A design method and application of porous concrete mix proportion based on two-dimensional morphological characteristics of recycled coarse aggregate.

By quantifying the two-dimensional morphological characteristics of recycled coarse aggregate and its water absorption behavior during the mixing process, a closed-loop design process of morphological correction, water absorption compensation, and volume balance is constructed. This solves the problems of particle shape differences and water absorption mismatch in the mix design of recycled coarse aggregate concrete, and realizes efficient and stable mix design of concrete.

CN123072579APending Publication Date: 2026-11-10CHINA THREE GORGES CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611189173.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies fail to effectively consider the two-dimensional morphological characteristics of recycled coarse aggregate concrete mix design, resulting in water absorption mismatch, workability fluctuations, uneven slurry coating, and unstable skeleton stacking structure during the mixing process. It is difficult to achieve synergistic optimization of porosity and strength, and the design process relies on experience-based adjustments, which is time-consuming, labor-intensive, and unstable.

Method used

By employing systematic steps such as target porosity constraints, quantification of two-dimensional morphological parameters of recycled coarse aggregates, construction of morphological correction coefficients, compensation for water absorption in the initial mixing stage, and solution of volume balance, a mix design method for porous concrete with recycled coarse aggregates suitable for permeable concrete and vegetation concrete is formed. The method quantifies and compensates for the influence of aggregate particle shape differences and establishes a closed-loop design process.

Benefits of technology

It achieves accurate description of aggregate particle shape differences and stable compensation of water volume during mixing under the constraint of target porosity, improves the design pertinence and batch stability of concrete, reduces trial mixing iterations, and enhances engineering applicability and strength consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of ecological hydraulic engineering materials technology, specifically to a design method and application of porous concrete mix proportions based on the two-dimensional morphological characteristics of coarse aggregates using recycled coarse aggregates. The design method includes the following steps: determining the target porosity and target performance of the concrete; collecting the two-dimensional morphological parameters of the recycled coarse aggregates and the reference aggregates; dividing the two-dimensional morphological parameters of the recycled coarse aggregates by the two-dimensional morphological parameters of the reference aggregates to obtain normalized dimensionless two-dimensional morphological parameters; and constructing a morphological correction coefficient α based on the normalized dimensionless two-dimensional morphological parameters. m ; Use morphological correction factor α m Calculate the amount of coarse aggregate correction and the total water correction. This invention proposes for the first time a porous concrete mix design method based on the morphological characteristics of recycled coarse aggregate, transforming the influence of aggregate particle shape differences on skeleton packing and paste requirements into a calculable correction mechanism, thereby improving the design's relevance and repeatability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ecological hydraulic materials technology, specifically to a design method and application of porous concrete mix proportions made from recycled coarse aggregate based on the two-dimensional morphological characteristics of coarse aggregate. Background Technology

[0002] Permeable concrete is mainly used for road paving, achieving rapid drainage and alleviating urban flooding through its interconnected porous structure. Vegetated concrete is often used for slope protection; its internal porous structure is designed to accommodate soil and plant roots, achieving soil stabilization, slope protection, and ecological restoration. Currently, when designing mix proportions for both permeable and vegetated concrete, the target porosity is often used as the core control indicator, combined with empirical or volumetric methods to determine parameters such as coarse aggregate dosage, paste dosage, and water-cement ratio.

[0003] Patent application CN112094082A discloses a method for preparing permeable concrete based on the paste-aggregate ratio and cementitious materials. The paste-aggregate ratio is determined based on the proportions of cementitious slurry and coarse aggregate in the permeable concrete, the amount of cementitious materials used in the permeable concrete is determined, the water consumption is calculated, and finally, the mix proportion is determined. Patent application CN112115409A discloses a mix proportion design method for high-strength, high-permeability concrete based on aggregate characteristics, including the following steps: setting the target strength grade of the permeable concrete; setting the target permeability coefficient of the permeable concrete; determining the amount of aggregate per unit volume and calculating the compact packing porosity of the aggregate; calculating the strength of the cementitious slurry based on the relationship between the target strength of the permeable concrete and the strength of the cementitious slurry; determining the amount of cementitious slurry per unit volume in the permeable concrete; and obtaining the concrete mix proportion based on the amount of aggregate per unit volume, the amount of slurry, and the composition of the cementitious slurry.

[0004] When using recycled coarse aggregate, engineering practices typically improve workability by pre-wetting treatment or by increasing the amount of additional water based on the water absorption rate. However, due to the irregular particle shape, more pronounced needle-like and flaky characteristics, rough surface, and rapid water absorption in the initial mixing stage of recycled coarse aggregate, existing technologies still have significant drawbacks: Firstly, the basis for additional water absorption compensation during the mixing stage does not match the mixing process. Existing technologies often use a 24-hour water absorption rate or a fixed time (such as 30 hours). The method of determining the amount of water to add based on the water absorption rate (min) is insufficient to reflect the rapid water absorption behavior in the early stage of mixing, which can easily lead to insufficient effective mixing water or excessive water addition during the mixing process, resulting in problems such as workability fluctuations, uneven slurry coating, or local pore blockage. Secondly, the quantitative difference in the two-dimensional morphology of recycled coarse aggregates is not incorporated into the mix proportion calculation chain. Existing designs lack measurable and calculable input parameters for key morphological characteristics of aggregates, such as sphericity, angularity, surface texture, degree of needle-like and flaky features, and contour complexity. They are often replaced by empirical coefficients or simple needle-like and flaky content indicators, which are difficult to accurately describe the impact of morphology on skeleton packing density, skeleton void structure, and slurry requirements. Thirdly, the skeleton-slurry-effective water matching under the design porosity constraint lacks synergistic optimization for the characteristics of recycled aggregates. Given a design porosity, if the changes in packing structure caused by particle shape and the effective water loss due to water absorption in the initial mixing stage are not considered, contradictions can easily arise, such as "meeting the design porosity but having low strength and large dispersion" or "sacrificing interconnected pore structure to pursue strength." Fourth, the mix proportion relies on trial mixing experience and lacks repeatability. Due to the superposition of uncertainties in water absorption and particle shape, multiple rounds of trial mixing are often required in engineering to repeatedly adjust the water and paste dosages to meet the porosity and strength / permeability requirements. This is time-consuming, labor-intensive, and results in poor batch stability, which is not conducive to large-scale promotion and application. Therefore, it is urgent to develop a concrete mix design method that can compensate for additional water absorption during the mixing stage, quantify the differences in the morphology of recycled coarse aggregates, and can be promoted and applied on a large scale. Summary of the Invention

[0005] To address the aforementioned deficiencies or improvement needs of existing technologies, this invention establishes a systematic approach for designing mix proportions of porous concrete using recycled coarse aggregates, applicable to permeable concrete and vegetation concrete. This approach involves target porosity constraints, quantification of two-dimensional morphological parameters of recycled coarse aggregates (AIMS), construction of morphological correction coefficients, compensation for water absorption during initial mixing, volume balance calculation, and verification iterations.

[0006] To achieve the above objectives, the specific technical solution is as follows: In a first aspect, the present invention provides a method for designing the mix proportion of porous concrete using recycled coarse aggregate, comprising the following steps: Step 1: Determine the target porosity and target performance of the recycled coarse aggregate porous concrete; collect the two-dimensional morphological parameters of the recycled coarse aggregate and the reference aggregate, divide the two-dimensional morphological parameters of the recycled coarse aggregate by the two-dimensional morphological parameters of the reference aggregate respectively, and calculate the normalized dimensionless two-dimensional morphological parameters, which include sphericity Sp, edge angle An, texture value Te, fractal dimension D, sheet parameter FR and needle parameter ER; Furthermore, the reference aggregate is selected from natural coarse aggregate, engineering qualified recycled coarse aggregate, or aggregates that have been verified in a historical database to meet the target porosity and target performance requirements.

[0007] Furthermore, the two-dimensional morphological parameters of the reference aggregate are the average or median values ​​obtained with the recycled coarse aggregate under the same particle size range, the same image acquisition conditions, and the same statistical methods, and are used as normalized reference values ​​within the mix design system.

[0008] Furthermore, the target performance includes, but is not limited to, one or more of the following: mixture encapsulation state, slurry flow or pore blockage, molding stability, 28-day compressive strength, compressive strength dispersion, permeability coefficient, interconnected porosity, suitable pore structure for vegetation, and durability indicators; the target performance is determined according to the application scenario of the porous concrete. When the porous concrete is used for permeable concrete, the target performance includes one or more of the following: compressive strength, permeability coefficient, interconnected porosity, mixture encapsulation state, and molding stability; when the porous concrete is used for vegetation concrete, the target performance includes one or more of the following: compressive strength, suitable porosity or pore size range for vegetation, interconnected porosity, degree of slurry pore blockage, mixture encapsulation state, strength dispersion, and durability indicators.

[0009] Furthermore, the reference aggregate can be natural coarse aggregate that has stable performance in engineering, meets the specifications, and has been used in the mix design of conventional porous concrete. Alternatively, qualified recycled coarse aggregate that has been screened and washed and has a relatively stable morphology can be selected. The two-dimensional morphological parameters of the reference aggregate serve to provide a relative benchmark for the normalization of the two-dimensional morphological parameters of the recycled coarse aggregate, so that the sphericity, edge angle, texture value, fractal dimension, and needle-like parameters of recycled coarse aggregate from different batches or sources can be converted into dimensionless input parameters.

[0010] Step 2: Based on the two-dimensional morphological parameters collected in Step 1, construct the morphological correction coefficient α. m And calibrate it; Furthermore, α m The basic construction formula is: α m =1+γ1[β1(An-1)-β2(Sp-1)] In the formula, γ1 is the scaling factor, and β1 and β2 are the weighting factors; Furthermore, α m The enhanced construct is: α m =1+γ2[β3An-β4Te+β5D+β6FR+β7ER-β8Sp] In the formula, γ2 is the scaling factor, and β3, β4, β5, β6, β7, and β8 are weighting factors; Furthermore, the α calculated by the basic construction formula and the enhanced component formula m The value is limited to the range of 0.85 to 1.25. When the calculated value is less than 0.85, α is taken as... m =0.85, when the calculated value is greater than 1.25, take α. m =1.25, or the weighting coefficient can be readjusted based on the engineering trial mix results to avoid excessive correction of coarse aggregate dosage and compensation water due to morphological factors.

[0011] Furthermore, the basic construct is suitable for scenarios where morphological parameters are limited or where rapid engineering design is required. It uses angularity and sphericity as the main control indicators to characterize the impact of enhanced particle angularity and reduced overall roundness on skeleton stacking and slurry requirements. The enhanced construct is suitable for scenarios where complete two-dimensional morphological parameters have been obtained. Based on the basic construct, it further considers the impact of texture value, fractal dimension, sheet parameters, and needle parameters on slurry encapsulation, skeleton voids, and mixing water absorption compensation.

[0012] Furthermore, α m Basic construction and α m The calibration method for enhanced constructs involves determining the performance target of the porous concrete to be prepared, using it as the calibration target, and determining α through regression analysis of historical databases. m Scaling and weighting factors in basic constructs; Furthermore, when using the basic construct, a small-sample calibration experiment can be used to verify the scaling and weighting coefficients in the basic construct; when using the enhanced construct, the small-sample calibration experiment is used to verify α. m The scaling factor γ is selected or modified to enhance the multiple weight coefficients in the construct, which are preferably determined by regression of historical databases or by preset weighting.

[0013] Furthermore, in the small-sample calibration test, more than two groups of recycled coarse aggregates with different two-dimensional morphological characteristics were selected, and specimens were prepared under the same target porosity, water-cement ratio, and mixing process. The target porosity and target performance were used as evaluation indicators to determine or verify the corresponding α. m Values; Furthermore, the morphological correction factor α was confirmed. m After obtaining the value, α can be verified through a single trial mixing.m The value is corrected; Furthermore, the historical database regression, when multiple batches of historical data are available, uses the normalized dimensionless two-dimensional morphological parameters as independent variables, and assigns the α value corresponding to meeting the target porosity and performance requirements. m The γ and β parameters were obtained by fitting the data as dependent variables.

[0014] Step 3: Coarse aggregate correction amount (m) g The calculation formula is as follows:

[0015] Where ρ s To determine the close packing density of the recycled coarse aggregate, α m Morphological correction factor, α0 is the baseline factor, and α0 takes a value of 0.95 to 1.00; Step 4: Establish the volume balance equation for concrete per unit volume under the constraint of the target design porosity P, as shown in the following equation:

[0016] In the formula, m g ρ is the amount of coarse aggregate per unit volume of concrete. g The apparent density of coarse aggregate is m. b ρ is the total amount of cementitious materials used per unit volume of concrete. b The apparent density of the cementitious material is given by m. When the cementitious material is multi-component, a weighted density method can be used. w0 ρ is the target effective water consumption per unit volume of concrete. w Let m be the density of water. ad ρ is the amount of admixture per unit volume of concrete. ad Density of the admixture; Combining the target effective water-cement ratio λ with the admixture mass fraction k and the total amount of cementitious material m b Target effective water consumption (m) w0 Admixture dosage per unit volume of concrete (m³) ad The relationship is shown in the following formula:

[0017] In the formula, The target effective water-cement ratio; This refers to the mass fraction of the admixture. By solving the simultaneous equations, the total amount of cementitious material, m, can be calculated. b With the target effective water consumption m w0 :

[0018] Step 5: Total water usage correction (m)w Calculation: The recycled coarse aggregate was dried to constant weight to obtain a dry mass m0. After soaking in water, a sample was taken at time t, and after surface drying treatment, the mass was obtained as m(t). The water absorption rate was calculated.

[0019] The actual time from the addition of water to the recycled coarse aggregate to the end of mixing is t. mix When t=t mix At that time, the water absorption rate ω a (t mix This is used to indicate the additional water absorption of recycled coarse aggregate during the mixing stage; The moisture content ω of the aggregate before mixing was determined by the drying-to-constant-weight method. c ; Total water usage correction (m) w The calculation formula is as follows:

[0020]

[0021] In the formula, ω c ω represents the moisture content of the recycled coarse aggregate before mixing. a (t mix () represents the water absorption rate of the aggregate from before mixing to the end of mixing.

[0022] Moisture content ω of aggregates before mixing c ≥ω a (t mix When this occurs, the additional water absorption compensation volume will no longer be calculated.

[0023] Secondly, the present invention provides an application of designing porous concrete mix proportions using the above-mentioned design method, wherein the application is in the field of permeable concrete or vegetation concrete.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. A quantitative design method for porous concrete mix proportion that considers the morphological characteristics of recycled coarse aggregate is proposed for the first time. Under the constraint of target porosity, the influence of aggregate particle shape difference on skeleton packing and paste demand is transformed into a calculable correction mechanism, replacing simple empirical trial mix design and improving the design pertinence and reproducibility. 2. This invention proposes an additional water absorption compensation method for recycled aggregate that matches the mixing process. In response to the problem of fluctuations in effective mixing water caused by rapid water absorption of recycled aggregate during the mixing stage, a compensation calculation based on water absorption behavior during the mixing stage is established to make the effective water (effective water-cement ratio) more stable and reduce workability fluctuations and the risk of pore blockage / segregation. 3. This invention constructs a collaborative closed-loop design process of "morphological correction - water absorption compensation - volume balance solution", which realizes the coordinated determination of coarse aggregate, cementitious materials and water consumption. Under the premise of meeting the permeability / vegetation function porosity, it improves the strength level and consistency, reduces trial mixing iterations, and improves the engineering applicability and batch stability. Detailed Implementation

[0025] The present invention will be further described below with reference to embodiments, but the scope of protection of the present invention is not limited thereto. It should be noted that the implementation steps in the embodiments can be further adjusted according to the specific experimental environment, and the implementation steps not specified are usually conditions in conventional experiments. All compounds involved in the following embodiments are commercially available pharmaceutical products.

[0026] Example 1 Taking porous vegetation concrete made from recycled coarse aggregate for ecological slope protection as an example, the target design porosity P=28%, the target effective water-cement ratio λ=0.30, the admixture mass fraction k=0.4%, and the mixing time t mix =4 min. PO 42.5 ordinary Portland cement was used, with a cementitious material density of 3100 kg / m³. 3 The density of water is taken as 1000 kg / m³ 3 The density of the admixture is taken as 1050 kg / m³. 3 The recycled coarse aggregate has a particle size range of 16~31.5 mm, consisting of three particle sizes: 16~20 mm, 20~26.5 mm, and 26.5~31.5 mm.

[0027] 1. Basic physical property testing The apparent density ρ of recycled coarse aggregate was measured. g =2550 kg / m 3 Close packing density ρ s =1450 kg / m 3 Moisture content ω before mixing c =1.2%. Take the baseline coefficient α0=0.98.

[0028] 2. Two-dimensional morphological parameter testing and normalization Two-dimensional morphological tests were performed on recycled coarse aggregate and reference aggregate using the AIMS system. The reference aggregate was selected from qualified natural coarse aggregate of the same particle size range, and its morphological parameters were used as the normalization benchmark.

[0029] The recycled coarse aggregate was measured to have a sphericity Sp = 0.65 and an edge angle An = 320°; the reference aggregate was measured to have a sphericity Sp0 = 0.72 and an edge angle An0 = 280°. Therefore: Sp =0.65 / 0.72=0.903; An =3200 / 2800=1.143.

[0030] 3. α m Calibration and Calculation This embodiment uses a basic constructivist approach to calculate α. m Based on existing historical data from multiple batches, normalized dimensionless two-dimensional morphological parameters were used as independent variables, and the corresponding αm that met the target porosity and performance requirements was used as the dependent variable to fit the γ and β parameters. Taking γ1=0.50, β1=0.70, and β2=0.30, then: α m =1+0.50×[0.70×(1.143 1) 0.30×(0.903 1)] α m =1+0.50×(0.100+0.029) α m =1.065.

[0031] The value is in the range of 0.85 to 1.25, so no truncation correction is needed.

[0032] 4. Calculation of coarse aggregate usage The standard dosage of coarse aggregate is: m g0 =α 0· ρ s =0.98×1450=1421 kg / m 3 .

[0033] After introducing the morphology correction factor, the amount of coarse aggregate to be corrected is: m g =α m ·m g0 =1.065×1421=1514 kg / m 3 .

[0034] Considering the accuracy of engineering measurements, m can be taken. g =1510 kg / m 3 .

[0035] 5. Solving for cementitious materials and target effective water consumption using volume equilibrium. In a unit volume of 1 m 3 In porous concrete, establish volume equilibrium: m g / ρ g + m b / ρ b + m w0 / ρ w + mad / ρ ad + P = 1.

[0036] Where, m w0 =λ·m b m ad =k·m b Substituting P=0.28 and m... g =1510 kg / m 3 ρ g =2550 kg / m 3 ρ b =3100kg / m 3 ρ w =1000 kg / m 3 ρ ad =1050 kg / m 3 Given λ=0.30 and k=0.004, solving the equations simultaneously yields the amount of cementitious material used, m. b And target effective water consumption m w0 .

[0037] After rounding up the engineering measurements, take m. b =240 kg / m 3 m w0 =72 kg / m 3 m ad =1.0 kg / m 3 .

[0038] 6. Additional water absorption compensation during the mixing stage After the recycled coarse aggregate was dried to constant weight, a water absorption kinetics test was conducted to measure the water absorption rate ω at 4 min. a (t mix )=2.0%, moisture content ω before mixing c If the water absorption rate is 1.2%, then the water absorption rate difference that needs to be compensated during the mixing stage is 0.8%.

[0039] The additional water absorption compensation volume is: m add =α m ·m g ·max[ω a (t mix ) ωc,0] m add =1.065 × 1510 × 0.008 = 12.9 kg / m 3 .

[0040] The revised total water consumption is: m w =m w0 +madd =72 + 12.9 = 84.9 kg / m 3 The engineering measurement is taken as 85 kg / m³. 3 .

[0041] 7. Output the mix proportions and verification results. The final output mix proportion is: cement 240 kg / m³ 3 1510 kg / m³ of recycled coarse aggregate 3 The target effective mixing water is 72 kg / m³. 3 Additional water absorption compensation of approximately 13 kg / m³ 3 Total water consumption: 85 kg / m³ 3 Additive 1.0 kg / m 3 .

[0042] The concrete was formed using the "cement-coated stone method" and cured for 28 days. The measured porosity was 27.4%, which was 0.6 percentage points lower than the target porosity of 28%. The 28-day compressive strength was 10.8 MPa. The mixture showed no obvious segregation, bleeding, or local pore blockage, meeting the requirements for ecological slope protection vegetation concrete.

[0043] Example 2 Taking porous vegetation concrete made from recycled coarse aggregate for ecological slope protection as an example, the target design porosity P=28%, the target effective water-cement ratio λ=0.30, the admixture mass fraction k=0.4%, and the mixing time t mix =4 min. PO 42.5 ordinary Portland cement was used, with a cementitious material density of 3100 kg / m³. 3 The density of water is taken as 1000 kg / m³ 3 The density of the admixture is taken as 1050 kg / m³. 3 The recycled coarse aggregate has a particle size range of 16~31.5 mm, consisting of three particle sizes: 16~20 mm, 20~26.5 mm, and 26.5~31.5 mm.

[0044] 1. Basic physical property testing The apparent density ρ of recycled coarse aggregate was measured. g =2550 kg / m 3 Close packing density ρ s =1450 kg / m 3 Moisture content ω before mixing c =1.2%. Take the baseline coefficient α0=0.98.

[0045] 2. Two-dimensional morphological parameter testing and normalization Two-dimensional morphological tests were performed on recycled coarse aggregate and reference aggregate using the AIMS system. The reference aggregate was selected from qualified natural coarse aggregate of the same particle size range, and its morphological parameters were used as the normalization benchmark.

[0046] The recycled coarse aggregate was measured to have a sphericity Sp = 0.65, an edge angle An = 3200, a texture value Te = 3200, a fractal dimension D = 1.18, a lamellar parameter FR = 0.22, and a acicular parameter ER = 0.28. The reference aggregate was measured to have a sphericity Sp0 = 0.72, an edge angle An0 = 2800, a texture value Te0 = 700, a fractal dimension D0 = 1.12, a lamellar parameter FR0 = 0.18, and a acicular parameter ER0 = 0.20. Therefore: Sp =0.65 / 0.72=0.903; An =3200 / 2800=1.143; Te =1.214, D =1.054, FR =1.222, ER =1.400.

[0047] 3. α m Calibration and Calculation This embodiment employs enhanced constructivist computation α. m Based on existing historical data from multiple batches, the normalized dimensionless two-dimensional morphological parameters are used as independent variables, and the α value corresponding to meeting the target porosity and performance requirements is defined. m As dependent variables, the parameters γ and β were obtained through fitting. The values ​​were γ2=0.37, β3=0.30, β4=0.20, β5=0.15, β6=0.15, β7=0.10, and β8=0.10.

[0048] Substitute α m =1+γ2[β3An -β4Te +β5D +β6FR +β7ER -β8Sp ]; α m =1.213 The value is in the range of 0.85 to 1.25, so no truncation correction is needed.

[0049] 4. Calculation of coarse aggregate usage The standard dosage of coarse aggregate is: m g0 =α 0· ρ s =0.98×1450=1421 kg / m 3 .

[0050] After introducing the morphology correction factor, the amount of coarse aggregate to be corrected is: m g =α m ·m g0 =1.213×1421≈1724 kg / m 3 .

[0051] Considering the accuracy of engineering measurements, m can be taken. g =1720kg / m 3 .

[0052] 5. Solving for cementitious materials and target effective water consumption using volume equilibrium. In a unit volume of 1 m 3 In porous concrete, establish volume equilibrium: m g / ρ g + m b / ρ b + m w0 / ρ w + m ad / ρ ad + P = 1.

[0053] Where, m w0 =λ·m b m ad =k·m b Substituting P=0.28 and m... g =1720 kg / m 3 ρ g =2550 kg / m 3 ρ b =3100kg / m 3 ρ w =1000 kg / m 3 ρ ad =1050 kg / m 3 Given λ=0.30 and k=0.004, solving the equations simultaneously yields the amount of cementitious material used, m. b And target effective water consumption m w0 .

[0054] After rounding up the engineering measurements, take m. b =72 kg / m 3 m w0 =22 kg / m 3 m ad =0.3 kg / m 3 .

[0055] 6. Additional water absorption compensation during the mixing stage After the recycled coarse aggregate was dried to constant weight, a water absorption kinetics test was conducted to measure the water absorption rate ω at 4 min. a (t mix )=2.0%, moisture content ω before mixing c If the water absorption rate is 1.2%, then the water absorption rate difference that needs to be compensated during the mixing stage is 0.8%.

[0056] The additional water absorption compensation volume is: m add =α m ·m g ·max[ω a (t mix ) ωc,0] m add =1.213 × 1720 × 0.008 = 16.7 kg / m 3 .

[0057] The revised total water consumption is: m w =m w0 +m add =22 + 16.7 = 38.7 kg / m 3 The engineering measurement is taken as 39 kg / m³. 3 .

[0058] 7. Output the mix proportions and verification results. The final output mix proportion is: cement 72 kg / m³ 3 1720 kg / m³ of recycled coarse aggregate 3 The target effective mixing water is 22 kg / m³. 3 Additional water absorption compensation is approximately 16.7 kg / m³. 3 Total water consumption: 38.7 kg / m³ 3 Additive 0.3 kg / m 3 .

[0059] The concrete was formed using the "cement-coated stone method" and cured for 28 days. The measured porosity was 27.8%, which was 0.2 percentage points lower than the target porosity of 28%. The 28-day compressive strength was 10.9 MPa. The mixture showed no obvious segregation, bleeding, or local pore blockage, meeting the requirements for ecological slope protection vegetation concrete.

Claims

1. A method for designing the mix proportion of porous concrete using recycled coarse aggregate, characterized in that, Including the following steps: Determine the target porosity and target properties of concrete; Two-dimensional morphological parameters of recycled coarse aggregate and reference aggregate are collected. The two-dimensional morphological parameters of the recycled coarse aggregate are divided by the two-dimensional morphological parameters of the reference aggregate to obtain normalized dimensionless two-dimensional morphological parameters. Based on the normalized dimensionless two-dimensional morphological parameters, a morphological correction coefficient α is constructed. m ; Using morphological correction factor α m Calculate the amount of coarse aggregate correction and the total water correction; The reference aggregate is selected from natural coarse aggregate, qualified recycled coarse aggregate, or aggregates from historical databases that have been verified to meet the target porosity and target performance requirements of the recycled coarse aggregate porous concrete. The two-dimensional morphological parameters of the reference aggregate are the average or median obtained with the recycled coarse aggregate under the same particle size range, the same image acquisition conditions, and the same statistical methods.

2. The design method according to claim 1, characterized in that, The normalized dimensionless two-dimensional morphological parameters include sphericity Sp, edge angle An, texture value Te, fractal dimension D, sheet parameter FR, and needle parameter ER.

3. The design method according to claim 2, characterized in that, The α m The basic construction formula is: a m =1+γ1[β1(An-1)-β2(Sp-1)] In the formula, γ1 is the scaling factor, and β1 and β2 are the weighting factors; The α m The enhanced construct is: a m =1+γ2[β3An-β4Te+β5D+β6FR+β7ER-β8Sp] In the formula, γ2 is the scaling factor, and β3, β4, β5, β6, β7, and β8 are weighting factors; The α m The range is 0.85~1.25, when α m When <0.85, take α m =0.85, when α m When α > 1.25, take α. m =1.

25.

4. The design method according to claim 3, characterized in that, The α m Basic construction and α m The method for calibrating the scaling factor and weighting factor in the enhanced construction is to determine the performance target of the concrete, and then calibrate them based on the target performance and target porosity of the concrete through regression analysis of a historical database.

5. The design method according to claim 4, characterized in that, The historical database regression, when multiple batches of historical data are available, uses the normalized dimensionless two-dimensional morphological parameters as independent variables, and assigns the α value corresponding to meeting the target porosity and performance requirements. m The γ and β parameters were obtained by fitting the data as dependent variables.

6. The design method according to any one of claims 1-5, characterized in that, The amount of recycled coarse aggregate used for correction is m g The calculation formula is as follows: In the formula, ρ s To determine the close packing density of the recycled coarse aggregate, α m α0 is the morphological correction coefficient, and α0 is the baseline coefficient, with a value of 0.95 to 1.

00.

7. The design method according to claim 6, characterized in that, The amount of admixture per unit volume of the recycled coarse aggregate porous concrete (m³) ad Target effective water consumption per unit volume of concrete (m³) w0 and the amount of cementitious material per unit volume of concrete (m) b The calculation method is as follows: The volume balance equation for a unit volume of concrete is established as follows: In the formula, m g ρ is the amount of coarse aggregate per unit volume of concrete. g The apparent density of coarse aggregate is m. b ρ is the amount of cementitious material per unit volume of concrete. b The apparent density of the cementitious material is m. w0 ρ is the target effective water consumption per unit volume of concrete. w Let m be the density of water. ad ρ is the amount of admixture per unit volume of concrete. ad Where P is the density of the admixture and P is the target porosity; Given the target effective water-cement ratio λ and the admixture mass fraction k, λ, k and m w0 m b and m ad The relationship is as follows: The volume balance equation is compared with λ, k, and m. w0 m b and m ad Solving the simultaneous equations, we get: m can then be calculated ad、 m b and m w0 The value of .

8. The design method according to claim 7, characterized in that, The target effective water content per unit volume of concrete (m) w0 After morphological correction factor α m Corrected total water usage (m) w The calculation formula is as follows: In the formula, ω c The moisture content of the aggregate before mixing was measured by the drying to constant weight method. ω a (t mix () represents the water absorption rate of the recycled coarse aggregate from before mixing to the end of mixing; m add The water absorption of coarse aggregate, in m g The amount of coarse aggregate per unit volume of concrete; m w0 The target effective water consumption per unit volume of concrete.

9. The design method according to claim 8, characterized in that, The ω a (t mix The calculation method for ) is as follows: The recycled coarse aggregate was dried to constant weight to obtain a dry mass m0. After soaking in water, a sample was taken at time t, and after surface drying treatment, the mass was obtained as m(t). The water absorption rate was calculated using the following formula: The actual time from adding water to the recycled coarse aggregate to the end of mixing is t. mix When t=t mix ω a (t mix This refers to the water absorption rate of recycled coarse aggregate from before mixing to the end of mixing.

10. An application of the design method described in any one of claims 1-9 for designing porous concrete mix proportions, characterized in that, The application areas are permeable concrete or vegetation concrete.

Citation Information

Patent Citations

  • Preparation method of pervious concrete based on slurry-bone ratio and cementing material

    CN112094082A

  • High-strength and high-permeability concrete mix proportion design method based on aggregate characteristics

    CN112115409A