Simulated contamination compositions and their preparation methods; simulation methods for localized abnormal temperature rise at cable terminals.
By constructing a non-uniform contamination layer structure using a specific combination of ash materials and water-soluble salts, the problem of simulating local abnormal temperature rise in porcelain-sheathed cable terminals was solved, achieving a stable and effective temperature rise effect, which is suitable for cable terminal cleaning process verification.
Patent Information
- Application Number
- CN202610958101.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies are unable to stably and effectively simulate the localized abnormal temperature rise phenomenon caused by dirt accumulation in porcelain-sheathed cable terminals. Traditional dirt-retaining formulations perform poorly in simulating abnormal temperature rises and are difficult to reproduce the actual situation.
A non-uniform fouling layer structure is formed by using a specific combination of ash materials, water-soluble salts, and dispersion media. Abnormal temperature rise is induced by voltage application. Kaolin or diatomaceous earth is used as a solid framework, and water-soluble salts provide ionic conductivity and hygroscopicity, forming conductive channels with concentrated local current density.
It successfully reproduces the abnormal temperature rise phenomenon of porcelain-insulated cable terminals, making it suitable for verifying cable terminal cleaning processes and ensuring the stability and effectiveness of the simulation results.
Smart Images

Figure CN123066518A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of power equipment technology, and in particular to a method for simulating pollution compositions and their preparation methods, and a method for simulating local abnormal temperature rise at cable terminals. Background Technology
[0002] Porcelain-sheathed outdoor cable terminals need to operate in natural environments for extended periods. Due to the deposition of dust, industrial particles, salt, and other pollutants, a natural dust layer gradually forms on their surface. The presence of this natural dust layer can cause problems such as increased leakage current, localized corona discharge, surface discharge, and abnormal temperature rise, which are detrimental to the long-term stable operation of the cable. Therefore, how to efficiently clean the surface of cable terminals has become one of the key research focuses in this field.
[0003] Before conducting research on cleaning cable terminal surfaces, it is usually necessary to artificially construct simulated contamination layers to carry out experiments and tests under relatively controlled conditions. Currently, traditional artificial contamination formulations are mostly aimed at reproducing the impact of dirt on cable insulation performance, and they perform poorly in simulating abnormal temperature rises, only occasionally showing weak and scattered temperature rise points, making it difficult to stably and effectively simulate the local abnormal temperature rise phenomenon caused by dirt accumulation on the porcelain bushing surface. Summary of the Invention
[0004] To address the aforementioned issues, this application provides a simulated contamination composition that can stably and effectively induce abnormal temperature rise on the surface of cable terminals, a method for preparing the same, and a method for simulating localized abnormal temperature rise in cable terminals.
[0005] In a first aspect, this application provides a composition for simulating filth.
[0006] A simulated filth composition comprising ash material, water-soluble salt, and dispersion medium; wherein the ash material comprises one or more of kaolin and diatomaceous earth; wherein the water-soluble salt comprises one or more of sodium salt, potassium salt, and calcium salt; wherein the dispersion medium comprises water; and wherein the mass ratio of the water-soluble salt to the ash material is 1:(3~10).
[0007] In some embodiments, the mass ratio of the ash material to the dispersion medium is 1:(0.8~1.2).
[0008] In some embodiments, the ash material comprises kaolin and diatomaceous earth, and the mass ratio of the kaolin to the diatomaceous earth is 1:(0.5~2).
[0009] In some embodiments, the water-soluble salt includes one or more of sodium chloride, sodium sulfate, potassium chloride, potassium sulfate, calcium chloride, and calcium sulfate.
[0010] In some embodiments, the water-soluble substances include sodium chloride, sodium sulfate, and calcium chloride.
[0011] In some embodiments, the water-soluble salt comprises, by weight, 10 to 20 parts sodium chloride, 5 to 15 parts sodium sulfate, and 2 to 10 parts calcium chloride.
[0012] A second aspect of this application provides a method for preparing a simulated filth composition.
[0013] A method for preparing the above-mentioned simulated sewage composition includes the following steps:
[0014] A dispersion is prepared by mixing a water-soluble salt with a dispersion medium.
[0015] The ash material and the dispersion are mixed to prepare the simulated filth composition.
[0016] In a third aspect, this application provides a method for simulating localized abnormal temperature rise in cable terminals.
[0017] A method for simulating local abnormal temperature rise in cable terminals involves forming a contamination layer using the simulated contamination composition described above or the simulated contamination composition prepared by the above preparation method, and generating an abnormal temperature rise by applying a preset voltage to the contamination layer.
[0018] In some implementations, the following steps are included:
[0019] The simulated contamination composition was coated onto the porcelain sheath surface of the cable terminal, and after drying, an adhesion amount of 2 mg / cm² per unit area was obtained. 2 ~50mg / cm 2 A dry layer of contaminants;
[0020] A preset voltage is applied to the cable terminal, causing an abnormal temperature rise through the dry contamination layer.
[0021] In some implementations, the following steps are included:
[0022] The simulated contamination composition was coated onto the porcelain sheath surface of the cable terminal and dried to obtain an adhesion amount of 2 mg / cm² per unit area. 2 ~50mg / cm 2 A dry layer of contaminants;
[0023] The dry dirt layer is sprayed to prepare a wet dirt layer;
[0024] A preset voltage is applied to the cable terminal, causing an abnormal temperature rise through the wet contamination layer.
[0025] The simulated contamination composition provided in this application, through the combination of specific ash materials, water-soluble salts, and dispersion media, can effectively control the particle packing morphology and conductivity of the contamination layer, thereby forming non-uniform local conductive channels under an applied electric field and stably reproducing the abnormal temperature rise phenomenon of porcelain-sheathed cable terminals. Specifically, kaolin or diatomaceous earth in the ash materials acts as a solid framework, constructing a porous, rough structure with good water retention on the porcelain sheath surface, which helps to facilitate the local aggregation of ions. The water-soluble salt provides ionic conductivity and a certain degree of hygroscopic capacity, dissolving and releasing freely moving ions when damp, thus forming a non-uniform conductivity distribution within the contamination layer. This results in conductive channels with concentrated local current density when voltage is applied, triggering the abnormal temperature rise phenomenon. Through the synergistic effect of the above components, this simulated contamination composition can stably induce abnormal temperature rise on the surface of the cable terminal, facilitating subsequent process verification. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0027] Figure 1 This is an infrared temperature rise diagram of the simulated soiled composition in Example 1 of this application under a wet state. Detailed Implementation
[0028] To make the above-mentioned objectives, features, and advantages of this application more readily understood, a detailed description of specific embodiments of this application is provided below. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.
[0029] In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified. In this application, "at least one" means one or more, such as one, two, or more than two. "Multiple" or "several" means at least two, such as two, three, etc.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0031] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0032] Unless otherwise specified, all steps in this application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0033] In this application, "above" or "below" includes the number itself. For example, "below 1" includes 1.
[0034] Unless otherwise specified, the temperature parameters in this application are permitted to be either constant-temperature treatment or variations within a certain temperature range. It should be understood that the constant-temperature treatment allows temperature fluctuations within the precision range of the instrument control, such as ±5℃, ±4℃, ±3℃, ±2℃, or ±1℃.
[0035] The first aspect of this application provides a simulated contamination composition that can stably induce abnormal temperature rise on the surface of a cable terminal.
[0036] For example, the simulated filth composition comprises ash material, water-soluble salt, and dispersion medium. The ash material includes one or more of kaolin and diatomaceous earth; the water-soluble salt includes one or more of sodium, potassium, and calcium salts; the dispersion medium includes water; and the mass ratio of water-soluble salt to ash material is 1:(3~10).
[0037] The simulated contamination composition provided in this application, through the combination of specific ash materials, water-soluble salts, and dispersion media, can effectively control the particle packing morphology and conductivity of the contamination layer, thereby forming non-uniform local conductive channels under an applied electric field and stably reproducing the abnormal temperature rise phenomenon of porcelain-sheathed cable terminals. Specifically, kaolin or diatomaceous earth in the ash materials serve as a solid framework, constructing a porous, rough structure with good water retention on the porcelain sheath surface, which facilitates the formation of local ion aggregation. The water-soluble salt provides ionic conductivity and a certain degree of hygroscopic capacity, dissolving and releasing freely moving ions when damp, thus forming a non-uniform conductivity distribution within the contamination layer. This generates conductive channels with concentrated local current density when voltage is applied, triggering the abnormal temperature rise phenomenon. Through the synergistic effect of the above components, this simulated contamination composition can stably induce abnormal temperature rise on the surface of the cable terminal, making it suitable for cleaning process verification.
[0038] In this embodiment, the mass ratio of water-soluble salt to ash material is 1:(3~10). Optionally, the mass ratio of water-soluble salt to ash material can be, but is not limited to, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or other values within the range of 1:(3~10). Studies have shown that maintaining the mass ratio of water-soluble salt to ash material within the above-mentioned range helps to form a contamination layer structure on the ceramic sleeve surface, with ash material as a continuous framework and water-soluble salt in a discrete distribution. This structure not only ensures good adhesion of the contamination layer through a high proportion of ash material, providing a framework for ion migration in a humid environment, but also avoids the tendency for the overall conductivity of the contamination layer to be too high and the local current channel characteristics to be annihilated due to excessive water-soluble salt, thereby facilitating the stable triggering of local abnormal temperature rise caused by non-uniform conductivity distribution under an applied electric field.
[0039] In some embodiments, the mass ratio of ash material to dispersion medium is 1:(0.8~1.2). Optionally, the mass ratio of ash material to dispersion medium can be, but is not limited to, other values within the range of 1:0.8, 1:0.9, 1:1.1, 1:1.2, or 1:(0.8~1.2). Studies have shown that maintaining the mass ratio of ash material to dispersion medium within the above-mentioned range helps the simulated dirt composition obtain suitable rheological properties during the coating stage, forming a simulated dirt layer of moderate thickness, dense structure, and strong adhesion to the substrate after drying. This avoids problems such as poor slurry flowability and difficulty in forming uniform coverage due to insufficient dispersion medium, or insufficient layer thickness and loose structure after drying due to excessive dispersion medium.
[0040] In some embodiments, the ash material comprises kaolin and diatomaceous earth, with a mass ratio of kaolin to diatomaceous earth of 1:(0.5~2). Optionally, the mass ratio of kaolin to diatomaceous earth can be, but is not limited to, 1:0.5, 1:0.7, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, or other values within the range of 1:(0.5~2). By compounding kaolin and diatomaceous earth in this proportion, it helps to synergistically leverage the excellent adhesion and water retention properties of kaolin and the porous framework structure and adsorption capacity of diatomaceous earth. Maintaining the above-mentioned mass ratio range helps to construct a robust dirt layer framework with excellent internal conductive channels. This not only promotes the retention and capillary aggregation of water-soluble salt solutions within the pores, forming micro-regions of localized ion enrichment, but also, when voltage is applied, utilizes the pore structure to induce a non-uniform distribution of the electric field, thereby effectively triggering an abnormal temperature rise.
[0041] In some embodiments, the water-soluble salt includes one or more of sodium chloride, sodium sulfate, potassium chloride, potassium sulfate, calcium chloride, and calcium sulfate.
[0042] In some embodiments, the water-soluble salts include sodium chloride, sodium sulfate, and calcium chloride.
[0043] In some embodiments, the water-soluble salt comprises, by mass parts, 10 to 20 parts sodium chloride, 5 to 15 parts sodium sulfate, and 2 to 10 parts calcium chloride. Sodium chloride provides basic ionic conductivity and a certain degree of hygroscopicity; the solubility and hygroscopic point of sodium sulfate vary significantly with temperature, which helps to regulate conductivity behavior under different humidity levels; calcium chloride is highly hygroscopic, thus preferentially absorbing moisture and slowly dissolving at lower relative humidity levels, forming initial localized high-conductivity liquid bridges. Using a compound system and maintaining the above-mentioned content relationships among the components helps to construct a simulated fouling layer that can effectively respond and stably induce abnormal temperature rises under both dry and wet environments.
[0044] A second aspect of this application provides a method for preparing a simulated filth composition.
[0045] An exemplary method for preparing a simulated soil composition includes the following steps:
[0046] A dispersion is prepared by mixing a water-soluble salt with a dispersion medium.
[0047] Ash materials and dispersions are mixed to prepare a simulated filth composition.
[0048] In a third aspect, this application provides a method for simulating localized abnormal temperature rise in cable terminals.
[0049] For example, the method for simulating local abnormal temperature rise at cable terminals uses the simulated contamination composition described above or the simulated contamination composition prepared by the above preparation method to form a contamination layer, and applies a preset voltage to the contamination layer to generate an abnormal temperature rise.
[0050] In some implementations, the method for simulating localized abnormal temperature rise at cable terminals includes the following steps:
[0051] The simulated contamination composition was coated onto the porcelain sheath surface of the cable terminal, and after drying, an adhesion amount of 2 mg / cm² per unit area was obtained. 2 ~50mg / cm 2 A dry layer of contaminants;
[0052] A preset voltage is applied to the cable terminal, causing an abnormal temperature rise through the dry contamination layer.
[0053] In some implementations, the method for simulating localized abnormal temperature rise at cable terminals includes the following steps:
[0054] The simulated contamination composition was coated onto the porcelain sheath surface of the cable terminal, and after drying, an adhesion amount of 2 mg / cm² per unit area was obtained. 2 ~50mg / cm 2 A dry layer of contaminants;
[0055] A wet dirt layer is prepared by spraying the dry dirt layer.
[0056] A preset voltage is applied to the cable terminal, causing an abnormal temperature rise through the wet contamination layer.
[0057] In some embodiments, the moisture content of the wet sludge layer is 10% to 40%. Optionally, the moisture content of the wet sludge layer can be, but is not limited to, 10%, 15%, 20%, 25%, 30%, 35%, 40%, or other values within the range of 10% to 40%.
[0058] In some embodiments, the spray liquid used in the spray treatment includes water.
[0059] In some implementations, the process of applying a preset voltage to the cable terminal includes:
[0060] Within the range of 0kV to 60kV, the voltage is gradually increased in increments of 10kV to 20kV and maintained for 5 to 10 minutes.
[0061] The present application will be further described in detail below with reference to specific embodiments.
[0062] Unless otherwise specified, the raw materials used in the following specific embodiments and comparative examples are all commercially available products; the instruments used are all commercially available products; and the processes used are all conventionally selected by those skilled in the art unless otherwise specified.
[0063] Example 1
[0064] This embodiment provides a simulated filth composition.
[0065] The composition of the simulated soil composition, by parts by weight, is as follows:
[0066] 50 parts kaolin, 50 parts diatomaceous earth, 12 parts sodium chloride, 6 parts sodium sulfate, 2 parts calcium chloride, and 100 parts deionized water.
[0067] The method for preparing the simulated filth composition is as follows: Sodium sulfate, sodium chloride, and calcium chloride are added to deionized water and stirred until completely dissolved to obtain a dispersion;
[0068] Kaolin and diatomaceous earth were mixed and divided into two equal parts. The mixture was added to the dispersion in two separate batches and stirred for 20 minutes to obtain a simulated filth composition.
[0069] Example 2
[0070] This embodiment provides a simulated filth composition.
[0071] The composition of the simulated soil composition, by parts by weight, is as follows:
[0072] 50 parts kaolin, 50 parts diatomaceous earth, 20 parts sodium chloride, and 100 parts deionized water.
[0073] The method for preparing the simulated filth composition is as follows: Sodium chloride is added to deionized water and stirred until completely dissolved to obtain a dispersion;
[0074] Kaolin and diatomaceous earth were mixed and divided into two equal parts. The mixture was added to the dispersion in two separate batches and stirred for 20 minutes to obtain a simulated filth composition.
[0075] Example 3
[0076] This embodiment provides a simulated filth composition.
[0077] The composition of the simulated soil composition, by parts by weight, is as follows:
[0078] 100 parts kaolin, 12 parts sodium chloride, 6 parts sodium sulfate, 2 parts calcium chloride, and 100 parts deionized water.
[0079] The method for preparing the simulated filth composition is as follows: Sodium sulfate, sodium chloride, and calcium chloride are added to deionized water and stirred until completely dissolved to obtain a dispersion;
[0080] Kaolin was divided into two equal parts and added to the dispersion in two batches, and the mixture was stirred for 20 minutes to obtain a simulated filth composition.
[0081] Example 4
[0082] This embodiment provides a simulated filth composition.
[0083] The composition of the simulated soil composition, by parts by weight, is as follows:
[0084] 100 parts diatomaceous earth, 12 parts sodium chloride, 6 parts sodium sulfate, 2 parts calcium chloride, and 100 parts deionized water.
[0085] The method for preparing the simulated filth composition is as follows: Sodium sulfate, sodium chloride, and calcium chloride are added to deionized water and stirred until completely dissolved to obtain a dispersion;
[0086] Kaolin was divided into two equal parts and added to the dispersion in two batches, and stirred for 20 minutes to obtain a simulated filth composition.
[0087] Comparative Example 1
[0088] The composition of the simulated soil composition, by parts by weight, is as follows:
[0089] 150 parts kaolin, 10 parts sodium chloride, and 150 parts deionized water.
[0090] The method for preparing the simulated filth composition is as follows: Sodium chloride is added to deionized water and stirred until completely dissolved to obtain a dispersion;
[0091] Kaolin was divided into two equal parts and added to the dispersion in two batches, and stirred for 20 minutes to obtain a simulated filth composition.
[0092] Test case
[0093] (1) Dry state test: The uniformly mixed simulated contaminant composition was brushed onto the lower middle skirt, adjacent small skirt area, and outer surface area corresponding to the internal stress cone of the ceramic bushing of the cable terminal. It was then allowed to dry naturally at room temperature, resulting in an average dry state adhesion amount of 20 mg / cm². 2 A dry, foul-smelling layer.
[0094] Voltage was applied to the cable terminal in stages, and the temperature distribution on the porcelain bushing surface was recorded using an infrared thermal imager. The voltage was increased stepwise from 0 kV, 15 kV, 30 kV, 45 kV, to 60 kV, and each voltage level was held for 5 minutes. Infrared images were recorded after each voltage stage was held for 5 minutes. The test environment was 25°C room temperature and 65% relative humidity. The test results are shown in Table 1.
[0095] (2) Wet test: The uniformly mixed simulated contaminant composition was brushed onto the lower middle skirt, adjacent small skirt area, and outer surface area corresponding to the internal stress cone of the ceramic bushing of the cable terminal. It was then allowed to dry naturally at room temperature, resulting in an average dry adhesion amount of 20 mg / cm². 2 A dry, foul-smelling layer.
[0096] Spray water mist onto the dry dirt layer, allowing it to gradually absorb moisture and clean the surface until no water droplets remain, resulting in a wet dirt layer. The moisture content of the wet dirt layer is controlled at 25%, calculated as follows:
[0097] Moisture content = (Wet fouling layer mass - Dry fouling layer mass) / Dry fouling layer mass × 100%
[0098] Voltage was applied to the cable terminals in stages, and the temperature distribution on the porcelain bushing surface was recorded using an infrared thermal imager. The voltage was increased progressively at 0 kV, 15 kV, 30 kV, 45 kV, and 60 kV, with each voltage level held for 5 minutes. Infrared images were recorded after each voltage stage was held for 5 minutes. The test environment was 25°C room temperature and 65% relative humidity. The test results are shown in Table 1. Additionally, for wet contamination layers, the infrared temperature rise test should be completed within 40 minutes after spray treatment to ensure the contamination layer remains in a stable wet state. Please refer to [link to relevant documentation]. Figure 1 , Figure 1 This is an infrared temperature rise diagram of the simulated dirt composition in Example 1 of this application under a wet state, wherein the black box area is the area coated with a wet dirt layer.
[0099] Table 1 Performance Comparison of Examples
[0100]
[0101] As shown in Table 1, compared to Comparative Example 1, Examples 1-4 can stably induce a large-scale abnormal temperature rise on the surface of the cable terminal under stepped voltage, making them suitable for cleaning process verification. Specifically, Example 1, by compounding kaolin and diatomaceous earth in a certain proportion, allows the contaminant layer to possess both the good adhesion and water retention properties of kaolin and the porous framework structure and adsorption capacity of diatomaceous earth. Based on this, by selecting specific water-soluble salt components, sodium chloride provides basic ionic conductivity and hygroscopicity, and calcium chloride and sodium sulfate adjust the hygroscopic capacity, ultimately resulting in a significant temperature rise. Example 2, using only single-component sodium chloride, shows a significantly lower temperature rise effect in the wet state compared to Example 1. Examples 3 and 4, using only single-component ash materials, cannot form an effective conductive path compared to Example 1, resulting in varying degrees of decreased temperature rise.
[0102] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0103] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this invention patent should be determined by the appended claims, and the specification can be used to interpret the content of the claims.
Claims
1. A composition simulating filth, characterized in that, It comprises ash material, water-soluble salt, and dispersion medium; the ash material includes one or more of kaolin and diatomaceous earth; the water-soluble salt includes one or more of sodium salt, potassium salt, and calcium salt; the dispersion medium includes water; the mass ratio of the water-soluble salt to the ash material is 1:(3~10).
2. The simulated filth composition according to claim 1, characterized in that, The mass ratio of the ash material to the dispersion medium is 1:(0.8~1.2).
3. The simulated filth composition according to any one of claims 1 to 2, characterized in that, The ash material comprises kaolin and diatomaceous earth, and the mass ratio of kaolin to diatomaceous earth is 1:(0.5~2).
4. The simulated filth composition according to any one of claims 1 to 2, characterized in that, The water-soluble salts include one or more of sodium chloride, sodium sulfate, potassium chloride, potassium sulfate, calcium chloride, and calcium sulfate.
5. The simulated filth composition according to claim 4, characterized in that, The water-soluble substances include sodium chloride, sodium sulfate, and calcium chloride.
6. The simulated filth composition according to claim 5, characterized in that, The water-soluble salt comprises, by mass, 10 to 20 parts sodium chloride, 5 to 15 parts sodium sulfate, and 2 to 10 parts calcium chloride.
7. A method for preparing the simulated filth composition according to any one of claims 1 to 6, characterized in that, Includes the following steps: A dispersion is prepared by mixing a water-soluble salt with a dispersion medium. The ash material and the dispersion are mixed to prepare the simulated filth composition.
8. A method for simulating localized abnormal temperature rise in cable terminals, characterized in that, A soiled layer is formed by using the simulated soiled composition according to any one of claims 1 to 6 or the preparation method according to claim 7, and an abnormal temperature rise is generated by applying a preset voltage to the soiled layer.
9. The method for simulating local abnormal temperature rise in cable terminals according to claim 8, characterized in that, Includes the following steps: The simulated contamination composition was coated onto the porcelain sheath surface of the cable terminal and dried to obtain an adhesion amount of 2 mg / cm² per unit area. 2 ~50mg / cm 2 A dry layer of contaminants; A preset voltage is applied to the cable terminal, causing an abnormal temperature rise through the dry contamination layer.
10. The method for simulating local abnormal temperature rise in cable terminals according to claim 8, characterized in that, Includes the following steps: The simulated contamination composition was coated onto the porcelain sheath surface of the cable terminal and dried to obtain an adhesion amount of 2 mg / cm² per unit area. 2 ~50mg / cm 2 A dry layer of contaminants; The dry dirt layer is sprayed to prepare a wet dirt layer; A preset voltage is applied to the cable terminal, causing an abnormal temperature rise through the wet contamination layer.