chemical protection. Ultimately, this results in the coating of this invention having a 200-300 hour longer neutral salt spray test resistance time compared to existing technologies, and a 30%-50% improvement in long-term corrosion resistance.
[0033] (2) Improved coating adhesion In this invention, polyaniline-modified kaolinite is combined with montmorillonite nanoclay to construct a dual physical anchoring structure. Specifically, the polyaniline-modified kaolinite possesses a nanoscale porous or layered structure with a surface rich in active hydroxyl groups. During melt extrusion and curing, the molten polyester resin penetrates into the nanopores or interlayer gaps of the porous material, forming a "resin anchor" structure after curing, resulting in a physical interlocking effect. When external force is applied to the coating, the peeling process overcomes not only the van der Waals forces at the resin-filler interface (approximately 0.1 J / m² to 0.5 J / m²), but also the shear yield force of 10 J / m² to 50 J / m², pulling the resin anchor out of the nanopores—the latter being two orders of magnitude higher. Simultaneously, the layered structure of the montmorillonite nanoclay further enhances the interfacial bonding. Ultimately, this invention improves the coating's cross-cut adhesion from level 1 in existing technologies to level 0, achieving a pull-out adhesion test value of 13 MPa to 15 MPa. After a 500-hour damp heat aging test at 50°C and 95% humidity, the adhesion retention rate can still reach over 90%, while existing technologies typically drop to less than 70% of the original value under the same conditions.
[0034] (3) It can significantly improve impact resistance. This invention introduces polyaniline-modified kaolinite as a porous material, utilizing its porous structure and lamellar morphology to synergistically dissipate impact energy. The density difference between polyaniline-modified kaolinite and resin is significantly reduced, resulting in a 60-70% reduction in inertial stress concentration. Simultaneously, the porous structure of the material undergoes elastic deformation during compression, converting impact kinetic energy into stored deformation energy instead of directly transferring it to the interface. The kaolinite lamellars in the polyaniline-modified kaolinite possess a high aspect ratio of 20-100, forming a three-dimensional network structure within the coating. According to fracture mechanics principles, when a crack propagates to the lamellar interface, the modulus difference alters the stress field at the crack tip, causing the crack to deflect or bifurcate, consuming propagation energy, lengthening the crack propagation path, and increasing the critical crack length, thereby inhibiting the formation of penetrating cracks. Ultimately, the coating of this invention remains crack-free under a 50 cm·kg impact strength in both positive and negative impact tests, while existing technologies often exhibit fine cracks under the same conditions. In drop hammer impact tests, the coating absorbs 20% to 30% more impact energy than existing technologies, and its impact toughness is significantly improved.
[0035] (4) The weather resistance and thermal stability of the matrix have been greatly improved. This invention provides a limited acid value, glass transition temperature, and melt viscosity at 200°C for a carboxyl polyester resin. It utilizes the steric hindrance effect of the gem-dimethyl group in neopentyl glycol to impart hydrolysis resistance to the main chain during the esterification stage. The rigid alicyclic structure of cyclohexanediethanol significantly enhances the rigidity of the molecular chain segments during the polycondensation stage. These two elements synergistically form the basis for the resin skeleton's weather resistance and thermal stability. The introduction of trimellitic anhydride at the acid desealing stage not only provides precise acid value control but also forms branching points on the polyester molecular chain, ensuring that the carboxyl polyester resin possesses good hydrolysis resistance and weather resistance. Ultimately, it constructs a denser three-dimensional cross-linked network during the powder coating curing process, guaranteeing the coating's high corrosion resistance and long-term protective performance from the resin source.
[0036] (5) Low-zinc formula design, economical and environmentally friendly This invention reduces the amount of zinc phosphate used from 30-50 parts in existing technologies to 5-10 parts, a reduction of over 80%. This invention replaces most of the zinc salt with environmentally friendly porous materials, reducing zinc ore resource consumption, reducing zinc-containing wastewater discharge, and reducing the heavy metal environmental burden after coating disposal. Simultaneously, it achieves superior anti-corrosion performance while reducing zinc content primarily through the electrochemical passivation of polyaniline and the intelligent release mechanism of porous materials.
[0037] Therefore, the metal multi-element anti-corrosion powder coating provided by the present invention can prepare a new type of protective coating on the surface of hydraulic supports, which has ultra-long service life, strong and tough bonding, inhibits the spread of damage corrosion, and has active defense function, so as to ensure the long-term safe and stable operation of heavy equipment in coal mines. Attached Figure Description
[0038] Figure 1 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating of Embodiment 1 of the present invention.
[0039] Figure 2 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating in Embodiment 2 of the present invention.
[0040] Figure 3 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating in Example 3 of the present invention.
[0041] Figure 4 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating of Comparative Example 1 of this invention.
[0042] Figure 5 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating of Comparative Example 2 of this invention.
[0043] Figure 6 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating of Comparative Example 3 of this invention.
[0044] Figure 7 This is a photograph of the rust spread width at the scratches in the salt spray test of the coating of Comparative Example 4 of this invention.
[0045] Figure 8 These are photographs of the coating adhesion test results from Embodiment 1 of the present invention.
[0046] Figure 9 These are photos of the coating adhesion test in Embodiment 2 of the present invention.
[0047] Figure 10 These are photos of the coating adhesion test in Embodiment 3 of the present invention. Detailed Implementation
[0048] The technical solution of the present invention will be further described in detail below through specific embodiments.
[0049] Unless otherwise specified, all terms used in this invention are commonly used in the relevant field. The technical means employed in the embodiments, such as preparation processes and testing methods, are conventional methods well-known to those skilled in the art. All reagents and products used are commercially available. The source, trade name, and, where necessary, the components of any reagents are indicated upon their first appearance.
[0050] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention. Example 1
[0051] This embodiment provides a metal multi-element anti-corrosion powder coating, which, by weight, comprises the following components: 600 parts of carboxylated polyester resin; 27 parts of curing agent; 100 parts of titanium dioxide; 15 parts of montmorillonite nano-clay; 0.5 parts of curing accelerator; 5 parts of adhesion accelerator; 10 parts of leveling agent; 5 parts of defoamer; 10 parts of anti-yellowing agent; 2 parts of wetting and dispersing agent; 8 parts of zinc phosphate; 40 parts of polyaniline; 30 parts of polyaniline-modified kaolinite; and 150 parts of barium sulfate. In this embodiment, the curing agent is triglycidyl isocyanurate, and the curing accelerator is benzyltriphenylphosphine chloride. The adhesion accelerator is H-300 type. The leveling agent is Sheng SAS-550. The defoamer is benzoin. The anti-yellowing agent is preferably Tinuvin 144. The wetting and dispersing agent is Evonik TEGO® Powder Aid D01. Intrinsic or doped polyaniline can be used.
[0052] This embodiment also provides a method for preparing a metal multi-element anti-corrosion powder coating, the specific steps of which include: Mixing: Mix all solid raw materials at 1200 rpm for 8 minutes. Specifically, first add a large proportion of the base material and additives, namely carboxylated polyester resin, curing agent, wetting and dispersing agent, adhesion promoter, leveling agent, defoamer, anti-yellowing agent, and curing accelerator. Start the mixer for initial mixing; the frictional force of the large proportion of materials generates heat, which helps soften the carboxylated polyester resin. Then add functional fillers, namely barium sulfate, zinc phosphate, titanium dioxide, montmorillonite nanoclay, and polyaniline. Finally, add polyaniline-modified kaolinite to reduce moisture absorption and agglomeration. The material temperature must be monitored during mixing and should generally not exceed 60℃.
[0053] Melt extrusion: The mixed material is placed in a twin-screw melt extruder for melt extrusion. Utilizing heat and shear force, the mixture is melted, allowing the resin to completely encapsulate the filler and ensuring that preservative components such as polyaniline and nano-clay are dispersed at the molecular level within the resin matrix. Simultaneously, the curing agent is uniformly incorporated. The temperature control in each zone of the twin-screw melt extruder is as follows: feed zone 100℃, mixing zone 120℃, discharge zone 115℃, and screw speed 600 rpm. The extruded viscous material is pressed into thin sheets by compression rollers and immediately conveyed to a cooling press for forced cooling, rapidly reducing it to room temperature to prevent further curing and facilitate subsequent crushing.
[0054] Crushing and Classifying Mill: An air classifier mill is used to crush the cooled, brittle, flaky material into powder with a D50 of 30-50 micrometers to meet the process requirements of electrostatic spraying. The crushed powder is then introduced into a cyclone separator along with the airflow. Utilizing the principle of centrifugal sedimentation, ultrafine powder with a particle size less than 10 micrometers is efficiently separated and collected. By controlling the proportion of this micro-powder to below 10%, the overall flowability of the powder system can be significantly optimized. During electrostatic spraying, this effectively suppresses dust dispersion, improves the uniformity of coating thickness and surface quality, and reduces defects such as orange peel texture. The powder after cyclone separation then enters a rotary vibrating screen, typically with a mesh size of 150 to 200, to remove coarse particles larger than 80 micrometers and any trace amounts of gel particles, ensuring their content is also below 10%. This classification process effectively prevents particle protrusions or foreign matter inclusions on the coating surface, thus ensuring the smoothness and purity of the final coating film. The humidity in the crushing workshop should be controlled at ≤50%. Porous materials will lose powder flowability and powder application rate after absorbing moisture.
[0055] This embodiment also provides a coating method for a hydraulic support, including the following steps: A metal multi-component anti-corrosion powder coating as described above is provided; First, the hydraulic support is shot-blasted / sandblasted to remove rust, achieving a Sa2.5 grade. Then, the workpiece is placed in a preheating furnace and dried at 110℃ for 20 minutes. Using a high-pressure electrostatic spray gun at an 80 KV electrostatic spraying voltage, a multi-element anti-corrosion powder coating is applied to the surface of the hydraulic support, controlling the coating thickness to 100 μm. Finally, the coating is baked at 200℃ for 180 minutes using a combined heating mode of "gas-fired infrared radiation + hot air convection" for high-temperature curing.
[0056] The present invention also provides an anti-corrosion coating applied to the surface of a hydraulic support, the anti-corrosion coating being prepared by the coating method.
[0057] In this embodiment, the polyaniline-modified layered kaolinite is prepared by in-situ oxidative polymerization, and the specific preparation steps include: Kaolin pretreatment: Commercially available kaolin is repeatedly washed with deionized water and separated by sedimentation to remove impurities. After drying at 110℃ to constant weight, it is pulverized and passed through a 325-mesh sieve to obtain purified kaolin.
[0058] Aniline adsorption: Pretreated kaolin was dispersed in deionized water to prepare a suspension with a solid content of 15%. The kaolin flakes were fully dispersed under high-speed stirring at 800 rpm. Aniline monomer at 0.5 times the mass of kaolin was slowly added dropwise to the suspension, and stirring was continued for 60 minutes to allow aniline to be uniformly adsorbed on the surface of the kaolin flakes.
[0059] In-situ oxidative polymerization: Add hydrochloric acid at 2.0 times the molar amount of aniline as a dopant to the above suspension. Under the conditions of 30℃ and pH≤2, slowly add ammonium persulfate oxidant solution at 1.4 times the molar amount of aniline over 60 minutes. Control the polymerization temperature at room temperature and continue stirring for 24 hours to allow aniline to undergo in-situ oxidative polymerization on the surface of kaolinite flakes, generating nanofiber polyaniline that is tightly bonded to the surface of kaolinite flakes.
[0060] Washing and purification: The polymerization product is separated by vacuum filtration or centrifugation, and washed 4 times alternately with deionized water and dilute hydrochloric acid until the filtrate is colorless and transparent and the pH is at the center, to remove unreacted monomers, oligomers and excess acid.
[0061] Drying and pulverizing: The washed product is spray-dried with an inlet air temperature of 180°C and an outlet temperature of 80°C until the moisture content is less than or equal to 10%. After grinding and passing through a 200-mesh sieve, the polyaniline-modified layered kaolinite lightweight porous anti-rust pigment is obtained.
[0062] The specific preparation steps of the carboxyl polyester resin include: Esterification stage: Under nitrogen protection, neopentyl glycol and cyclohexanediol were first added to the reactor, along with 0.15% dibutyltin oxide as a catalyst and 0.3% triphenyl phosphite as a heat stabilizer. The temperature was raised to 180°C to melt the polyols, and then terephthalic acid and isophthalic acid were gradually added. The temperature was gradually increased to 250°C at a rate of 10°C / hour, and the reaction was maintained at this temperature for 10 hours under normal pressure until the acid value at the esterification endpoint dropped to 20 mg KOH / g. In this stage, the rigid benzene ring structure of terephthalic acid and the asymmetric molecular structure of isophthalic acid complete the initial block copolymerization, laying the foundation for the resin's rigid-flexible main chain structure.
[0063] Acid decomposition and sealing stage: Cool the system to 240℃, add trimellitic anhydride (calculated according to the target acid value, accounting for about 12% of the total feed), and carry out acid decomposition reaction at this temperature for 3 hours, so that the anhydride group of trimellitic anhydride reacts with the hydroxyl group at the end of the polyester molecular chain, introduces carboxyl groups on the molecular chain and attaches branched structure, and the acid value at the end of acid decomposition is controlled at 50mgKOH / g.
[0064] Vacuum polycondensation stage: Vacuum is drawn to a system vacuum degree ≤100Pa using a gradient decompression method, and polycondensation is carried out at 235℃ for 2 hours. The reaction is driven towards higher molecular weight by removing the small molecule water generated by polycondensation, and finally a carboxylated polyester resin with an acid value of 38mgKOH / g, a glass transition temperature of 65℃, and a melt viscosity of 6000mPa·s at 200℃ is obtained.
[0065] Post-processing: The reaction product is cooled to 200℃ and then melted and discharged. It is then cooled by steel belt and crushed into ≤5mm flakes or granules, and sealed in inner plastic and outer woven bags. Example 2
[0066] This embodiment provides a metal multi-element anti-corrosion powder coating, which, by weight, includes the following components: 700 parts of carboxylated polyester resin; 30 parts of TGIC curing agent, 120 parts of titanium dioxide, 10 parts of zinc phosphate, 45 parts of polyaniline, 20 parts of montmorillonite nano-clay, 35 parts of polyaniline-modified kaolinite, 138 parts of barium sulfate; 1 part of curing accelerator, 6 parts of adhesion accelerator, 12 parts of leveling agent, 6 parts of defoamer, 20 parts of anti-yellowing agent, and 3 parts of wetting and dispersing agent.
[0067] This embodiment also provides a method for preparing a metal multi-element anti-corrosion powder coating, the steps of which include: Weigh the above raw materials according to their respective weight proportions; Mixing: Place the weighed anti-corrosion powder coating raw materials into a mixer and mix at 1000 rpm for 5 minutes to obtain a mixture. During mixing, control the temperature of the materials to not exceed 60°C. Melting: The mixture is melt-extruded using a screw extruder, with the screw speed controlled at 500 rpm, the feeding zone temperature at 80°C, the melt mixing zone temperature at 110°C, and the melt homogenization zone temperature at 112°C. The molten material extruded from the screw extruder die is then rapidly cooled at 15°C and pressed into a continuous sheet with a thickness of 1.5 mm. Crushing: First, the continuous thin sheet is coarsely crushed using a pulverizer, and then finely ground and classified using an air classifier mill to obtain finely ground powder with a median particle size D50 of 30μm to 60μm; then, the finely ground powder is sieved and separated sequentially using a cyclone separator and a rotary vibrating screen, controlling the content of fine particles with a particle size less than 10μm and the content of coarse particles with a particle size greater than 80μm in the finely ground powder to be less than 10% respectively, to obtain the metal multi-element anti-corrosion powder coating.
[0068] This embodiment also provides a coating method for a hydraulic support, the steps of which include: Electrostatic spraying: The metal multi-element anti-corrosion powder coating is electrostatically sprayed onto the mining hydraulic support under an electrostatic spraying voltage of 60 KV, and the coating thickness is controlled to be 60 μm. Crosslinking and curing: The hydraulic support after electrostatic spraying is placed on the coating line of the curing oven, and the mining hydraulic support is baked at 190°C for 4 hours using infrared radiation and hot air convection to crosslink and cure the metal multi-element anti-corrosion powder coating on the hydraulic support. Example 3
[0069] This embodiment provides a metal multi-element anti-corrosion powder coating, which, by weight, includes the following components: 500 parts of carboxylated polyester resin; 24 parts of TGIC curing agent, 80 parts of titanium dioxide, 5 parts of zinc phosphate, 35 parts of polyaniline, 10 parts of montmorillonite nano-clay, 20 parts of polyaniline-modified kaolinite, 168 parts of barium sulfate; 0.3 parts of curing accelerator, 3 parts of adhesion accelerator, 8 parts of leveling agent, 4 parts of defoamer, 6 parts of anti-yellowing agent, and 1 part of wetting and dispersing agent.
[0070] This embodiment also provides a method for preparing a metal multi-element anti-corrosion powder coating, the steps of which include: Weigh the above raw materials according to their respective weight proportions; Mixing: Place the weighed anti-corrosion powder coating raw materials into a mixer and mix at 1200 rpm for 3 minutes to obtain a mixture. During mixing, control the temperature of the materials to not exceed 60°C. Melting: The mixture is melt-extruded using a screw extruder, with the screw speed controlled at 600 rpm, the feeding zone temperature at 90°C, the melt mixing zone temperature at 120°C, and the melt homogenization zone temperature at 115°C. The molten material extruded from the screw extruder die is then rapidly cooled at 10°C and pressed into a continuous sheet with a thickness of 2 mm. Crushing: First, the continuous thin sheet is coarsely crushed using a pulverizer, and then finely ground and classified using an air classifier mill to obtain finely ground powder with a median particle size D50 of 30μm to 60μm; then, the finely ground powder is sieved and separated sequentially using a cyclone separator and a rotary vibrating screen, controlling the content of fine particles with a particle size less than 10μm and the content of coarse particles with a particle size greater than 80μm in the finely ground powder to be less than 10% respectively, to obtain the metal multi-element anti-corrosion powder coating.
[0071] This embodiment also provides a coating method for a hydraulic support, the steps of which include: Electrostatic spraying: The metal multi-element anti-corrosion powder coating is electrostatically sprayed onto the mining hydraulic support under an electrostatic spraying voltage of 90 KV, and the coating thickness is controlled to be 150 μm. Crosslinking and curing: The hydraulic support after electrostatic spraying is placed on the coating line of the curing oven, and the mining hydraulic support is baked at 220°C for 4 hours using infrared radiation and hot air convection to crosslink and cure the metal multi-element anti-corrosion powder coating on the hydraulic support. Comparative Example 1 omits both polyaniline and polyaniline-modified kaolinite.
[0072] Comparative Example 1 provides a metal multi-element anti-corrosion powder coating. The main difference between this and Example 1 is that, based on Example 1, the mass fractions of zinc phosphate, polyaniline, polyaniline-modified kaolinite, and barium sulfate are changed. The change in the mass fraction of barium sulfate is to ensure that the total mass fractions of zinc phosphate, polyaniline, polyaniline-modified kaolinite, and barium sulfate remain constant in each comparative example.
[0073] Specifically, the following materials were selected: 40 parts zinc phosphate, 0 parts polyaniline, 0 parts polyaniline-modified kaolinite, and 188 parts barium sulfate. Comparative Example 2 omitted polyaniline-modified kaolinite and added zinc phosphate.
[0074] Comparative Example 2 provides a metal multi-element anti-corrosion powder coating. The main difference between this and Example 1 is that, based on Example 1, the mass proportions of zinc phosphate, polyaniline, polyaniline-modified kaolinite, and barium sulfate are changed.
[0075] Specifically, the following materials were selected: 40 parts zinc phosphate, 40 parts polyaniline, 0 parts polyaniline-modified kaolinite, and 148 parts barium sulfate. Comparative Example 3 (polyaniline omitted)
[0076] Comparative Example 3 provides a metal multi-element anti-corrosion powder coating. The main difference from Example 1 is that, based on Example 1, the mass proportions of zinc phosphate, polyaniline, polyaniline-modified kaolinite, and barium sulfate are changed. Specifically, the following materials were selected: 40 parts zinc phosphate, 0 parts polyaniline, 30 parts polyaniline-modified kaolinite, and 158 parts barium sulfate. Comparative Example 4 (zinc phosphate omitted)
[0077] Comparative Example 4 provides a metal multi-element anti-corrosion powder coating. The main difference from Example 1 is that, based on Example 1, the mass proportions of zinc phosphate, polyaniline, polyaniline-modified kaolinite, and barium sulfate are changed.
[0078] Specifically, the following materials were selected: 0 parts zinc phosphate, 40 parts polyaniline, 30 parts polyaniline-modified kaolinite, and 158 parts barium sulfate. Comparative Example 5 omits both polyaniline-modified kaolinite and montmorillonite nanoclay.
[0079] Comparative Example 5 provides a metal multi-element anti-corrosion powder coating. The main difference from Example 1 is that, based on Example 1, the mass fractions of polyaniline-modified kaolinite, montmorillonite nanoclay, and barium sulfate are changed. The change in the mass fraction of barium sulfate is to ensure that the total mass fractions of polyaniline-modified kaolinite, montmorillonite nanoclay, and barium sulfate remain constant in each comparative example.
[0080] Specifically, 0 parts of polyaniline-modified kaolinite, 0 parts of montmorillonite nano-clay, and 195 parts of barium sulfate were selected. Comparative Example 6 (omitting polyaniline-modified kaolinite)
[0081] Comparative Example 6 provides a metal multi-element anti-corrosion powder coating. The main difference from Example 1 is that, based on Example 1, the mass fractions of polyaniline-modified kaolinite, montmorillonite nanoclay, and barium sulfate are changed.
[0082] Specifically, the following materials were selected: 0 parts of polyaniline-modified kaolinite, 15 parts of montmorillonite nano-clay, and 180 parts of barium sulfate. Comparative Example 7 (omitted: montmorillonite nano-clay)
[0083] Comparative Example 7 provides a metal multi-element anti-corrosion powder coating. The main difference from Example 1 is that, based on Example 1, the mass parts of polyaniline-modified kaolinite, montmorillonite nanoclay, and barium sulfate are changed. Specifically, 30 parts of polyaniline-modified kaolinite, 0 parts of montmorillonite nanoclay, and 165 parts of barium sulfate are selected. Comparative Example 8: Liquid coating prepared using waterborne carboxylated polyester resin
[0084] Comparative Example 8 provides a liquid coating, the main difference from Example 1 being that, based on Example 1, it uses a water-based carboxylated polyester resin. The specific components, by weight, include: 600 parts water-based carboxylated polyester resin, 27 parts curing agent, 100 parts titanium dioxide, 15 parts montmorillonite nano-clay, 40 parts polyaniline, 30 parts polyaniline-modified kaolinite, 8 parts zinc phosphate, 150 parts barium sulfate, 0.5 parts curing accelerator, 5 parts adhesion accelerator, 10 parts leveling agent, 5 parts defoamer, 10 parts anti-yellowing agent, 2 parts wetting and dispersing agent, 15 parts triethylamine neutralizer, 20 parts propylene glycol methyl ether (PMA) cosolvent, and an appropriate amount of deionized water (added according to 45-55% of the solids content).
[0085] In the specific preparation of liquid coatings, the above-mentioned raw materials weighed are mixed and stirred using the mixing steps of Example 1 of this invention.
[0086] It should be noted that the embodiments and comparative examples of this invention are based on practical applications and production costs. That is, considering production costs, the weight proportions of raw materials are designed within a reasonable upper limit range. Performance testing
[0087] Adhesion, impact, and pencil hardness tests were conducted on Examples 1 to 3 and Comparative Examples 1 to 8, respectively. Salt spray tests were also conducted on Examples 1 to 3, Comparative Examples 1 to 4, and Comparative Example 8. It should be noted that Comparative Examples 5 to 7 were designed primarily to verify the anchoring effect between montmorillonite nanoclay and polyaniline-modified kaolinite. Based on experimental costs and the salt spray test results of Comparative Examples 1 to 4, salt spray tests were not conducted on Comparative Examples 5 to 7. However, it can be inferred that the salt spray test results could not achieve the results of Examples 1 to 3 of this invention.
[0088] The test sample used a 150mm×75mm×4mm Q235 steel plate as the substrate for electrostatic spraying of the coating, and the surface was shot-blasted to Sa2.5 grade. The spraying distance was 250mm, and the curing conditions were 160℃ for 10 minutes. The dry film thickness of the coating was 120μm. Specific test standards are shown in Table 1, and specific test results are shown in Tables 2 and 3. Figures 1 to 10 As shown.
[0089] Table 1. Test Items and Methods Test Project Test Standards Test methods neutral salt spray test GB / T10125-2021 5% NaCl, 35℃, continuous spraying Adhesion (cross-cut test) GB / T9286-2021 2mm grid spacing Adhesion (pull-out test) GB / T5210-2006 Pulling method Impact test GB / T1732-2020 The drop hammer weighs 1kg and has a height of 50mm. Pencil hardness GB / T6739-2022 Mitsubishi Pencil Table 2. Mechanical Test Results Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Adhesion (cross-cut test) Level 0 Level 0 Level 0 Level 1 Level 1 Level 0 Level 1 Level 2 Level 1 Level 0 Level 2 Adhesion (pull-out) unit MPa 19.5 19.6 17.5 10.2 11.3 16.8 10.8 10.2 12.3 14.6 9.2 Pencil hardness 2H 2H 2H H H 2H H H H 2H H Impact test No cracks No cracks No cracks minor cracks No cracks No cracks minor cracks crack minor cracks No cracks wrinkles Table 3. Rust spread width at scratches in salt spray test (unit: mm) Test time Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 8 480h 0.5 0.5 0.7 1.5 1.1 0.9 1.2 1.8 600h 1.2 1.1 1.4 2.8 1.8 1.5 2.5 3.2 720h 1.8 1.6 2.0 5.1 2.8 2.5 4.1 8.7 816h 2.2 2.2 2.5 8.6 5.3 4.2 5.6 termination (1) Comparison of mechanical properties Specifically, from Table 2, Table 3, Figure 1 , Figure 2 , Figure 3 , Figure 8 , Figure 9 and Figure 10 It can be seen from this: The coatings prepared by cross-cut adhesion testing in Examples 1, 2, and 3 of this invention all achieved an adhesion level of 0. The maximum pull-out adhesion was 19.6 MPa in Example 2 and 17.5 MPa in Example 3. The pencil hardness of all samples reached 2H, and no cracks were observed in the impact test. After 720 hours of salt spray testing, the maximum rust width was only 2.0 mm, and after 812 hours, the rust width was 2.2 mm. A clear "self-healing" phenomenon was observed at the scratches, which is essentially due to the formation of a passivation film induced by polyaniline on the exposed metal surface, combined with the intelligent release of the corrosion inhibitor, effectively suppressing rust expansion.
[0090] Analysis suggests that the significant improvement in adhesion is attributed to the physical anchoring effect of the kaolinite layers in the polyaniline-modified kaolinite. The layered structure of kaolinite provides numerous anchoring points for the resin. The molten resin penetrates into the interlayer gaps, forming a "resin anchor" structure after curing, transforming the interface bonding from physical encapsulation to physical interlocking. The improved impact performance is due to the porous structure of the polyaniline-modified kaolinite acting as a "stress buffer," with pore compression deformation absorbing impact energy. Simultaneously, the high aspect ratio of the kaolinite layers deflects crack propagation, consuming propagation energy. The improved corrosion resistance is attributed to the coexistence of zinc phosphate, polyaniline-modified kaolinite, and polyaniline in the same coating system, forming a triple active protection mechanism of rapid chemical passivation response, continuous non-consumable electrochemical passivation, and intelligent release for long-term replenishment, achieving stable corrosion protection throughout the entire lifecycle. Furthermore, as can be seen from Examples 1 to 3, performance gradually improves with increasing component content. Considering production costs, the components defined in this invention were specifically selected.
[0091] (2) Synergistic effect of polyaniline and polyaniline-modified kaolinite Compared to Example 1 of the present invention, Comparative Example 1, by omitting both polyaniline and polyaniline-modified kaolinite, failed to construct a dual physical anchoring structure, resulting in a drop in cross-cut adhesion to grade 1, a pull-out adhesion to 10.2 MPa, a pencil hardness to H, and slight cracks appearing in the impact test, indicating weaker adhesion and impact resistance. Meanwhile, as... Figure 4 As shown, Comparative Example 1 also suffered from weak corrosion resistance because it could not utilize polyaniline-modified kaolinite as a long-lasting slow-release component, resulting in an 8.6 mm rust width after 816 hours.
[0092] (3) Long-lasting sustained-release effect of polyaniline-modified kaolinite Compared to Example 1 of this invention, Comparative Example 2, due to the omission of polyaniline-modified kaolinite, suffers from a reduced coating strength (grade 1 in cross-cut adhesion), a reduced pull-out adhesion to 11.3 MPa, and a reduced pencil hardness to H, indicating weaker adhesion, as the coating cannot form a dual physical anchoring structure. Meanwhile, as... Figure 5 As shown, Comparative Example 2 could not utilize polyaniline-modified kaolinite as a long-lasting slow-release component, but retained polyaniline, resulting in an 816h corrosion width expansion to 5.3mm. Its corrosion resistance was weaker, but improved compared to Comparative Example 1, indicating that polyaniline can significantly slow down corrosion expansion.
[0093] (4) Electrochemical passivation effect of polyaniline Compared to Example 1 of this invention, Comparative Example 3, by omitting polyaniline, cannot utilize polyaniline to transfer the electrochemical corrosion reaction at the metal interface from the metal surface to the interior of the coating, nor can it continuously transfer electrons to the metal interface, thus failing to inhibit the corrosion reaction at its electrochemical source. Consequently, although Comparative Example 3 exhibits strong adhesion and impact resistance, with a cross-cut adhesion rating of 0, a pull-out adhesion rating of 16.8 MPa, and a pencil hardness of 2H, it still falls short of the requirements of Example 3. Figure 6 As shown, the rust width of Comparative Example 3 expanded to 4.2 mm after 816 hours, and its corrosion resistance was improved compared to Comparative Example 1, indicating that polyaniline-modified kaolinite can improve the active corrosion protection capability of the coating.
[0094] (5) Rapid response effect of zinc phosphate Compared to Example 1 of this invention, Comparative Example 4, by omitting zinc phosphate, lacked protective capability in the initial stage, resulting in a decrease in cross-cut adhesion to grade 1, pull-out adhesion to 10.8 MPa, and pencil hardness to H, indicating weaker adhesion. Meanwhile, as... Figure 7 As shown, in Comparative Example 4, the rust width expanded to 4.1 mm after 720 hours, indicating the most severe rust condition. This demonstrates that initial protection with zinc phosphate is essential.
[0095] (6) Impact resistance of montmorillonite nano-clay Compared to Example 1 of the present invention, Comparative Example 5 omits both polyaniline-modified kaolinite and montmorillonite nanoclay, resulting in the coating being unable to construct a dual physical anchoring structure and unable to utilize polyaniline-modified kaolinite to improve impact resistance. Consequently, the cross-cut adhesion of Comparative Example 5 drops to level 2, the pull-out adhesion drops to 10.2 MPa, the pencil hardness drops to H, and cracks appear during the impact test, indicating weak adhesion and impact resistance.
[0096] (7) The combination of polyaniline-modified kaolinite and montmorillonite nano-clay provides a dual physical anchoring effect. Compared to Example 1 of this invention, Comparative Example 6, by omitting polyaniline-modified kaolinite, failed to construct a dual physical anchoring structure in its coating. Consequently, the cross-cut adhesion of Comparative Example 6 decreased to level 1, the pull-out adhesion decreased to 12.3 MPa, the pencil hardness decreased to H, and slight cracks appeared during the impact test, indicating weaker adhesion. However, compared to Comparative Example 5, the pull-out adhesion of Comparative Example 6 improved due to the addition of montmorillonite nanoclay, demonstrating that the anchoring ability of montmorillonite nanoclay alone is limited.
[0097] (8) Effect of montmorillonite nano-clay Compared to Example 1 of this invention, Comparative Example 7, by omitting montmorillonite nano-clay, cannot construct a dual physical anchoring structure in its coating. Although Comparative Example 7 achieves a cross-cut adhesion rating of 0, a pull-out adhesion rating of 14.6 MPa, a pencil hardness of 2H, and no cracks during impact testing, it still does not meet the performance of this invention, indicating that the anchoring ability of polyaniline-modified kaolinite alone is limited.
[0098] (9) Differences between water-based coatings and powder coatings Compared to Example 1 of this invention, Comparative Example 8, due to the use of ordinary water-based carboxylated polyester resin, requires multiple applications on the surface of the hydraulic support during coating preparation. Furthermore, compared to Comparative Example 8, the powder coating of this invention exhibits significantly superior anti-corrosion performance compared to liquid coatings, and a dense coating of 60μm~80μm can be formed with a single application. Its effective salt spray time (≥816h) is more than 1.7 times that of water-based coatings. The powder coating also demonstrates significantly better mechanical properties, with adhesion grade 0 (19.5MPa), no cracking at 50cm·kg impact, and a hardness of 2H, all superior to water-based coating systems. In summary, the powder coating of this invention significantly outperforms water-based coating solutions with the same formulation in both salt spray corrosion protection and mechanical properties, demonstrating the inherent advantages of powder coating technology in anti-corrosion applications.
[0099] The above experimental results demonstrate that this invention, through a three-component synergistic anti-corrosion system of zinc phosphate, polyaniline, and polyaniline-modified kaolinite, provides synergistic protection through chemical passivation, electrochemical passivation, and physical shielding. Furthermore, by combining the dual physical anchoring interface enhancement technology of polyaniline-modified kaolinite and montmorillonite nanoclay, the interface bonding is upgraded from physical encapsulation to physical interlocking and chemical bonding. The impact resistance of polyaniline-modified kaolinite further contributes to a comprehensive breakthrough in the overall performance of the powder coating. Simultaneously, the solvent-free, one-step film formation of the powder coating ensures a dense and defect-free coating, fully utilizing the design functions of each component. This results in a coating with an adhesion grade of 0, a pull-out value of up to 19.6 MPa, a pencil hardness of 2H, no cracking under normal impact, and resistance to neutral salt spray for 816 hours. This enables the preparation of a novel protective coating on the surface of hydraulic supports that combines ultra-long lifespan, strong and tough bonding, inhibition of corrosion spread, and active defense functions, ensuring the long-term safe and stable operation of heavy equipment in coal mines.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them; although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications can still be made to the specific implementation of the present invention or equivalent substitutions can be made to some technical features without departing from the spirit of the technical solutions of the present invention, and all such modifications and substitutions should be covered within the scope of the technical solutions claimed in the present invention.
Claims
1. A metal multi-element anti-corrosion powder coating, characterized in that, The raw materials include the following parts by weight: 500-700 parts of carboxylated polyester resin, 35-45 parts of polyaniline, 20-35 parts of polyaniline-modified kaolinite, 5-10 parts of zinc phosphate, 10-20 parts of montmorillonite nano-clay, and 24-30 parts of curing agent.
2. The metal multi-element anti-corrosion powder coating according to claim 1, characterized in that, The polyaniline-modified kaolinite is prepared by using kaolin and aniline monomers as raw materials and generating nano-sized polyaniline on the surface of the kaolin sheets through in-situ oxidative polymerization.
3. The metal multi-element anti-corrosion powder coating according to claim 2, characterized in that, It also includes the following raw materials in parts by weight: 140-170 parts barium sulfate, 80-120 parts titanium dioxide, 0.3-1 part curing agent accelerator, 3-6 parts adhesion accelerator, 8-12 parts leveling agent, 4-6 parts defoamer, 6-20 parts anti-yellowing agent, and 1-3 parts wetting and dispersing agent.
4. The metal multi-element anti-corrosion powder coating according to claim 3, characterized in that, The curing agent is triglycidyl isocyanurate, the curing accelerator is benzyltriphenylphosphine chloride, the adhesion accelerator is H-300 type adhesion accelerator, the leveling agent is polybutyl acrylate, the defoamer is benzoin, the anti-yellowing agent is hindered amine light stabilizer, and the wetting and dispersing agent is a polymeric wetting and dispersing agent.
5. A method for preparing a metal multi-element anti-corrosion powder coating for hydraulic supports, comprising: The raw materials of the metal multi-component anti-corrosion powder coating according to any one of claims 1 to 4 are uniformly mixed to obtain raw material mixed powder, and the raw material mixed powder is melt-extruded, rapidly cooled, crushed and sieved to obtain metal multi-component anti-corrosion powder coating for hydraulic supports.
6. The preparation method according to claim 5, characterized in that, When the raw material mixture powder is melt-extruded and rapidly cooled, a screw extruder is used for melt extrusion. The screw speed is controlled at 300 rpm to 600 rpm, the feeding zone temperature is 70℃ to 90℃, the melt mixing zone temperature is 100℃ to 120℃, and the melt homogenization zone temperature is 105℃ to 115℃. The molten material extruded from the screw extruder die is rapidly cooled at a temperature of 10℃ to 20℃ and then pressed into continuous sheets with a thickness of 1 mm to 2 mm.
7. The preparation method according to claim 6, characterized in that, During the crushing and sieving process, the continuous thin sheet is first coarsely crushed using a pulverizer, and then finely ground and classified using an air classifier mill to obtain finely ground powder with a median particle size D50 of 30 μm to 60 μm. The finely ground powder is then sieved and separated sequentially using a cyclone separator and a rotary vibrating screen, controlling the content of fine particles with a particle size less than 10 μm and the content of coarse particles with a particle size greater than 80 μm in the finely ground powder to be less than 10% respectively, thus obtaining the metal multi-element anti-corrosion powder coating.
8. A metal multi-element anti-corrosion powder coating for hydraulic supports is prepared by the preparation method described in any one of claims 5 to 7.
9. A method for painting a hydraulic support, comprising the following steps: Electrostatic spraying: The metal multi-element anti-corrosion powder coating for hydraulic supports as described in claim 8 is electrostatically sprayed onto the mining hydraulic supports using the electrostatic spraying method; Crosslinking and curing: The hydraulic support after electrostatic spraying is baked to crosslink and cure the metal multi-element anti-corrosion powder coating on the hydraulic support.
10. The coating method according to claim 9, characterized in that, In the electrostatic spraying step, the electrostatic spraying voltage is controlled to be 60 KV to 90 KV, and the coating thickness on the mining hydraulic support is controlled to be 60 μm to 150 μm. In the cross-linking and curing step, the mining hydraulic support is baked at 190℃ to 220℃ for 2 h to 4 h using infrared radiation and hot air convection.
11. The coating method according to claim 10, characterized in that, The electrostatic spraying step also includes first performing shot blasting to remove rust on the hydraulic support before spraying the metal multi-element anti-corrosion powder coating, and then placing the hydraulic support in a preheating furnace for preheating.
12. An anti-corrosion coating applied to the surface of a hydraulic support, characterized in that, The anti-corrosion coating is obtained by the coating method according to any one of claims 10 to 11.
13. The application of the metal multi-element anti-corrosion powder coating according to any one of claims 1 to 4 in the preparation of anti-corrosion coatings on the surface of metal materials.
Citation Information
Patent Citations
Polyaniline nano composite material for anticorrosive paint, preparation method of polyaniline nano composite material and polyaniline composite anticorrosive paint
CN117659758A