A heat treatment method for coordinated temperature control in high-speed steel forging
By using a heat treatment method that coordinates temperature control during high-speed steel forging, the problem of dynamic generation and reduction of carbide-related micropores during high-speed steel forging was solved, achieving uniform cooling and performance improvement of forgings, and enhancing the material's impact absorption energy and internal quality.
Patent Information
- Application Number
- CN202611576230.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies have failed to effectively control the dynamic generation and reduction of carbide-related micropores during high-speed steel forging, leading to increased internal damage to forgings and affecting material properties.
A high-speed steel forging temperature-coordinated heat treatment method is adopted. By controlling the final forging temperature, rapid cooling rate and temperature difference between the near-surface and core, uniform cooling of the forging is achieved. This includes preheating, homogenization control, multi-stage forging, rapid cooling and controlled heat exchange. Combined with the circulation and temperature regulation of the gas medium, the temperature uniformity of the forging is ensured in the later stage of forging.
While reducing carbide-related micropores, it improves the room temperature impact absorption energy of forgings, reduces the area fraction of carbide-related pores and the average aperture of interfacial pores, and enhances the overall performance of the material.
Smart Images

Figure CN123063579A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-speed steel hot working and heat treatment technology, and in particular to a heat treatment method for coordinating temperature control during high-speed steel forging. Background Technology
[0002] High-speed steel contains a lot of alloying elements such as W, Mo, Cr, and V. During solidification, it is easy to form primary carbides such as M2C, MC, and M6C. Forging is an important step in the preparation of high-speed steel. It can break up coarse and network carbides through plastic deformation, improve the distribution of carbides, and control the microstructure by combining it with post-forging heat treatment.
[0003] Existing technologies mainly promote the crushing and homogenization of coarse carbides by adjusting forging temperature, deformation method, and deformation degree. For example, Chinese patent CN113355584A discloses a high-cobalt, high-molybdenum ultra-hard high-speed steel and a method for improving its hot working properties. Different forging methods are used depending on the forging temperature; light forging at higher temperatures reduces cracking tendency, while heavy forging at lower temperatures promotes carbide crushing. The hot working microstructure of the high-speed steel is improved by controlling the number of forgings and the total forging ratio. Chinese patent CN102418042A... A Chinese patent discloses a manufacturing process for forging round bars of high-carbon, high-chromium cold work die steel. This process involves sequentially performing symmetrical deformation forging, asymmetrical deformation forging, and finished product forging, while controlling the amount of deformation per pass at different stages to break up large carbide particles, improve the inhomogeneity of eutectic carbides, and reduce forging cracks. Another Chinese patent, CN116497197A, discloses a method for refining carbides in high-carbon alloy steel. This method involves repeatedly breaking down and dissolving primary carbides through thermomechanical deformation and isothermal diffusion cycles, thereby obtaining smaller and more uniformly distributed carbides.
[0004] However, the above-mentioned technologies have not fully considered the evolutionary characteristics of carbide-related micropores, which have both dynamic generation and dynamic reduction during continuous hot deformation. Hou Zhiyuan et al.'s study on "Pore Formation and Evolution Mechanism during Hot Deformation of M50 Bearing Steel" published in Acta Metallurgica Sinica pointed out that non-coordinated deformation between M2C and MC carbides and the matrix will generate pores at the interface between carbides and the matrix, and carbide breakage will also promote the formation of pores inside. Further quantitative studies show that the number of pores does not increase continuously with the degree of deformation. The number of pores reaches a high level under moderate deformation, but after further increasing plastic deformation, some existing pores will be compressed and self-welded due to the further plastic flow of the surrounding matrix, which will cause the number of pores to decrease. Summary of the Invention
[0005] The technical problem to be solved by this invention is: after high-speed steel has completed final forging and stopped forging, while reducing the further breakage of primary carbides and the addition of new carbide-related micropores caused by additional plastic deformation, we further regulate the carbide-related micropores already formed in the final forging stage. To this end, we propose a heat treatment method for co-controlling the forging temperature of high-speed steel.
[0006] This invention provides a heat treatment method for temperature synergistic control during high-speed steel forging, comprising the following steps:
[0007] S1: Select high-speed steel billet, clean the surface of the billet, heat the billet to 550-650℃ for the first stage of preheating, then raise the temperature to 800-900℃ for the second stage of preheating, and then raise the temperature to 1120-1140℃ so that the cross section of the billet reaches the homogeneous heating state required for forging before it is taken out of the furnace for forging.
[0008] The solubility state refers to the core temperature of the billet reaching within ±10℃ of the set forging heating temperature, and the absolute value of the difference between the near-surface temperature and the core temperature not exceeding 30℃. The near-surface temperature and core temperature can be determined by a process monitoring sample with the same material as the billet to be forged and the same cross-sectional shape and equivalent cross-sectional size. The process monitoring sample and the forging to be processed undergo the corresponding heating or heat exchange environment synchronously in the same posture, and are used to determine the temperature control system for the corresponding specification forging after pre-calibration.
[0009] The high-speed steel is either W6Mo5Cr4V2 high-speed steel or M35 high-speed steel.
[0010] S2: The high-speed steel billet that has been preheated before forging is forged and plastically deformed by at least one of upsetting, drawing, and die forging.
[0011] During the forging process before final forging, forging is stopped when the temperature of the forging drops below 900°C. The forging is then reheated to 1120-1140°C. Forging continues after the cross-section of the forging reaches the homogenized state described in step S1. During the final forging, the forging reaches the target size, and the forging characterization temperature T1 at the end of the final forging is controlled at 890-910°C. Forging deformation is stopped after the target size is reached.
[0012] S3: Within 5-60 seconds after the final forging, the forging that retains the residual heat of the final forging is transferred to a controlled heat exchange environment with a temperature lower than T1. A gaseous heat exchange medium is used to flow through multiple outer surfaces of the forging simultaneously. The heat exchange intensity of each outer surface of the forging is adjusted by circulating the heat exchange medium, changing the relative position between the forging and the heat exchange medium, or a combination of both, so that each outer surface of the forging enters a controlled forced convection heat exchange state.
[0013] The gas heat exchange medium is nitrogen or argon.
[0014] S4: The temperature at a distance of 5-10 mm from the surface of the forging is taken as the near-surface temperature, the temperature at the center of the forging cross-section is taken as the core temperature, and the arithmetic mean of the near-surface temperature and the core temperature is taken as the forging characterization temperature. After the forging enters the controlled heat exchange environment, the forging characterization temperature at this time is recorded as T0. By adjusting the temperature and flow rate of the heat exchange medium, the forging characterization temperature is reduced from T0 to the rapid cooling termination temperature T2 of 800-870℃ at an average cooling rate of 0.8-2.0℃ / s; where (T1-T2) is 40-110℃. After the forging enters the controlled heat exchange environment, its cooling process is controlled by adjusting the temperature and flow rate of the heat exchange medium.
[0015] The average cooling rate is calculated according to the following formula: ;
[0016] Wherein, T0 is the forging characterization temperature when the forging enters the controlled heat exchange environment, Δt is the time it takes for the forging characterization temperature to decrease from T0 to T2, and the average cooling rate is used to characterize the controlled rapid cooling rate of the forging from T0 to T2 after entering the controlled heat exchange environment.
[0017] The heat exchange conditions are adjusted based on the current cooling rate of the forging's characteristic temperature and the absolute value of the temperature difference between the near-surface and core layers. When the temperature difference between the near-surface and core layers is less than 40°C, the heat exchange conditions are adjusted according to the current cooling rate. When the current cooling rate is less than 0.8°C / s, the flow rate of the gas heat exchange medium is increased and / or the temperature of the gas heat exchange medium is decreased. When the current cooling rate is greater than 2.0°C / s, the flow rate of the gas heat exchange medium is decreased and / or the temperature of the gas heat exchange medium is increased. When the temperature difference between the near-surface and core layers reaches or exceeds 40°C, the flow rate of the gas heat exchange medium is preferentially decreased and / or the temperature of the gas heat exchange medium is increased, and the forging is rotated and / or the flow direction of the gas heat exchange medium is changed. When the temperature difference between the near-surface and core layers decreases to below 30°C, the flow rate and / or temperature of the gas heat exchange medium are adjusted according to the current cooling rate to continue cooling the forging.
[0018] S5: When the forging characterization temperature reaches T2±10℃, the forging is held within the T2±10℃ range for 1-5 minutes. During the holding period, no further mechanical forging is performed. The transition holding can be achieved in the original controlled heat exchange environment by adjusting the temperature of the gas heat exchange medium to T2±10℃ and reducing the gas flow rate. Alternatively, the forging can be transferred to a constant temperature holding environment with the temperature set at T2±10℃ within a specified time. Preferably, the gas heat exchange medium flow rate is reduced to 20-30% of the flow rate during the rapid cooling stage.
[0019] S6: After the transition holding is completed, no independent reheating process is set. The first annealing temperature T3 is 800-870℃, and T2≥T3 is satisfied. When T2 equals T3, after the transition holding is completed, continue to hold at T3 for 1-6 hours. When T2 is higher than T3, let the forging continue to decrease from T2 to T3 at a rate of 0.1-2℃ / min, and then hold at T3 for 1-6 hours.
[0020] S7: After the first annealing, reduce the temperature of the forging to 650-750℃ at an average cooling rate of 5-30℃ / h, then furnace cool to no higher than 500℃ and air cool to room temperature, or continue furnace cooling to room temperature.
[0021] Depending on the high-speed steel grade, forging hardness, and subsequent machining requirements, after completing the slow cooling treatment in step S7, spheroidizing annealing or isothermal annealing can be performed. Spheroidizing annealing involves reheating the forging to the spheroidizing annealing temperature of the corresponding steel grade, holding it at that temperature, and then slowly cooling it to make the carbides tend to spheroidize. Isothermal annealing involves heating the forging to the annealing temperature of the corresponding steel grade, holding it at that temperature, cooling it to the isothermal transformation temperature and holding it until the microstructure transformation is complete, and then cooling it to room temperature. The subsequent annealing is used to adjust the hardness and microstructure of the forging and is not a necessary step for controlling the micropore state of carbides in steps S4 to S6.
[0022] The near-surface temperature and core temperature can be measured using process monitoring samples with the same material, cross-sectional shape, and equivalent cross-sectional dimensions as the forging to be processed. Temperature sensors are installed at the process monitoring samples at a distance of 5-10 mm from the surface and at the center of the cross-section. The relationship between the near-surface temperature and core temperature and the processing time is obtained through the process monitoring samples, and a temperature control system for the corresponding specifications of forgings is established in advance. During the final forging process, the forging characterization temperature T1 at the end of the final forging can be determined according to the pre-calibrated temperature control system. During the controlled heat transfer process after the final forging, the near-surface temperature and core temperature of the forging can be measured by the synchronously set process monitoring samples or determined according to the pre-calibrated relationship.
[0023] The technical effects and advantages of this invention are as follows:
[0024] Compared with conventional cooling after final forging, this invention, after stopping mechanical deformation during final forging, simultaneously controls the average cooling rate between the final forging temperature and the rapid cooling termination temperature, as well as the maximum temperature difference between the near-surface layer and the core. This results in a final forging with a lower carbide-related void area fraction and a smaller average interface void opening. Without a significant increase in the proportion of primary carbide breakage, room temperature impact energy absorption is improved, and a synergistic relationship is observed between rapid cooling and the control of the near-surface layer and the core temperature difference. Attached Figure Description
[0025] The disclosure of this invention is illustrated with reference to the accompanying drawings. It should be understood that the drawings are for illustrative purposes only and are not intended to limit the scope of protection of this invention. In the drawings:
[0026] Figure 1 This is a flowchart of the high-speed steel forging temperature coordinated control heat treatment method of the present invention. Detailed Implementation
[0027] Example 1: As Figure 1 As shown, this embodiment uses W6Mo5Cr4V2 high-speed steel as the test material, and a cylindrical billet with dimensions of φ240mm×1200mm is used. The specific processing steps are as follows:
[0028] S1: Clean the surface of the high-speed steel billet to remove oxide scale and visible surface defects, and place the billet in a heating furnace for graded heating.
[0029] First, heat the billet to 600℃ for the first stage of preheating. When the core temperature of the billet reaches 600±10℃ and the absolute value of the temperature difference between the near-surface layer and the core temperature is no greater than 20℃, hold it at that temperature for 10 minutes. Then, raise the temperature to 850℃ for the second stage of preheating. When the core temperature of the billet reaches 850±10℃ and the absolute value of the temperature difference between the near-surface layer and the core temperature is no greater than 20℃, hold it at that temperature for 10 minutes. After that, continue to raise the temperature to 1140℃ for pre-forging heating.
[0030] Temperature monitoring was performed using a process monitoring sample with the same material and cross-sectional dimensions as the billet to be forged. Thermocouples were placed at a distance of 8 mm from the surface of the process monitoring sample and at the center of the cross-section. The temperature detected at a distance of 8 mm from the surface was taken as the near-surface temperature, and the temperature detected at the center of the cross-section was taken as the core temperature. When the core temperature reached 1130±10℃ and the absolute value of the difference between the near-surface temperature and the core temperature was not greater than 20℃, the pre-forging heating was completed and the sample was taken out of the furnace for forging.
[0031] S2: First, the φ240mm×1200mm billet is forged in multiple passes. During the forging process before the final forging, when the temperature of the forging drops to 900℃, the forging is stopped and the forging is reheated to 1120-1140℃. After the forging reaches the homogeneous state, the forging continues.
[0032] During the final forging, forging continues until the diameter of the forging reaches 95mm, and the characterization temperature T1 of the forging at the end of the final forging is controlled at 900±10℃. When the forging reaches the above target size, the forging pressure is stopped, and no forging, upsetting, drawing or die forging operations are performed on the forging from the end of the final forging until the end of the subsequent heat treatment.
[0033] S3: Within 15 seconds after the final forging is completed, the forging that retains the residual heat of the final forging will be transferred to a controlled heat exchange environment with a temperature lower than the final forging temperature.
[0034] Nitrogen is used as the heat exchange medium, and the circulating nitrogen flows through the circumferential outer surface and two end faces of the forging simultaneously. At the beginning of rapid cooling, the temperature of the circulating nitrogen is controlled at 760±10℃, and the nitrogen is circulated along the outer surfaces of the forging through the circulating fan and the guide channel.
[0035] During the cooling process, the heat transfer intensity of different outer surfaces of the forging is adjusted by regulating the flow rate of circulating nitrogen and by rotating the forging around its longitudinal axis or changing the direction of nitrogen flow as needed, based on the temperature drop of different outer surfaces of the forging.
[0036] S4: The rapid cooling process is monitored synchronously using a process monitoring sample with the same material and cross-sectional dimensions as the forging to be treated. Thermocouples are set at 8 mm from the surface of the process monitoring sample and at the center of the cross-section. The temperature at 8 mm from the surface is taken as the near-surface temperature, and the temperature at the center of the cross-section is taken as the core temperature. The arithmetic mean of the near-surface temperature and the core temperature is taken as the forging characterization temperature.
[0037] By adjusting the temperature and flow rate of circulating nitrogen, the forging temperature is rapidly reduced from 900±10℃ to 850±10℃. After the forging enters the controlled nitrogen heat exchange environment, the forging's characteristic temperature upon entering the environment is used as the starting temperature for rapid cooling. By adjusting the temperature and flow rate of circulating nitrogen, the forging's characteristic temperature is reduced to 850±10℃. The average cooling rate during this controlled rapid cooling phase is controlled at 1.5±0.3℃ / s. After the forging enters the controlled nitrogen heat exchange environment, the temperature and flow rate of circulating nitrogen are adjusted based on the current cooling rate and the temperature difference between the near-surface and core layers, controlling the temperature difference between the near-surface and core layers to be no greater than 30℃.
[0038] During rapid cooling, when the temperature difference between the near-surface layer and the core is less than 25℃, the current cooling rate is calculated based on the decrease in the forging's characteristic temperature and the corresponding time interval between two adjacent temperature sampling times. When the current cooling rate is below 1.2℃ / s, the circulating nitrogen flow rate is increased and / or the circulating nitrogen temperature is decreased. When the current cooling rate is above 1.8℃ / s, the circulating nitrogen flow rate is decreased and / or the circulating nitrogen temperature is increased. When the temperature difference between the near-surface layer and the core reaches or exceeds 25℃, the circulating nitrogen flow rate is preferentially reduced, and the forging is rotated around the longitudinal axis and / or the flow direction of the circulating nitrogen is changed. When the temperature difference between the near-surface layer and the core decreases to below 20℃, the circulating nitrogen flow rate and / or the circulating nitrogen temperature are adjusted according to the current cooling rate to continue cooling the forging.
[0039] When the forging temperature reaches 850±10℃, the circulating nitrogen temperature is adjusted to 850±10℃, and the circulating nitrogen flow rate is reduced to 20-30% of the flow rate during the rapid cooling phase, so that the forging enters the transition holding phase from the state of controlled rapid cooling between the near-surface layer and the core.
[0040] S5: Continue to keep the forging in the controlled nitrogen environment of step S4, and maintain the temperature of the forging at 850±10℃ for 3 minutes. During the holding process, maintain nitrogen circulation to reduce the temperature difference between different positions of the forging. Do not perform forging, upsetting, drawing or die forging operations on the forging.
[0041] S6: After completing the 3-minute transition hold, continue to maintain the controlled ambient temperature at 850±10℃, allowing the forging to directly enter the first annealing stage. Continue to hold at 850±10℃ for 3 hours. After the first annealing is completed, reduce the temperature of the forging from 850℃ to 700℃ at an average cooling rate of 15℃ / h. Then, cool it in the furnace to below 500℃, and finally remove the forging from the furnace and air cool it to room temperature.
[0042] Example 2: This example uses M35 high-speed steel. The remaining processing steps are the same as in Example 1, except that: the forging characterization temperature T1 at the end of the final forging is controlled at 900±10℃. Within 20 seconds after the end of the final forging, the forging is transferred to a controlled nitrogen forced convection heat exchange environment. The circulating nitrogen temperature is 780±10℃ at the start of rapid cooling. The forging characterization temperature when the forging enters the controlled heat exchange environment is recorded as T0. By adjusting the temperature and flow rate of the circulating nitrogen, the forging characterization temperature is reduced from T0 to 860±10℃. The average cooling rate of this controlled rapid cooling stage is controlled at 1.2±0.3℃ / s. During the rapid cooling process, the temperature difference between the near-surface layer and the core layer is no more than 30℃.
[0043] When the forging characterization temperature reaches 860±10℃, the circulating nitrogen temperature is adjusted to 860±10℃ and the circulating nitrogen flow rate is reduced to allow the forging to enter the transition holding stage. After holding at 860±10℃ for 3 minutes, no independent reheating step is set, and the first annealing treatment is carried out by holding at 860±10℃ for 3 hours.
[0044] Comparative Example 1: This comparative example uses the same W6Mo5Cr4V2 high-speed steel billet as Example 1. The pre-forging staged heating, forging forming, and final forging conditions are all the same as in Example 1. The only difference is that after the final forging at 900±10℃, the controlled rapid cooling of the near-surface and core temperature difference as described in Example 1 is not performed. Instead, the forging is directly transferred to a protective atmosphere furnace that has been stabilized at 850±10℃ within 15 seconds, allowing the forging to cool naturally in the furnace. When the characterization temperature of the forging drops to 850±10℃, it is first held at 850±10℃ for 3 minutes, and then held at this temperature for 3 hours for the first annealing treatment. After that, it is slowly cooled to room temperature in the manner of Example 1.
[0045] Comparative Example 2: Except for the rapid cooling method after final forging, the other steps in this comparative example are the same as in Example 1. Within 15 seconds after the final forging, the forging at 900±10℃ is transferred to a nitrogen forced convection cooling environment. Nitrogen gas at 760±10℃ is used to force-cool the outer surface of the forging. The average cooling rate of the forging is controlled to be 1.5±0.3℃ / s by adjusting the nitrogen flow rate.
[0046] During the cooling process, the cross-section is nearly isothermal controlled without rotating the forging, reversing the airflow, or adjusting the heat transfer intensity based on the temperature difference between the near-surface and core layers. This ensures that the maximum temperature difference between the near-surface and core layers of the forging reaches more than 80°C.
[0047] When the forging characterization temperature reaches 850±10℃, the ambient temperature is adjusted to 850±10℃, and the forging is held at 850±10℃ for 3 minutes. Then, it is held at this temperature for 3 hours for the first annealing treatment, and then slowly cooled to room temperature in accordance with the method of Example 1.
[0048] Comparative Example 3: Except for the temperature path after the transition, the other steps in this comparative example are the same as those in Example 1. According to the method of Example 1, the final forging is rapidly reduced from a near isothermal temperature of 900±10℃ to 850±10℃, and held at 850±10℃ for 3 minutes.
[0049] After the transition holding period, instead of directly entering the first annealing stage, the forging is heated from 850±10℃ to 900±10℃ at a heating rate of 5℃ / min and held at 900±10℃ for 10min. Then, the temperature is lowered back to 850±10℃ at a cooling rate of 5℃ / min and held at 850±10℃ for 3h for the first annealing treatment. Finally, it is slowly cooled to room temperature in accordance with the method in Example 1.
[0050] Comparative Example 4: This comparative example uses the same W6Mo5Cr4V2 high-speed steel billet as Example 1. The pre-forging staged heating, forging forming, final forging temperature and transfer time after final forging are the same as in Example 1. The difference lies in the cooling rate after final forging.
[0051] Within 15 seconds after the final forging at 900±10℃, the forging is transferred to a controlled nitrogen forced convection heat exchange environment, using nitrogen as the heat exchange medium. By reducing the circulating nitrogen flow rate and adjusting the circulating nitrogen temperature, the average cooling rate of the forging during the process of decreasing from 900±10℃ to 850±10℃ is controlled to be 0.15±0.05℃ / s.
[0052] During the cooling process, the flow rate of circulating nitrogen is adjusted according to the changes in near-surface temperature and core temperature. The forging is rotated around the longitudinal axis and / or the flow direction of circulating nitrogen is changed as needed to keep the temperature difference between the near-surface and core temperatures no greater than 30°C.
[0053] When the forging characterization temperature reaches 850±10℃, the circulating nitrogen temperature is adjusted to 850±10℃ and the circulating nitrogen flow rate is reduced to put the forging into a locked holding state. After holding at 850±10℃ for 3 minutes, no independent reheating step is set, and the forging is held at 850±10℃ for 3 hours for the first annealing treatment. Then, it is slowly cooled to room temperature according to the method in Example 1.
[0054] Experimental Example 1: High-speed steel forgings processed in Examples 1, 2 and Comparative Examples 1-4 were selected for carbide-related micropore detection. To reduce the influence of sampling location differences on the detection results, samples were taken from the middle of the length direction of each forging, and metallographic observation surfaces were taken at 1 / 4 of the cross-sectional thickness from the surface of the forging.
[0055] Each sample was wet-ground sequentially using 240-mesh, 400-mesh, 800-mesh, 1200-mesh, and 2000-mesh SiC sandpaper, and then mechanically polished using 3μm and 1μm diamond polishing agents until there were no obvious scratches on the observation surface. After polishing, the sample was cleaned with anhydrous ethanol and dried. No corrosion treatment was performed to avoid confusion between corrosion pits and carbide-related pores.
[0056] Backscattered electron imaging was performed using a field emission scanning electron microscope. The electron beam accelerating voltage was set to 15kV, the working distance was 8-12mm, and the magnification was uniformly set to 2000x. Ten non-overlapping fields of view were randomly selected for each group of samples, and the selection of fields of view avoided the sample edges, obvious oxidation areas, and mechanical sample preparation defects.
[0057] Image analysis software was used to binarize each field of view and perform manual verification. Black pore-like defects with an equivalent diameter of not less than 0.2 μm located inside the primary carbide or at the interface between the primary carbide and the high-speed steel matrix were counted as carbide-related pores. For carbide-matrix interface pores, the maximum opening width was measured along the direction perpendicular to the local interface, and the arithmetic mean of the opening widths of all interface pores in each field of view was used as the average opening of the interface pores.
[0058] The area fraction of carbide-related pores, i.e., the percentage of the total area of carbide-related pores in 10 fields of view to the total area of the corresponding fields of view; the average aperture of the interface pores; and the primary carbide fragmentation ratio, i.e. the percentage of primary carbides with penetrating cracks or obvious separation fractures to the total number of primary carbides counted, were calculated respectively. The results are shown in Table 1.
[0059] The carbide-related void area fraction is calculated using the following formula: ;
[0060] Among them, P A A represents the carbide-related pore area fraction; i Let A be the area of the i-th carbide-related pore on the observation surface; n is the total number of carbide-related pores counted; A T This represents the total area of the entire statistical field of view.
[0061] The average aperture of the interface holes is calculated using the following formula: ;
[0062] in, W represents the average aperture of the interface holes. j is the maximum opening width of the j-th carbide-matrix interface pore measured along the direction perpendicular to the local interface; m is the total number of interface pores counted.
[0063] The proportion of carbide crushing in one step is calculated using the following formula: ;
[0064] Among them, P F The proportion of carbide crushing in a single step; N F The amount of primary carbides with penetrating fractures or clearly separated fracture surfaces; N T The total number of primary carbides counted: Table 1. Detection results of micropores related to carbides in each group of forgings ;
[0065] As can be seen from Table 1, the carbide-related pore area fraction and the average opening of interface pores in Example 1 are lower than those in Comparative Examples 1-4. After using M35 high-speed steel and adjusting the rapid cooling termination temperature and cooling rate accordingly, the pore area fraction and the average opening of interface pores in Example 2 are at a similar level to those in Example 1, indicating that the processing approach shows the same trend under the conditions of the two high-speed steel materials.
[0066] The final forging and first annealing processes of Example 1 and Comparative Example 1 are basically the same, but Comparative Example 1 omits the controlled rapid cooling of the near-surface-core temperature difference after final forging; the pore area fraction and the average opening of the interface pores in Comparative Example 1 are both higher than those in Example 1, indicating that there is a corresponding relationship between the controlled rapid cooling after final forging and the lower level of carbide-related micropores.
[0067] Comparative Example 2 has an average cooling rate and a termination cooling temperature close to that of Example 1, but the temperature difference between the near-surface layer and the core exceeds 80°C during the cooling process; Comparative Example 4 controls the temperature difference between the near-surface layer and the core to within 30°C, but the average cooling rate is lower than that of Example 1; the pore area fraction and the average opening of the interface pores in both groups are higher than those in Example 1, indicating that the treatment effect should not be simply attributed to either rapid cooling or a small cross-sectional temperature difference.
[0068] Comparative Example 3, after completing the same rapid cooling and transition holding as Example 1, introduced an independent return temperature path including reheating, high-temperature holding, and recooling. Its final pore area fraction and average interface pore opening were higher than those of Example 1, indicating that under the experimental conditions of this group, the independent return temperature path did not achieve the same micropore control effect as directly and continuously entering the first annealing.
[0069] The proportion of primary carbide breakage in each group was in a narrow range of 18.7-20.1%. Example 1 did not show a trend of increasing primary carbide breakage. Combined with the changes in pore area fraction and average pore opening at the interface, it can be considered that the pore reduction trend in Example 1 did not depend on the continued increase in mechanical deformation after final forging.
[0070] Experimental Example 2: To evaluate the effect of different final forging treatments on the overall toughness of forgings, samples were taken from the middle of the length of the forgings treated in Example 1 and Comparative Examples 1-4. According to the Charpy V-notch impact test specimen form specified in GB / T 229-2020 "Metallic Materials Charpy Pendulum Impact Test Method", each group of materials was processed into 10mm×10mm×55mm specimens, and a V-notch with a depth of 2mm and an included angle of 45° was machined in the middle of the specimen.
[0071] Three parallel specimens were prepared for each group, and impact tests were conducted using a pendulum impact testing machine at 20±2℃. The impact absorbed energy of each specimen was recorded, and the arithmetic mean of the three parallel specimens was taken as the impact absorbed energy of the group. The results are shown in Table 2. Table 2 Room temperature impact energy of forgings in each group ;
[0072] As can be seen from Table 2, the average room temperature impact absorption energy of Example 1 is 16.8 J, which is higher than that of Comparative Examples 1-4. Combined with the test results of Experiment 1, Example 1 has both a lower carbide-related pore area fraction and a smaller average interface pore opening, indicating that there is a corresponding relationship between the reduction of internal carbide-related micro-damage level and the increase of impact absorption energy.
[0073] In Comparative Example 1, after eliminating the controlled rapid cooling with a large temperature difference between the near-surface and the core, the average impact absorption energy was 13.6 J; in Comparative Example 2, after rapid cooling with a large temperature difference between the near-surface and the core, it was 14.2 J; in Comparative Example 4, after slow cooling with a smaller temperature difference between the near-surface and the core, it was 13.9 J; and in Comparative Example 3, after adding an independent reheating step, it was 14.8 J. The above results are basically consistent with the changing trends of the pore area fraction and the average aperture of the interface pores in Experimental Example 1.
[0074] Experimental Example 3: To determine whether different cooling paths after final forging form detectable differences in the micropore state of carbides before the first annealing, and to verify whether there is a synergistic effect between rapid cooling and the temperature difference control between the near-surface and the core, stage interruption tests were conducted using Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 4 as experimental objects. The stage interruption test conditions for each group are shown in Table 3.
[0075] All groups used the same W6Mo5Cr4V2 high-speed steel billet, pre-forging heating regime, forging method, and final forging conditions as in Example 1. Final forging was completed at 900±10℃, and forging pressure was stopped after reaching the target dimensions. After final forging, the temperature was lowered to 850±10℃ according to the corresponding example or comparative example. Processing was immediately interrupted upon reaching 850±10℃, without subsequent 3-minute holding and 3-hour first annealing. Table 3. Interruption test conditions for each group ;
[0076] After reaching 850±10℃, the high-temperature treatment of each group was immediately terminated, and the same interrupted cooling regime was used to cool to room temperature. No transition holding or first annealing was performed, and samples were taken from the same locations. The sample preparation, SEM-BSE observation, and statistical methods for carbide-related pore area fraction and average interface pore aperture were the same as in Experiment 1. Three independent samples were set up for each group, and 10 non-overlapping fields of view were randomly selected for each sample. The results are shown in Table 4. Table 4. Detection results of micropores related to carbides in samples from each group with interrupted stages. ;
[0077] As can be seen from Table 4, in Example 1, when only the near-surface and core temperature difference was controlled and rapidly cooled from 900°C to 850°C after final forging, without transition holding and first annealing, the carbide-related pore area fraction and the average aperture of interface pores in the stage interruption sample were 0.096% and 0.71 μm, respectively. Compared with Comparative Example 1, which used a normal cooling method, these figures were reduced by approximately 35.6% and 34.9%, respectively. This indicates that the differences in carbide-related micropore states formed by different cooling paths after final forging could already be detected in the stage interruption sample before the start of the first annealing, demonstrating a correspondence between the controlled and rapid cooling stage of the near-surface and core temperature difference and the aforementioned differences in micropore states.
[0078] Comparative Example 2 has the same rapid cooling rate as Example 1, but the temperature difference between the near-surface layer and the core is greater than 80°C, and its pore area fraction and average aperture are 0.136% and 0.97 μm, respectively. Comparative Example 4 also controls the temperature difference between the near-surface layer and the core to within 30°C, but the cooling rate is only 0.15±0.05°C / s, and the corresponding values are 0.137% and 0.99 μm, respectively. Both results are higher than those of Example 1, indicating that neither rapid cooling alone nor reducing the cross-sectional temperature difference alone can achieve the same micropore control effect as Example 1.
[0079] Experimental Example 4: To verify whether controlling the temperature difference between the near-surface layer and the core can reduce the adverse effects caused by uneven temperature distribution in the cross section during rapid cooling while maintaining a high cooling rate, W6Mo5Cr4V2 high-speed steel forgings from Example 1, Comparative Example 2, and Comparative Example 4 were selected for comparative experiments.
[0080] Each group used the same high-speed steel billet, pre-forging graded heating system, forging forming method and final forging conditions as in Example 1. The final forging was completed at 900±10℃ and the same target size was achieved before the forging deformation was stopped.
[0081] Example 1: Within 15 seconds after final forging, the sample was placed in a controlled nitrogen forced convection heat exchange environment, and the temperature was reduced from 900±10℃ to 850±10℃ at an average cooling rate of 1.5±0.3℃ / s, while the temperature difference between the near-surface layer and the core was controlled within 30℃. Comparative Example 2: The same average cooling rate as Example 1 was used, but the temperature difference between the near-surface layer and the core was not controlled, so that the maximum temperature difference was greater than 80℃. Comparative Example 4: The temperature difference between the near-surface layer and the core was controlled within 30℃, but the average cooling rate was controlled at 0.15±0.05℃ / s.
[0082] After each group of forgings reaches 850±10℃, the corresponding cooling stage is immediately terminated without subsequent transition holding and first annealing. The same subsequent cooling conditions are used to reduce the impact of different thermal histories on crack observation results after 850℃.
[0083] Metallographic specimens were prepared at the same cross-sectional position in the middle of the length of the forging in each group. After grinding and polishing, the specimens were not subjected to corrosion treatment. They were first screened at low magnification using an optical microscope, and then the suspected microcrack areas were verified using a scanning electron microscope.
[0084] Each group consisted of 3 independent specimens. For each specimen, 10 non-overlapping fields of view were randomly selected. Linear defects with a length of not less than 20 μm, exhibiting continuous crack morphology and excluding polishing scratches, inclusion pits, and carbide pull-out pits were counted as microcracks. The number of microcracks per unit observation area and the total crack length per unit observation area were counted to characterize the degree of adverse damage related to thermal stress under different cooling conditions. Table 5. Cross-sectional temperature difference and microcrack detection results under different cooling methods ;
[0085] As shown in Table 5, Example 1 and Comparative Example 2 have the same average cooling rate, but the maximum temperature difference between the near-surface temperature and the core temperature in Example 1 is controlled within 30°C, while the maximum temperature difference in Comparative Example 2 reaches 86°C. Under the same rapid cooling conditions, the number of microcracks and the crack line density in Comparative Example 2 are higher than those in Example 1, indicating a corresponding relationship between the larger cross-sectional temperature difference and the adverse effects of thermal stress during rapid cooling. The maximum temperature difference between the near-surface and core in Example 1 and Comparative Example 4 is controlled within 30°C, but the average cooling rate of Example 1 is higher than that of Comparative Example 4. The number of microcracks and the crack line density in the two groups are at similar levels, indicating that under the experimental conditions of this group, by limiting the temperature difference between the near-surface temperature and the core temperature, a higher cooling rate can be maintained while preventing the forging from exhibiting a microcrack increase trend comparable to rapid cooling with a large temperature difference.
[0086] Based on the comparison results of Example 1, Comparative Example 2, and Comparative Example 4, it can be seen that the present invention does not obtain a smaller cross-sectional temperature difference by reducing the cooling rate, but rather controls the temperature difference between the near-surface layer and the core while maintaining a specified rapid cooling rate, thereby coordinating rapid cooling with cross-sectional temperature uniformity. This temperature control method is beneficial to reducing the adverse effects caused by a large cross-sectional temperature gradient during rapid cooling and provides further experimental evidence for the implementation of the rapid cooling stage after final forging.
[0087] The technical scope of this invention is not limited to the content described above. Those skilled in the art can make various modifications and variations to the above embodiments without departing from the technical concept of this invention, and all such modifications and variations should fall within the protection scope of this invention.
Claims
1. A heat treatment method for coordinated temperature control in high-speed steel forging, characterized in that, Includes the following steps: S1: The temperature at a distance of 5-10 mm from the surface of the forging is taken as the near-surface temperature, the temperature at the center of the forging cross-section is taken as the core temperature, and the arithmetic mean of the near-surface temperature and the core temperature is taken as the forging characterization temperature. The absolute value of the difference between the near-surface temperature and the core temperature is taken as the near-surface and core temperature difference. The high-speed steel billet is preheated and forged. The final forging is completed when the forging characterization temperature is 890-910℃. The temperature is recorded as T1. After the forging reaches the target size, the forging deformation is stopped. S2: Within 5-60 seconds after the final forging is completed, transfer the forging to a controlled heat exchange environment with a temperature lower than T1. S3: After the forging enters the controlled heat exchange environment, the current forging temperature is recorded as T0. Forced convection heat exchange is performed between the gas heat exchange medium and multiple outer surfaces of the forging, so that the forging temperature decreases from T0 to a rapid cooling termination temperature of 800-870℃ at an average cooling rate of 0.8-2.0℃ / s, where T1-T2 is 40-110℃. The ratio of the decrease in the forging temperature between two adjacent temperature sampling times to the corresponding time interval is used as the current cooling rate. The temperature and flow rate of the gas heat exchange medium are adjusted based on the current cooling rate and the temperature difference between the near-surface layer and the core. During the cooling process, the temperature difference between the near-surface layer and the core is not greater than 50℃. S4: After the forging reaches T2, it is held for 1-5 minutes within the range of T2±10℃ to form a transition holding stage; S5: After the transition holding is completed, the first annealing stage is entered, and after the end, the forging is subjected to slow cooling treatment.
2. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: The high-speed steel billet is W6Mo5Cr4V2 high-speed steel or M35 high-speed steel.
3. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: The pre-forging heating in step S1 includes heating the high-speed steel billet to 550-650℃ for the first stage of preheating, then raising the temperature to 800-900℃ for the second stage of preheating, and then raising the temperature to 1120-1140℃ for forging heating to reach a homogeneous state before taking it out of the furnace for forging.
4. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 3, characterized in that: The so-called uniform heating state refers to the temperature of the billet core reaching within ±10℃ of the set forging heating temperature, and the absolute value of the difference between the near-surface temperature and the core temperature not exceeding 30℃.
5. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: The forging process in step S1 employs one or more of upsetting, drawing, and die forging.
6. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: In step S3, the gas heat exchange medium is nitrogen or argon.
7. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 3, characterized in that: During the forging process before final forging, forging is stopped when the temperature of the forging drops below 900°C, and the forging is reheated to 1120-1140°C to reach the homogeneous state before forging continues.
8. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: The feedback adjustment in step S3 specifically involves the following steps: When the temperature difference between the near-surface layer and the core is less than 40°C, the heat exchange conditions are adjusted according to the current cooling rate. When the current cooling rate is less than 0.8°C / s, the flow rate of the gas heat exchange medium is increased and / or the temperature of the gas heat exchange medium is decreased. When the current cooling rate is greater than 2.0°C / s, the flow rate of the gas heat exchange medium is decreased and / or the temperature of the gas heat exchange medium is increased. When the temperature difference between the near-surface layer and the core reaches or exceeds 40°C, the flow rate of the gas heat exchange medium is preferentially decreased and / or the temperature of the gas heat exchange medium is increased, and the forging is rotated and / or the flow direction of the gas heat exchange medium is changed. When the temperature difference between the near-surface layer and the core decreases to below 30°C, the flow rate and / or temperature of the gas heat exchange medium are continued to be adjusted according to the current cooling rate to allow the forging to continue cooling down.
9. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: In step S5, the temperature T3 of the first annealing stage is 800-870℃, and T2≥T3 is satisfied.
10. The heat treatment method for coordinated temperature control in high-speed steel forging according to claim 1, characterized in that: The slow cooling process in step S5 includes cooling the forging to 650-750°C at an average cooling rate of 5-30°C / h, then cooling it in the furnace to below 500°C, and finally air cooling it to room temperature after it is removed from the furnace.
Citation Information
Patent Citations
Novel manufacturing process of phi 300 mm-phi 700 mm high-carbon high-chromium cold-working die steel forged round steel
CN102418042A
High-cobalt high-molybdenum superhard high-speed steel and method for improving hot working performance thereof
CN113355584A
Method for refining carbide in high-carbon alloy steel
CN116497197A