High-concentration light-excited negative oxygen ion release type full-nano ceramic after-loaded heat insulation film and preparation method thereof
By optimizing the all-inorganic nano-ceramic material system, the problems of insufficient negative oxygen ion release and metal oxidation failure of the heat insulation film were solved, achieving a combination of efficient negative oxygen ion release and heat insulation performance, and ensuring the stability and electromagnetic compatibility of the product.
Patent Information
- Application Number
- CN202611396006.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-10
AI Technical Summary
Existing photocatalytic negative oxygen ion releasing materials suffer from problems such as insufficient negative oxygen ion release, limited spectral response range, insufficient surface active sites, and insufficient consideration of environmental factors. Furthermore, existing heat insulation films suffer from metal oxidation failure and electromagnetic signal shielding issues.
By employing an all-inorganic nano-ceramic material system, a thermal insulation functional layer is constructed through carrier separation, spectral response, and environmental synergistic optimization. This layer includes an infrared shielding component, a photocatalytic negative oxygen ion release component, and a structural reinforcement component. This avoids the use of a metal layer and utilizes oxygen vacancy defects and Z-shaped heterojunctions to achieve efficient charge separation and continuous release of negative oxygen ions.
It achieves continuous release of high concentrations of negative oxygen ions across a wide spectral range, while also possessing high transparency and heat insulation properties. It maintains functional stability during long-term use, does not affect electromagnetic signals, and meets the normal operating requirements of electronic devices.
Smart Images

Figure CN123063089A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional thin film materials technology, and in particular to a high-concentration photo-excited negative oxygen ion releasing all-nano ceramic post-installed heat insulation film and its preparation method. Background Technology
[0002] Photocatalytic negative ion releasing materials have broad application prospects in the field of functional films for automotive and architectural glass. These materials can generate negative oxygen ions under light irradiation, thereby achieving continuous purification of air inside vehicles or rooms. However, existing photocatalytic negative ion releasing technologies face significant concentration bottlenecks in practical applications, with their negative ion release rates typically only reaching 500-2000 ions / cm³. 3 This cannot meet the growing demand for air purification.
[0003] The main reasons for the aforementioned concentration bottleneck are as follows. First, the electron-hole recombination rate of traditional TiO2 photocatalysts is as high as 90% or more, resulting in low quantum efficiency and limiting the yield of negative oxygen ions. Second, the spectral response range of TiO2 is limited to the ultraviolet region below 388nm, with a utilization rate of only 3-5% for visible light. Furthermore, traditional photocatalytic materials have insufficient surface active sites and low surface hydroxyl content, limiting the effective adsorption of water and oxygen molecules. Simultaneously, existing technologies lack synergistic design for environmental factors, failing to fully consider the impact of humidity, temperature, and other conditions on photocatalytic efficiency, thus failing to achieve a significant improvement in negative oxygen ion release efficiency under different environmental conditions. On the other hand, existing automotive or architectural window films with heat insulation functions mostly use metal or metal oxide coatings for their heat insulation layers, achieving heat insulation by reflecting infrared rays. However, metal layers are prone to oxidation and failure during long-term use, leading to a decline in heat insulation performance. Additionally, the shielding effect of metal layers on electromagnetic signals such as GPS and 5G in vehicles can also affect the normal operation of electronic devices.
[0004] Therefore, how to achieve the continuous release of high concentrations of negative oxygen ions over a wide spectral response range while maintaining high transparency and heat insulation performance through systematic optimization of photocatalytic materials without any metal layer has become an urgent technical challenge. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a high-concentration photo-excited negative oxygen ion releasing all-nano-ceramic post-installed heat insulation film and its preparation method. The photocatalytic system is systematically optimized from the perspectives of carrier separation, spectral response, surface adsorption, and environmental synergy. A heat insulation functional layer is constructed using an all-inorganic nano-ceramic material system, containing no elemental metals, metal coatings, or continuous conductive metal layers. This fundamentally avoids metal oxidation failure, ensuring the functional stability of the product during long-term use and achieving continuous release of environmentally adaptive negative oxygen ions.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A high-concentration photo-excited negative oxygen ion releasing all-nano-ceramic post-installed heat insulation film comprises a functional integrated nano-ceramic coating, a PET substrate, and a pressure-sensitive adhesive layer stacked sequentially. The functional integrated nano-ceramic coating includes an infrared shielding component, a highly active photocatalytic negative oxygen ion releasing component, a structural reinforcement component, and a film-forming matrix. The infrared shielding component includes cesium tungsten bronze nanoparticles and lanthanum hexaboride nanoparticles. The highly active photocatalytic negative oxygen ion releasing component includes iron-lanthanum co-doped nitrogen-doped titanium dioxide, and composite nanosheets composed of bismuth vanadate with oxygen vacancy defects and bismuth tungstate with oxygen vacancy defects. The structural reinforcement component includes porous silica nanospheres, nano-montmorillonite, fumed silica, and polyethylene glycol. The film-forming matrix includes silica sol and an aqueous polyurethane dispersion.
[0008] Preferably, the aforementioned functional integrated nano-ceramic coating comprises the following components per 100 parts by weight: 8-12 parts cesium tungsten bronze nanoparticles, 3-5 parts lanthanum hexaboride nanoparticles, 4-6 parts iron-lanthanum co-doped nitrogen-doped titanium dioxide, 4.5-7.5 parts composite nanosheets, 3-5 parts porous silica nanospheres, 1-2 parts nano-montmorillonite, 0.1-1 parts fumed silica, 0.5-1.5 parts polyethylene glycol, 20-30 parts silica sol, 10-20 parts aqueous polyurethane dispersion, with the balance being water.
[0009] Preferably, the particle size of the aforementioned cesium tungsten bronze nanoparticles is 20-40 nm; the particle size of the lanthanum hexaboride nanoparticles is 50-80 nm.
[0010] Preferably, in the aforementioned iron-lanthanum co-doped nitrogen-doped titanium dioxide, the atomic doping amount of Fe is 1.5-2.5 at%, the atomic doping amount of La is 0.5-1.0 at%, the atomic doping amount of N is 5-10 at%, and the particle size of the iron-lanthanum co-doped nitrogen-doped titanium dioxide is 8-15 nm.
[0011] Preferably, the aforementioned composite nanosheet is a Z-shaped heterojunction composite nanosheet composed of bismuth vanadate with oxygen vacancy defects and bismuth tungstate with oxygen vacancy defects, wherein the mass ratio of bismuth vanadate with oxygen vacancy defects to bismuth tungstate with oxygen vacancy defects is 2-3:1-2; and the oxygen vacancy density of both bismuth vanadate with oxygen vacancy defects and bismuth tungstate with oxygen vacancy defects is 1×10⁻⁶. 18 -1×10 20 cm -3 .
[0012] Preferably, the aforementioned porous silica nanospheres have a particle size of 50-100 nm and a pore size of 5-10 nm.
[0013] Preferably, the dry film thickness of the aforementioned functional integrated nano-ceramic coating is 3-4 μm, the thickness of the PET substrate is 50-100 μm, and the thickness of the pressure-sensitive adhesive layer is 5-10 μm.
[0014] The preparation method of the aftermarket heat insulation film includes the following steps:
[0015] S1. Preparation of iron-lanthanum co-doped nitrogen-doped titanium dioxide powder;
[0016] S2. Prepare bismuth vanadate powder with oxygen vacancy defects and bismuth tungstate powder with oxygen vacancy defects, and combine the bismuth vanadate powder with oxygen vacancy defects and the bismuth tungstate powder with oxygen vacancy defects to form composite nanosheets.
[0017] S3. Prepare porous silica nanospheres by dispersing iron-lanthanum co-doped nitrogen-doped titanium dioxide powder and composite nanosheets, and then mixing them with porous silica nanosphere slurry so that the photocatalytic component is loaded into the pore structure of the porous silica nanospheres.
[0018] S4. Add cesium tungsten bronze, lanthanum hexaboride, silica sol, waterborne polyurethane dispersion and silane coupling agent to the loaded slurry, heat to carry out modification reaction, then add nano montmorillonite, fumed silica and polyethylene glycol, mix evenly and filter to obtain functional integrated coating.
[0019] S5. Apply the functional integrated coating to the surface of the PET substrate, dry and cure it to form a functional integrated nano-ceramic coating.
[0020] S6. Apply pressure-sensitive adhesive to the other surface of the PET substrate to form a pressure-sensitive adhesive layer, and then laminate with a release film.
[0021] Preferably, in step S4 above, after adding 0.5-2.0 parts by weight of silane coupling agent, the reaction is carried out at 55-65°C for 1.5-2.5 h; after mixing evenly, the pH value is adjusted to 8-9.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] (1) This invention systematically optimizes the photocatalytic system from the aspects of carrier separation, spectral response, surface adsorption and environmental synergy; it utilizes oxygen vacancy engineering to capture photogenerated electrons, and combines the built-in electric field of the crystal plane with the Z-type heterojunction to achieve efficient charge separation; Fe / La co-doping simultaneously achieves band gap narrowing and grain refinement, broadens the spectral response range and increases the density of active sites; it is conducive to the generation and stable existence of surface hydroxyl groups, further enhancing the adsorption capacity of oxygen and water molecules; the hygroscopic and water-retaining components can maintain a local high humidity microenvironment on the membrane surface, realizing the continuous release of environmentally adaptive negative oxygen ions;
[0024] (2) The present invention uses an all-inorganic nano-ceramic material system to construct the heat insulation functional layer, which does not contain metal elements, metal coatings and continuous metal conductive layers. This avoids the problem of metal oxidation failure from the material essence level and ensures the functional stability of the product during long-term use. The film layer has no shielding effect on electromagnetic signals and can meet the normal use requirements of electronic devices such as vehicle GPS and 5G communication. Attached Figure Description
[0025] Figure 1 The graph shows the test results of negative oxygen ion release concentration of each membrane sample in Examples 1-3 and Comparative Examples 1-4;
[0026] Figure 2 These are the optical performance test results of each film sample in Examples 1-3 and Comparative Examples 1-4;
[0027] Figure 3 The graphs show the photocatalytic activity test results of each membrane sample in Examples 1-3 and Comparative Examples 1-4. Detailed Implementation
[0028] To clearly illustrate the technical features of this solution, the following detailed implementation method will be used to explain the solution.
[0029] A high-concentration photo-excited negative oxygen ion releasing type all-nano-ceramic post-installed heat insulation film includes a functional integrated nano-ceramic coating, a PET substrate and a pressure-sensitive adhesive layer stacked sequentially. The functional integrated nano-ceramic coating includes an infrared shielding component, a highly active photocatalytic negative oxygen ion releasing component, a structural reinforcement component and a film-forming matrix.
[0030] Infrared shielding components include cesium tungsten bronze nanoparticles (Cs). 0.33 Cesium tungsten bronze nanoparticles (WO3) and lanthanum hexaboride nanoparticles (LaB6) have a particle size of 20-40 nm and a particle size of 50-80 nm.
[0031] The highly active photocatalytic negative oxygen ion releasing components include Fe-La co-doped N-TiO2, and composite nanosheets Ov-BiVO4 / Ov-Bi2WO6 composed of bismuth vanadate (BiVO4) and bismuth tungstate (Bi2WO6) with oxygen vacancy defects. In the iron-lanthanum co-doped nitrogen-doped titanium dioxide, the atomic doping amount of Fe is 1.5-2.5 at%, the atomic doping amount of La is 0.5-1.0 at%, and the atomic doping amount of N is 5-10 at%. The particle size of the iron-lanthanum co-doped nitrogen-doped titanium dioxide is 8-15 nm. The composite nanosheets are Z-shaped heterojunction composite nanosheets composed of bismuth vanadate and bismuth tungstate with oxygen vacancy defects, wherein the mass ratio of bismuth vanadate to bismuth tungstate with oxygen vacancy defects is 2-3:1-2; the oxygen vacancy density of both bismuth vanadate and bismuth tungstate with oxygen vacancy defects is 10¹⁸-10²⁰ cm⁻¹. -3 .
[0032] The structural reinforcement components include porous silica nanospheres and a moisture-absorbing and water-retaining component. The porous silica nanospheres have a particle size of 50-100 nm and a pore size of 5-10 nm. The moisture-absorbing and water-retaining component includes nano-montmorillonite, fumed silica, and polyethylene glycol PEG-400.
[0033] The film-forming matrix includes silica sol and aqueous polyurethane dispersion.
[0034] The functional integrated nano-ceramic coating comprises the following components by weight: 8-12 parts cesium tungsten bronze nanoparticles, 3-5 parts lanthanum hexaboride nanoparticles, 4-6 parts iron-lanthanum co-doped nitrogen-doped titanium dioxide, 4.5-7.5 parts composite nanosheets, 3-5 parts porous silica nanospheres, 1-2 parts nano-montmorillonite, 0.1-1 parts fumed silica, 0.5-1.5 parts polyethylene glycol, 20-30 parts silica sol, and 10-20 parts aqueous polyurethane dispersion.
[0035] The dry film thickness of the integrated functional nano-ceramic coating is 3-4 μm, the thickness of the PET substrate is 50-100 μm, and the thickness of the pressure-sensitive adhesive layer is 5-10 μm.
[0036] The preparation method of the aftermarket heat insulation film includes the following steps:
[0037] S1. Preparation of iron-lanthanum co-doped nitrogen-doped titanium dioxide powder;
[0038] S2. Prepare bismuth vanadate powder with oxygen vacancy defects and bismuth tungstate powder with oxygen vacancy defects, and combine the bismuth vanadate powder with oxygen vacancy defects and the bismuth tungstate powder with oxygen vacancy defects to form composite nanosheets.
[0039] S3. Prepare porous silica nanospheres by dispersing iron-lanthanum co-doped nitrogen-doped titanium dioxide powder and composite nanosheets, and then mixing them with porous silica nanosphere slurry so that the photocatalytic component is loaded into the pore structure of the porous silica nanospheres.
[0040] S4. Add cesium tungsten bronze, lanthanum hexaboride, silica sol, waterborne polyurethane dispersion and silane coupling agent to the loaded slurry. After adding the silane coupling agent, keep the reaction at 55-65℃ for 1.5-2.5 h. After the coating is prepared, adjust the pH value to 8-9, then add nano montmorillonite, fumed silica and polyethylene glycol, mix evenly and filter to obtain the functional integrated coating.
[0041] S5. Apply the functional integrated coating to the surface of the PET substrate, dry and cure it to form a functional integrated nano-ceramic coating.
[0042] S6. Apply pressure-sensitive adhesive to the other surface of the PET substrate to form a pressure-sensitive adhesive layer, and then laminate with a release film.
[0043] The functionally integrated coating of this invention contains multiple photocatalytic materials. When these materials are exposed to sunlight or indoor lighting, their valence band electrons transition to the conduction band, leaving positively charged holes in situ. The electrons transitioning to the conduction band are captured by oxygen molecules in the surrounding environment, generating superoxide radical anions; while the valence band holes react with water molecules or surface hydroxyl groups, generating hydroxyl radicals. In this process, the oxygen vacancies in the coating act as electron-capturing centers, effectively suppressing the recombination of electrons and holes, allowing more charge carriers to participate in surface chemical reactions, thereby significantly improving quantum efficiency. Through iron and lanthanum co-doping and the introduction of nitrogen, the band gap of the photocatalytic material is narrowed, extending its photoresponse range from the ultraviolet region to the visible light region, maintaining high photocatalytic activity even under ordinary indoor lighting. The introduction of crystal plane engineering creates a built-in electric field between different crystal planes, driving photogenerated electrons and holes to migrate to different crystal planes, achieving effective spatial separation and further reducing the recombination probability. Porous silica nanospheres, acting as a carrier, not only prevent the aggregation of photocatalytic particles but also enrich oxygen and water vapor in the air due to their mesoporous structure, increasing the local concentration of reactants. Simultaneously, nano-montmorillonite and polyethylene glycol added to the coating exert hygroscopic and water-retaining functions, maintaining a relatively humid microenvironment on the membrane surface and continuously supplying water molecules for the photocatalytic reaction. These enhancement strategies work synergistically to systematically improve the generation rate of active species in the photocatalytic reaction, ultimately resulting in the release of high concentrations of negative oxygen ions. The heat insulation function stems from the strong absorption of near-infrared light by cesium tungsten bronze and lanthanum hexaboride. These two materials dissipate the absorbed infrared light energy as heat, achieving highly efficient infrared blocking without any metal components. The entire film layer is prepared on a PET substrate through coating and can be directly bonded to existing glass surfaces, offering convenient application.
[0044] Example 1
[0045] The preparation method of the aftermarket heat insulation film includes the following steps:
[0046] S1. Preparation of Fe-La co-doped N-TiO2
[0047] (1) Tetrabutyl titanate and anhydrous ethanol were mixed at a volume ratio of 1:4 to obtain solution A;
[0048] (2) Dissolve Fe(NO3)3, La(NO3)3 and urea in deionized water, with Fe / Ti ratio of 2.0 at%, La / Ti ratio of 0.7 at%, and molar ratio of urea to Ti atoms of 3:1, and disperse uniformly to obtain solution B;
[0049] (3) Under vigorous stirring, solution B was added dropwise to solution A, stirred at room temperature for 3 hours to obtain a light yellow sol, aged at 80°C for 24 hours, dried at 100°C, and calcined at 350°C for 2 hours (N2 atmosphere) to obtain Fe-La-N-TiO2 nanoparticles.
[0050] S2, Preparation of Ov-BiVO4
[0051] Bi(NO3)3 was dissolved in dilute nitric acid to prepare a 0.2M solution. NH4VO3 was added, with a Bi to V molar ratio of 1:1. 0.5 g / L SDBS was added as a crystal facet control agent. Ethylene glycol was added at a volume ratio of 1:1 with water to adjust the pH to 2-3. The solution was transferred to a hydrothermal reactor and reacted at 180℃ for 12 h. After cooling to room temperature, the solution was centrifuged and washed. The solution was dried at 60℃ to obtain pyramidal BiVO4. BiVO4 was dispersed in a 0.1M NaBH4 solution and stirred at room temperature for 2 h. After centrifugation and washing, the solution was dried at 60℃ to obtain Ov-BiVO4.
[0052] S3, Preparation of Ov-Bi2WO6
[0053] Bi(NO3)3 and Na2WO4 were dissolved in an ethylene glycol-water mixed solvent at a volume ratio of 1:1; the pH was adjusted to 1-2, and the mixture was stirred for 30 min; the mixture was transferred to a hydrothermal reactor and reacted at 160 °C for 12 h; the mixture was cooled to room temperature, centrifuged and washed; and dried at 60 °C to obtain Bi2WO6 nanosheets; Bi2WO6 was dispersed in a 0.1 M NaBH4 solution and stirred at room temperature for 2 h; the mixture was centrifuged and washed, and dried at 60 °C to obtain Ov-Bi2WO6 nanosheets.
[0054] S4. Preparation of Ov-BiVO4 / Ov-Bi2WO6 composite nanosheets
[0055] Ov-BiVO4 and Ov-Bi2WO6 were dispersed in deionized water at a mass ratio of 2:1; ultrasonic dispersion was performed for 1 h, followed by magnetic stirring for 2 h; the mixture was reacted at 180 °C for 6 h to form a tight heterojunction interface; the mixture was then centrifuged, washed, and freeze-dried to obtain Ov-BiVO4 / Ov-Bi2WO6 composite nanosheets.
[0056] S5. Preparation of porous SiO2 nanospheres
[0057] CTAB was dissolved in an ethanol-water mixture, and the pH was adjusted to 10-11 with ammonia. TEOS was added dropwise, and the mixture was stirred at room temperature for 6 hours. After centrifugation and washing, the nanospheres were dried at 60°C and calcined at 550°C for 4 hours to obtain mesoporous SiO2 nanospheres with a pore size of 5-8 nm and a specific surface area >500 m². 2 / g.
[0058] S6, Preparation of Functional Integrated Coatings
[0059] (1) Predispersion of nanoparticles
[0060] Take 10 portions of Cs 0.33 WO3 and 4 parts of LaB6 were dispersed in deionized water, sonicated for 30 min, and ball-milled for 2 h; 5 parts of Fe-La-N-TiO2 and 6 parts of Ov-BiVO4 / Ov-Bi2WO6 were dispersed, sonicated for 30 min, and ball-milled for 1 h; 4 parts of porous SiO2 nanospheres, 1.5 parts of nano-montmorillonite, 0.5 parts of fumed SiO2 and 1 part of polyethylene glycol PEG-400 were dispersed and sonicated for 20 min.
[0061] (2) Carrier load
[0062] Fe-La-N-TiO2 and Ov-BiVO4 / Ov-Bi2WO6 slurries were mixed and then added to porous SiO2 slurry. The mixture was stirred for 2 hours to load the photocatalytic material into the porous SiO2 channels.
[0063] (3) Preparation of mixed slurry
[0064] Join Cs 0.33 WO3 and LaB6 slurry; add 25 parts silica sol and 15 parts waterborne polyurethane dispersion, and stir at high speed for 1 hour.
[0065] (4) Interface modification
[0066] Add 1.5 parts of KH-570 silane coupling agent and stir at 60°C for 2 hours to form Si-OM bonds.
[0067] (5) Adding additives
[0068] Add MMT, fumed SiO2, and PEG-400; add leveling agent, 0.8g nano ZrO2, and 0.2g defoamer; adjust pH to 8-9 and viscosity to 50-70 cP; filter to obtain a functional integrated coating.
[0069] S7. Preparation of heat insulation film
[0070] The functional integrated coating is applied to the surface of a PET substrate, with a wet film thickness of 45μm and a coating speed of 5-10m / min. Drying and curing are then carried out using the following curing process: first stage 80℃×5min (pre-baking); second stage 100℃×5min (drying); third stage 120℃×10min (curing); fourth stage 140℃×5min (post-curing); resulting in a dry film thickness of 3.5μm, forming a functional integrated nano-ceramic coating. Pressure-sensitive adhesive is then applied to the other surface of the PET substrate to form a pressure-sensitive adhesive layer, and a release film is laminated to obtain the heat insulation film product.
[0071] Example 2
[0072] The difference from Example 1 lies in the amount of each component, specifically: 8 parts cesium tungsten bronze, 3 parts lanthanum hexaboride, 6 parts iron-lanthanum co-doped nitrogen-doped titanium dioxide, 7.5 parts Ov-BiVO4 / Ov-Bi2WO6 composite nanosheets, 5 parts porous silica nanospheres, 2 parts nano-montmorillonite, 1.0 part fumed silica, 1.5 parts polyethylene glycol PEG-400, 30 parts silica sol, and 20 parts aqueous polyurethane dispersion. The preparation method is the same as in Example 1.
[0073] Example 3
[0074] The difference from Example 1 lies in the amount of each component, specifically: 12 parts of cesium tungsten bronze, 5 parts of lanthanum hexaboride, 4 parts of iron-lanthanum co-doped nitrogen-doped titanium dioxide, 4.5 parts of Ov-BiVO4 / Ov-Bi2WO6 composite nanosheets, 3 parts of porous silica nanospheres, 1.0 part of nano-montmorillonite, 0.1 part of fumed silica, 0.5 parts of polyethylene glycol, 20 parts of silica sol, and 10 parts of aqueous polyurethane dispersion.
[0075] Comparative Example 1
[0076] In Example 1, all iron-lanthanum co-doped nitrogen-doped titanium dioxide and Ov-BiVO4 / Ov-Bi2WO6 composite nanosheets were replaced with commercial P25 TiO2 (21 nm particle size, undoped, oxygen-vacancy-free), in an amount of 11 parts. The remaining components and preparation process were the same as in Example 1.
[0077] Comparative Example 2
[0078] Compared to Example 1, porous silica nanospheres, nano-montmorillonite, fumed silica, and polyethylene glycol were removed. Five parts of Fe-La-N-TiO2 and six parts of Ov-BiVO4 / Ov-Bi2WO6 were directly dispersed in a mixture of silica sol and aqueous polyurethane, without pore loading or a moisture-absorbing and water-retaining system. The remaining components and amounts were the same as in Example 1.
[0079] Comparative Example 3
[0080] A metal Ag layer heat insulation film prepared using commercially available magnetron sputtering technology was used as a control. Its structure consisted of a 75 μm PET substrate, a 0.1 μm Ag metal coating, and an 8 μm pressure-sensitive adhesive layer.
[0081] Comparative Example 4
[0082] Compared with Example 1, the specific differences are as follows: the infrared shielding component retains only 10 parts of cesium tungsten bronze, and lanthanum hexaboride is removed; the photocatalytic component is replaced with an undoped, oxygen-vacant simple physical mixture of BiVO4 / Bi2WO6 at a mass ratio of 2:1, totaling 11 parts. The remaining components are the same as in Example 1.
[0083] Performance testing
[0084] (1) Test of negative oxygen ion release concentration
[0085] The membrane samples from Examples 1-3 and Comparative Examples 1-4 were cut into 10cm × 10cm pieces and fixed to a 1m... 3 Inside a sealed acrylic testing chamber, the temperature was 25±2℃ and the relative humidity was 50±5%. An air negative ion concentration meter was used for testing, with three lighting conditions set: Condition A: Sunlight simulator, xenon lamp, AM1.5G filter, irradiance 100mW / cm². 2 Condition B: Indoor white LED light, color temperature 4000K, illuminance 500 lux; Condition C: Aluminum foil wrapping for light protection. Each sample was tested continuously for 120 minutes under each condition, and the negative oxygen ion concentration at 120 minutes was recorded. Specific results are shown in [link to results]. Figure 1 .
[0086] Depend on Figure 1 It can be seen that all three examples achieved high-concentration negative oxygen ion release. Example 2 showed the best data because the total content of the photocatalytic components was increased, and the Fe / La doping amount in Fe-La-N-TiO2 was at its upper limit, while the N doping amount reached 10 at%, resulting in the most significant bandgap narrowing effect; simultaneously, the oxygen vacancy density of Ov-BiVO4 / Ov-Bi2WO6 reached 1×10⁻⁶. 20 cm -3The highest concentration of negative oxygen ions was achieved by increasing the amount of porous SiO2 support to 5 parts, providing more reactant enrichment sites, and increasing PEG-400 to 1.5 parts, which enhanced the surface microenvironment humidity maintenance. These factors simultaneously enhanced carrier separation, spectral response, surface adsorption, and environmental synergy, resulting in the highest concentration of negative oxygen ions. Example 3 showed a relatively lower concentration due to a reduction in the total amount of photocatalytic components and an increase in the proportion of infrared shielding components. Although the concentration of negative oxygen ions decreased, it still reached 9800 ions / cm³. 3 .
[0087] Comparative Example 1: Only 1800 / cm² under sunlight 3 Only 120 per cm under LED light 3 This study verified three major bottlenecks of traditional TiO2: high electron-hole recombination rate: P25 lacks oxygen vacancy trapping centers and a Z-shaped heterojunction interface electric field, resulting in a recombination rate >90% and very few charge carriers participating in surface reactions; narrow spectral response: P25 has a band gap of approximately 3.2 eV, responding only to ultraviolet light below 388 nm, a band almost entirely absent in LEDs, thus exhibiting extremely low activity under visible light; and insufficient surface active sites: lacking crystal plane engineering control, the surface hydroxyl density is low, limiting the adsorption of water molecules and oxygen. Comparative Example 2 showed 5200 active sites / cm² under sunlight. 3 Although higher than Comparative Example 1, it was significantly lower than Example 1. This indicates that even with excellent photocatalytic materials, the lack of a porous SiO2 support leads to nanoparticle aggregation, a decrease in effective specific surface area, and insufficient exposure of active sites. The absence of montmorillonite and PEG-400 prevents the membrane surface from maintaining a localized high-humidity microenvironment. Under 50% RH conditions, the water molecule supply rate becomes the rate-limiting step, restricting the generation of hydroxyl radicals and ultimately negative oxygen ions. Comparative Example 3 released almost no negative oxygen ions because it completely lacked a photocatalytic functional layer. Comparative Example 4 fell between Comparative Example 1 and Examples 1-3, indicating that while a single infrared shielding material and an unmodified photocatalyst have basic functions, they lack synergistic optimization. The absence of LaB6 resulted in incomplete coverage of the infrared absorption band; the lack of oxygen vacancies and Z-shaped heterojunctions led to low carrier separation efficiency; and the lack of doping resulted in a wide band gap and poor visible light utilization.
[0088] (2) Thermal insulation and optical performance testing
[0089] The transmittance of each sample in the 280-2500 nm wavelength range was measured using a UV-Vis-NIR spectrophotometer. Visible transmittance (VLT, 380-780 nm), UV blocking rate (280-380 nm), and near-infrared blocking rate (NIR, 780-2500 nm) were calculated. The infrared lamp-temperature difference method was used. The sample was placed over the window of an insulated chamber, with a thermocouple thermometer and a 250W infrared lamp placed inside at a distance of 30 cm. Irradiation was performed for 30 minutes, and the temperature rise inside the chamber and the temperature difference compared to the blank control were recorded. Specific results are shown in [link to results]. Figure 2 See Table 1.
[0090] Table 1 Thermal insulation performance of Examples 1-3 and Comparative Examples 1-4
[0091]
[0092] pass Figure 2 As shown in Table 1, the NIR blocking rates of Examples 1-3 are all greater than 89%, with Example 3 reaching as high as 95.8%, and the VLTs are all greater than 68%, meeting the light transmittance regulations for automotive windshield films and architectural glass films. This proves that Cs 0.33 Synergistic effect of WO3 and LaB6, Cs 0.33 The free electrons and polarons in WO3 exhibit strong absorption in the 900-1500nm near-infrared band; the plasmon resonance absorption of LaB6 mainly covers the 1000-2000nm band. The two complement each other, covering the entire near-infrared band and dissipating infrared energy as heat rather than reflection. Comparative Example 3 has an NIR blocking rate of 96.5% and a temperature difference of 13.8℃, slightly higher than Example 3, which is a typical characteristic of metal reflective thermal insulation. However, the advantages of metal films are only reflected in static thermal insulation data; their long-term stability and electromagnetic compatibility have serious defects. Comparative Example 4 has an NIR blocking rate of only 85.2%, indicating that a single infrared absorbing material is difficult to cover the entire band, and the supplementary absorption of long-wavelength near-infrared by LaB6 is crucial. The thermal insulation data of Comparative Examples 1 and 2 are close to those of Example 1, indicating that the infrared shielding performance is mainly determined by Cs. 0.33 The presence of WO3 and LaB6 indicates that the photocatalytic and structural reinforcement components have relatively little impact on the coating, reflecting the functional independence of each component in the integrated functional coating.
[0093] (3) Photocatalytic activity test
[0094] In 1m 3 In a sealed environment testing chamber, formaldehyde standard gas was injected to achieve an initial concentration of 1.00 ± 0.05 mg / m³. 3 Membrane samples (10cm × 10cm) from Examples 1-3 and Comparative Examples 1-4 were attached to the inner wall of the chamber, and irradiated with a solar simulator for 4 hours. The formaldehyde concentration inside the chamber was measured every hour using a phenol reagent spectrophotometer, and the formaldehyde degradation rate over 4 hours was calculated. Specific results are shown in [link to results]. Figure 3 .
[0095] Depend on Figure 3It can be seen that the formaldehyde degradation rate in Examples 1-2 was greater than 92% in 4 hours, and in Example 2 it reached 97%, indicating that the photocatalytic system of the present invention has extremely high quantum efficiency. The reason is that: oxygen vacancies, as electron trapping centers, significantly suppress electron-hole recombination; the conduction band electrons of Ov-BiVO4 and the valence band holes of Ov-Bi2WO6 recombine through the interface, retaining the high oxidizing valence band holes of Ov-BiVO4 and the high reducing conduction band electrons of Ov-Bi2WO6, thereby maximizing the redox capacity; the band gap is narrowed to below 2.5 eV, the spectral response is extended to above 500 nm, and the utilization rate of sunlight is significantly improved.
[0096] The degradation rate of Comparative Example 1 was only 22%, further confirming the shortcomings of traditional TiO2, such as severe electron-hole recombination and no visible light response. The degradation rate of Comparative Example 2 was 58%, higher than Comparative Example 1 but lower than Example 1. This is because although the photocatalytic material itself has high activity, the lack of a porous SiO2 support leads to agglomeration, reducing the effective reaction area; simultaneously, the lack of hygroscopic and water-retaining components results in insufficient adsorption of gaseous formaldehyde and water molecules on the membrane surface, limiting the reaction rate. This data, from the perspective of pollutant degradation, corroborates the importance of porous structure and humidity regulation for enhanced surface adsorption. The degradation rate of Comparative Example 4 was 45%, indicating that although undoped, oxygen-vacancy-free BiVO4 / Bi2WO6 has basic visible light activity, the lack of a Z-type heterojunction charge separation mechanism and oxygen vacancy trapping centers results in a short carrier lifetime and a significant decrease in degradation efficiency.
[0097] (4) Electromagnetic signal transmittance test
[0098] The transmittance of the sample to electromagnetic waves in the GPS L1 band (1575.42MHz) and the 5G n78 band (3.5GHz) was tested using a vector network analyzer or the signal source-power meter method. The sample size was 10cm × 10cm, and the tests were conducted in a microwave anechoic chamber. Insertion loss was recorded, and the specific results are shown in Table 2.
[0099] Table 2 Electromagnetic signal transmittance test results of Examples 1-3 and Comparative Examples 1-4
[0100]
[0101] As shown in Table 2, the electromagnetic transmission loss of Examples 1-3 and Comparative Examples 1, 2, and 4 is all <0.3dB, equivalent to a signal transmittance >97%, fully meeting the normal usage requirements of in-vehicle GPS navigation, ETC communication, and 5G mobile phone signals. This is because the functional integrated coating of the present invention is entirely composed of inorganic oxides, nitrides, and borides, without any continuous metal layers or high-concentration free-electron metal components. The material has a low intrinsic dielectric constant and does not produce an electromagnetic shielding effect. Comparative Example 3 shows a loss of 28.5dB in the GPS band and 35.2dB in the 5G band, with the signal almost completely shielded. The high conductivity of the Ag metal layer causes strong electromagnetic wave reflection, which is an inherent defect of metal heat insulation films and directly affects the function of in-vehicle electronic equipment.
[0102] (5) Weather resistance and functional stability test
[0103] QUV accelerated aging: Following ASTM G154 standards, using UVA-340 lamps, the illumination cycle was 60℃ / 8h, and the condensation cycle was 50℃ / 4h, for a continuous period of 1000h. High temperature and high humidity aging: Placed at 85℃ / 85%RH for 1000h. The concentration of negative oxygen ions released (sunlight, 120min) and NIR blocking rate were measured before and after aging. Specific results are shown in Table 3.
[0104] Table 3. Weather resistance and functional stability test results
[0105]
[0106] As shown in Table 3, after rigorous aging, Examples 1 and 3 exhibited a negative oxygen ion retention rate greater than 89% and an NIR blocking rate retention rate greater than 98%, demonstrating excellent functional stability. This is because Fe-La-N-TiO2 and Ov-BiVO4 / Ov-Bi2WO6 are both crystalline inorganic oxides / nitrides, and the photogenerated carriers participate in the surface redox reaction without being consumed by the material itself; furthermore, the photocatalytic components are loaded within the porous SiO2 channels, protected by the support, and are less prone to agglomeration and deactivation. 0.33 WO3 and LaB6 are entirely inorganic ceramic materials and do not have the problem of metal oxidation. Cs 0.33 The Cs⁺ in WO3 stabilizes the oxygen vacancies in the WO3 lattice, while the boride structure of LaB6 provides strong chemical inertness. After the silica sol cures, it forms a Si-O-Si network, and the waterborne polyurethane provides flexibility. The entire coating is dense, blocking the penetration of water vapor and oxygen.
[0107] Comparative Example 3, after 85 / 85 aging, saw its NIR blocking rate plummet from 96.5% to 75.8%. This is because the Ag metal layer underwent electrochemical corrosion and oxidation under high temperature and humidity conditions, generating insulating oxides such as Ag₂O, which disrupted the continuity and conductivity of the metal layer, leading to a sharp decrease in infrared reflectivity. Comparative Example 1 exhibited a negative oxygen ion retention rate of only 58.3%. This is because P₂₅ is prone to photocorrosion under light and lacks carrier protection. Furthermore, the nanoparticles agglomerated and grew during the aging process, resulting in a decrease in specific surface area and a reduction in active sites.
[0108] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any way, and all technical solutions obtained by equivalent substitution or equivalent transformation fall within the protection scope of the present invention.
Claims
1. A high-concentration photo-excited negative oxygen ion releasing all-nano ceramic post-installed heat insulation film, characterized in that, The product comprises a functional integrated nano-ceramic coating, a PET substrate, and a pressure-sensitive adhesive layer stacked sequentially. The functional integrated nano-ceramic coating includes an infrared shielding component, a highly active photocatalytic negative oxygen ion releasing component, a structural reinforcement component, and a film-forming matrix. The infrared shielding components include cesium tungsten bronze nanoparticles and lanthanum hexaboride nanoparticles; The highly active photocatalytic negative oxygen ion releasing component includes iron-lanthanum co-doped nitrogen-doped titanium dioxide, and composite nanosheets composed of bismuth vanadate with oxygen vacancy defects and bismuth tungstate with oxygen vacancy defects. The structural reinforcement components include porous silica nanospheres, nano-montmorillonite, fumed silica, and polyethylene glycol; The film-forming matrix includes silica sol and aqueous polyurethane dispersion.
2. The photo-excited negative oxygen ion releasing type all-nano ceramic post-installed heat insulation film according to claim 1, characterized in that, The functional integrated nano-ceramic coating comprises the following components per 100 parts by weight: 8-12 parts cesium tungsten bronze nanoparticles, 3-5 parts lanthanum hexaboride nanoparticles, 4-6 parts iron-lanthanum co-doped nitrogen-doped titanium dioxide, 4.5-7.5 parts composite nanosheets, 3-5 parts porous silica nanospheres, 1-2 parts nano-montmorillonite, 0.1-1 parts fumed silica, 0.5-1.5 parts polyethylene glycol, 20-30 parts silica sol, 10-20 parts aqueous polyurethane dispersion, with the balance being water.
3. The photo-excited negative oxygen ion releasing type all-nano ceramic post-installed heat insulation film according to claim 1, characterized in that, The cesium tungsten bronze nanoparticles have a particle size of 20-40 nm; the lanthanum hexaboride nanoparticles have a particle size of 50-80 nm.
4. The photo-excited negative oxygen ion releasing type all-nano ceramic post-installed heat insulation film according to claim 1, characterized in that, In the iron-lanthanum co-doped nitrogen-doped titanium dioxide, the atomic doping amount of Fe is 1.5-2.5 at%, the atomic doping amount of La is 0.5-1.0 at%, the atomic doping amount of N is 5-10 at%, and the particle size of the iron-lanthanum co-doped nitrogen-doped titanium dioxide is 8-15 nm.
5. The photo-excited negative oxygen ion releasing type all-nano ceramic post-installed heat insulation film according to claim 1, characterized in that, The composite nanosheet is a Z-shaped heterojunction composite nanosheet composed of bismuth vanadate with oxygen vacancy defects and bismuth tungstate with oxygen vacancy defects, wherein the mass ratio of bismuth vanadate with oxygen vacancy defects to bismuth tungstate with oxygen vacancy defects is 2-3:1-2; the oxygen vacancy density of both bismuth vanadate with oxygen vacancy defects and bismuth tungstate with oxygen vacancy defects is 1×10⁻⁶. 18 -1×10 20 cm -3 .
6. The photo-excited negative oxygen ion releasing type all-nano ceramic post-installed heat insulation film according to claim 1, characterized in that, The porous silica nanospheres have a particle size of 50-100 nm and a pore size of 5-10 nm.
7. The photo-excited negative oxygen ion releasing type all-nano ceramic post-installed heat insulation film according to claim 1, characterized in that, The dry film thickness of the integrated functional nano-ceramic coating is 3-4 μm, the thickness of the PET substrate is 50-100 μm, and the thickness of the pressure-sensitive adhesive layer is 5-10 μm.
8. A method for preparing a retrofitted heat insulation film according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Preparation of iron-lanthanum co-doped nitrogen-doped titanium dioxide powder; S2. Prepare bismuth vanadate powder with oxygen vacancy defects and bismuth tungstate powder with oxygen vacancy defects, and combine the bismuth vanadate powder with oxygen vacancy defects and the bismuth tungstate powder with oxygen vacancy defects to form composite nanosheets. S3. Prepare porous silica nanospheres by dispersing iron-lanthanum co-doped nitrogen-doped titanium dioxide powder and composite nanosheets, and then mixing them with porous silica nanosphere slurry so that the photocatalytic component is loaded into the pore structure of the porous silica nanospheres. S4. Add cesium tungsten bronze, lanthanum hexaboride, silica sol, waterborne polyurethane dispersion and silane coupling agent to the loaded slurry, heat to carry out modification reaction, then add nano montmorillonite, fumed silica and polyethylene glycol, mix evenly and filter to obtain functional integrated coating. S5. Apply the functional integrated coating to the surface of the PET substrate, dry and cure it to form a functional integrated nano-ceramic coating. S6. Apply pressure-sensitive adhesive to the other surface of the PET substrate to form a pressure-sensitive adhesive layer, and then laminate with a release film.
9. The preparation method according to claim 8, characterized in that, In step S4, after adding the silane coupling agent, the mixture is kept at 55-65°C for 1.5-2.5 h; after mixing evenly, the pH value is adjusted to 8-9.
10. The application of the aftermarket heat insulation film according to any one of claims 1-7 in the application of film to the surface of architectural or automotive glass.