A long-lasting negative ion antistatic methoxy composite fiber and its preparation method

By coating the somati nanoparticles with porous silica and modifying them with hydrophobic fluorosilane, combined with core-sheath composite spinning and heat setting crosslinking, the problems of uneven powder dispersion and poor compatibility in somati composite fibers were solved, and the durability and longevity of the negative ion antistatic function were achieved.

CN123063889APending Publication Date: 2026-11-10ZHEJIANG SHUANGDUN TEXTILE TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611351876.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the existing technology, Somato-based composite fibers have problems such as uneven dispersion of functional powders, poor compatibility with polymer matrix, and insufficient durability of negative ion antistatic function.

Method used

Long-lasting negative ion antistatic somati composite fiber was prepared by coating somati nanoparticles with porous silica and modifying their surface with fluorosilane hydrophobic agents, combined with core-sheath composite spinning and cross-linking treatment with epoxy silane coupling agents during heat setting.

Benefits of technology

It significantly improves the dispersibility and interfacial compatibility of functional powders in polymer matrix, achieves surface enrichment of negative ion release and antistatic functions, ensures the mechanical strength and durability of fibers, and enhances the long-term performance and water resistance of fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for preparing long-lasting negative ion antistatic somatite composite fiber, comprising the following steps: S1: Melt-blending and extruding granulation of functionally modified somatite composite powder, reduced graphene, and a first polymer resin to obtain a somatite functional masterbatch; S2: Using this masterbatch as the sheath layer material and a second polymer resin as the core layer material, melt-spinning is performed through a sheath-core type composite spinneret to obtain nascent fibers; S3: The masterbatch is subsequently subjected to cooling, stretching, and heat-setting post-treatments to obtain long-lasting negative ion antistatic somatite composite fiber. The preparation method of this invention effectively solves the problems of somatite powder dispersion and interfacial compatibility in the polymer matrix, achieving maximum enrichment of functional components on the fiber surface, while ensuring the overall mechanical strength of the fiber and significantly improving the functional durability and washability of the fiber. The resulting composite fiber possesses both long-lasting negative ion release performance and antistatic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of composite fibers, and more particularly to a long-lasting negative ion antistatic methoxy composite fiber and its preparation method. Background Technology

[0002] Somatid is a microscopic energy source found in natural minerals, believed to possess multiple functions including releasing negative ions, anti-aging, antibacterial and deodorizing, and far-infrared radiation. In recent years, with the increasingly widespread application of functional fibers in the textile industry, introducing somatid into fiber preparation to endow products with health benefits such as negative ion release and antistatic properties has become a research hotspot in the industry.

[0003] Currently, the preparation of functional composite fibers mainly employs the blend spinning method, which involves directly mixing functional inorganic powders with polymeric resins (such as polyester and nylon) and then melt spinning. However, this process faces numerous technical challenges. First, nanoscale inorganic powders have a large specific surface area and high surface energy, making them prone to agglomeration in the polymer matrix and difficult to achieve uniform dispersion. Second, due to differences in specific gravity, temperature, and properties, the interfacial bonding between inorganic powders and polymeric resins is poor, leading to decreased spinnability of the fibers during spinning and accompanying deterioration of mechanical properties such as fiber strength and elongation. Furthermore, some existing technologies use post-treatment methods to attach functional particles to the fiber surface. While this is simple to operate, the functional components lack a strong bond with the fiber matrix, resulting in poor washability and difficulty in maintaining functionality. Regarding somati itself, due to the characteristics of the biological environment, existing technologies also have limitations, such as difficulty in large-scale extraction and cultivation, and limited applicability as an industrial composite material.

[0004] To address this, Chinese patent CN105332074B discloses a method for manufacturing multifunctional fibers using somati quantum energy bio-fusion masterbatch sheets. The method involves extracting somati from natural minerals, pulverizing it to 0.2–2 micrometers, mixing it with ethylene glycol to form a slurry, then melt-blending it with a polymer resin, extruding and granulating it to obtain masterbatch sheets, and finally melt-spinning it into fibers. This technology represents a preliminary application of somati in fibers, but it still suffers from drawbacks such as the functional powder not being surface-modified, poor interfacial compatibility with the polymer matrix, easy agglomeration, and the functional components not being evenly distributed throughout the fiber, thus failing to maximize surface enrichment.

[0005] Therefore, there is an urgent need to develop a somatoti-based composite fiber and its preparation method that can effectively improve the dispersibility of functional powders, enhance interfacial compatibility with polymer matrices, and possess long-lasting functional stability. Summary of the Invention

[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing long-lasting negative ion antistatic methoxy composite fiber to solve the technical problems such as uneven dispersion of functional powders, poor compatibility with polymer matrix, and insufficient durability of negative ion antistatic function in methoxy-based composite fiber.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a long-lasting negative ion antistatic methoxy composite fiber, the method comprising the following steps:

[0009] S1: Functional modified somati composite powder, reduced graphene and first polymer resin are melt-blended, extruded and granulated to obtain somati functional masterbatch;

[0010] S2: Using the Somati functional masterbatch obtained in step S1 as the skin layer raw material and the second polymer resin as the core layer raw material, melt spinning is performed through a skin-core type composite spinneret to obtain nascent fibers.

[0011] S3: The nascent fibers obtained in step S2 are subjected to cooling, stretching, and heat setting post-treatment to obtain long-lasting negative ion antistatic somato composite fibers.

[0012] As a preferred technical solution, the mass ratio of the functionally modified somati composite powder, reduced graphene and the first polymer resin is 3-5:1-2:15-30.

[0013] As a preferred technical solution, the modification method of the functionally modified somatostatin composite powder includes the following steps:

[0014] S1-1: Somati nanoparticles are dispersed in an alcohol-water mixed solvent, a template agent is added and stirred to form a uniform dispersion, a silicon source is added dropwise and the system is adjusted to alkalinity to allow silica sol to grow in situ on the surface of the nanoparticles; after separation, washing, removal of the template agent and drying of the reaction product, porous silica-coated somati composite powder is obtained.

[0015] S1-2: The porous silica-coated somati composite powder obtained in step S1-1 is added to a fluorosilane hydrophobic agent solution for surface modification treatment, and then dried to obtain functionally modified somati composite powder.

[0016] As a preferred technical solution, the template agent is at least one of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (F127).

[0017] As a preferred technical solution, the silicon source is tetraethyl orthosilicate and / or methyl orthosilicate.

[0018] As a preferred technical solution, the fluorosilane hydrophobic agent is at least one selected from 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and 1H,1H,2H,2H-perfluorooctyltriethoxysilane.

[0019] As a preferred technical solution, the first polymer resin and the second polymer resin are each independently selected from at least one of polyethylene terephthalate (PET), polyamide 6 (PA6), polyamide 66 (PA66), polyethylene (PE), polypropylene (PP), and polybutylene terephthalate (PBT).

[0020] As a preferred technical solution, the heat setting method is as follows: during the heat setting process, a finishing liquid containing an epoxy silane coupling agent is applied to the fiber surface, and after drying and curing, a cross-linked network structure is formed on the fiber surface.

[0021] As a preferred technical solution, the mass fraction of the epoxy silane coupling agent in the finishing solution is 0.5-5%.

[0022] As a preferred technical solution, the epoxy silane coupling agent is at least one of 3-glycidyl etheroxypropyltrimethoxysilane, 3-glycidyl etheroxypropyltriethoxysilane, and 5,6-epoxyhexyltriethoxysilane.

[0023] As a preferred technical solution, in step S2, the spinning temperature of the melt spinning is 230-290℃; in step S3, the draw ratio of the drawing is 2.5-5.0 times, and the heat setting temperature is 120-200℃.

[0024] Another aspect of the present invention is to provide a long-lasting negative ion antistatic methoxy composite fiber, wherein the composite fiber is prepared by the preparation method of the long-lasting negative ion antistatic methoxy composite fiber described above.

[0025] The beneficial effects of this invention are:

[0026] This invention discloses a method for preparing long-lasting negative ion antistatic methoxygenated composite fibers. By innovatively coating methoxygenated nanoparticles with porous silica and combining this with surface modification using fluorosilane hydrophobic agents, the technical challenges of uneven dispersion and easy agglomeration of inorganic functional powders in a polymer matrix are effectively solved, significantly improving the interfacial compatibility between the functional powders and the polymer resin. Simultaneously, by using a functional masterbatch as the sheath layer and a pure polymer resin core layer in a sheath-core composite spinning process, not only is the surface enrichment of negative ion release and antistatic functions maximized, but the overall mechanical strength and durability of the fiber are also ensured to remain unaffected by the functional filler. This design not only enhances the fiber's long-lasting negative ion release capacity and antistatic properties but also maintains its good spinnability and wearability, helping to broaden the application range of functional composite fibers in the textile field.

[0027] Furthermore, this invention introduces an epoxy silane coupling agent during the heat setting process to crosslink the fiber surface, forming a stable crosslinked network structure on the fiber surface, which further enhances the fiber's functional durability and water resistance.

[0028] In summary, the long-lasting negative ion antistatic methoxy composite fiber of the present invention not only has excellent negative ion release performance and antistatic performance, but also has long-lasting function and good washability, which can meet the requirements of functional textiles for long-term durability and stability. Detailed Implementation

[0029] The following description is intended to disclose the invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art.

[0030] Example 1

[0031] The preparation method of the long-lasting negative ion antistatic methoxy composite fiber in this embodiment includes the following steps:

[0032] S1: Preparation of Functionally Modified Somati Composite Powder: Somati nanopowder was dispersed in a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 1:1. A template agent, cetyltrimethylammonium bromide (CTAB), was added, with a CTAB to somati nanopowder mass ratio of 1:5. The mixture was stirred for 30 min to form a uniform dispersion. Tetraethyl orthosilicate (TEOS) was added dropwise to the dispersion, with a TEOS to somati nanopowder mass ratio of 1:2. Simultaneously, ammonia was added dropwise to adjust the pH of the system to 9–10. The mixture was stirred at room temperature for 6 h to allow silica sol to grow in situ on the surface of the somati nanopowder. The reaction product was then subjected to… Centrifugation was performed, followed by washing three times with deionized water and anhydrous ethanol. The sample was then calcined in a muffle furnace at 550°C for 4 hours to remove the template agent, yielding porous silica-coated somaturite composite powder with a silica shell thickness of 20 nm. The obtained porous silica-coated somaturite composite powder was added to an ethanol solution of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane at a mass ratio of 2% (powder to solution) at a mass ratio of 1:10. The mixture was stirred at 80°C for 4 hours to perform surface hydrophobic modification treatment. The reaction product was centrifuged and then vacuum dried at 80°C for 12 hours to obtain functionally modified somaturite composite powder.

[0033] Preparation of Somati functional masterbatch: The above-mentioned functional modified somati composite powder, reduced graphene and the first polymer resin polyethylene terephthalate (PET) were mixed at a mass ratio of 4:1:20. A dispersant (BYK-110) accounting for 1% of the mass of the functional modified somati composite powder was added. The mixture was stirred at 1000 rpm for 15 min in a high-speed mixer. Then, the mixture was melt-blended and extruded and granulated at 260℃ using a twin-screw extruder to obtain the somati functional masterbatch.

[0034] Somatome nanoparticles were prepared according to the method in Example 1 of CN105332074B: natural minerals (a mixture of maifanite and tourmaline) containing SiO2, Al2O3, Fe2O3, MgO, and K were collected and pulverized to below 320 mesh. They were then heat-treated at 600℃ for 1.5 hours to remove impurities and residual organic matter. The mineral powder and water were mixed at a mass ratio of 1:1 and fermented at room temperature of 25℃ for 30 days. The matured mixture was dried at 180℃ for 1 hour and then heated and dried again at 500℃ for 3 hours to extract mineral-bound somatome. The obtained mineral-bound somatome was heated at 1000℃ for 10 hours for high-temperature and high-pressure sterilization and screening to retain only the surviving components. Finally, it was dried at 200℃ for 5 hours and pulverized to an average particle size of 800 nm to obtain somatome nanoparticles.

[0035] S2: Core-Sheath Composite Melt Spinning: The above-mentioned Somati functional masterbatch was vacuum dried at 120℃ for 2 hours and used as the sheath material. The second polymer resin PET chips were vacuum dried at 120℃ for 1 hour and used as the core material. Melt spinning was performed using a core-sheath composite spinneret. The mass ratio of sheath to core was 3:7. The sheath spinning temperature was 265℃, the core spinning temperature was 275℃, the spinning speed was 60m / min, the side-blowing cooling temperature was 20℃, and the wind speed was 0.5m / s to obtain nascent fibers.

[0036] S3: Post-treatment: The above-mentioned nascent fibers are subjected to primary drawing (drawing temperature 90℃, drawing ratio 1.8 times) and secondary drawing (drawing temperature 110℃, drawing ratio 2.0 times); then heat-set at 150℃ for 2 minutes. During the heat-setting process, a finishing solution containing 3% by mass of 3-glycidyl etheroxypropyltrimethoxysilane and 5% by mass of triethylenetetramine curing agent is applied to the fiber surface (the finishing solution is an aqueous emulsion system, and the coupling agent is pre-hydrolyzed). After drying and curing, a cross-linked network structure is formed on the fiber surface, and finally long-lasting negative ion antistatic methoxysilane composite fiber is obtained.

[0037] Example 2

[0038] The preparation method of the long-lasting negative ion antistatic somato composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, methyl orthosilicate is used instead of ethyl orthosilicate as the silicon source.

[0039] Example 3

[0040] The preparation method of the long-lasting negative ion antistatic methoxy composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the fluorosilane hydrophobic agent is replaced by 1H,1H,2H,2H-perfluorooctyltrimethoxysilane instead of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane.

[0041] Example 4

[0042] The preparation method of the long-lasting negative ion antistatic methoxy composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the fluorosilane hydrophobic agent is replaced by 1H,1H,2H,2H-perfluorodecyltriethoxysilane instead of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane.

[0043] Example 5

[0044] The preparation method of the long-lasting negative ion antistatic methoxy composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the fluorosilane hydrophobic agent is replaced by 1H,1H,2H,2H-perfluorooctyltriethoxysilane instead of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane.

[0045] Example 6

[0046] The preparation method of the long-lasting negative ion antistatic methoxy composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the epoxy silane coupling agent is 3-glycidyl etheroxypropyltriethoxysilane instead of 3-glycidyl etheroxypropyltrimethoxysilane.

[0047] Example 7

[0048] The preparation method of the long-lasting negative ion antistatic methoxy composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the epoxy silane coupling agent is 5,6-epoxyhexyltriethoxysilane instead of 3-glycidyl etheroxypropyltrimethoxysilane.

[0049] Example 8

[0050] The preparation method of the long-lasting negative ion antistatic somatoti composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the mass ratio of the functional modified somatoti composite powder, reduced graphene and the first polymer resin is 3:1:15.

[0051] Example 9

[0052] The preparation method of the long-lasting negative ion antistatic somati composite fiber in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this embodiment, the mass ratio of the functional modified somati composite powder, reduced graphene and the first polymer resin is 5:2:30.

[0053] Comparative Example 1

[0054] The preparation method of this comparative example of long-lasting negative ion antistatic somati composite fiber is basically the same as that of Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this comparative example, the somati nanopowder is not coated with porous silica and modified with fluorosilane hydrophobic treatment. The unmodified somati nanopowder is directly melt-blended with the first polymer resin PET at a mass ratio of 2:8 and extruded and granulated to obtain somati functional masterbatch.

[0055] Comparative Example 2

[0056] The preparation method of this comparative example of long-lasting negative ion antistatic Somato composite fiber is basically the same as that of Example 1 in terms of raw material composition and preparation steps. The difference is that in this comparative example, the preparation method does not use a core-sheath type composite spinning structure. Instead, Somato functional masterbatch is mixed with PET chips in a certain proportion and then the fiber is made by conventional single-component melt spinning process.

[0057] Comparative Example 3

[0058] The preparation method of this comparative example of long-lasting negative ion antistatic methoxyl composite fiber is basically the same as that of Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this comparative example, no finishing liquid containing epoxy silane coupling agent is applied during the heat setting process. That is, the heat setting step is only a conventional heat drying treatment.

[0059] Comparative Example 4

[0060] The preparation method of this comparative example of long-lasting negative ion antistatic somatoti composite fiber is basically the same as that of Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this comparative example, the raw material of the outer layer is pure PET resin and the raw material of the core layer is somatoti functional masterbatch (that is, the functional component is located in the core layer rather than the outer layer).

[0061] Comparative Example 5

[0062] The preparation method of the long-lasting negative ion antistatic somati composite fiber in this comparative example is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation method of this comparative example, the somati nanopowder is only coated with porous silica, but is not subjected to hydrophobic modification treatment with fluorosilane.

[0063] The long-lasting negative ion antistatic somati composite fibers prepared in Examples 1-9 and Comparative Examples 1-5 were subjected to performance tests, and the performance results are shown in Table 1.

[0064] The tensile strength was measured according to GB / T14337-2022. An electronic fiber tensile tester was used to stretch a single fiber at a constant elongation rate of 100 mm / min until fracture. The tensile load was recorded and divided by the linear density to calculate the tensile strength (cN / dtex). At least 30 fibers were tested for each sample, and the average value was taken. The negative ion release was measured according to GB / T30128-2013 using the friction method. The sample was installed between the upper and lower friction discs of the friction testing device. A pressure of 7.5 N was applied to the upper disc, and the lower disc rotated at a speed of 93 r / min to stimulate negative ions. The concentration of negative ions (cN / cm³) in the stable phase within the friction chamber was measured using a negative ion measuring instrument. 3For each sample, at least 3 sets were tested and the average value was taken. For the resistance value, refer to GB / T12703.4-2010. Use a surface resistance tester (high resistance meter) to apply a DC voltage of 100V to the fiber sample. After 1 minute of power-on, read the stable surface resistance (Ω). For each sample, at least 5 different locations were measured and the average value was taken. For the washability, according to GB / T8629 "Home Washing and Drying Procedures for Textile Testing", wash 50 times at 40℃ water temperature and standard detergent. After each wash, rinse thoroughly, dehydrate and air dry. Then calculate the percentage of negative ion release after 50 washes relative to the release before washing (negative ion retention rate), and the percentage of resistance value before washing relative to the resistance value after washing (resistance retention rate, since the lower the resistance, the better the antistatic property, so the former divided by the latter indicates the degree of performance retention).

[0065] Table 1

[0066] Table 1 shows the test results: Compared with the comparative examples, the composite fibers of each embodiment of the present invention exhibit excellent performance in terms of breaking strength, negative ion release and its water wash retention rate, antistatic properties and its water wash retention rate. Among them, Examples 1 to 7 maintain good comprehensive performance under different raw material substitutions; Example 8, due to its relatively high total solid content of functional powder and reduced graphene, has a negative ion release of 5120 ions / cm³. 3 The tensile strength is 4.1 cN / dtex; in Example 9, due to the relatively low powder content, the negative ion release is 5060 ions / cm³. 3 Its tensile strength is 4.0 cN / dtex, but due to its higher proportion of reduced graphene, its resistivity is significantly reduced to 3.2 × 10⁻⁶. 6 The Ω-coated surface area and 92% retention rate demonstrate the optimizing effect of graphene on the conductive network. Comparative Example 1, due to severe agglomeration of the unmodified powder, exhibited the worst performance across all aspects. Comparative Example 2, due to the use of single-component spinning resulting in overall distribution of functional components, showed significantly lower negative ion release and retention rates compared to the examples. Comparative Example 3, lacking cross-linking finishing during heat setting, experienced a significant decrease in functional retention after washing. Comparative Example 4, with its functional layer located in the core layer, had a negative ion release of only 2500 ions / cm². 3 The surface enrichment effect was the worst; Comparative Example 5, due to lack of hydrophobic modification, had insufficient interfacial compatibility and its overall performance was significantly lower than all other examples.

[0067] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A method for preparing a long-lasting negative ion antistatic methoxyl composite fiber, characterized in that, The preparation method includes the following steps: S1: Functional modified somati composite powder, reduced graphene and first polymer resin are melt-blended, extruded and granulated to obtain somati functional masterbatch; S2: Using the Somati functional masterbatch obtained in step S1 as the skin layer raw material and the second polymer resin as the core layer raw material, melt spinning is performed through a skin-core type composite spinneret to obtain nascent fibers. S3: The nascent fibers obtained in step S2 are subjected to cooling, stretching, and heat setting post-treatment to obtain long-lasting negative ion antistatic somato composite fibers.

2. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 1, characterized in that, The mass ratio of the functionally modified somati composite powder, reduced graphene, and the first polymer resin is 3-5:1-2:15-30.

3. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 1, characterized in that, The modification method of the functionally modified somatostatin composite powder includes the following steps: S1-1: Somati nanoparticles are dispersed in an alcohol-water mixed solvent, a template agent is added and stirred to form a uniform dispersion, a silicon source is added dropwise and the system is adjusted to alkalinity to allow silica sol to grow in situ on the surface of the nanoparticles; after separation, washing, removal of the template agent and drying of the reaction product, porous silica-coated somati composite powder is obtained. S1-2: The porous silica-coated somati composite powder obtained in step S1-1 is added to a fluorosilane hydrophobic agent solution for surface modification treatment, and then dried to obtain functionally modified somati composite powder.

4. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 2, characterized in that, The template agent is at least one of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer.

5. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 2, characterized in that, The silicon source is tetraethyl orthosilicate and / or methyl orthosilicate.

6. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 2, characterized in that, The fluorosilane hydrophobic agent is at least one of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and 1H,1H,2H,2H-perfluorooctyltriethoxysilane.

7. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 1, characterized in that, The first polymer resin and the second polymer resin are each independently selected from at least one of polyethylene terephthalate, polyamide 6, polyamide 66, polyethylene, polypropylene, and polybutylene terephthalate.

8. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 1, characterized in that, The heat setting method is as follows: during the heat setting process, a finishing liquid containing an epoxy silane coupling agent is applied to the fiber surface, and after drying and curing, a cross-linked network structure is formed on the fiber surface.

9. The preparation method of the long-lasting negative ion antistatic methoxy composite fiber as described in claim 1, characterized in that, In step S2, the spinning temperature of the melt spinning is 230-290℃; in step S3, the draw ratio of the drawing is 2.5-5.0 times, and the heat setting temperature is 120-200℃.

10. A long-lasting negative ion antistatic methoxyl composite fiber, characterized in that, The composite fiber is prepared using the preparation method of long-lasting negative ion antistatic methoxy composite fiber as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for manufacturing multifunctional fiber using soma Quantum energy bio-fusion master batch contained in the mineral world of natural minerals

    CN105332074B