A warm, moisture-conducting, breathable and flame-retardant home textile fabric and a preparation process thereof

By constructing an aminoquinone crosslinking network and undergoing esterification on the fiber surface, and combining chitosan and isophorone diisocyanate to prepare a phosphorus-nitrogen finishing agent, the problems of weak flame retardant bonding and poor washability of flame-retardant home textile fabrics are solved, achieving a balance between flame retardant performance and comfort performance.

CN123064005APending Publication Date: 2026-11-10CHANGXING HONGFENG PRINTING & DYEING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611445871.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing flame-retardant home textile fabrics have shortcomings in balancing flame retardancy and comfort, especially in the weak bonding between flame retardants and fibers, poor washability, and decreased breathability and moisture wicking after finishing.

Method used

The fiber surface is treated with an aminosilane coupling agent, and a phosphorus-nitrogen finishing agent is prepared by combining chitosan and isophorone diisocyanate. A strong flame-retardant layer is formed on the fiber surface through an aminoquinone cross-linking network and esterification reaction, which enhances the fiber bonding force. Phytic acid and glycine are used to form a phosphorus-nitrogen synergistic flame-retardant system.

Benefits of technology

It achieves durable flame retardant properties and improved comfort performance, enhances the bonding force between the cellulose fiber surface and the finishing agent, maintains good air permeability and moisture wicking, and significantly improves water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064005A_ABST
    Figure CN123064005A_ABST
Patent Text Reader

Abstract

This application belongs to the field of home textile fabric technology, specifically providing a warm, moisture-wicking, breathable, and flame-retardant home textile fabric and its preparation process. The fabric includes a base fabric and a composite functional layer loaded on the surface of the base fabric. The composite functional layer includes: modified chitosan obtained from chitosan amino groups and gallic acid; a finishing agent obtained from phytic acid, glycine, and isophorone diisocyanate; and an ester cross-linking structure formed by citric acid and fiber hydroxyl groups. The preparation process includes fiber surface amylation pretreatment, preparation of modified chitosan solution, preparation of finishing agent, preparation of finishing solution, and padding and baking finishing steps. This fabric can balance warmth, moisture wicking, breathability, and flame retardancy, exhibiting good flame retardant durability and maintaining a high flame retardant level even after multiple washes. It is suitable for bedding, curtains, blankets, and other home textile products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of home textile fabric technology, specifically relating to a warm, moisture-wicking, breathable, and flame-retardant home textile fabric and its preparation process. Background Technology

[0002] Home textile fabrics are widely used in everyday home settings such as bedding, curtains, blankets, and sofa covers, directly impacting users' sleep quality and residential safety. The fiber raw materials of home textiles are mostly blends of cellulose and synthetic fibers. Cellulose fibers have good moisture absorption and a soft feel, but a low limiting oxygen index, making them prone to continuous combustion when exposed to open flames. Synthetic fibers, on the other hand, exhibit combustion behaviors such as heat shrinkage and dripping. With increasing demands for home fire safety, flame retardancy has become a crucial performance indicator for home textile fabrics. Furthermore, home textile products worn close to the skin require fabrics with good warmth retention, moisture wicking, and breathability to ensure thermal and humid comfort.

[0003] There are two main types of finishing methods for existing flame-retardant home textile fabrics. One type is halogen-based flame-retardant finishing, which has a high flame-retardant efficiency, but the finished fabric produces a large amount of toxic fumes during combustion. Furthermore, the environmental and health risks of some halogen-based flame retardants are increasingly restricted by stringent regulations, leading to a shrinking application space. The other type is halogen-free phosphorus-based flame-retardant finishing, which exerts its flame-retardant effect by promoting char formation of cellulose at high temperatures and isolating heat and oxygen. However, conventional phosphorus-based finishing agents are mostly small-molecule compounds, lacking a strong chemical bond with cellulose fibers. They mainly adhere to the fiber surface through physical adsorption or weak hydrogen bonding. After repeated washing, a large amount of flame retardant is lost, resulting in a significant decrease in flame-retardant performance and poor wash resistance. In addition, to ensure flame-retardant effects, conventional finishing often requires a high amount of finishing agent, resulting in a stiff hand feel, covered pores, significantly reduced breathability and moisture wicking, and compromised warmth and wearing comfort.

[0004] It is evident that existing flame-retardant finishing methods generally face two interrelated problems: First, it is difficult to simultaneously achieve flame retardancy with comfort properties such as moisture wicking, breathability, and warmth retention; high levels of flame retardant reduce comfort, while low levels fail to meet flame retardancy standards. Second, the bonding force between flame retardant agents and fibers is weak, resulting in insufficient wash resistance and difficulty in maintaining flame retardant function after multiple washes. How to construct a multifunctional finishing system on the fiber surface that is firmly bonded to the fiber and possesses both hydrophilicity and flame-retardant char-forming ability, enabling home textile fabrics to simultaneously achieve durable flame retardancy and good warmth retention, moisture wicking, and breathability, is a pressing technical problem to be solved in the home textile fabric industry. Summary of the Invention

[0005] To address the aforementioned issues, this application provides a warm, moisture-wicking, breathable, and flame-retardant home textile fabric and its preparation process.

[0006] This application first provides a preparation process for a warm, moisture-wicking, breathable, and flame-retardant home textile fabric, including the following steps: S1: The base fabric is immersed in a solution containing an aminosilane coupling agent to impregnate the surface of the base fabric fibers, thereby obtaining a pretreated base fabric; S2: Dissolve chitosan in a buffer solution, add gallic acid solution to the chitosan solution, and stir the reaction under the action of an oxidant to obtain a modified chitosan solution; S3: Phytic acid and glycine are mixed in water, and the resulting mixture is dispersed in an anhydrous organic solvent. Isophorone diisocyanate is added, and the mixture is reacted under an inert atmosphere. After precipitation, filtration and drying, a phosphorus-nitrogen-containing finishing agent is obtained. S4: Mix the modified chitosan solution with the phosphorus-nitrogen finishing agent, add citric acid and sodium hypophosphite, stir evenly, and prepare a finishing solution; S5: The pretreated base fabric is immersed in the finishing solution, and after two dips and two nips, pre-drying and baking, and then washed and dried, a warm, moisture-wicking, breathable and flame-retardant home textile fabric is obtained.

[0007] In one embodiment, in S1, the aminosilane coupling agent is 3-aminopropyltriethoxysilane, the solution is a mixture of ethanol and water with a volume ratio of ethanol to water of 95:5, the mass concentration of 3-aminopropyltriethoxysilane is 2%, and the pH of the solution is adjusted to 4.5-5.5 with acetic acid; the impregnation temperature is 60°C, the impregnation time is 60 min; after impregnation, it is rinsed 3 times with deionized water and pre-dried at 60°C for 10 min.

[0008] In one embodiment, in S2, the buffer solution is an acetate-sodium acetate buffer solution with pH 5.5, and the mass concentration of chitosan is 2%; the concentration of gallic acid solution is 1.5 wt%, and the mass ratio of chitosan to gallic acid is 2:1; the oxidant is ammonium persulfate, and the amount of ammonium persulfate is 5 wt% of the mass of gallic acid; the reaction is stirred at room temperature for 30 min.

[0009] In one embodiment, in S3, the ratio of phytic acid, glycine, and deionized water is 10g:12g:200mL, and the reaction is carried out in water at 80°C for 2 hours with stirring. The anhydrous organic solvent is anhydrous N,N-dimethylformamide, and the amount used is 100mL. The amount of isophorone diisocyanate is 5g, the reaction temperature is 60°C, the reaction time is 4 hours, and the inert atmosphere is nitrogen. Anhydrous diethyl ether is used for precipitation.

[0010] In one embodiment, in S4, the mass ratio of the modified chitosan solution to the phosphorus-nitrogen finishing agent is 10:1, citric acid accounts for 3 wt% of the total mass of the finishing solution, and sodium hypophosphite accounts for 1.5 wt% of the total mass of the finishing solution.

[0011] In one embodiment, in step S5, the impregnation bath ratio is 1:20, the impregnation temperature is room temperature, and the impregnation time is 30 min; the roll residue of the two-dip and two-roll process is 75%; the pre-drying temperature is 80°C, and the pre-drying time is 5 min; the baking temperature is 160°C, and the baking time is 3 min.

[0012] In one embodiment, in step S5, deionized water is used for washing, the washing bath ratio is 1:50, the washing temperature is 50°C, the washing time is 10 minutes per wash, and the number of washes is 3; the drying temperature is 80°C.

[0013] This application also provides a warm, moisture-wicking, breathable, and flame-retardant home textile fabric, which is prepared using the above-described method.

[0014] In one embodiment, the above-mentioned fabric is used to prepare bedding, curtains, blankets or sofa covers and other home textile products.

[0015] Compared with the prior art, this application has the following beneficial effects: 1. This application constructs an aminoquinone crosslinking network on the fiber surface by chitosan amino groups and gallic acid, which can improve the wetting and wicking capacity of the fabric and facilitate the rapid conduction and dissipation of sweat and moisture. At the same time, the phenolic hydroxyl groups of gallic acid can promote char formation on the fiber surface when heated at high temperature, forming a dense char layer barrier, thereby providing a char formation basis for flame retardant performance.

[0016] 2. This application utilizes the isocyanate groups of isophorone diisocyanate to react with amino groups to generate urea groups, grafting a phosphorus-nitrogen-containing finishing agent onto an aminoquinone crosslinking network. Phytic acid, a high-phosphorus-content organic phosphoric acid, can promote the dehydration and char formation of cellulose and release phosphorus-based free radicals to quench species when heated; glycine provides nitrogen, forming a phosphorus-nitrogen synergistic flame-retardant system with phosphorus, which can simultaneously exert condensed-phase char formation and gas-phase dilution effects. The urea group has strong polarity and hydrogen bonding ability, which can enhance the binding force between the finishing agent and cellulose fibers and improve the anchoring strength of the finishing agent on the fiber surface.

[0017] In addition, this application utilizes citric acid to undergo esterification with the hydroxyl groups in the cellulose and aminoquinone crosslinking network under high-temperature baking conditions to form ester bonds. On the one hand, this firmly anchors the aminoquinone crosslinking network and the phosphorus-nitrogen-containing finishing agent to the fiber surface. On the other hand, it forms a three-dimensional crosslinking structure inside the functional layer, which restricts the migration and dissolution of finishing agent molecules during the washing process, thereby significantly improving the wash resistance durability of the flame retardant function. Attached Figure Description

[0018] Figure 1 Forest plot of multifactor Cox proportional hazards analysis for the wash resistance durability of each group of samples in this application. Detailed Implementation

[0019] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0020] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0021] The present application will be further illustrated by the following examples, but these examples do not limit the scope of the present application.

[0022] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in this application, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. All reagents or instruments whose manufacturers are not specified are conventional products that can be purchased commercially. In addition to the specific methods, equipment, and materials used in the embodiments, based on the knowledge of the prior art possessed by one of ordinary skill in the art and the description in this application, any prior art methods, equipment, and materials similar to or equivalent to those described, used, or made by the methods, equipment, and materials in the embodiments of this application may be used to implement this application.

[0023] Example 1 The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric in this embodiment includes the following steps: S1: Fiber surface amination pretreatment A cotton / polyester blended knitted base fabric with a cotton / polyester ratio of 60 / 40 and an areal density of 200 g / m² was immersed in an ethanol / water mixture of KH-550 (ethanol:water = 95:5, v / v), with a KH-550 concentration of 2 wt%. The pH was adjusted to 4.5-5.5 using acetic acid. The immersion was carried out at 60°C for 60 min. After immersion, the fabric was rinsed three times with deionized water to remove unreacted KH-550, and then pre-dried at 60°C for 10 min to obtain the pretreated base fabric. S2: Preparation of modified chitosan solution An acetate-sodium acetate buffer solution with pH 5.5 was prepared, and chitosan was dissolved in this buffer solution at a concentration of 2 wt%. The solution was stirred until completely dissolved to obtain a chitosan solution. Gallic acid was dissolved in deionized water at a concentration of 1.5 wt%. The gallic acid solution was slowly added dropwise to the chitosan solution, with the mass ratio of chitosan to gallic acid controlled at 2:1. Ammonium persulfate was added as an oxidant, with the amount of ammonium persulfate being 5 wt% of the mass of gallic acid. The mixture was stirred at room temperature for 30 min to obtain a modified chitosan solution. S3: Preparation of finishing agent 10 g of phytic acid and 12 g of glycine were dissolved in 200 mL of deionized water and stirred at 80 °C for 2 h to obtain a phytic acid-glycine mixture. Subsequently, the obtained phytic acid-glycine mixture was dispersed in 100 mL of anhydrous DMF, and 5 g of IPDI was added. The mixture was reacted at 60 °C for 4 h under nitrogen protection. After the reaction was complete, the product was precipitated with anhydrous diethyl ether, filtered, and vacuum dried to obtain the finishing agent. S4: Preparation of finishing solution The modified chitosan solution obtained in S2 and the finishing agent obtained in S3 were mixed at a mass ratio of 10:1. 3 wt% citric acid and 1.5 wt% sodium hypophosphite were added and stirred evenly to prepare the finishing solution. S5: Fabric Finishing The pretreated base fabric obtained from S1 was immersed in the finishing solution at a liquor ratio of 1:20 for 30 minutes at room temperature. A two-dip, two-nip process was used, with the pick-up percentage controlled at 75%. Subsequently, it was pre-dried at 80°C for 5 minutes, and then baked at 160°C for 3 minutes. After baking, the fabric was thoroughly washed with deionized water (liquor ratio 1:50, washing at 50°C for 10 minutes, repeated 3 times) to remove unreacted finishing agents, and then dried at 80°C to obtain the final product.

[0024] Example 2 The difference between this embodiment and Embodiment 1 lies in the process parameters of S1 and S2: in S1, the mass concentration of KH-550 is adjusted to 1.5wt%, and the impregnation time is adjusted to 45min; in S2, the mass concentration of chitosan is adjusted to 2.5wt%, the gallic acid solution concentration is maintained at 1.5wt%, and the mass ratio of chitosan to gallic acid is maintained at 2:1. The remaining steps are the same as in Embodiment 1.

[0025] This embodiment investigates the effects of amination degree and network precursor concentration on performance by reducing the coupling agent concentration, shortening the impregnation time, and increasing the chitosan concentration. The resulting fabric has slightly lower flame retardant and moisture-wicking properties than that of Example 1, but is still within an acceptable range.

[0026] Example 3 The difference between this embodiment and Embodiment 1 lies in the process parameters of S3 and S5: in S3, the amounts of phytic acid, glycine, and IPDI are adjusted to 8g, 10g, and 4g, respectively, while the amounts of deionized water and DMF are maintained at 200mL and 100mL, respectively; in S5, the baking temperature is adjusted to 180℃, and the baking time is adjusted to 2min. The remaining steps are the same as in Embodiment 1.

[0027] This embodiment examines the effects of finishing agent dosage ratio and baking conditions on the degree of crosslinking of functional layers and fiber strength. The limiting oxygen index of the resulting fabric is slightly higher than that of Example 1, but the breaking strength retention rate is reduced.

[0028] Example 4 The difference between this embodiment and Embodiment 1 lies in the base fabric specifications and the finishing solution ratio: the base fabric is a cotton / polyester blended knitted base fabric with a cotton / polyester mass ratio of 50:50 and an areal density of 180 g / m²; the mass ratio of the modified chitosan solution to the phosphorus-nitrogen-containing finishing agent in S4 is adjusted to 15:1. The remaining steps are the same as in Embodiment 1.

[0029] This embodiment examines the influence of the composition of the base fabric and the proportion of functional layer components on the overall performance. The resulting fabric has slightly better moisture-wicking properties due to the reduced proportion of polyester and the increased proportion of hydrophilic components, but its flame-retardant properties are slightly lower than those of Example 1.

[0030] Comparative Example 1 The difference between this comparative example and Example 1 is that the S1 fiber surface amination pretreatment step is omitted, and the base fabric is directly used for S5 fabric finishing. The remaining steps are the same as in Example 1.

[0031] This comparative example is used to investigate the contribution of fiber surface amination pretreatment to the covalent anchoring of finishing agents and flame retardant durability.

[0032] Comparative Example 2 The difference between this comparative example and Example 1 is that gallic acid is not added in S2; instead, an unmodified chitosan solution is used instead of the modified chitosan solution. All other preparation and finishing conditions remain unchanged. The remaining steps are the same as in Example 1.

[0033] This comparative example is used to investigate the contribution of quinone groups and aminoquinone crosslinking networks generated by gallic acid oxidation to moisture conductivity and flame retardant charring properties.

[0034] Comparative Example 3 The difference between this comparative example and Example 1 is that the S3 finishing agent preparation step is omitted, and in S4, only the modified chitosan solution is mixed with citric acid and sodium hypophosphite to prepare the finishing solution, without containing phosphorus-nitrogen finishing agents. The remaining steps are the same as in Example 1.

[0035] This comparative example is used to examine the contribution of phosphorus-nitrogen-containing finishing agents to flame retardant properties.

[0036] Comparative Example 4 The difference between this comparative example and Example 1 is that citric acid and sodium hypophosphite are not added in S4, and the finishing solution is only prepared by mixing modified chitosan solution and phosphorus-nitrogen-containing finishing agent at a mass ratio of 10:1. The remaining steps are the same as in Example 1.

[0037] This comparative example is used to investigate the contribution of the citrate crosslinking structure to the water-wash-resistant anchoring strength of the functional layer.

[0038] Comparative Example 5 This comparative example uses a commercially available phosphate ester-based phosphorus flame retardant to perform conventional padding and baking finishing on a cotton / polyester blended knitted base fabric with a cotton / polyester mass ratio of 60:40 and an areal density of 200 g / m². The amount of finishing agent used, based on solids content, is equivalent to that of the finishing solution in Example 1. The padding residue is 75%, pre-drying is performed at 80°C for 5 min, and baking is performed at 160°C for 3 min. The washing and drying conditions after finishing are the same as in Example 1.

[0039] Performance testing 1. The performance of the fabrics obtained in each embodiment and comparative example was tested according to the following methods: Limiting oxygen index was tested according to GB / T 5454-1997; damage length, afterflame time and smoldering time were tested according to GB / T 5455-2014 vertical burning method; wicking height was tested according to FZ / T 01071-2008; moisture permeability was tested according to GB / T 12704.1-2009 evaporation method (temperature 38℃, relative humidity 90%); air permeability was tested according to GB / T 5453-1997 (pressure difference 100Pa); thermal resistance was tested according to GB / T 11048-2018 flat plate method; breaking strength was tested according to GB / T 3923.1-2013, and the breaking strength retention rate was the ratio of the breaking strength of the finished fabric to that of the original fabric; standard washing was carried out according to GB / T 8629-2017 (type A washing machine, 4N program). The comprehensive performance test results are shown in Table 1.

[0040] Table 1. Comprehensive fabric performance test data for the examples and comparative examples. As shown in Table 1, the limiting oxygen index of the fabrics obtained in Examples 1 to 4 was 31.9% to 33.8%, all of which were not less than 30%, the damaged length was 92mm to 118mm, and the afterflame time and smoldering time were basically zero, achieving a good flame retardant level. The limiting oxygen index of Comparative Examples 1 to 5 was 26.8% to 29.1%, all of which were less than 30%, and the damaged length was more than 135mm. Among them, the damaged length of Comparative Example 3 (without phosphorus and nitrogen finishing agent) reached 178mm and the afterflame time reached 4.8s, indicating that the flame retardant performance was obviously insufficient. In terms of comfort performance, the wicking height of Examples 1 to 4 ranged from 121 mm / 30 min to 135 mm / 30 min, the moisture permeability from 8390 g / (m²·24h) to 8720 g / (m²·24h), the air permeability from 206 mm / s to 243 mm / s, and the thermal resistance from 0.159 m²·K / W to 0.172 m²·K / W, all remaining at levels comparable to or better than the original fabric. In contrast, Comparative Example 5, after conventional phosphorus treatment, showed a decrease in air permeability to below 262 mm / s and a wicking height to 96 mm / 30 min, resulting in a significant decline in comfort performance. The breaking strength retention rate of Examples 1 to 4 was above 91.8%, indicating that the damage to fabric strength caused by the finishing process was controllable.

[0041] 2. The limiting oxygen index of the fabrics obtained in Examples 1 to 4 and Comparative Examples 1 to 5 was tested after 20 and 50 standard washes, respectively. The results are shown in Table 2.

[0042] Table 2. Test data on wash resistance durability of fabrics in the examples and comparative examples. As shown in Table 2, after 50 standard water washes, the limiting oxygen index (LOI) of Examples 1 to 4 remained at 28.4% to 30.6%, and the flame retardancy retention rate (LOI ratio after 50 washes to LOI before washing) was 89.0% to 91.6%. In contrast, the limiting oxygen index of Comparative Examples 1 to 4 decreased to 23.0% to 24.8% after 50 washes, and that of Comparative Example 5 decreased to 22.7%. Comparative Example 1, lacking amination pretreatment, had a lack of covalent grafting sites for the finishing agent, resulting in significant loss after washing. Comparative Example 4, lacking citrate ester crosslinking, had weak functional layer anchoring and experienced the fastest decline in flame retardant performance. These results indicate that the synergistic effect of amination pretreatment, the aminoquinone crosslinking network, and the ester crosslinking structure plays a crucial role in flame retardant durability.

[0043] 3. To further investigate the influence of process factors such as modified chitosan solution and finishing agent on flame retardant durability and their relative importance, 42 process combination samples were designed according to the process parameter ranges of Examples 1 to 4 and Comparative Examples 1 to 5, and a multi-factor Cox ratio risk analysis of water wash resistance durability was conducted.

[0044] The event endpoint was defined as follows: after N standard washes, the limiting oxygen index of the sample, measured according to GB / T 5454-1997, was below 27.0%, which was considered as flame retardant failure. The time variable was the number of washes required to reach failure; samples that did not fail within 60 washes were censored. Covariates included: X1, the mass concentration of chitosan in the modified chitosan solution (wt%, 0.5 to 2.0); X2, the mass ratio of gallic acid to chitosan (0.5 to 3.0); X3, the mass ratio of modified chitosan solution to phosphorus-nitrogen finishing agent (5:1, 10:1, 20:1, with 10:1 as the reference level); X4, the mass concentration of citric acid in the finishing solution (0, 1.5, 3.0, 4.5 wt%, with 3.0 wt% as the reference level); X5, the baking temperature (140, 160, 180℃, with 160℃ as the reference level). The factor combinations, the number of washes required to reach failure, and the censoring of the 42 sample groups are shown in Table 3.

[0045] Table 3. Factor combinations, number of washes reaching failure, and deletion status for each sample. The Cox proportional hazards model was fitted using the data in Table 3. The Efron method was used to process the concurrent failure times to obtain the hazard ratios (HR) and 95% confidence intervals for each covariate. The results are shown in Table 4.

[0046] Table 4. Fitting data for each group of samples like Figure 1As shown in the figure and in conjunction with Table 4, the modified chitosan concentration has a significant protective effect on flame retardant durability (HR = 0.196, P = 0.002). For every 1 wt% increase in chitosan concentration, the risk of flame retardant failure decreases by approximately 80%. An increase in the gallic acid / chitosan mass ratio also shows a protective trend (HR = 0.553, P = 0.070), indicating that the density of the aminoquinone cross-linked network is an important influencing factor on flame retardant durability. When the mass ratio of modified chitosan solution to finishing agent increases from 10:1 to 20:1, the risk of flame retardant failure increases significantly (HR = 6.722, P = 0.002), indicating that insufficient relative amounts of phosphorus-nitrogen finishing agents significantly weaken flame retardant durability. However, there is no statistically significant difference between the 5:1 and 10:1 levels (HR = 0.717, P = 0.592), indicating that when the finishing agent is relatively excessive, flame retardant durability no longer improves. When the citric acid concentration decreased from 3.0 wt% to 0, the risk of flame retardant failure increased significantly (HR = 6.559, P = 0.001), confirming that the ester crosslinking structure is a key anchoring factor for flame retardant durability. When the citric acid concentration increased to 4.5 wt%, the HR approached 1 (P = 0.860), indicating that the optimal crosslinking level was close to 3.0 wt%. When the baking temperature decreased from 160℃ to 140℃, the risk of failure increased significantly (HR = 6.106, P = 0.008), and the risk also increased when the baking temperature increased to 180℃ (HR = 2.432, P = 0.138), indicating that the area around 160℃ is a relatively optimal balance point between sufficient crosslinking reaction and fiber thermal damage.

[0047] In summary, within the scope of the investigation, the modified chitosan concentration, gallic acid / chitosan mass ratio, modified chitosan solution to finishing agent mass ratio, citric acid concentration, and baking temperature all affect flame retardancy and durability. Among these, the effects of modified chitosan concentration, relative amount of finishing agent, citric acid concentration, and baking temperature are statistically significant. The process parameters used in Example 1 (chitosan concentration 2.0 wt%, gallic acid / chitosan mass ratio 2:1, modified chitosan solution to finishing agent mass ratio 10:1, citric acid concentration 3.0 wt%, baking temperature 160℃) are within the optimal range for each factor, which is consistent with the test results in Tables 1 and 2.

[0048] Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A preparation process for a warm, moisture-wicking, breathable, and flame-retardant home textile fabric, characterized in that: Includes the following steps: S1: The base fabric is immersed in a solution containing an aminosilane coupling agent to aminate the surface of the base fabric fibers, thereby obtaining a pretreated base fabric; S2: Dissolve chitosan in a buffer solution, add gallic acid solution to the chitosan solution, and stir the reaction under the action of an oxidant to obtain a modified chitosan solution; S3: Phytic acid and glycine are mixed in water, and the resulting mixture is dispersed in an anhydrous organic solvent. Isophorone diisocyanate is added, and the mixture is reacted under an inert atmosphere. After precipitation, filtration and drying, a phosphorus-nitrogen-containing finishing agent is obtained. S4: Mix the modified chitosan solution with the phosphorus-nitrogen finishing agent, add citric acid and sodium hypophosphite, stir evenly, and prepare a finishing solution; S5: The pretreated base fabric is immersed in the finishing solution, and after two dips and two nips, pre-drying and baking, and then washed and dried, a warm, moisture-wicking, breathable and flame-retardant home textile fabric is obtained.

2. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: In S1, the aminosilane coupling agent is 3-aminopropyltriethoxysilane, and the solution is a mixture of ethanol and water with a volume ratio of ethanol to water of 95:

5.

3. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 2, characterized in that: The mass concentration of the 3-aminopropyltriethoxysilane is 1.5-3%, and the pH of the solution is adjusted to 4.5-5.5 with acetic acid; the impregnation temperature is 60℃, and the impregnation time is 60 min; after impregnation, it is rinsed 3 times with deionized water and pre-dried at 60℃ for 10 min.

4. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: In step S2, the buffer solution is an acetate-sodium acetate buffer solution with a pH of 5.5, and the chitosan mass concentration is 1.5-3%; the gallic acid solution has a concentration of 1-3 wt%, and the mass ratio of chitosan to gallic acid is 1.5-3:1; the oxidant is ammonium persulfate, and the amount of ammonium persulfate is 3-6 wt% of the mass of gallic acid; the reaction is stirred at room temperature for 30 min.

5. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: In step S3, the ratio of phytic acid, glycine, and deionized water is 10g:12g:200mL, and the mixture is stirred in water at 80°C for 2 hours. The anhydrous organic solvent is anhydrous N,N-dimethylformamide, and the amount used is 100mL. The amount of isophorone diisocyanate is 5g, the reaction temperature is 60°C, the reaction time is 4 hours, and the inert atmosphere is nitrogen. The precipitation is carried out using anhydrous diethyl ether.

6. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: In step S4, the mass ratio of the modified chitosan solution to the phosphorus-nitrogen finishing agent is 8-15:1, the citric acid accounts for 2-5 wt% of the total mass of the finishing solution, and the sodium hypophosphite accounts for 1-2 wt% of the total mass of the finishing solution.

7. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: In step S5, the impregnation bath ratio is 1:20, the impregnation temperature is room temperature, and the impregnation time is 30 min; the roll residue of the two-dip and two-roll process is 75%; the pre-drying temperature is 80℃, and the pre-drying time is 5 min; the baking temperature is 160℃, and the baking time is 3 min.

8. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: In step S5, deionized water is used for washing, the washing ratio is 1:50, the washing temperature is 50℃, the washing time is 10 minutes each time, and the number of washing cycles is 3; the drying temperature is 80℃.

9. The preparation process of the warm, moisture-wicking, breathable, and flame-retardant home textile fabric according to claim 1, characterized in that: The base fabric is a cotton / polyester blended knitted base fabric, wherein the mass ratio of cotton to polyester in the cotton / polyester blended knitted base fabric is 60:40, and the areal density is 200g / m².

10. A warm, moisture-wicking, breathable, and flame-retardant home textile fabric, characterized in that: It is prepared using the preparation process described in any one of claims 1-9.