A detection method and system for solid-liquid hybrid batteries
By using an adiabatic accelerated calorimeter and thermal correction relationship calculations, the problem of accurately detecting the quality of liquid electrolyte in solid-liquid hybrid batteries was solved, enabling high-precision quality measurement without disassembling the battery.
Patent Information
- Application Number
- CN202611189722.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-06
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies cannot accurately identify the remaining mass of liquid electrolyte in solid-liquid hybrid batteries without disassembling the battery, resulting in inaccurate test results and systematic errors.
Adiabatic accelerated calorimeter was used to perform calorimetric tests on the battery. The measured heat was determined by integral compensation power, and the mass of the liquid electrolyte was calculated using thermal correction relationship and unit enthalpy of fusion, avoiding errors caused by disassembly and sample transfer.
This technology enables accurate measurement of liquid electrolyte mass without disassembling the battery, reducing measurement errors caused by evaporation and transfer, and improving the accuracy and reliability of the detection.
Smart Images

Figure CN123066162A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of new energy technology, and in particular to a detection method and system for solid-liquid hybrid batteries. Background Technology
[0002] Solid-liquid hybrid batteries, also known as semi-solid batteries, retain a certain amount of liquid electrolyte or electrolyte components capable of forming a liquid phase within a battery system containing a solid electrolyte. This liquid electrolyte improves the interfacial contact between the solid electrolyte and the electrodes and provides ion transport channels; therefore, its content affects the battery's cycle performance, rate performance, safety performance, and lifespan.
[0003] During battery manufacturing, storage, and recycling, the liquid electrolyte may decrease due to poor sealing, evaporation, leakage, interfacial film formation, or side reactions. To assess battery sealing, electrolyte retention, and overall health, it is necessary to determine the amount of electrolyte remaining in the encapsulated battery that can still participate in melting as a liquid electrolyte.
[0004] Existing methods for detecting electrolyte content typically include disassembly and weighing, theoretical estimation, chemical analysis, or imaging detection. Disassembly and weighing requires opening the battery and separating, cleaning, or drying internal components. Electrolyte is prone to evaporation or loss during disassembly and transfer, rendering the tested battery unusable. Theoretical estimation is usually calculated based on the initial fill volume and pore volume, making it difficult to reflect actual consumption after cycling or storage. Chemical analysis methods such as gas chromatography and ion tracing require removing the electrolyte or adding tracer substances to the battery, constituting destructive or invasive detection. While methods like neutron imaging can observe electrolyte distribution, the equipment is expensive, data processing is complex, and it's not easy to directly obtain the total electrolyte mass.
[0005] Therefore, how to accurately identify the remaining mass of liquid electrolyte in a solid-liquid hybrid battery without disassembling the battery under test is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0006] This application provides a method and system for detecting solid-liquid hybrid batteries, which at least solves the problem that the calorimetric results of a complete battery simultaneously include the endothermic melting of the liquid electrolyte and the thermal contribution of battery components other than the liquid electrolyte, making it impossible to directly and accurately determine the quality of the liquid electrolyte participating in the melting in the packaged battery.
[0007] The first aspect of this application provides a method for testing a solid-liquid hybrid battery. For a battery under test with a target specification, the target specification includes at least the dry cell specification of the battery under test and the electrolyte type of the electrolyte in the battery under test. First, based on the melting temperature zone corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric testing on the battery under test, and the compensation power of the battery under test within the melting temperature zone is integrated to determine the measured heat of the battery under test. Second, the measured heat is processed according to the thermal correction relationship corresponding to the dry cell specification to obtain the melting endothermic heat of the electrolyte under test. This thermal correction relationship is determined based on the first calibration heat of a first reference battery with the same dry cell specification and without liquid electrolyte, and is used to characterize the thermal contribution of battery components other than the liquid electrolyte within the melting temperature zone. Finally, the mass of the electrolyte participating in melting in the battery under test is determined according to the ratio of the melting endothermic heat to the unit enthalpy of melting corresponding to the electrolyte type.
[0008] A second aspect of this application provides a testing system for solid-liquid hybrid batteries. The testing system includes testing equipment and a computing device connected to the testing equipment. The testing equipment includes at least an adiabatic accelerated calorimeter. The computing device controls the testing equipment to execute the testing method described in the first aspect and processes the test data acquired by the testing equipment.
[0009] This application uses the latent heat of phase change during the melting process of liquid electrolyte as a mass detection medium, converting the mass of the liquid electrolyte inside the packaged battery, which is difficult to weigh directly, into heat that can be obtained through calorimetry. The battery under test does not need to be completely disassembled to obtain the electrolyte, thus reducing measurement errors caused by electrolyte evaporation, sample transfer, and component separation. Simultaneously, a pre-calibrated first reference battery, which does not contain liquid electrolyte, can characterize the dry cell background—the thermal contribution of battery components other than the liquid electrolyte, such as the casing, electrodes, current collector, separator, binder, and solid electrolyte, under the same test conditions—by using a thermal correction relationship determined based on the first calibration heat to process the measured heat of the battery under test, avoiding the erroneous conversion of this background thermal contribution into the mass of the electrolyte under test.
[0010] Therefore, this application can determine the melting temperature range and unit enthalpy of melting based on the electrolyte type, and determine the thermal correction relationship based on the dry cell specifications, so that the mass conversion can be adapted to the differences in electrolyte materials and battery structures. By selecting a low temperature range where the liquid electrolyte melts but the solid electrolyte and electrode materials do not undergo interfering phase transitions, the specificity of the test results for liquid electrolytes can also be improved. Attached Figure Description
[0011] Figure 1 This is an exemplary structural block diagram of a solid-liquid hybrid battery detection system provided in some embodiments of this application.
[0012] Figure 2 This is an exemplary flowchart of a solid-liquid hybrid battery detection method provided in some embodiments of this application.
[0013] Figure 3 An exemplary flowchart illustrating the device correction parameter calibration process provided for some embodiments of this application.
[0014] Figure 4 An exemplary flowchart illustrating the thermal correction relationship calibration process provided for some embodiments of this application.
[0015] Figure 5 An exemplary flowchart illustrating the unit enthalpy of fusion calibration process provided for some embodiments of this application.
[0016] Figure 6 The compensated power curves of the battery under test provided in some embodiments of this application are obtained by calorimetry testing using an adiabatic accelerated calorimeter.
[0017] Figure 7 The net heat flow curves of the liquid electrolyte provided in some embodiments of this application are obtained by measuring the unit enthalpy of fusion using a differential scanning calorimeter.
[0018] Figure 8 The table shows test results for actual embodiments and comparative examples of the detection method based on this application. Detailed Implementation
[0019] The embodiments of this application will now be described with reference to the accompanying drawings. It should be understood that the described embodiments are for illustrative purposes only and are not intended to limit the scope of this application. Technical features in different embodiments may be combined with each other where there is no conflict.
[0020] It should be noted that the expressions "may," "for example," and "in some embodiments" used in the embodiments of this application are all used to describe optional implementation methods and should not be construed as limiting the essential technical features. The reference numerals, device classifications, step numbers, arrow directions, and execution order in the accompanying drawings are used to assist in illustrating the detection and calibration process; unless otherwise expressly defined in the claims, they do not indicate that each process must be executed by independent hardware, independent program processes, or in a fixed order. The device models, temperature ranges, times, masses, power, heat, ratios, and test parameters listed herein are all exemplary contents for ease of understanding and can be selected or adjusted according to the specifications of the battery under test, the type of electrolyte, and the capabilities of the calorimetric equipment.
[0021] In this application's embodiments, ordinal numbers such as "first" and "second" are used only to distinguish different objects, different data, or different processing procedures, and should not be construed as indicating or implying relative importance, order of precedence, or a fixed quantity. "And / or" in this document refers to any one or any combination of the listed related objects; "multiple" can mean two or more; "at least one" can mean one or more. Terms such as "including," "comprising," and "having" in this document are open-ended expressions, and unless explicitly defined by the context, they do not exclude the inclusion of other objects, steps, modules, units, data items, or processing logic. Technical features in different embodiments can be combined and implemented where there is no conflict. A process described in one embodiment can also be split into multiple processing modules or devices for execution, or merged with other processes into the same processing module or device for execution.
[0022] As mentioned in the background, to avoid battery damage caused by invasive electrolyte mass measurement methods such as battery disassembly, and considering that the physical state of liquid electrolyte changes with temperature, this application uses thermal weighing to measure the mass of the electrolyte. Thermal weighing refers to measuring the total heat absorbed or released by the target substance in a predetermined thermal event, and using the heat per unit mass corresponding to that thermal event to convert the total heat into the mass of the substance participating in that thermal event. This method is based on the fact that when the type of substance, the thermal event, and its temperature boundary are consistent, there is a corresponding relationship between the total heat of the target thermal event and the mass of the substance participating in that thermal event.
[0023] Therefore, the thermal events used for heat integration should be consistent with the calibration events per unit mass of heat.
[0024] In practice, thermal weighing is generally achieved using a calorimeter, which measures the heat absorbed or released by a sample during temperature changes, thereby deriving its mass based on this heat change. For liquid electrolytes, this application finds that weighing can be performed during their melting process. Specifically, liquid electrolytes absorb heat during the melting process as they transition from a solid to a liquid state, and there is a corresponding relationship between the heat absorbed during melting and the mass of the electrolyte involved in the melting process.
[0025] This application further discovers that when directly calorimetricizing a complete battery, the measurement results may also include the heat contribution generated by battery components other than the liquid electrolyte within the same temperature range, such as the battery casing, electrodes, current collectors, separator, binder, and solid electrolyte. If the measured heat of the complete battery is directly determined as the melting endothermic heat of the electrolyte under test, systematic errors will be introduced due to interference from battery components.
[0026] To address this issue, this application first performs calorimetric testing on the battery under test within the melting temperature range corresponding to the electrolyte type of the electrolyte under test, obtaining the measured heat of the complete battery by integrating the compensated power; then, it processes the measured heat using a thermal correction relationship formed based on the first calibrated heat of a first reference battery that corresponds to the dry cell specifications of the battery under test and at least does not contain liquid electrolyte, separating the heat of melting attributable to the melting process of the electrolyte under test; finally, it determines the mass of the electrolyte under test participating in the melting by using the ratio between the heat of melting and the unit enthalpy of melting of the corresponding electrolyte type.
[0027] Therefore, this application converts the mass of the electrolyte inside the encapsulated battery, which is difficult to weigh directly, into heat that can be obtained without disassembling the battery for sampling. Before performing heat-mass conversion, it excludes or constrains the heat contribution generated by battery components other than liquid electrolyte in the same temperature range, thereby reducing electrolyte loss caused by disassembly and sample transfer, and reducing systematic errors caused by heat contribution from non-target battery components.
[0028] Before further describing the solid-liquid hybrid battery detection method provided in this application, the hardware structure upon which the solid-liquid hybrid battery detection method of this application relies will be explained first. Specifically, this application also provides an exemplary structural block diagram of a solid-liquid hybrid battery detection system (…). Figure 1 ), Figure 1 The solid-liquid hybrid battery testing system 100 shown can perform a solid-liquid hybrid battery testing method and its pre-calibration process, wherein the pre-calibration process can provide the various parameters required in the solid-liquid hybrid battery testing method to avoid repeated measurements.
[0029] like Figure 1 As shown, the solid-liquid hybrid battery testing system 100 may include a testing device 110 and a computing device 120, which are communicatively connected. When the object under test is set in a specific device within the testing device 110, the computing device 120 can drive the corresponding specific device to execute the corresponding test method to determine the corresponding test result.
[0030] In the specific testing method for solid-liquid hybrid batteries, the testing equipment 110 may include an adiabatic accelerated calorimeter 111. During the execution of the method, the battery under test can be placed in the adiabatic accelerated calorimeter 111, and the computing device 120 drives the adiabatic accelerated calorimeter 111 to execute the testing method of this application to obtain the test results of the adiabatic accelerated calorimeter 111. Then, calibrated parameters are called to calculate the mass of the electrolyte in the battery under test.
[0031] Test equipment 110 refers to a collection of one or more devices that apply a predetermined temperature program to the object under test and obtain corresponding thermal response test data. Test equipment 110 includes at least a device capable of performing calorimetric testing on a complete battery under test; when pre-calibrating the required parameters, test equipment 110 may also include a device for measuring the heat flow of small-mass standard samples or electrolyte samples. Specifically, each device can exchange control commands and test data with computing device 120 through a wired communication interface, a wireless communication interface, or a data file interface.
[0032] An adiabatic accelerated calorimeter 111 is a calorimetric device capable of accommodating the battery under test, establishing adiabatic or quasi-adiabatic test conditions under a controlled temperature program, recording compensation power, and outputting complete battery thermal response data. Specifically, the adiabatic accelerated calorimeter 111's test temperature range covers the melting temperature range of the electrolyte under test and has temperature control, compensation power sampling, and data output capabilities. Specifically, an ARC device with a low-temperature control module and supporting a heating-wait-search procedure can be used; its sample chamber size can be configured according to the size of pouch cells, prismatic cells, cylindrical cells, or battery modules.
[0033] In some embodiments, the adiabatic accelerated calorimeter 111 can be adapted to test objects of different sizes by changing the sample chamber, sample holder, or corresponding temperature control accessories. The testable objects can range from coin cells, single-cell pouch cells, prismatic cells, or cylindrical cells to large-size automotive batteries or battery modules. Changing the sample chamber size does not alter the processing logic that uses the compensated power integral result within the melting temperature zone as the heat input; when the sample chamber or its thermal configuration changes, the corresponding device correction parameters can be recalibrated in the manner described above.
[0034] The computing device 120 refers to a data processing device capable of communicating with the testing device 110, sending test control information to the testing device 110, receiving test data, and performing heat calculations and mass conversions. The computing device 120 can be integrated with the testing device 110 or set up independently relative to the testing device 110. Specifically, the computing device 120 can be a testing device controller, an industrial computer, a server, a workstation, or an embedded control device.
[0035] In some embodiments, the computing device 120 may further include a processor 121 and a memory 122. The processor 121 is communicatively connected to the memory 122, and the processor 121 is capable of reading and executing program instructions in the memory 122 and accessing calibration results and test data in the memory 122. The processor 121 can also communicate with the testing device 110 through the communication interface of the computing device 120 to send control information to the corresponding calorimetric device and receive its test results.
[0036] Processor 121 refers to a computing unit that executes program instructions and performs test control, data processing, and result output. Processor 121 may include a central processing unit, a microcontroller, a digital signal processor, a field-programmable gate array, an application-specific integrated circuit, or a combination thereof. Specifically, processor 121 may perform one or more of the following processes: target specification acquisition, calibration result matching, compensated power integration, device response correction, dry cell background correction, and electrolyte quality calculation.
[0037] Memory 122 refers to a storage component that stores program instructions, calibration results, target specifications, test parameters, and test data for access by processor 121. Memory 122 may include random access memory, read-only memory, flash memory, solid-state memory, disk drive, network memory, or a combination thereof. Specifically, memory 122 may associate melting temperature range and unit enthalpy of melting with electrolyte type, thermal correction relationships with dry cell specifications, and device correction parameters and calorimetric test parameters with the adiabatic accelerated calorimeter 111 and its test configuration.
[0038] Therefore, in actual execution, the memory 122 can pre-store program instructions for implementing the detection method, as well as melting temperature range, unit enthalpy of fusion, thermal correction relationship, and equipment correction parameters obtained from the calibration process. After the battery under test is placed in the adiabatic accelerated calorimeter 111, the processor 121 can retrieve the matching calibration results from the memory 122 according to the target specifications of the battery under test, generate or retrieve calorimetric test parameters, and control the adiabatic accelerated calorimeter 111 to perform calorimetric tests accordingly.
[0039] After the adiabatic accelerated calorimeter 111 returns the compensated power data, the processor 121 can integrate the compensated power within the melting temperature range to obtain the measured heat. When configuring the equipment correction parameters, the measured heat is first converted into battery endothermic heat using the equipment correction parameters. Then, the melting endothermic heat of the electrolyte under test is obtained using the thermal correction relationship, and this melting endothermic heat is divided by the unit enthalpy of fusion to obtain the mass of the electrolyte under test that participated in the melting. The calibration process and the actual detection process can therefore be separated in time. During actual detection, only the existing calibration results matching the current object need to be called.
[0040] In addition to the testing process, the aforementioned adiabatic accelerated calorimeter 111 can also be used in the calibration process. Specifically, the equipment correction parameters of the adiabatic accelerated calorimeter 111 can be calibrated by performing calorimetric tests on a standard with a known true enthalpy of fusion; alternatively, the first calibration heat and the second calibration heat can be obtained by performing calorimetric tests on the first reference cell and the second reference cell respectively, and the thermal correction relationship can be calibrated accordingly. All of the above calibration results can be stored in association with the corresponding equipment configuration, dry cell specifications, or electrolyte type, as detailed in [reference needed]. Figure 3 , Figure 4 Related descriptions.
[0041] Given the diversity of liquid electrolytes, their unit enthalpy of fusion is generally difficult to determine directly and requires an additional calibration process. To calibrate the unit enthalpy of fusion of liquid electrolytes, the aforementioned testing equipment 110 may also include a differential scanning calorimeter 112 in the calibration process.
[0042] The differential scanning calorimeter 112 is a calorimetric device that measures the heat flow difference between the sample end and the reference end under programmed temperature conditions and outputs a heat flow curve. Specifically, the differential scanning calorimeter 112 is used for heat flow measurement of small-mass liquid electrolyte samples, and its test temperature range covers the target melting process. Specifically, the differential scanning calorimeter 112 can have liquid nitrogen cooling, nitrogen purging, and sealed aluminum crucible testing capabilities, and can record the sample heat flow curve and blank baseline according to a preset heating rate. The differential scanning calorimeter 112 is used for pre-calibrating the unit enthalpy of fusion and is not a necessary piece of equipment for every actual test of the battery under test.
[0043] When obtaining the unit enthalpy of fusion using the differential scanning calorimeter 112, the same temperature program can be used to test both the sample crucible containing a known mass of target type liquid electrolyte and the blank reference crucible without liquid electrolyte. After subtracting the blank baseline from the sample heat flow curve, the resulting net heat flow curve mainly retains the increased heat flow contribution of the liquid electrolyte relative to the crucible and the test baseline. Integrating the net heat flow curve within the melting temperature region yields the sample fusion heat, which, when divided by the known mass of the liquid electrolyte, gives the unit enthalpy of fusion for the corresponding electrolyte type. For detailed calibration procedures, please refer to [link to calibration procedure]. Figure 5 And its related descriptions.
[0044] Based on the aforementioned solid-liquid hybrid battery testing system, this application also provides an exemplary flowchart of a solid-liquid hybrid battery testing method ( Figure 2 In actual implementation, Figure 2 The detection method P200 shown can be executed by the aforementioned computing device 120.
[0045] Considering that the selection of the test battery requires manual intervention in actual battery testing, the specific specifications of the test battery are known before testing, and these known specifications can be denoted as the target specifications. That is, the aforementioned P200 can test the test battery under the target specifications. The test battery refers to the solid-liquid hybrid battery set up in the adiabatic accelerated calorimeter, with the corresponding mass of its internal electrolyte as the detection output. The test battery can be a battery after manufacturing, storage, cycling, or in service. Specifically, the test battery can be a lithium-ion battery, a sodium-ion battery, or other secondary battery containing a solid electrolyte and a liquid electrolyte, and can be packaged in a pouch, square, or cylindrical manner.
[0046] In other embodiments, the battery under test may also be a zinc-based battery, a magnesium-based battery, a nickel-based battery, or another battery that simultaneously contains a solid electrolyte and a liquid electrolyte, and the liquid electrolyte exhibits an identifiable target melting process. Different battery systems can be adapted by separately associating electrolyte type, melting temperature range, unit enthalpy of fusion, and dry cell specifications.
[0047] This application does not specifically limit the material type and formation process of the solid electrolyte. The solid electrolyte can be an oxide, sulfide, halide, polymer, composite solid electrolyte, or other solid material capable of providing ion conduction in the battery, and can be formed using coating, pressing, sintering, in-situ polymerization, composite film formation, or other processes suitable for the corresponding battery system. The specific materials and processes can be included as part of the dry cell specifications to select a thermal correction relationship comparable to the thermal background.
[0048] The battery under test can be a commercially available battery, or a battery in the research, development, trial production, or manufacturing process; it can serve as a power source or energy storage unit for electrical devices. Corresponding devices may include mobile terminals, laptops, pure electric vehicles, hybrid vehicles, plug-in hybrid vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, robots, electric trains, ships, satellites, and energy storage systems. The above uses are only for illustrating the testable objects and do not change the method of handling the molten heat response during the testing process.
[0049] The target specification refers to a set of specifications sufficient to match the electrolyte thermal characteristics benchmark and dry cell background benchmark for the current battery under test. Specifically, the target specification is used to retrieve matching melting temperature range, unit enthalpy of fusion, thermal correction relationship, and calorimetric testing parameters. The target specification can be entered by the operator, read from the battery identification code, provided by the manufacturing execution system, or obtained from pre-stored product information, and can be a combination of dry cell specification identifier and electrolyte type identifier.
[0050] Considering the requirements of subsequent measurements, the target specifications should include at least the dry cell specifications of the battery under test and the electrolyte type of the electrolyte to be tested in the battery under test.
[0051] Dry cell specifications refer to a set of structural and state specifications that make the thermal contributions of battery components within the melting temperature range comparable when no liquid electrolyte is present. Dry cell specifications must cover at least the items that have a substantial impact on this thermal contribution. Specifically, dry cell specifications may include one or more of the following: battery system, packaging form, capacity, positive and negative electrode materials, current collectors, separator, solid electrolyte, conductive agent, binder, component amounts, and state of charge. Dry cell specifications are used to define the comparability of background heat and do not require different batteries to be identical in all manufacturing parameters unrelated to background heat contribution.
[0052] Electrolyte type refers to the composition or model category that enables a group of liquid electrolytes to share the target melting process and corresponding unit mass heat of fusion. Specifically, electrolyte type is used to match melting temperature range and unit enthalpy of fusion. Electrolyte type can be determined based on one or more of the following: solvent, solute, concentration, additives, and model designation.
[0053] Based on the battery under test with the aforementioned target specifications, such as Figure 2 As shown, P200 may include the following steps: S210. Based on the melting temperature zone corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric tests on the battery under test, and the compensation power of the battery under test in the melting temperature zone during the calorimetric test is integrated to determine the measured heat of the battery under test.
[0054] S220. Process the measured heat according to the thermal correction relationship corresponding to the dry cell specifications to obtain the heat of melting absorption of the electrolyte in the battery under test.
[0055] S230. Determine the mass of the electrolyte that participates in melting in the battery under test based on the ratio of the heat absorbed by melting to the unit enthalpy of melting corresponding to the electrolyte type.
[0056] In the aforementioned S210, the melting temperature zone refers to the temperature range that covers the target melting process of the electrolyte under test and serves as the boundary for heat integration. The melting temperature zone corresponds to the electrolyte type because changes in the electrolyte composition or type may alter the position and width of its solidification and melting peaks. The boundary of the melting temperature zone covers the target melting endothermic process and excludes adjacent non-target thermal processes.
[0057] In some embodiments, the melting temperature range is also selected to suppress non-target side reactions between the electrodes, electrolyte, and interface, so that the integrated heat primarily corresponds to the target melting process of the electrolyte under test. For the small endothermic heat generated by the binder near the glass transition temperature, or other background thermal responses that cannot be completely eliminated by temperature range selection alone, the first reference cell and the liquid-containing reference cell can use the same binder and the same test conditions, and the thermal response can be incorporated into the equivalent thermal contribution of the non-liquid electrolyte component through a thermal correction relationship.
[0058] Because the selected low-temperature testing range can be far below the temperature threshold at which irreversible chemical reactions occur in the battery materials, the battery under test can return to a working state of matter after the temperature recovers, provided that no irreversible reaction is triggered and the battery package remains intact. This recoverability depends on the specific battery system, the upper limit of the test, and the safety control conditions, and does not mean that all batteries subjected to arbitrary temperature programs will necessarily maintain unchanged performance.
[0059] When the instrument's heat flux resolution and temperature resolution meet the requirements, the aforementioned molten heat-to-mass conversion can also be used to identify approximately 1% to 2% changes in electrolyte mass. For example, an adiabatic accelerating calorimeter or differential scanning calorimeter capable of capturing microwatt-level heat flux changes and milliKelvin-level temperature changes can be selected. This value describes the instrument's capabilities and the effects of optional implementations, and does not constitute a necessary performance limitation for all equipment.
[0060] Calorimetry refers to a test that subjects an object to a controlled temperature process and obtains its thermal response data. Compensation power refers to the power data provided or recorded by the equipment to maintain preset thermal conditions during calorimetry, and whose time integral can characterize the corresponding heat change. Measured heat refers to the calorimetric result obtained by integrating the compensation power of the battery under test within its melting temperature range. Measured heat is the input to the thermal correction relationship and is not directly equivalent to the melting heat absorption of the electrolyte under test.
[0061] In some embodiments, S210 is used to obtain the complete battery thermal response covering the target melting process without opening the battery under test. The battery under test can be first placed in an adiabatic accelerated calorimeter, and the melting temperature zone and the test temperature range covering that zone can be selected according to the electrolyte type. Then, the adiabatic accelerated calorimeter is controlled to change the temperature of the battery under test and record the compensation power. If the compensation power is denoted as Pcomp(t), and the integration start and end times corresponding to the melting temperature zone are ta and tb respectively, then the measured heat can be expressed as... The integration interval is from ta to tb.
[0062] Integration can be performed numerically on continuously sampled data by a computing device, or it can be achieved by integrating the compensation power within each temperature step and then summing the results. The integration boundary should cover the target melting process of the electrolyte under test and be consistent with the target thermal event used for subsequent unit enthalpy of melting. Specifically, calorimetry testing can be performed in a heating-waiting-search mode.
[0063] The heating-waiting-search mode refers to the cyclical procedure by which the adiabatic accelerated calorimeter sequentially executes temperature rise steps, waits for thermal equilibrium, and searches for self-heating or thermal response. During the heating phase, the device raises the temperature of the object under test from the current temperature to the next set temperature. During the waiting phase, the test conditions are maintained or adjusted to reduce the temperature difference between the sample, sample chamber, and sensor. During the search phase, the device monitors whether the temperature rise rate or the corresponding thermal response reaches the preset sensitivity, and accordingly enters the next control state or the next temperature step.
[0064] The heating-waiting-search procedure parameters may include the starting temperature, ending temperature, temperature step size, waiting time, search sensitivity, and compensation power sampling parameters. Specifically, the starting temperature can be -60℃, the ending temperature can be 0℃, the temperature step size can be 2℃ to 5℃, the waiting time after each temperature step can be 30 min to 60 min, and the search sensitivity can be 0.01℃ / min to 0.02℃ / min. The above values are used to illustrate a feasible setting and do not limit other settings that can cover the target melting process and obtain stable compensation power data.
[0065] In some embodiments, the starting temperature T1 of the calorimetric test can be selected within the range of -80°C to -55°C, for example, -80°C, -75°C, -70°C, -65°C, -60°C, or -55°C; the ending temperature T2 can be selected within the range of -5°C to 10°C. Preferably, the test temperature range can be -60°C to 0°C. Here, the test temperature range is used to subject the object under test to a complete temperature program, and the melting temperature zone is the target temperature range used to compensate for the power integral; the two do not necessarily have the same boundary.
[0066] The test temperature range needs to cover the target melting process. If the range is too narrow, the start or end of the target melting peak may fall outside the test range, causing the heat of melting involved in the integration to be underestimated; if the range is too wide, it may introduce more non-target background thermal response and noise, and increase the time required for cooling, waiting, and heating. Therefore, based on the preliminary thermal analysis results of the corresponding electrolyte, the non-target temperature range can be limited while fully covering the target melting process.
[0067] When using the heating-wait-search mode, the waiting period after each temperature step allows the complete cell to gradually approach an isothermal or quasi-isothermal state, and the electrolyte's melting endothermic plateau near the corresponding temperature is tracked by compensated power data. Compared to the continuous heating mode without step-by-step thermal equilibrium, this approach reduces the risk of thermal inertia of the complete cell and the risk of internal temperature gradients masking weak endothermic signals. The continuous heating mode is not entirely unusable; it can also be used as an alternative temperature program when it provides comparable thermal equilibrium levels and complete integration of the target thermal events.
[0068] Temperature steps are used to strike a balance between the test cycle and the temperature resolution of the target melting process. If the temperature step is too small, more heating, waiting, and searching cycles are required to complete the same temperature range, significantly extending the test cycle. If the temperature step is too large, it may cross the local melting endothermic plateau of the electrolyte under test, resulting in insufficient acquisition of the corresponding compensation power, leading to an underestimation of integrated heat or the omission of target thermal events. Therefore, 2℃ to 5℃ can be considered a suitable temperature step range for low-temperature melting tests.
[0069] Waiting time is used to ensure that, under conditions of low temperature and limited internal thermal conductivity of the battery, a comparable degree of thermal equilibrium is achieved between the battery's interior and surface, as well as between the test object, sample chamber, and sensor. Waiting times shorter than 30 minutes may result in insufficient internal temperature equilibrium, potentially leading to a lower compensated power integral result; waiting times longer than 60 minutes generally allow for testing, but increase the overall testing time. Therefore, a waiting time of 30 to 60 minutes strikes a balance between thermal equilibrium and testing efficiency.
[0070] The search sensitivity corresponds to the criterion used by the adiabatic accelerated calorimeter to determine whether spontaneous temperature rise or other thermal responses requiring tracking have occurred. If the sensitivity is set too high (i.e., the threshold is too low), equipment noise or minor temperature fluctuations may trigger a control state switch; if the sensitivity is set too low (i.e., the threshold is too high), weaker thermal responses may be missed. Therefore, the threshold can be set within a validated range of 0.01℃ / min to 0.02℃ / min, or other parameters, based on the equipment noise level and the thermal response intensity of the target battery.
[0071] In the aforementioned S220, the thermal correction relationship refers to the processing relationship that uses the first calibrated heat as at least one determining basis to exclude or constrain the thermal contribution of battery components other than liquid electrolyte from the calorimetric results to be processed.
[0072] The first reference cell refers to a reference cell whose dry cell specifications are consistent with those of the battery under test and which does not contain liquid electrolyte. The first calibrated heat is the calibrated calorific result obtained by integrating the compensated power of the first reference cell within the melting temperature range. The first reference cell can be a cell that is not filled with liquid but whose electrodes, separator, solid electrolyte, and casing meet the corresponding dry cell specifications. Its first calibrated heat thus provides an object-level background heat reference for the non-liquid electrolyte battery components.
[0073] Hot correction relationships can be achieved using fixed background subtraction, proportional relationships, lookup tables, or function relationships.
[0074] For example, when the thermal contribution of the non-liquid electrolyte battery components under the same dry cell specification can be approximated as a fixed background, the first calibration heat can be subtracted from the heat to be processed; when the ratio of the background thermal contribution to the thermal response of the complete reference cell is stable, a proportionality coefficient can be used; when the background thermal contribution varies with electrolyte mass, wetting state, or interface state, a functional relationship can be established using multiple reference cells with the same dry cell specification but different known liquid electrolyte masses. The common effect of all these methods is to separate the heat attributed to the target melting process of the electrolyte from the calorimetric results of the battery under test.
[0075] The heat of melting endothermic reaction refers to the heat of melting that is attributed to the target melting process of the electrolyte after thermal correction, and can be denoted as Q1. This heat is different from the measured heat that includes the mixed thermal response of the complete battery. When the input calibrator used for thermal correction is consistent with its calibration calibrator, the processing result can be used as the mass conversion numerator in S230.
[0076] In the aforementioned S230, the unit enthalpy of fusion refers to the heat absorbed by a unit mass of the corresponding electrolyte to complete the target melting process, which can be denoted as ΔH, and the unit can be J / g. The mass of the electrolyte participating in the melting refers to the mass of the electrolyte in the test battery that contributes to the target melting thermal response in the selected melting temperature range, which can be denoted as m1. The conversion relationship between the two can be expressed as: m1=Q1 / ΔH.
[0077] Wherein, Q1 and ΔH should correspond to the same electrolyte type and the same target melting process. Electrolyte source components that have undergone irreversible reactions and no longer exhibit the target melting response can be excluded from the melt-contributing mass; therefore, this test result represents the current mass of the electrolyte that can contribute to the target melting thermal response, and is not necessarily equivalent to the initial electrolyte mass injected during manufacturing.
[0078] When the initial electrolyte mass m0 of the battery under test or the electrolyte mass at another reference time is known, the electrolyte loss and conventional weight loss rate can be determined based on the mass m1 of the electrolyte that participated in melting. The electrolyte loss Δm can be expressed as Δm = m0 - m1, and the conventional weight loss rate λ can be expressed as λ = (m0 - m1) / m0 × 100%. This conventional weight loss rate uses the initial electrolyte mass or the reference electrolyte mass as the denominator to represent the proportion of reduction relative to that reference.
[0079] Unlike conventional weight loss rate, the parameter calculated using η = m1 / M represents the ratio of the mass m1 of the electrolyte currently participating in melting to the total battery mass M. To avoid confusion with the aforementioned conventional weight loss rate, this paper refers to η as the electrolyte residual rate or simply η, i.e., η = m1 / M × 100%. The electrolyte residual rate reflects the weight level of the electrolyte currently carrying the battery that can participate in melting within the entire battery. In practical applications, m1 can be directly output, or the conventional weight loss rate λ and the electrolyte weight index η can be output after obtaining m0 and M, respectively. The appropriate index can be selected based on the specific evaluation criteria.
[0080] Therefore, S210 first converts the changes in the internal state of matter of the packaged battery into an integrable complete battery thermal response; S220 then uses a first reference battery of the same dry cell specifications but without liquid electrolyte to provide background heat data, separating the heat of melting of the electrolyte under test from the complete battery thermal response; S230 finally completes the heat-mass conversion using the unit enthalpy of melting corresponding to the electrolyte type. The battery under test does not need to be completely disassembled to obtain the electrolyte, reducing measurement losses caused by disassembly, evaporation, and sample transfer; simultaneously, the background heat contribution of non-liquid electrolyte battery components is not directly converted into mass as electrolyte melting heat, thereby reducing systematic errors in the detection results. This effect is consistent with the technical effects described in the invention.
[0081] In practical applications, considering the numerous pre-calibrated parameters in the aforementioned processing, the target rules can be directly invoked before actual execution, followed by the execution of P200. This allows the target specifications of the battery under test to be obtained in response to its placement on the adiabatic accelerated calorimeter. The melting temperature zone is determined based on the electrolyte type in the target specifications, and the thermal correction relationship is determined based on the dry cell specifications. Calorimetric test parameters are then determined based on the melting temperature zone and the adiabatic accelerated calorimeter, and these parameters are used to control the adiabatic accelerated calorimeter to perform calorimetric testing on the battery under test.
[0082] During this parameter retrieval process, calorimetric test parameters refer to the set of parameters determined based on the melting temperature range and the current adiabatic accelerated calorimeter, used to control the adiabatic accelerated calorimeter to perform calorimetric tests. These calorimetric test parameters may include one or more of the following: starting temperature, ending temperature, temperature step, waiting time, search sensitivity, and compensation power sampling parameters. The term "determining" here can include parameters generated by the computing device according to rules, or it can include directly retrieving existing parameters from calibration records associated with the target specifications and equipment configuration.
[0083] In one implementation, a calibration database is set up in the memory. A record in the database may include battery system, packaging form, capacity, state of charge, positive and negative electrode materials, solid electrolyte, electrolyte type, melting temperature range, enthalpy of fusion, thermal correction relationship, device identifier, device correction parameters, and calorimetric test parameters. After the battery under test is set in the adiabatic accelerated calorimeter, the calculation device obtains its target specifications, retrieves the melting temperature range and enthalpy of fusion by electrolyte type, retrieves the thermal correction relationship by dry cell specification, and then calls up the calorimetric test parameters in combination with the device identifier and configuration of the current adiabatic accelerated calorimeter.
[0084] Record matching can employ complete matching, preset priority matching, or matching based on parameters falling within a preset range. When no record meets the comparability requirements, the computing device can output a recalibration prompt or stop automatic testing without invoking the mismatched thermal correction relationship. After matching is complete, the computing device uses the calorimetric test parameters to drive the adiabatic accelerated calorimeter to execute S210, and continues executing S220 and S230 after obtaining the test data.
[0085] Through the above processing, the pre-calibration process is separated from the actual testing process of each battery under test. The computing device calls the melting temperature range and unit enthalpy of melting according to the electrolyte type, the thermal correction relationship according to the dry cell specifications, and the calorimetric test parameters according to the current equipment, so that the calibration results with different physical meanings are respectively bound to their determining factors. This reduces the time required for repeated calibration before each test and also reduces the risk of incorrectly applying the calibration results of one electrolyte or one dry cell structure to another.
[0086] In practical applications, the adiabatic accelerated calorimeter, sample chamber, sample cell, sensor, and their test configuration may exhibit differences in thermal inertia, heat transfer paths, and response sensitivity, leading to a response deviation between the measured heat obtained from the compensated power integration and the actual heat corresponding to the tested object. This device response deviation differs from the background heat contribution from non-liquid electrolyte components in the tested battery: the former originates from the calorimeter and its configuration, while the latter originates from the tested battery itself. To address these two types of influences separately, the measured heat can be processed according to the adiabatic accelerated calorimeter's device correction parameters before using thermal correction relationships to eliminate the battery component background.
[0087] Specific sources of equipment response deviations may include thermal radiation loss between the sample and the furnace body, thermal conductivity of the sample support structure, sample cavity heat capacity, sensor installation position, and compensation control delay. Equipment correction parameters incorporate the combined response of these factors under the current equipment and test configuration into the calibration, without requiring separate measurement of each loss. By establishing corresponding equipment correction parameters for different adiabatic accelerated calorimeters or different calorimetric platforms, the measurement results can be converted to the same known true heat range, thereby improving the comparability of test results across equipment or platforms.
[0088] Therefore, the aforementioned S220 may include the following sub-steps: S221. Process the measured heat according to the equipment correction parameters of the adiabatic accelerated calorimeter to obtain the heat absorbed by the battery under test.
[0089] S222. Process the heat absorption of the battery according to the thermal correction relationship corresponding to the dry cell specifications to obtain the heat absorption of the electrolyte in the battery under test.
[0090] In S221, the equipment correction parameter refers to the response parameter established based on the known true heat and the corresponding equipment measured heat, used to convert the calorimetric results of the adiabatic accelerated calorimeter into the corresponding true heat.
[0091] Battery heat absorption refers to the intermediate heat of the battery under test obtained after the measured heat has been processed by the equipment correction parameters, but before the background of the dry cell has been eliminated using the thermal correction relationship. When the equipment correction parameter uses a proportional coefficient α, if the measured heat is Qtotal, then the battery heat absorption Qcell can be expressed as: Qcell = αQtotal.
[0092] The equipment correction parameters should correspond to the current adiabatic accelerated calorimeter, its sample chamber, sensors, and test configuration. The equipment correction parameters can be recalibrated when the equipment or configurations that significantly affect the equipment response are changed.
[0093] In S222, the heat absorbed by the battery is used as the input to the thermal correction relationship corresponding to the dry cell specifications, and the heat absorbed by the melting of the electrolyte to be tested is obtained.
[0094] For example, when using a fixed background subtraction relationship, the first calibration heat can be subtracted from the Qcell; when using a proportional relationship, the Qcell can be multiplied by the corresponding thermal correction factor. The input of the thermal correction relationship should be consistent with the heat caliber used during calibration: if the first and second calibration heats have been corrected by the equipment response, then the Qcell should also use the caliber corrected by the equipment response.
[0095] S221 first standardizes the equipment calorimetry results to the corresponding actual heat range, and S222 then processes the heat contribution from the non-liquid electrolyte components of the battery under test. By correcting according to the order of "equipment response impact - battery component background", it is possible to avoid using a single ambiguous correction amount to simultaneously bear two types of errors, and to reduce the further transmission of equipment response deviation to the electrolyte mass conversion results.
[0096] In some embodiments, the aforementioned device correction parameters can be determined through a calibration process. To further illustrate the process, this application also provides an exemplary flowchart of the device correction parameter calibration process (…). Figure 3 ).
[0097] like Figure 3 As shown, the equipment correction parameter calibration process P300 may include the following steps: S310. Based on the melting temperature range corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric testing on the melting enthalpy standard, and the compensation power of the melting enthalpy standard in the melting temperature range during the calorimetric test is integrated to determine the third calibration heat.
[0098] S320. Determine equipment correction parameters based on the ratio of standard melting heat to third calibration heat.
[0099] In S310, to determine the degree of response of the adiabatic accelerated calorimeter to a known enthalpy of fusion, a calibration object is needed that allows the actual enthalpy of fusion to be predetermined and whose corresponding thermal response can be measured by the adiabatic accelerated calorimeter. Based on this function, a enthalpy of fusion standard refers to a calibration sample whose mass and unit enthalpy of fusion are known and which can undergo a repeatable melting process under target calorimetric conditions.
[0100] In some embodiments, the melting process of the enthalpy of fusion standard falls within the temperature range covered by the adiabatic accelerated calorimeter, and no non-target reactions occur within the melting temperature range used for integration that would alter the true heat of fusion baseline. The enthalpy of fusion standard can be a non-battery standard with a known unit enthalpy of fusion, or a liquid electrolyte sample whose unit enthalpy of fusion has been determined through independent calorimetric testing. When selecting a standard, its melting temperature range can be the same as or adjacent to the temperature range used by the device to be calibrated for subsequent battery testing to reduce extrapolation errors caused by temperature variations in the device response.
[0101] In one specific implementation, the enthalpy of fusion standard is 50g of high-purity n-decane, whose known enthalpy of fusion is 201.4 J / g. Alternatively, n-octane, n-nonane, cyclohexane, adamantane, or other substances with known melting thermal properties and chemical stability within the calibration temperature range can be used. When using a liquid electrolyte sample as the enthalpy of fusion standard, it can be pre-tested... Figure 5 The unit enthalpy of fusion calibration process shown determines its unit enthalpy of fusion.
[0102] In some embodiments, the non-cell standard material with known enthalpy of fusion may be selected from one or more of alkanes, cycloalkanes or isoalkanes, halogenated hydrocarbons, common organic solvents and alcohols, acids, and eutectic mixtures. Alkanes may include n-octane, n-nonane, n-decane, and adamantane; cycloalkanes or isoalkanes may include cyclohexane, methylcyclohexane, and neopentane; halogenated hydrocarbons may include chloroform, carbon tetrachloride, 1,2-dichloroethane, and chlorobenzene; common organic solvents and alcohols may include benzene, ethylene glycol, and tert-butanol; acids may include benzoic acid and sebacic acid; and eutectic mixtures may include sodium chloride-water eutectic, calcium chloride-water eutectic, magnesium chloride-water eutectic, and naphthalene-biphenyl mixtures.
[0103] Enthalpy of fusion standards can be selected based on chemical inertness, thermal stability, known thermophysical properties, high purity, and temperature coverage. Chemical inertness reduces the likelihood of the standard reacting with the sample cell or test atmosphere; thermal stability ensures a repeatable composition within the calorimetric program; known thermophysical properties provide a traceable standard heat of fusion; high purity minimizes melting point and enthalpy of fusion deviations caused by impurities; and temperature coverage ensures that the melting process of the standard falls within the range that can be accurately measured by the target equipment and the target test temperature range. When these conditions are met, the difference between the measured value of the standard and the standard heat of fusion primarily reflects the thermal response of the equipment and its test configuration, rather than uncontrollable chemical changes occurring in the standard itself.
[0104] To provide a true thermal baseline for equipment measurement results, the standard heat of fusion refers to the true heat of fusion determined based on the known mass and known unit enthalpy of fusion of a standard sample. If the mass of the standard sample is mstd and the known unit enthalpy of fusion is ΔHstd, then the standard heat of fusion Qstd can be expressed as: Qstd = mstd × ΔHstd.
[0105] In some embodiments, the mass and unit enthalpy of fusion are multiplied using compatible units of measurement, and the melting process corresponding to this unit enthalpy of fusion is made consistent with the target melting process integrated in the adiabatic accelerated calorimeter. Thus, the standard heat of fusion is not a reading from the adiabatic accelerated calorimeter, but rather a known, true quantity used to evaluate that reading.
[0106] In the aforementioned n-decane example, the standard heat of fusion is 50 × 201.4 = 10070 J.
[0107] In order to obtain the actual reading of the above-mentioned true melting heat of the current adiabatic accelerated calorimeter and its test configuration, the third calibration heat refers to the heat obtained by integrating the compensation power in the corresponding melting temperature range when the adiabatic accelerated calorimeter performs calorimetric testing on the melting enthalpy standard.
[0108] In some embodiments, a melting enthalpy standard is placed in the sample chamber of an adiabatic accelerated calorimeter, and a calorimetric program covering the melting process of the standard is executed. Compensation power is collected within the temperature range where the standard transitions from a solid to a liquid state, and the compensation power is integrated over time. The third calibration heat can be associated and stored with the adiabatic accelerated calorimeter's device identifier, sample chamber, temperature sensor, compensation heating configuration, and calorimetric program parameters. When the above configuration undergoes a change sufficient to alter the heat response, the third calibration heat can be recalibrated.
[0109] In one specific implementation, the adiabatic accelerated calorimeter adopts a heating-waiting-search mode with an initial temperature of -60℃, an ending temperature of 0℃, a temperature step of 5℃, and a waiting time of 45min after each temperature step. The third calibration heat Q3 = 9590.5J is obtained by integrating the compensated power in the melting temperature range of n-decane.
[0110] In S320, in order to convert the equipment readings to the true heat caliber, the equipment correction parameter refers to the parameter established based on the standard heat of fusion of the same enthalpy standard and the third calibration heat, which is used to correct the heat response of the adiabatic accelerated calorimeter.
[0111] In some embodiments, the device correction parameter can be represented by a proportional, piecewise proportional, or calibration function. When the device response within the target calorimetric range can be approximated by a proportional approach, the device correction parameter α can be expressed as: α = Qstd / Q3.
[0112] Therefore, multiplying α by the measured heat obtained under the same equipment and comparable test configuration yields the heat corrected according to the standard true heat caliber. α represents the ratio of the true heat to the heat measured by the equipment, without presupposing that it must be greater than 1 or less than 1; α is greater than 1 when the third calibration heat is less than the standard melting heat, and less than 1 when the third calibration heat is greater than the standard melting heat. If the equipment's response in different heat ranges is not a single proportion, multiple known masses of melting enthalpy standards can be used to establish a piecewise function or fitting function, and the corresponding function value can be called according to the range of heat to be corrected.
[0113] In the aforementioned n-decane example, α = 10070 / 9590.5 = 1.05.
[0114] The P300 allows the compensation power integral result of the adiabatic accelerated calorimeter to be converted to a heat caliber consistent with the known heat of fusion. Since the standard heat of fusion and the third calibration heat of fusion correspond to the same standard and the same melting process, the resulting equipment correction parameters mainly compensate for the thermal response deviation of the current equipment and test configuration, reducing the impact of this deviation on the heat absorption and mass results of the electrolyte under test.
[0115] In some embodiments, the aforementioned thermal correction relationship can be characterized as a thermal correction coefficient, or as a fixed background subtraction relationship, a piecewise relationship, a fitting function, or a lookup table. The gap that the thermal correction relationship needs to fill is that the calorimetric results of the complete cell simultaneously include the target molten heat contribution of the electrolyte under test and the equivalent thermal contribution of the non-liquid electrolyte components under the calorimetric conditions of the complete cell; without establishing a separation rule between the two, the heat of the complete cell cannot be reliably attributed to the electrolyte under test.
[0116] The equivalent thermal contribution here refers not only to the intrinsic phase transition enthalpy measured independently for each of the non-liquid electrolyte components, but also to the combined contribution of these components to the compensated power integral result in terms of the heat transfer path, thermal capacity coupling, wetting state, and interfacial state of the complete cell. Although the amount of non-liquid electrolyte components can remain constant, changes in the mass of the liquid electrolyte may alter the wetting degree of the electrodes and separator, the thermal contact between components, and local interfacial thermal processes. Therefore, its equivalent thermal contribution in the complete cell can be a fixed amount or vary with the mass of electrolyte involved in the melting process.
[0117] When the equivalent heat contribution can be approximated as a fixed background, the difference relationship Q1 = Qcell - Qdry can be used. This implementation directly subtracts the first calibration heat Qdry provided by the first reference cell of the same dry cell specification from the heat absorbed by the cell under test Qcell, which is suitable for specification ranges where the background heat is not sensitive to changes in electrolyte quality.
[0118] When the ratio of the equivalent thermal contribution to the full battery thermal response is approximately stable within the target specifications and target mass range, a thermal correction factor k can be used, and the melting heat absorption can be determined according to Q1 = kQcell. This proportional relationship is equivalent to extracting the electrolyte melting heat contribution from the full thermal response according to a calibrated ratio, suitable for scenarios where the required accuracy can be obtained using a first reference battery and a liquid-containing reference battery.
[0119] When the equivalent heat contribution varies with the mass of the electrolyte involved in melting, it can be expressed as a function of mass, B(m). If the mass of the electrolyte to be measured is represented by the unknown quantity x, then the heat of the complete battery can be expressed as Qcell = xΔH + B(x), or x = [Qcell - B(x)] / ΔH. The computing device can solve this equation analytically, numerically, or by looking up a table based on a pre-calibrated B(x), thereby simultaneously obtaining the unknown mass x and the background heat contribution corresponding to that mass.
[0120] To calibrate B(m), multiple reference cells with the same dry cell specifications, containing the same type of liquid electrolyte as the electrolyte under test, but with different known liquid electrolyte masses mi, can be set up. The calibration heat Qi is obtained for each reference cell under the same thermal caliber, and the equivalent background heat contribution at the corresponding mass point is obtained according to Bi = Qi - miΔH. Multiple (mi, Bi) calibration points can be used to establish linear functions, piecewise functions, nonlinear fitting functions, or lookup tables.
[0121] As an equivalent implementation, a complete reference heat function G(m) with respect to the mass of the liquid electrolyte can be directly established using multiple (mi, Qi) calibration points. After testing the battery under test and obtaining Qcell, the unknown mass x is determined by solving Qcell = G(x), and then the melting heat is obtained according to Q1 = xΔH. For cases where two calibration points can support a linear approximation, G(m) = am + b, where a = (Qb - Qa) / (mb - ma), b = Qa - a·ma, thus obtaining x = (Qcell - b) / a. The mass of the liquid electrolyte corresponding to the first reference battery is zero, which can also be used as the zero-mass calibration point in the above fitting.
[0122] In some embodiments, k(m) can be calibrated separately for different electrolyte mass ranges, or one or more of the following can be used as inputs to a function or lookup table: electrolyte mass, wetting state characterization, cycling state, and state of charge. Regardless of whether a fixed value, proportional coefficient, or mass-related function is used, the calibration data and the test data use the same or convertible equipment correction caliber, calorimetric program, and integral temperature range to ensure that the invoked thermal correction relationship is comparable to the current test battery.
[0123] The first reference cell is used to represent the background heat contribution of the battery components (excluding the liquid electrolyte) in the test battery within the melting temperature range. Therefore, the first reference cell refers to a reference cell with the same dry cell specifications as the test battery but without liquid electrolyte.
[0124] In some embodiments, the first reference cell is consistent with or comparable to the cell under test in at least one of the following aspects affecting background heat contribution: electrodes, current collectors, separator, binder, solid electrolyte, casing, dimensions, and state of charge, and employs a calorimetric program and integrated temperature range comparable to the cell under test. The first reference cell may be a dry cell without electrolyte filling, or a reference object assembled with the same structure without introducing liquid electrolyte.
[0125] In one specific implementation, the first reference battery is an unfilled cell with the same dry cell structure as the 50Ah lithium-ion pouch battery under test.
[0126] The first calibration heat is used to quantify the background heat contribution mentioned above. Therefore, the first calibration heat refers to the compensated power integral result of the first reference cell in the melting temperature region, which can be denoted as Qdry.
[0127] In some embodiments, the first calibration heat is stored in association with the dry cell specifications of the battery under test and the calorimetric procedure used to obtain the heat. The first calibration heat can be either subtracted directly from the heat absorbed by the battery as a fixed background quantity, or it can be used as background calibration data in a proportional or functional relationship.
[0128] In the aforementioned specific implementation, the compensation power integral of the first reference battery within the range of -50℃ to -10℃ yields Qdry = 142.76J.
[0129] The second reference cell is used to provide a complete reference thermal response when containing the target type of liquid electrolyte. Therefore, the second reference cell refers to a reference cell with the same dry cell specifications as the battery under test and containing a liquid electrolyte of the same type as the electrolyte under test.
[0130] In some embodiments, the second reference battery preferably uses electrodes, current collectors, separators, solid electrolytes, and casings from the same batch or at least with comparable thermal backgrounds as the first reference battery; the formulation or type of the liquid electrolyte in the second reference battery is the same as the electrolyte type of the electrolyte to be tested. The second reference battery uses a calorimetric program and integrated temperature range comparable to the first reference battery and the battery to be tested. The second reference battery can be a finished battery with a known electrolyte injection volume, or a specially prepared reference battery with a known electrolyte injection volume.
[0131] In one specific embodiment of a reference battery pair, the first and second reference batteries are identical in their battery system, packaging form, nominal capacity, state of charge, type and proportion of positive electrode active material, type and proportion of negative electrode active material, type and proportion of conductive agent, type and proportion of binder, current collector, separator, solid electrolyte, and casing. The difference between the two is at least that the first reference battery does not contain liquid electrolyte, while the second reference battery contains a known mass of target type liquid electrolyte. By making the design parameters affecting the background heat contribution identical, the structural differences between the reference objects that are incorporated into the thermal correction relationship can be reduced.
[0132] A typical cell structure for a reference battery may include a positive electrode, a negative electrode, a separator disposed between the positive and negative electrodes and allowing ions to pass through, a solid electrolyte, and a casing. The positive electrode may include a positive current collector and a layer of positive active material disposed on one or both sides of the positive current collector; the negative electrode may include a negative current collector and a layer of negative active material disposed on one or both sides of the negative current collector. The second reference battery also includes a liquid electrolyte, while the first reference battery does not include a liquid electrolyte during the corresponding background calibration.
[0133] In some embodiments, the positive or negative electrode sheet can be prepared by adding the corresponding active material, conductive agent, and binder to a solvent and dispersing them at high speed to form a slurry, then coating the slurry onto one or both sides of a current collector, and obtaining the electrode sheet through drying, rolling, slitting, and die-cutting. The active material, conductive agent, binder, and solvent can be materials commonly used in the corresponding battery system, as long as the required dry cell thermal background comparability is maintained between the first reference cell, the second reference cell, and the battery under test.
[0134] In some embodiments, the positive electrode, separator, and negative electrode can be stacked sequentially, or the corresponding layers can be wound, followed by baking, electrolyte injection, formation, and encapsulation as needed to form a second reference cell or a cell under test. The first reference cell can omit the electrolyte injection step and adopt appropriate assembly and encapsulation methods. The material and shape of the separator, the specific composition of the liquid electrolyte, and the battery assembly process are not particularly limited, but the aforementioned comparability conditions should be met between reference cells used in the same set of calibrations.
[0135] In one specific implementation, the second reference battery is a finished battery cell with the same dry cell specifications as the first reference battery and which has been injected with EL1 type liquid electrolyte.
[0136] The second calibration heat is used to characterize the complete reference thermal response of the second reference cell within the same melting temperature range. Therefore, the second calibration heat refers to the compensated power integral result of the second reference cell within the melting temperature range, which can be denoted as Qwet.
[0137] In some embodiments, the second calibration heat and the first calibration heat are corrected using the same equipment for aperture correction and integration boundary. The second calibration heat can be obtained by subtracting the first calibration heat from the first calibration heat, or it can be used together with the first calibration heat as calibration data for a multi-mass point function or lookup table.
[0138] In the aforementioned specific implementation, the compensation power integral of the second reference battery within the range of -50℃ to -10℃ yields Qwet = 3568.9J.
[0139] The calibrated melt endothermic heat is used to separate the increased reference thermal contribution of the liquid electrolyte from the complete reference thermal response of the second reference cell. Therefore, the calibrated melt endothermic heat is the difference between the second calibrated heat and the first calibrated heat, which can be denoted as Qcal: that is, Qcal = Qwet - Qdry.
[0140] In some embodiments, when both the first and second calibration heat values are corrected by the equipment, they use the same equipment correction parameters; when the equipment influence is included in the calibration calibrator of the thermal correction relationship, the subsequent measured heat values of the battery under test are processed using the same calibrator. This avoids directly subtracting or comparing values under different heat calibrators.
[0141] When a proportional thermal correction relationship is used, the thermal correction coefficient k indicates the proportion of heat attributable to the melting process of the target type liquid electrolyte after background constraints from the first reference cell, within the complete reference thermal response of the second reference cell. It can be expressed as: k = Qcal / Qwet = (Qwet - Qdry) / Qwet.
[0142] In some embodiments, k is stored in association with the dry cell specifications, electrolyte type, melting temperature range, and calorimetric program of the battery under test. When using independent device correction, the measured heat of the battery under test can be processed according to the device correction parameters to obtain the battery endothermic heat Qcell, and then the melting endothermic heat of the electrolyte under test can be obtained according to Q1 = kQcell. When the calibration calibrator of the thermal correction relationship already includes the influence of device response or when device response correction is not performed separately, the measured heat can be processed directly according to the same calibrator as the calibration.
[0143] In the aforementioned specific implementation, k = (3568.9 - 142.76) / 3568.9 = 96%.
[0144] The aforementioned first calibration heat, second calibration heat, and thermal correction relationship can be pre-calibrated using an adiabatic accelerated calorimeter and directly invoked according to the dry cell specifications and electrolyte type during battery testing. To further illustrate the calibration process, this application also provides an exemplary flowchart of the thermal correction relationship calibration process (…). Figure 4 ).
[0145] like Figure 4 As shown, the thermal correction relationship calibration process P400 may include the following steps: S410. Based on the melting temperature zone corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric testing on the first reference cell, and the compensation power of the first reference cell in the melting temperature zone during the calorimetric testing is integrated to determine the first calibration heat.
[0146] S420. Based on the melting temperature zone corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric testing on the second reference cell, and the compensation power of the second reference cell in the melting temperature zone during the calorimetric testing is integrated to determine the second calibration heat.
[0147] S430. Determine the thermal correction relationship based on the first and second calibration heat.
[0148] In the implementation of S410, a first reference cell is placed in an adiabatic accelerated calorimeter and tested according to a calorimetric program that matches the melting temperature range of its corresponding electrolyte type. The compensation power is integrated only within that melting temperature range. The first reference cell does not contain liquid electrolyte, so that the obtained first calibrated heat can be used as a background heat reference for the non-liquid electrolyte battery components.
[0149] In one specific implementation of S410, a heating-waiting-search procedure with an initial temperature of -60℃, an ending temperature of 0℃, a temperature step of 5℃, and a waiting time of 45min is used to test unfilled soft-pack cells, and integration is performed within the range of -50℃ to -10℃ to obtain Qdry = 142.76J.
[0150] In the implementation of S420, a second reference cell is placed in the same adiabatic accelerated calorimeter and tested under a calorimetric program comparable to that of S410, with the compensated power integrated over the same melting temperature range. The second reference cell contains a liquid electrolyte of the same type as the electrolyte under test, enabling the second calibration heat to provide a complete reference thermal response with the same object basis as the first calibration heat.
[0151] In one specific implementation of S420, a finished cell with the same dry cell specifications as the first reference cell and containing EL1 type liquid electrolyte is used as the second reference cell. The same procedure as S410 is used and integration is performed within -50℃ to -10℃ to obtain Qwet = 3568.9J.
[0152] In the implementation of S430, the thermal correction relationship can be selected according to the stability of the background thermal contribution of the non-liquid electrolyte battery components. When the background thermal contribution can be regarded as a fixed amount, a difference relationship with Qdry as the deduction amount is established; when the ratio of the background thermal contribution to the thermal response of the complete battery is relatively stable, a thermal correction coefficient k is established; when the background thermal contribution changes with the mass or wetting state of the liquid electrolyte, multiple calibration points are obtained using multiple second reference batteries with different known liquid electrolyte masses, and a fitting function or lookup table is established to output the melting heat endothermic attribution to the liquid electrolyte, using the liquid electrolyte mass or the complete reference thermal response as the independent variable.
[0153] In one specific implementation of S430, the calibrated heat of melting is first determined using Qwet-Qdry, and then the ratio of this calibrated heat of melting to Qwet is determined as k. S430 does not use a third calibrated heat; the third calibrated heat belongs to... Figure 3 The calibration process for the device correction parameters is shown.
[0154] The P400 achieves comparable calorimetry between unfilled reference cells and reference cells containing the target type of liquid electrolyte, ensuring that the background thermal response of non-liquid electrolyte battery components shares the same object basis as the complete thermal response with liquid electrolyte. The thermal correction relationship determined by these two methods can be pre-associated and stored with the dry cell specifications and electrolyte type, and can be directly retrieved during subsequent testing of the battery under test, eliminating the need for synchronized configuration of reference cells each time.
[0155] Considering that P200, P300 and P400 all use an adiabatic accelerated calorimeter for calorimetry, in order to avoid the difference in calorimetry program being mistaken for the difference in heat of the tested object, the relevant calibration test and the test of the battery under test can use comparable heating-wait-search program parameters.
[0156] Comparable heating-wait-search procedure parameters mean that each test maintains consistency at least in terms of the starting temperature, ending temperature, temperature step, waiting time, search sensitivity, compensation power sampling aperture, and integration temperature range, which are sufficient to affect the thermal comparison. Comparability here does not preclude implementing safety or range adaptations for different sized objects without changing the physical integration aperture.
[0157] In some embodiments, the heating phase raises the sample temperature by a preset temperature step from the current temperature; the waiting phase allows the sample, sample chamber, and sensor to reach a preset thermal equilibrium condition; the search phase determines whether the sample experiences spontaneous temperature rise or other thermal events according to a preset sensitivity, and proceeds to the next temperature step or corresponding tracking control accordingly. Regardless of whether the complete program contains multiple loops, the value used to determine the measured heat or calibration heat is the integral of the compensation power within the target melting temperature range, not the integral of all compensation heat over the entire test temperature range.
[0158] In one specific implementation, the first reference cell, the second reference cell, and the cell under test all employ a heating-wait-search procedure with an initial temperature of -60°C, an ending temperature of 0°C, a temperature step of 5°C, and a waiting time of 45 minutes, and integrate the power compensation within the range of -50°C to -10°C. Therefore, the differences between Qdry, Qwet, and Qtotal primarily stem from the tested object itself, rather than from different heating histories, waiting periods, or integration boundaries.
[0159] In some embodiments, the liquid electrolyte is composed of various solvents, lithium or sodium salts, and additives, and its unit enthalpy of fusion is difficult to accurately derive from the composition alone. Therefore, before testing the battery under test, a liquid electrolyte of the same type as the electrolyte under test can be calibrated for its unit enthalpy of fusion, and the calibration results can be used during actual testing.
[0160] Unlike adiabatic accelerated calorimetry (ACC) which measures the calorimetry of a complete or reference cell, differential scanning calorimetry (DSC) can be used to independently determine the enthalpy of fusion. A DSC is used to measure the difference in heat flow between the sample and reference ends during a programmed temperature change.
[0161] The unit enthalpy of fusion test refers to performing differential scanning calorimetry on a liquid electrolyte sample of the same type as the electrolyte being tested to determine its heat of fusion within a target melting temperature range, and then normalizing this heat of fusion to a unit mass heat using the known mass of the sample. This calibration result corresponds to the electrolyte type, avoiding the use of the unit enthalpy of fusion from another formulation or model for current mass conversion.
[0162] In some embodiments, the unit enthalpy of fusion can be pre-stored in the computing device according to the electrolyte type, starting temperature, heating rate, and integration temperature range. When actually testing the battery under test, the computing device directly calls the matching unit enthalpy of fusion, without needing to simultaneously perform differential scanning calorimetry (DSC) testing for each battery under test in an adiabatic accelerated calorimetry test.
[0163] To further illustrate the calibration of unit enthalpy of fusion, this application also provides an exemplary flowchart of the unit enthalpy of fusion calibration process ( Figure 5 ).
[0164] like Figure 5 As shown, the unit enthalpy of fusion calibration process P500 may include the following steps: S510. Place a known mass of liquid electrolyte of the same type as the electrolyte to be tested into a sample crucible, and seal the sample crucible by cold welding. Use an empty aluminum crucible of the same mass as the sample crucible as a blank reference crucible.
[0165] S520. The sample crucible and the blank reference crucible are respectively placed in the differential scanning calorimeter. The furnace body of the differential scanning calorimeter is precooled to the starting temperature of the unit melting enthalpy test using liquid nitrogen. The differential scanning calorimeter is controlled to heat up at a preset heating rate to obtain the sample heat flow curve corresponding to the sample crucible and the blank baseline corresponding to the blank reference crucible.
[0166] S530. Subtract the blank baseline from the sample heat flow curve, and integrate the sample heat flow curve after subtracting the blank baseline within the melting temperature region to obtain the sample melting heat of the liquid electrolyte.
[0167] S540. Determine the unit enthalpy of fusion based on the ratio of the sample's heat of fusion to the known mass of the liquid electrolyte.
[0168] In S510, in order for the heat of fusion measured by the differential scanning calorimeter to correspond to a specific mass of liquid electrolyte, it is necessary to limit electrolyte evaporation during the test and set a reference object that can be used to subtract the crucible background.
[0169] A sample crucible is a sealed crucible that contains a known mass of liquid electrolyte of the same type as the electrolyte to be tested. Its function is to maintain the known sample mass and to use the liquid electrolyte as the analyte at the sample end of the differential scanning calorimeter.
[0170] In some embodiments, the sample crucible is made of materials and structures compatible with the liquid electrolyte, capable of withstanding the unit enthalpy of fusion test temperature range, and suitable for differential scanning calorimetry. The mass of the liquid electrolyte can be determined by the difference in weight before and after sample addition; sample preparation and transfer can be performed in an argon-protected glove box or other environments that reduce the effects of moisture and volatilization.
[0171] Liquid electrolyte samples used for unit enthalpy calibration can be obtained from independently prepared samples, retained samples, or reference cells with the same electrolyte type as the test electrolyte. When it is necessary to verify the electrolyte composition within a specific cell and the cell has an injection or extraction port, a trace sample can also be obtained through existing ports. For fully sealed cells, a trace sample for differential scanning calorimetry can be obtained through a small, localized opening without disassembling the cell body. The above sampling methods are merely one option for obtaining pre-calibrated samples and do not require sampling for each test of the test cell, nor do they change the... Figure 2 The actual testing process shown can be performed without disassembling the battery under test.
[0172] In one specific implementation, the sample crucible is a high-pressure sealed aluminum crucible, filled with 8 mg to 15 mg of liquid electrolyte; in this example, 10 mg of EL1 type liquid electrolyte is used.
[0173] When the sample mass is too small, the heat flux signal generated by the melting of the liquid electrolyte is weak, which can easily lead to a decrease in the signal-to-noise ratio and increase the uncertainty of the peak area integral. When the sample mass is too large, the heat transfer inside the crucible may be uneven, causing a lag in the melting initiation temperature and broadening the peak shape. Using a sample mass of 8 mg to 15 mg can achieve a balance between the heat flux signal intensity and the heat transfer uniformity inside the sample, with 10 mg being a preferred specific sampling amount.
[0174] Cold welding sealing refers to forming a sealed structure in the sample crucible without significantly heating the sample. Its purpose is to reduce the volatilization of low-boiling-point solvents during sample preparation, transfer, and heating, and to prevent uncontrollable changes in the known sample mass before obtaining the heat flow profile.
[0175] In some embodiments, after sample addition and weighing are completed, the sample crucible can be sealed by mechanical pressing or a cold welding device adapted to the crucible structure, and the sealing strength meets the test conditions from the starting temperature to the ending temperature.
[0176] In one specific implementation, a high-pressure sealed aluminum crucible containing 10 mg of EL1 type liquid electrolyte is cold-welded sealed.
[0177] A blank reference crucible is an aluminum crucible that contains no liquid electrolyte and has the same mass as the sample crucible. Its purpose is to provide background heat flux for the crucible's own heat capacity, structure, and instrument baseline formation.
[0178] In some embodiments, the blank reference crucible and the sample crucible are made of the same material and have the same structure, and are tested under the same temperature program. Besides directly selecting empty crucibles of the same mass, the mass difference between the two can be kept within a preset tolerance range by screening or weighting.
[0179] In one specific implementation, an empty aluminum crucible with the same mass as a high-pressure sealed aluminum crucible containing 10 mg of electrolyte is used as a blank reference crucible.
[0180] In S520, the sample heat flow profile refers to the heat flow response curve formed by the sample crucible and the liquid electrolyte therein under a preset temperature program. This curve simultaneously includes the thermal response of the liquid electrolyte, the thermal capacity response of the sample crucible, and the influence of the instrument baseline.
[0181] In some embodiments, the sample crucible is placed at the sample end of the differential scanning calorimeter. The furnace body is pre-cooled to the starting temperature for the unit enthalpy of melting test using liquid nitrogen and the temperature field is stabilized. Then, the temperature is increased to the termination temperature at a preset heating rate, and the temperature and heat flow are recorded throughout the process. The test temperature range covers the target melting process.
[0182] In one specific implementation, the furnace body is pre-cooled to -60°C and stabilized, then heated from -60°C to 0°C at a rate of 1°C / min. The pre-cooling time can be 30 to 45 minutes, and the nitrogen purging flow rate can be 50 mL / min.
[0183] In some embodiments, the preset heating rate can be from 0.5°C / min to 2°C / min, and the pre-cooling stabilization time is preferably 40 min. After pre-cooling is completed, heating can begin once the furnace body, sample end, and reference end have been confirmed to have reached the preset stabilization conditions, without requiring a fixed time as the sole criterion.
[0184] If the precooling time is too short, the temperature field of the furnace body and the sample end may not be stable, resulting in blank baseline drift and increased melting peak integration error. If the precooling time is too long, it may increase the risk of excessive component shrinkage, moisture intrusion and frosting, and increased background noise in some equipment environments. 30 min to 45 min, and preferably 40 min, is used to balance low-temperature stability and testing efficiency.
[0185] When the heating rate is too low, the melting peak may broaden over a longer period, reducing the instantaneous heat flux amplitude and signal-to-noise ratio, and prolonging the testing time. When the heating rate is too high, the thermal hysteresis between the sample and the sensor may cause peak position shift, peak shape distortion, or overlap between the target melting peak and adjacent background peaks. Setting the heating rate in the range of 0.5℃ / min to 2℃ / min is beneficial for balancing testing efficiency, peak shape resolution, and integral accuracy of unit enthalpy of fusion.
[0186] The blank baseline refers to the background heat flow profile formed by a blank reference crucible under the same temperature program as the sample crucible. Its purpose is to provide a non-sample heat flow reference that can be subtracted from the sample heat flow profile.
[0187] In some embodiments, the blank baseline and the sample heat flow profile have the same or alignable temperature coordinates, time coordinates, and sampling aperture. The blank reference crucible can be tested separately from the sample crucible using the same procedure, or it can be tested synchronously in a differential scanning calorimeter equipped with a synchronous sample end and a reference end.
[0188] In one specific implementation, a blank baseline is obtained using an empty aluminum crucible of the same mass following a temperature program of -60°C to 0°C at a rate of 1°C / min.
[0189] In S530, the net heat flux profile refers to the heat flux profile of the sample after subtracting the blank baseline. Its purpose is to attribute the melting peak area primarily to the liquid electrolyte, rather than the crucible heat capacity or the instrument baseline.
[0190] In some embodiments, the temperature or time coordinates of the sample heat flux curve and the blank baseline are aligned before subtraction. Subtraction can be performed point by point, or it can be performed after fitting the blank baseline. The net heat flux curve after subtraction is integrated within the target melting temperature region, and the integration boundary is selected based on the principle of covering the target melting peak and excluding adjacent non-target peaks.
[0191] In one specific implementation Figure 7 The net heat flux curve of the EL1 type liquid electrolyte is shown, with the integration of the net heat flux curve over the range of -50℃ to -10℃.
[0192] The sample melting heat is the integral result of the net heat flux curve within the target melting temperature range, and can be denoted as Q2. Its function is to provide the melting heat molecule before normalization according to the sample mass.
[0193] In some embodiments, the melting process, integral temperature zone, and heat sign convention corresponding to Q2 are consistent with the unit enthalpy of fusion used for converting the mass of the battery under test.
[0194] In the aforementioned specific implementation, Q2 = 283.3 mJ.
[0195] In S540, the unit enthalpy of fusion refers to the ratio of the heat of fusion of the sample to the known mass of the liquid electrolyte in the sample. Its function is to provide a reference for the unit mass heat required to calculate the mass involved in the fusion from the heat absorbed during melting of the electrolyte. If the known mass of the liquid electrolyte is m, then: ΔH = Q² / m.
[0196] In some embodiments, when Q2 is expressed in joules and m in grams, the unit of ΔH is joules per gram. The unit enthalpy of fusion is stored in association with the electrolyte type, temperature program, and integration temperature zone; when recalled, its corresponding melting process is made consistent with the melting process integrated in the calorimetric test of the battery under test.
[0197] In the aforementioned specific implementation, ΔH = 283.3 mJ / 10 mg = 28.33 J / g.
[0198] By using sealed sample preparation, blank baseline subtraction, and integral processing of the same melting process in P500, the effects of liquid electrolyte evaporation, crucible heat capacity differences, and baseline drift on the unit enthalpy of fusion can be reduced. This unit enthalpy of fusion, after calibration, serves as a retrievable parameter corresponding to the electrolyte type for the heat-mass conversion of the battery under test.
[0199] In some embodiments, the unit enthalpy of fusion test and the calorimetric test of the battery under test can use the same starting temperature, and the integration temperature range of both tests can correspond to the same melting process of the electrolyte under test. The same melting process here means that the endothermic response integrated by the two tests both originate from the process of the target type liquid electrolyte changing from a solid state to a liquid state, and it is not required that the differential scanning calorimeter and the adiabatic accelerated calorimeter use the same temperature rise control method.
[0200] In actual testing, the melting temperature range can be determined through pre-calibration of the liquid electrolyte and stored according to the electrolyte type for recall during the testing process and in P300, P400, and P500. The melting temperature range is selected such that the solid electrolyte and electrode materials do not undergo a phase transition sufficient to interfere with the determination of the endothermic melting of the electrolyte under test, while the electrolyte under test undergoes the target melting process within this temperature range.
[0201] In one specific implementation, the melting temperature range is -50℃ to -10℃, and the test temperature ranges of both adiabatic accelerated calorimetry and differential scanning calorimetry cover this melting temperature range.
[0202] To further illustrate the actual implementation process of the detection method in this application, actual calibration, testing, and comparative testing were conducted, and the results were obtained. Figure 6 , Figure 7 and Figure 8 The results are shown. Figure 6 The compensated power curve is obtained by performing calorimetric testing on the battery under test using an adiabatic accelerated calorimeter. Figure 7 The net heat flow curve for the liquid electrolyte was obtained by measuring the unit enthalpy of fusion using a differential scanning calorimeter. Figure 8 This table presents the test results for each embodiment and comparative example. Figure 6 and Figure 7 The specific meaning of has been explained above.
[0203] The following provides a detailed description of the various embodiments and comparative examples of the actual calibration and testing of this application. The embodiments and comparative examples described below are... Figure 8 The specific test results.
[0204] Example 1: The battery under test in this embodiment is a 50Ah lithium-ion soft-pack solid-liquid hybrid battery A. The electrolyte under test is type EL1, the predetermined actual electrolyte mass is 80g, the state of charge is 0%, and the total battery mass is 1080g. The following specific values are for illustrative purposes. Figures 6 to 8 The process of obtaining the results shown is not intended to limit other battery systems, packaging forms, electrolyte volume, or electrolyte type.
[0205] First, the equipment calibration parameters are performed. Weigh 50g of high-purity n-decane as the melting enthalpy standard. The known unit melting enthalpy of n-decane is 201.4J / g, therefore the standard melting heat is: Qstd=50×201.4=10070J.
[0206] Calorimetric analysis of n-decane was conducted using a heating-waiting-search mode, with an initial temperature of -60℃ and an ending temperature of 0℃, in 5℃ increments, and a waiting time of 45 min after each temperature increment. The compensated power integral over the melting temperature range of n-decane yielded the third calibrated heat Q3 = 9590.5 J, from which we obtained: α = Qstd / Q3 = 10070 / 9590.5 = 1.05.
[0207] Then, the thermal correction relationship was calibrated. A first reference battery without electrolyte and a second reference battery containing EL1 type liquid electrolyte, both with the same dry cell specifications, were selected and tested under the same adiabatic accelerated calorimetry program as described above. The compensated power integral within the melting temperature range yielded the first calibrated heat Qdry = 142.76 J and the second calibrated heat Qwet = 3568.9 J. Therefore: k = (Qwet - Qdry) / Qwet = (3568.9 - 142.76) / 3568.9 = 96%.
[0208] The same heating-waiting-search procedure was then used to perform calorimetric testing on the battery under test. Figure 6 The compensated power curve of the battery under test during the test process from -60℃ to 0℃ is shown. Integrating the melting temperature range from -50℃ to -10℃, the measured heat Qtotal = 2244.2J is obtained. After first correcting the equipment response, and then processing with the thermal correction coefficient, the melting heat absorption of the electrolyte under test is obtained: Q1 = αkQtotal = 1.05 × 96% × 2244.2 = 2262.15J.
[0209] Perform a unit enthalpy test on the EL1 type liquid electrolyte. Take 10 mg of liquid electrolyte and place it in a high-pressure sealed aluminum crucible and cold weld it. Use an empty aluminum crucible of the same mass as a blank reference crucible. Pre-cool the differential scanning calorimeter furnace to -60℃ and stabilize it. Increase the temperature from -60℃ to 0℃ at a rate of 1℃ / min. Figure 7The net heat flow curve after subtracting the blank baseline is shown; integrating the net heat flow curve from -50℃ to -10℃, the heat of fusion of the sample is obtained as Q2 = 283.3 mJ. Therefore: ΔH = Q2 / m = 283.3 mJ / 10mg = 28.33 J / g.
[0210] Therefore, the mass of the electrolyte to be tested that participated in the melting is: m1=Q1 / ΔH=2262.15 / 28.33=79.85g.
[0211] The mass error for this test is -0.19% compared to the predetermined actual electrolyte mass of 80g. Figure 8 The ratio of the mass of the electrolyte to be melted to the total mass M of the battery was calculated according to η = m1 / M, and the result was 79.85 / 1080 = 7.39%. Figure 8 The column labeled "Battery Weight Loss Rate" uses the aforementioned electrolyte weight index η, not the conventional weight loss rate λ. If 80g is used as the initial electrolyte mass m0, the conventional weight loss rate should be calculated as λ = (m0 - m1) / m0 × 100%; these two parameters represent the reduction percentage relative to the initial electrolyte mass and the current electrolyte mass relative to the total battery mass, respectively.
[0212] Example 2: This embodiment uses the same pouch battery structure and EL1 type liquid electrolyte as Embodiment 1, the difference being that the predetermined actual liquid electrolyte mass is 150g. The same detection logic is used for this injection volume, and a thermal correction relationship matching its target specifications is invoked.
[0213] Example 3: This embodiment uses the same pouch battery structure and 80g of actual liquid electrolyte as in Embodiment 1, the difference being that the electrolyte type is EL2. During testing, the melting temperature range and unit enthalpy of fusion corresponding to the EL2 type liquid electrolyte are used, along with the thermal correction relationship matching the corresponding target specifications.
[0214] Example 4: The battery in this embodiment is a square solid-liquid hybrid battery, with an actual liquid electrolyte mass of 80g. During testing, the thermal correction relationship is called or recalibrated according to the dry cell specifications of the square battery, and the melting temperature range and unit melting enthalpy are called according to its electrolyte type.
[0215] Example 5: The battery in this embodiment is a cylindrical solid-liquid hybrid battery, with an actual liquid electrolyte mass of 80g. During testing, the thermal correction relationship is called or recalibrated according to the dry cell specifications of the cylindrical battery, and the melting temperature range and unit melting enthalpy are called according to the electrolyte type.
[0216] Example 6: The battery in this embodiment is a sodium-ion solid-liquid hybrid battery, with an actual liquid electrolyte mass of 80g. During testing, the melting temperature range and unit enthalpy of melting are determined based on the type of electrolyte used in the sodium-ion battery, and the thermal correction relationship is determined based on its dry cell specifications.
[0217] Except for the differences described above, the calibration, calorimetry, thermal correction, and mass conversion processes in Examples 2 to 6 can be performed in accordance with Example 1. The three test results and within-group ranges for each example are listed below. Figure 8 .
[0218] Comparative Example 1: This comparative example uses a destructive disassembly and weighing method on the same battery as in Example 1. The battery was disassembled in a glove box, free electrolyte was washed off each component, and each component was dried before weighing. The difference between the initial total mass of the battery and the total mass of all components after drying was taken as the electrolyte mass. This comparative example is used to compare the impact of disassembly, cleaning, drying, and sample transfer processes on measurement accuracy and repeatability.
[0219] Comparative Example 2: This comparative example uses the same test battery and other processing procedures as Example 1, except that the calibration of the equipment correction parameters shown on P300 is omitted, and the measured heat of the test battery is not processed using the equipment correction parameters. This comparative example is used to examine the impact of the response deviation of the adiabatic accelerated calorimeter and test configuration on the final mass conversion.
[0220] Comparative Example 3: This comparative example uses the same test cell and other processing procedures as Example 1, except that the thermal correction relationship calibration shown on P400 is omitted, and the thermal contribution of the non-liquid electrolyte battery components is not separated using the thermal correction relationship determined by the first and second reference cells. This comparative example is used to examine the impact of unconstrained background thermal contribution on the final mass conversion.
[0221] Figure 8 The results of repeated tests for Examples 1 to 6 and Comparative Examples 1 to 3 are shown. The electrolyte mass measurement errors for Examples 1 to 6 are all within ±0.8%. Figure 8 The listed mass percentage errors are all within ±0.08%; the mass range of electrolytes within each group in each embodiment is less than 0.9g, and the mass percentage range is less than 0.09%.
[0222] The three electrolyte mass measurements for Comparative Example 1 were 74.42 g, 76.17 g, and 72.28 g, with errors relative to the actual mass of 80 g of -6.98%, -4.79%, and -7.72%, respectively. The intra-group mass range was 3.89 g. The results are generally low and exhibit significantly increased dispersion, indicating that electrolyte evaporation, washing and sample transfer losses, and component separation differences during the disassembly process simultaneously introduce systematic bias and operational randomness.
[0223] The three electrolyte mass measurements for Comparative Example 2 were 77.69 g, 77.95 g, and 77.52 g, with errors of -2.89%, -2.56%, and -3.10%, respectively, and an intra-group mass range of 0.43 g. Compared to Example 1, Comparative Example 2, although still using the same melting heat-mass conversion logic, showed a large deviation in the same direction after omitting equipment correction, indicating that the equipment thermal response deviation is transmitted along the path of measured heat, melting heat absorption, and mass conversion.
[0224] The three electrolyte mass measurements for Comparative Example 3 were 78.02 g, 78.22 g, and 78.36 g, with errors of -2.48%, -2.23%, and -2.05%, respectively, and an intra-group mass range of 0.34 g. Compared to Example 1, Comparative Example 3, even after omitting the thermal correction relationship, also exhibited a significant systematic deviation, indicating that equipment response correction alone is insufficient to reliably attribute the heat of the complete battery to the electrolyte under test; it is also necessary to use the thermal correction relationship formed by a reference object with the same dry cell specifications to constrain the thermal contribution of the non-liquid electrolyte battery components. Since the thermal correction relationship can take different forms such as a fixed background, scale, function, or lookup table, this application does not limit the deviation to necessarily being a positive or negative deviation.
[0225] The above results verify the technical effectiveness of this application from the perspectives of the complete detection chain, equipment correction branch, and thermal correction branch, respectively. Examples 2 and 3 further demonstrate that by calling the melting temperature zone and unit melting enthalpy according to the electrolyte type and calling the thermal correction relationship according to the dry cell specification, the same heat-mass conversion logic can be adapted to different injection volumes and electrolyte types; Examples 4 and 5 demonstrate that this logic can be used for different packaging forms; Example 6 demonstrates that this logic can also be used for sodium-ion solid-liquid hybrid batteries.
[0226] Based on the mass of the electrolyte involved in melting, conventional weight loss rates, or electrolyte weight indicators, batteries with different storage times, cycle counts, manufacturing batches, or packaging structures can be compared for life degradation mechanism analysis, packaging structure optimization, electrolyte replenishment strategy formulation, production process monitoring, rapid quality inspection, and failure analysis. When the testing cycle time and equipment configuration meet production requirements, this detection logic can also be deployed in online or near-line quality monitoring systems during manufacturing or maintenance. The above applications pertain to the subsequent use of the test results and do not require corresponding actions to be performed during every quality inspection process.
[0227] The computing device 120 and its processing logic in this embodiment can be implemented through hardware, software, firmware, or a combination of both. Processes for parameter matching, test control, compensated power integration, equipment correction, thermal correction, and mass conversion can be integrated into the controller of the adiabatic accelerated calorimeter 111, or distributed across one or more computing devices communicating with the adiabatic accelerated calorimeter 111. Function names are used to describe the role of the corresponding process and do not require each process to be executed by independent hardware or a separate program module.
[0228] In some embodiments, the computing device 120 may include a processor 121, a memory 122, a communication interface, and a communication bus. The processor 121, memory 122, and communication interface can communicate with each other via the communication bus. The communication interface can be used to exchange control information and test data with the adiabatic accelerated calorimeter 111 and the differential scanning calorimeter 112 used in the calibration stage. The memory 122 can be used to store detection programs, target specifications, melting temperature range, thermal correction relationships, unit enthalpy of fusion, equipment correction parameters, calorimetric test parameters, and test data. The processor 121 can execute the program in the memory 122 to implement the detection method in any of the foregoing embodiments.
[0229] The processor described above may include a central processing unit (CPU), a graphics processing unit (GPU), a network processor, a digital signal processor (DSP), an application-specific integrated circuit (ASIC), a field-programmable gate array (FPGA), a programmable logic device (PLC), a microcontroller, a system-on-a-chip (SoC), or other devices with data processing capabilities, or a combination of the above devices. The memory described above may include random access memory (RAM), read-only memory (ROM), flash memory, a hard disk, an optical disk, a solid-state memory (SSD), a network memory, a cloud storage, or other storage media capable of storing data or programs, or a combination of the above storage media. The various steps executed by the processor may be performed serially, in parallel, interleaved, triggered, periodic, event-driven, or streaming manner as needed for actual deployment; unless expressly defined in the claims, the step numbers listed in the specification and drawings do not limit the actual execution order of the steps.
[0230] In some embodiments, this application may also provide a computer-readable storage medium storing a computer program, program instructions, or executable code; when the computer program, program instructions, or executable code is executed by a processor, the processor controls the adiabatic accelerated calorimeter 111 and performs the compensated power integration, device correction, thermal correction, unit enthalpy of fusion call, and electrolyte mass calculation in any of the foregoing embodiments. The computer-readable storage medium may be a non-transitory computer-readable storage medium and may include a read-only memory, random access memory, flash memory, hard disk, solid-state hard disk, optical disk, magnetic disk, memory card, or network storage space.
[0231] In some embodiments, this application may also provide a computer program product, which includes a computer program or program instructions; when the computer program or program instructions are executed by a processor, they implement the detection method in any of the foregoing embodiments. The computer program product may be provided in the form of a software installation package, a device control program, a firmware upgrade package, or other forms that can be loaded and executed by the computing device 120.
Claims
1. A method for detecting solid-liquid hybrid batteries, characterized in that, For the battery under test under target specifications, the target specifications include at least the dry cell specifications of the battery under test and the electrolyte type of the electrolyte to be tested in the battery under test, and the detection method includes: Based on the melting temperature zone corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric testing on the battery under test, and the compensation power of the battery under test in the melting temperature zone during the calorimetric testing is integrated to determine the measured heat of the battery under test. The measured heat is processed according to the thermal correction relationship corresponding to the dry cell specification to obtain the melting heat absorption of the electrolyte in the battery under test. The thermal correction relationship is determined based on the first calibrated heat of the first reference battery in the melting temperature range, and is used to characterize the heat contribution of the battery components other than the liquid electrolyte in the battery under test in the melting temperature range. The dry cell specification of the first reference battery is the same as that of the dry cell specification of the battery under test and does not contain liquid electrolyte. The mass of the electrolyte that participates in melting in the battery under test is determined based on the ratio of the heat absorbed during melting to the enthalpy of melting per unit corresponding to the electrolyte type.
2. The detection method according to claim 1, characterized in that, The thermal correction relationship is the ratio of the calibrated melting heat absorption to the second calibrated heat, wherein the calibrated melting heat absorption is the difference between the second calibrated heat and the first calibrated heat, the second calibrated heat is the calorimetric test result of the second reference battery in the melting temperature range, the dry cell specifications of the second reference battery are consistent with the dry cell specifications of the battery under test, and the second reference battery contains liquid electrolyte of the same type as the electrolyte under test.
3. The detection method according to claim 2, characterized in that, The thermal correction relationship is predetermined by the following calibration process: Based on the melting temperature range corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric tests on the first reference battery, and the compensation power of the first reference battery in the melting temperature range during the calorimetric test is integrated to determine the first calibrated heat. Based on the melting temperature zone corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric tests on the second reference battery, and the compensation power of the second reference battery in the melting temperature zone during the calorimetric test is integrated to determine the second calibration heat. The thermal correction relationship is determined based on the first calibrated heat and the second calibrated heat.
4. The detection method according to claim 1, characterized in that, The process of processing the measured heat according to the thermal correction relationship corresponding to the dry cell specification includes: The measured heat is processed according to the device correction parameters of the adiabatic accelerated calorimeter to obtain the battery heat absorption of the battery under test. The device correction parameters are determined based on the standard melting heat of the melting enthalpy standard and the third calibration heat of the melting enthalpy standard in the melting temperature range, and are used to characterize the response relationship between the calorimetric test results of the adiabatic accelerated calorimeter and the corresponding actual heat. The heat absorption of the battery is processed according to the thermal correction relationship corresponding to the specifications of the dry cell, and the heat absorption of the electrolyte in the battery under test is obtained.
5. The detection method according to claim 4, characterized in that, The equipment correction parameter is the ratio of the standard molten heat to the third calibrated heat, which is used to multiply the measured heat to obtain the heat absorbed by the battery. The standard molten heat is the product of the known mass of the enthalpy standard and the known unit enthalpy of molten heat. The equipment correction parameter is predetermined by the following calibration process: Based on the melting temperature range corresponding to the electrolyte type, an adiabatic accelerated calorimeter is used to perform calorimetric testing on the melting enthalpy standard, and the compensation power of the melting enthalpy standard in the melting temperature range during the calorimetric testing is integrated to determine the third calibration heat. The equipment correction parameters are determined based on the ratio of the standard melting heat to the third calibrated heat.
6. The detection method according to claim 4, characterized in that, The melting enthalpy standards include non-battery standard material samples with known mass and known unit melting enthalpy, and / or liquid electrolyte samples with known mass and known unit melting enthalpy.
7. The detection method according to claim 1, characterized in that, The calorimetric test is performed in a heating-waiting-search mode. The calorimetric test of the reference battery used to determine the thermal correction relationship and the calorimetric test of the battery under test use the same heating-waiting-search procedure parameters.
8. The detection method according to claim 1, characterized in that, The unit enthalpy of fusion is determined by performing a unit enthalpy test on a liquid electrolyte of the same type as the electrolyte to be tested using a differential scanning calorimeter.
9. The detection method according to claim 8, characterized in that, The unit enthalpy of fusion test includes: A known mass of liquid electrolyte of the same type as the electrolyte to be tested is placed in a sample crucible, and the sample crucible is sealed by cold welding. An empty aluminum crucible of the same mass as the sample crucible is used as a blank reference crucible. The sample crucible and the blank reference crucible are respectively placed in the differential scanning calorimeter. The furnace body of the differential scanning calorimeter is precooled to the starting temperature of the unit enthalpy of fusion test using liquid nitrogen. The differential scanning calorimeter is controlled to heat up at a preset heating rate to obtain the sample heat flow curve corresponding to the sample crucible and the blank baseline corresponding to the blank reference crucible. The blank baseline is subtracted from the sample heat flow curve, and the sample heat flow curve after subtracting the blank baseline is integrated within the melting temperature region to obtain the sample melting heat of the liquid electrolyte. The unit enthalpy of fusion is determined based on the ratio of the heat of fusion of the sample to the known mass of the liquid electrolyte.
10. The detection method according to claim 8, characterized in that, The unit enthalpy of fusion test and the calorimetric test have the same starting temperature, and the temperature range used to integrate the heat flux in the unit enthalpy of fusion test and the temperature range used to integrate the compensation power in the calorimetric test both correspond to the same melting process of the electrolyte under test.
11. The detection method according to claim 1, characterized in that, The melting temperature range is selected as a low-temperature melting temperature range in which the solid electrolyte and electrode materials do not undergo a phase transition that could interfere with the determination of the melting endothermic heat of the electrolyte under test, and in which the electrolyte under test melts within the melting temperature range.
12. The detection method according to claim 11, characterized in that, The melting temperature range is -50°C to -10°C, and the calorimetric test temperature range covers the melting temperature range.
13. The detection method according to claim 1, characterized in that, The detection method further includes: In response to the battery under test being placed on the adiabatic accelerated calorimeter, the target specifications of the battery under test are obtained; The melting temperature range is determined based on the electrolyte type in the target specification, and the thermal correction relationship is determined based on the dry cell specification in the target specification. The calorimetric test parameters are determined based on the melting temperature zone and the adiabatic accelerated calorimeter. These calorimetric test parameters are used to control the adiabatic accelerated calorimeter to perform the calorimetric test on the battery under test.
14. A detection system for a solid-liquid hybrid battery, characterized in that, The detection system includes: The testing equipment includes at least an adiabatic accelerated calorimeter; and A computing device connected to the testing device is used to control the testing device according to any one of claims 1 to 13, and process the test data obtained by the testing device when the battery under test is placed in the adiabatic accelerated calorimeter, so as to determine the mass of the electrolyte under test that participates in melting in the battery under test.