An energy-saving power cable with irregularly shaped conductor.
By using rare earth-graphene hybrid nanoparticles to modify the metal shaped monofilaments, combining the asymmetric shaped cross section with the sawtooth interlocking surface, and chemical bonding of the titanium carbide conductive conversion film and the titanate coupling agent transition layer in the shaped conductor power cable, the problem of synergistic matching between conductor materials and structural design is solved, achieving low AC resistance and stable contact of the conductor under thermal cycling conditions, thus achieving energy-saving effect.
Patent Information
- Application Number
- CN202611381369.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-10
AI Technical Summary
In existing power cables with irregularly shaped conductors, the microscopic performance control of conductor materials and the macroscopic irregular structure design are independent of each other and lack systematic coordination and matching. This leads to a gradual increase in the contact resistance between individual filaments under thermal cycling conditions, which increases transmission loss.
Metallic shaped monofilaments modified with rare earth-graphene hybrid nanoparticles are used to achieve interlayer interlocking through asymmetric irregular cross-sections and serrated interlocking surfaces. A titanium carbide conductive conversion film is composited in situ on the surface of the monofilaments, and a titanate coupling agent transition layer is set between the conductor and the cross-linked polyethylene insulation layer to achieve chemical bonding.
Maintaining stable contact resistance under thermal cycling conditions reduces AC resistance, decreases line operating losses, and achieves energy-saving operation.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of power cable technology, and specifically relates to an energy-saving power cable with an irregularly shaped conductor. Background Technology
[0002] High-voltage and ultra-high-voltage cross-linked polyethylene insulated power cables typically employ circular single-wire stranded compacted conductors or sector-shaped compacted conductor structures. As cable cross-sections continue to increase, the skin effect intensifies, and the conductor's AC resistance significantly exceeds its DC resistance. Simply increasing the cross-section is no longer an economical and effective way to improve current carrying capacity. To suppress the skin effect, current practices involve dividing large-section conductors into multiple insulated sector-shaped strands, then cabling them to form a circular conductor. This reduces the cross-sectional area of individual strands, thereby lowering the skin effect and proximity effect. Simultaneously, to reduce cable outer diameter, save materials, and improve fill factor, irregularly shaped conductors (such as Z-shaped, C-shaped, tile-shaped, and trapezoidal stranded conductors) are increasingly being used.
[0003] However, in existing power cables with irregularly shaped conductors, the microscopic performance control of conductor materials and the macroscopic irregular structure design are independent of each other, lacking systematic coordination and matching. The material performance advantages are difficult to fully utilize in irregularly shaped stranded structures. Moreover, irregularly shaped conductors are formed by twisting and pressing multiple irregularly shaped single wires together. The contact state between the single wires directly affects the overall conductivity of the conductor. However, the existing structure only focuses on the initial pressing state of the contact interface and does not consider the thermo-mechanical coupling effect caused by the periodic change of conductor temperature when the cable load fluctuates. This leads to a gradual increase in the contact resistance between single wires during long-term operation, and a corresponding increase in transmission loss. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide an energy-saving power cable with an irregularly shaped conductor to solve the problems mentioned in the background art. The specific solution is as follows:
[0005] The first aspect of this invention discloses an energy-saving power cable with an irregularly shaped conductor, comprising a central conductor layer and a cross-linked polyethylene insulation layer covering the outside of the central conductor layer; The central conductor layer is composed of multiple strands of irregularly shaped metal monofilaments twisted together in multiple layers; The metal shaped monofilament is prepared using rare earth modified oxygen-free copper or rare earth modified heat-resistant aluminum alloy, and rare earth-graphene hybrid nanoparticles are uniformly dispersed inside the matrix. The cross-section of the metal shaped monofilament is an asymmetric trapezoidal or arc-shaped variable cross-section structure, and adjacent layers of metal shaped monofilaments are interlocked and bonded to each other through serrated interlocking surfaces; The surface of the metal shaped monofilament is in situ coated with a titanium carbide conductive conversion film. A titanate coupling agent transition layer is provided between the titanium carbide conductive conversion film and the cross-linked polyethylene insulating layer. The titanate coupling agent transition layer is chemically bonded to the surface of the titanium carbide conductive conversion film and the cross-linked polyethylene insulating layer, respectively.
[0006] Furthermore, the outermost monofilament of the central conductor layer has a slightly convex arc surface, the radius of curvature of which is adapted to the radius of curvature of the inner wall of the cross-linked polyethylene insulation layer.
[0007] Furthermore, the mass fraction of rare earth-graphene hybrid nanoparticles in the metal matrix is 0.05% to 0.3%.
[0008] Furthermore, the thickness of the titanium carbide conductive conversion film is 50 nm to 200 nm, and the thickness of the titanate coupling agent transition layer is 5 nm to 50 nm.
[0009] Furthermore, along the radial direction of the central conductor layer from the inside out, the equivalent cross-sectional area of the metal shaped monofilaments in each layer decreases in a gradient, with the decrease ratio of the equivalent cross-sectional area between adjacent layers being 5% to 15%.
[0010] The second aspect of this invention discloses a method for preparing an energy-saving power cable with an irregularly shaped conductor, comprising the following steps: S1, high-purity copper liquid or aluminum liquid is melted under a protective atmosphere, rare earth-graphene intermediate alloy wire is added to it, and modified metal rod is prepared by continuous casting and rolling. S2, the modified metal rod is drawn through a continuous wire drawing machine in multiple passes, gradually drawn through a multi-pass transitional shaped wire drawing die, and then drawn into a shaped monofilament with a trapezoidal or arc-shaped cross section through an asymmetric shaped sizing die. S3, the irregular monofilament is continuously passed through the in-situ reaction chamber with built-in tetrabutyl titanate precursor, and a titanium carbide conductive conversion film is formed in-situ on the surface of the irregular monofilament. S4, the surface of the irregular monofilament with the titanium carbide conductive conversion film is coated with a tetrabutyl titanate coupling agent solution, and after drying and curing, a titanate coupling agent transition layer is formed. S5, multiple irregularly shaped monofilaments with titanium carbide conductive conversion film and titanate coupling agent transition layer are twisted in multiple layers, and radial compressive stress is applied at the converging mold, so that the irregularly shaped monofilaments in each layer are interlocked and pressed together by the sawtooth interlocking surface, thus obtaining the conductor. S6, the conductor is sequentially covered with a conductor shielding layer, a cross-linked polyethylene insulation layer, and an insulation shielding layer. After cross-linking treatment, the energy-saving irregular structure conductor power cable is obtained.
[0011] Furthermore, in step S1, the mass fraction of rare earth-graphene hybrid nanoparticles in the rare earth-graphene intermediate alloy wire is 1% to 5%, with the remainder being copper or aluminum.
[0012] Furthermore, in step S3, the temperature of the in-situ reaction chamber is 500℃~700℃, and the reaction time is 30s~120s.
[0013] Further, in step S4, the concentration of the tetrabutyl titanate coupling agent solution is 0.5wt% to 5.0wt%.
[0014] Furthermore, in step S5, the twisting diameter ratio of each layer is: inner layer 18-25, middle layer 15-22, and outer layer 10-16.
[0015] Compared with existing technologies, this invention has the following beneficial effects: This application systematically coordinates three aspects: conductor material modification, irregular structure design, and conductor-insulation interface strengthening. Rare earth-graphene hybrid nanoparticles are uniformly dispersed within the metal matrix, giving the conductor material both high conductivity and creep resistance, providing matching matrix support for the contact stability of the irregular stranded structure under thermal cycling conditions. The asymmetric irregular cross-section and serrated interlocking surface form a multi-tooth interlocking structure, with the equivalent cross-sectional area of each layer decreasing radially, collectively improving the current distribution inside the conductor. An in-situ composite titanium carbide conductive conversion film on the monofilament surface forms a low-resistance, oxidation-resistant conductive channel at the interlocking contact surface; a titanate coupling agent transition layer establishes a chemical bond between the titanium carbide film and the cross-linked polyethylene insulation layer, reducing the microscopic gaps at the interface. The synergistic cooperation of the above materials, structure, and interface enables the cable to maintain stable contact resistance under thermal cycling conditions and maintain a low AC resistance level throughout its entire life cycle, thereby achieving energy-saving operation. Detailed Implementation
[0016] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0017] During operation, the skin effect in high-voltage and ultra-high-voltage cross-linked polyethylene insulated power cables intensifies with increasing cross-sectional area, resulting in significantly higher AC resistance than DC resistance. Simply increasing the cross-section is insufficient to effectively improve current carrying capacity. Existing irregularly shaped conductor designs primarily focus on geometric optimization, with the microscopic performance control of the conductor material and the macroscopic irregular structure design remaining independent. Furthermore, attention to the contact interface is limited to the initial compaction state, neglecting the increased transmission losses caused by the gradual increase in contact resistance between single filaments under thermal cycling conditions. Therefore, this application provides an energy-saving irregularly shaped conductor power cable. It employs metal irregularly shaped single filaments modified with rare-earth-graphene hybrid nanoparticles, achieving interlayer interlocking through an asymmetric irregular cross-section and a serrated interlocking surface. A titanium carbide conductive conversion film is in-situ laminated onto the surface of the single filament, and a titanate coupling agent transition layer is placed between the conductor and the cross-linked polyethylene insulation layer to achieve bilateral chemical bonding. The technical solution of this application is described in detail below with reference to specific embodiments.
[0018] This invention provides an energy-saving power cable with an irregularly shaped conductor, comprising a central conductor layer and a cross-linked polyethylene insulation layer covering the outside of the central conductor layer. The central conductor layer is composed of multiple irregularly shaped metal monofilaments twisted together in multiple layers.
[0019] The metallic irregularly shaped monofilaments are prepared using rare-earth modified oxygen-free copper or rare-earth modified heat-resistant aluminum alloys, with rare-earth-graphene hybrid nanoparticles uniformly dispersed within the matrix. The rare-earth elements in the rare-earth-graphene hybrid nanoparticles synergistically interact with graphene, endowing the conductor material with high conductivity and good creep resistance, providing a material basis for maintaining contact stability of the irregularly stranded structure under thermal cycling conditions. In one specific implementation, the mass fraction of the rare-earth-graphene hybrid nanoparticles in the metal matrix is 0.05%–0.3%, and the rare-earth element is at least one selected from yttrium or cerium. Preferably, the particle size of the rare-earth-graphene hybrid nanoparticles is 50 nm–200 nm.
[0020] The cross-section of the shaped metal monofilament is an asymmetric trapezoidal or arc-shaped variable cross-section structure. An asymmetric trapezoidal structure refers to a monofilament cross-section where the lengths or inclination angles of the two sides of the waist are not equal; an arc-shaped variable cross-section structure refers to a monofilament cross-section where one or both sides have an arc-shaped transition. Adjacent layers of shaped metal monofilaments are interlocked and bonded together via serrated interlocking surfaces: serrated protrusions and serrated grooves are respectively provided on opposite sidewalls. Under radial compressive stress, the protrusions embed into the corresponding grooves, forming a multi-tooth interlocking structure. This structure, combined with the creep-resistant properties of the matrix material during thermal cycling, ensures stable contact pressure on the interlocking surfaces during thermal expansion and contraction. The tooth dimensions of the serrated interlocking surfaces are adapted to the wall thickness of the shaped monofilaments to ensure effective mechanical interlocking between adjacent layers of monofilaments after stranding and compression. It is understood that the specific values of the tooth dimensions can be adaptively adjusted according to the monofilament wall thickness and stranding process.
[0021] The central conductor layer comprises, from the inside out, an inner core wire, a middle transition wire, and an outer bonding wire. The outer bonding wire has a slightly convex arc surface on its outer surface. The radius of curvature of this arc surface matches the radius of curvature of the inner wall of the cross-linked polyethylene insulation layer, creating a uniform bonding interface between the outer surface of the conductor and the inner wall of the insulation layer. This helps alleviate local electric field concentration caused by irregularities on the conductor surface and improves the thermal conductivity of the conductor-insulation interface. Preferably, along the radial direction of the central conductor layer from the inside out, the equivalent cross-sectional area of each layer of shaped metal wires decreases in a gradient distribution, with a decrease of 5% to 15% between adjacent layers. The equivalent cross-sectional area refers to the area of an equivalent circular cross-section when the asymmetric cross-sectional area of the shaped wire is converted according to the principle of equal area. This gradient distribution facilitates uniform stress distribution among the shaped wires during the stranding and compaction process and, to some extent, improves the current distribution inside the conductor.
[0022] A titanium carbide conductive conversion film with a thickness of 50 nm to 200 nm is in situ laminated onto the surface of a shaped metal monofilament. This titanium carbide conductive conversion film is prepared by feeding the shaped monofilament into an in-situ reaction chamber filled with a titanium carbide-based precursor, and reacting at 500℃ to 700℃ for 30s to 120s under a protective atmosphere. A strong bond is formed between the titanium carbide conductive conversion film and the metal substrate through interfacial diffusion and localized reaction. This film layer exhibits good conductivity and high hardness, providing a low-resistance conductive channel at the monofilament contact interface. Its antioxidant properties also help to slow down the oxidation and deterioration of the contact surface during long-term cable operation. After drawing, some rare-earth-graphene hybrid particles are exposed on the surface of the shaped monofilament. These exposed particles can serve as nucleation sites for subsequent in-situ reactions to generate titanium carbide, which helps to improve the film density and the film-substrate bonding strength.
[0023] A titanate coupling agent transition layer is disposed between the titanium carbide conductive conversion film and the cross-linked polyethylene insulation layer. This titanate coupling agent transition layer is chemically bonded to both the surface of the titanium carbide conductive conversion film and the cross-linked polyethylene insulation layer. The thickness of the titanate coupling agent transition layer is 5 nm to 50 nm. One end of the titanate coupling agent molecule is bonded to the surface of the titanium carbide conductive conversion film, and the other end is bonded to the cross-linked polyethylene molecular chain during the cross-linking process, thereby constructing a chemically bonded interfacial transition layer between the conductor and the insulation layer. This interfacial transition layer helps to significantly reduce the microscopic interfacial gap between the conductor and the insulation layer, alleviate the electric field concentration at the interface, and reduce the probability of partial discharge. At the same time, the chemical bonding effect enhances the interfacial bonding strength between the conductor and the insulation layer, which can effectively inhibit the separation or relative slippage of the insulation layer from the conductor during cable bending or thermal cycling.
[0024] A conductor shielding layer and an insulating shielding layer are also provided outside the central conductor layer, with a cross-linked polyethylene insulating layer disposed between the conductor shielding layer and the insulating shielding layer. The conductor shielding layer is used to smooth out the protrusions on the conductor surface, uniformize the electric field on the conductor surface, and suppress electric field distortion on the conductor side; the insulating shielding layer is used to uniformly distribute the electric field on the outer surface of the insulating layer, matching the requirements of the cable shielding and grounding structure. The conductor shielding layer and the insulating shielding layer, together with the aforementioned conductor-insulation interface structure, jointly construct a complete electric field control system.
[0025] This invention also discloses a method for preparing an energy-saving power cable with an irregularly shaped conductor, which includes the following steps: S1. High-purity copper or high-purity aluminum is smelted under a protective atmosphere to obtain molten copper or molten aluminum at a smelting temperature of 1150℃~1250℃ (copper) or 710℃~750℃ (aluminum). Rare earth-graphene master alloy wire is added to the molten copper or aluminum through a continuous wire feeding method, and modified metal rods are prepared by continuous casting and rolling.
[0026] The preparation method of rare earth-graphene intermediate alloy wire is as follows: rare earth-graphene hybrid nanoparticles are melted and continuously cast and rolled with a copper or aluminum matrix to form an intermediate alloy wire. The mass fraction of rare earth-graphene hybrid nanoparticles in the intermediate alloy wire is 1% to 5%, with the balance being copper or aluminum. Adding the intermediate alloy wire in a continuous feeding manner facilitates the rapid melting and uniform dispersion of the rare earth-graphene hybrid nanoparticles in the molten copper or aluminum. During the continuous casting and rolling process, under the combined action of rolling deformation and recrystallization, the rare earth-graphene hybrid nanoparticles are further homogenized with the flow of the matrix metal, resulting in a uniformly dispersed microstructure within the modified metal rod.
[0027] S2, the modified metal rod obtained above is drawn in multiple passes through a continuous wire drawing machine, gradually passing through multiple transitional shaped wire drawing dies to gradually transform the cross-section of the monofilament from circular to elliptical, and then to a pre-formed irregular shape. Finally, it is drawn into an irregular monofilament with an asymmetric trapezoidal or arc-shaped variable cross-section structure through an asymmetric sizing die. The elongation coefficient of each drawing pass is 1.05–1.30, and the drawing speed is 5 m / min–15 m / min. The exit shape of the sizing die is consistent with the target cross-sectional shape of the irregular monofilament; by changing the sizing die, irregular monofilaments with different cross-sectional shapes and sizes can be adapted.
[0028] S3, the above-prepared irregular monofilament is continuously fed into an in-situ reaction chamber filled with a titanium carbide source precursor, and held at 500℃~700℃ for 30s~120s under a protective atmosphere to form a titanium carbide conductive conversion film in situ on the surface of the irregular monofilament.
[0029] The protective atmosphere in the reaction chamber is argon or nitrogen, with a flow rate of 0.5 L / min to 2.0 L / min. Titanium carbide is coated on the outer surface of the shaped monofilament in the form of a thin film. The thickness of the titanium carbide conductive conversion film is controlled by adjusting the linear velocity of the shaped monofilament through the reaction chamber, the reaction temperature, and the holding time; in this embodiment, it is controlled to be 50 nm to 200 nm.
[0030] S4, the surface of the irregular monofilament with the titanium carbide conductive conversion film is coated with a tetrabutyl titanate coupling agent solution, and after drying and curing, a titanate coupling agent transition layer is formed.
[0031] Specifically, tetrabutyl titanate coupling agent is dissolved in an organic solvent to prepare a coupling agent solution with a concentration of 0.5 wt% to 5.0 wt%. The organic solvent can be any one of anhydrous ethanol, isopropanol, or ethyl acetate. The coating method can be any one of dip coating, spray coating, or roller coating. After coating, it is dried and cured at a temperature of 60℃ to 100℃ for 30 min to 120 min, allowing the coupling agent molecules to chemically react with the active sites on the surface of the titanium carbide conductive conversion film to form chemical bonds, while simultaneously removing residual solvent. The thickness of the titanate coupling agent transition layer is controlled by adjusting the concentration of the coupling agent solution and the coating process parameters; in this embodiment, it is controlled to be 5 nm to 50 nm.
[0032] S5, multiple irregularly shaped monofilaments with titanium carbide conductive conversion film and titanate coupling agent transition layer are twisted in multiple layers through a cage stranding machine, and radial compressive stress is applied at the converging die, so that the irregularly shaped monofilaments in each layer are interlocked and pressed together by the sawtooth interlocking surface, thus obtaining the central conductor layer.
[0033] During the stranding process, the irregularly shaped monofilaments in each layer are stranded according to a predetermined arrangement and stranding pitch ratio. The stranding pitch ratios for each layer are: inner layer 18–25, middle layer 15–22, and outer layer 10–16. The inner layer uses a larger pitch ratio, and the outer layer uses a smaller pitch ratio. The radial compressive stress applied at the converging die ensures that the monofilaments in each layer are tightly bonded, and the serrated protrusions and serrated grooves on the opposite sidewalls interlock to form a multi-tooth interlocking structure. After stranding, the central conductor layer is obtained. During the stranding process, the titanate coupling agent transition layer in the interlocking area between the monofilaments is locally damaged due to extrusion and friction, exposing the titanium carbide conductive conversion film to the interlocking contact surface to provide conductive contact; while the titanate coupling agent transition layer in the outer arc surface area of the outer bonding wire remains intact, used to form a chemical bond with the cross-linked polyethylene insulation layer.
[0034] S6, the conductor is sequentially coated with a conductor shielding layer, a cross-linked polyethylene insulation layer, and an insulation shielding layer using a three-layer co-extrusion method. After the coating is completed, a cross-linking treatment is performed to obtain an energy-saving irregular-shaped conductor power cable.
[0035] The extrusion temperature for three-layer co-extrusion is 190℃~230℃ (die body) and 200℃~240℃ (die head). This temperature range allows the cross-linked polyethylene to fully melt and plasticize, exhibiting good fluidity, while preventing overheating and decomposition of the material. The three-layer co-extrusion process ensures clean and uncontaminated interfaces between layers, resulting in tight interlayer bonding.
[0036] The crosslinking process employs a dry crosslinking method: the coated cable is fed into a crosslinking pipeline and crosslinked under high-temperature, high-pressure steam conditions. The steam pressure in the crosslinking pipeline is 1.0 MPa to 2.5 MPa, the crosslinking temperature is 200℃ to 260℃, and the crosslinking time is 5 min to 15 min. Under these conditions, the crosslinked polyethylene insulation layer undergoes crosslinking. Simultaneously, the functional groups in the titanate coupling agent transition layer formed on the outermost layer of the conductor in step S4, facing the organic phase, participate in the crosslinking reaction and form chemical bonds with the crosslinked polyethylene molecular chains.
[0037] After cross-linking, a segmented water-cooling method is used for cooling and shaping: the cable is sequentially cooled in segments by passing it through a warm water bath at 40℃~60℃ and then a room temperature water bath. After cooling and shaping, an energy-saving power cable with an irregularly shaped conductor is obtained.
[0038] The energy-saving power cable with an irregularly shaped conductor, manufactured using the above method, features a core conductor layer where the irregularly shaped metal filaments are mechanically interlocked through serrated interlocking surfaces. Combined with the creep resistance of the matrix material, this effectively suppresses contact resistance degradation under thermal cycling conditions. The titanium carbide conductive conversion film and the titanate coupling agent transition layer work together to construct a chemically bonded interface transition layer between the conductor and insulation layers, which helps reduce partial discharge levels at the interface and improves interface peel strength. The gradient decrease in equivalent cross-sectional area of each layer, combined with the uniform adhesion of the conductor-insulation interface, improves the current distribution within the conductor and suppresses the skin effect to a certain extent. This synergistic combination of materials, structure, and interface ensures stable contact resistance under thermal cycling conditions and maintains a low AC resistance level throughout the cable's lifespan, thereby reducing line operating losses and achieving energy-saving operation.
[0039] To verify the effectiveness of the above material-structure-interface synergy scheme in reducing AC resistance and line loss, the following description, in conjunction with specific embodiments and comparative examples, provides further explanation.
[0040] Example 1: The specific preparation conditions for energy-saving power cables with irregularly shaped conductors are as follows.
[0041] The nominal cross-sectional area of the center conductor layer is 1000 mm². 2It is composed of 37 irregularly shaped metal monofilaments twisted together: 7 in the inner layer, 12 in the middle layer, and 18 in the outer layer. The metal monofilaments are prepared using rare-earth-modified oxygen-free copper. Rare-earth-graphene hybrid nanoparticles are uniformly dispersed within the matrix, with a mass fraction of 0.15%. The rare-earth elements used are a mixture of yttrium and cerium (mass ratio 1:1), and the nanoparticle size ranges from 80 nm to 120 nm. The cross-section of the metal monofilaments is an asymmetric trapezoidal structure, with adjacent layers interlocking and bonded together via serrated interlocking surfaces. The equivalent cross-sectional area decreases by 10% from the innermost layer to the outermost layer in the central conductor layer. The twisting pitch ratios are 22 for the inner layer, 18 for the middle layer, and 13 for the outer layer.
[0042] A titanium carbide conductive conversion film with a thickness of 100 nm is in situ laminated onto the surface of a metal shaped monofilament. A titanate coupling agent transition layer with a thickness of 20 nm is disposed between the titanium carbide conductive conversion film and the cross-linked polyethylene insulating layer.
[0043] The stranded and compressed conductor is coated with a conductor shielding layer, a cross-linked polyethylene insulation layer, and an insulation shielding layer in sequence using a three-layer co-extrusion method. The nominal thickness of the cross-linked polyethylene insulation layer is 16mm. The conductor is cross-linked for 10 minutes in a nitrogen atmosphere, at a pressure of 1.8MPa and a temperature of 230℃. After segmented water cooling and shaping, an energy-saving irregular-shaped conductor power cable sample is obtained.
[0044] Example 2: The difference from Example 1 is that the mass fraction of rare earth-graphene hybrid nanoparticles in the metal matrix is 0.05%, while the other conditions are the same as in Example 1.
[0045] Example 3: The difference from Example 1 is that the mass fraction of rare earth-graphene hybrid nanoparticles in the metal matrix is 0.30%, while the other conditions are the same as in Example 1.
[0046] Example 4: The difference from Example 1 is that the thickness of the titanium carbide conductive conversion film is 50 nm, while the other conditions are the same as in Example 1.
[0047] Example 5: The difference from Example 1 is that the thickness of the titanium carbide conductive conversion film is 200 nm, while the other conditions are the same as in Example 1.
[0048] Example 6: The difference from Example 1 is that the thickness of the titanate coupling agent transition layer is 5 nm, while the other conditions are the same as in Example 1.
[0049] Example 7: The difference from Example 1 is that the thickness of the titanate coupling agent transition layer is 50 nm, while the other conditions are the same as in Example 1.
[0050] Example 8: The difference from Example 1 is that the reduction ratio of the equivalent cross-sectional area between adjacent layers is 5%, while the other conditions are the same as in Example 1.
[0051] Example 9: The difference from Example 1 is that the reduction ratio of the equivalent cross-sectional area between adjacent layers is 15%, and the other conditions are the same as in Example 1.
[0052] Example 10: The difference from Example 1 is that the twisted diameter ratio of each layer is 25 for the inner layer, 22 for the middle layer, and 16 for the outer layer, while the other conditions are the same as in Example 1.
[0053] Example 11: The difference from Example 1 is that the twisting diameter ratio of each layer is 18 for the inner layer, 15 for the middle layer, and 10 for the outer layer, while the other conditions are the same as in Example 1.
[0054] Comparative Example 1: The conventional circular compacted conductor structure is adopted. The conductor is made of ordinary oxygen-free copper circular monofilaments of the same specification twisted and compacted. There is no TiC film and coupling agent layer on the surface of the monofilaments, and there is no coupling agent transition layer between the conductor and the insulation layer. The rest is the same as in Example 1.
[0055] Comparative Example 2: The difference from Example 1 is that the metal shaped monofilament is prepared using ordinary oxygen-free copper, and no rare earth-graphene hybrid nanoparticles are added inside the matrix. The other conditions are the same as in Example 1.
[0056] Comparative Example 3: The difference from Example 1 is that the cross-section of the metal shaped monofilament is a conventional circle, the monofilaments in each layer are conventionally twisted at point contact, and there is no serrated interlocking surface structure. The other conditions are the same as in Example 1.
[0057] Comparative Example 4: The difference from Example 1 is that the surface of the metal shaped monofilament does not have a titanium carbide conductive conversion film, that is, the S3 process is omitted, and the other conditions are the same as those in Example 1.
[0058] Comparative Example 5: The difference from Example 1 is that there is no titanate coupling agent transition layer between the titanium carbide conductive conversion film and the cross-linked polyethylene insulating layer, that is, step S4 is omitted, and the other conditions are the same as in Example 1.
[0059] Comparative Example 6: The difference from Example 1 is that the surface of the metal shaped monofilament has no titanium carbide conductive conversion film and no titanate coupling agent transition layer. That is, the S3 and S4 processes are omitted at the same time, and only the rare earth-graphene hybrid material and the shaped interlocking structure are retained. The other conditions are the same as those in Example 1.
[0060] Experimental example: The products obtained in the examples and comparative examples were subjected to relevant performance tests. The specific test methods are as follows: (1) DC resistance of conductor The test was conducted according to GB / T 3048.4-2025, using the double-arm bridge method to measure the DC resistance of the conductor under constant temperature conditions of 20℃.
[0061] (2) AC resistance of conductor Referring to the calculation methods for skin effect and proximity effect coefficients in IEC 60287-1-1 standard, and combining the measured DC resistance of the conductor, calculate the AC resistance of the conductor at a 50Hz power frequency, and calculate the ratio of AC resistance to DC resistance (AC / DC ratio).
[0062] (3) Rate of change of contact resistance during thermal cycling Referring to the thermal cycling test method specified in Clause 18.2.7 of GB / T 12706.2-2020, a periodic load current was applied to the cable sample, causing the conductor temperature to cycle between 20℃ and 120℃. The DC resistance of the conductor was measured at the end of the heating and cooling phases of each thermal cycle. Using the contact resistance value from the first cycle as a reference, the rate of change of contact resistance after the 100th cycle was calculated.
[0063] (4) Interfacial peel strength Cut a specimen of appropriate length from the cable sample, separate the cross-linked polyethylene insulation layer from the conductor, and perform a 180° peel test on a universal testing machine at a peel speed of 50 mm / min. Record the force value during the peel process and calculate the peel strength in N / cm.
[0064] (5) Partial discharge initiation voltage and partial discharge quantity The test was conducted in accordance with GB / T 3048.12-2025. The partial discharge initiation voltage was recorded in kV, and the partial discharge quantity at 1.5U0 voltage was recorded in pC.
[0065] The test results of each embodiment and comparative example are summarized in Table 1. All test data are the average values after testing three parallel samples.
[0066] Table 1 Comparison Test Results
[0067] Results analysis: (I) Electrical conductivity analysis As shown in Table 1, the DC resistance at 20℃ for each embodiment was 17.0–17.5 μΩ / m, and the AC / DC ratio was 1.10–1.14, both superior to the comparative examples. Comparative Example 1 used a conventional circular compacted oxygen-free copper conductor, with a DC resistance of 18.6 μΩ / m and an AC / DC ratio as high as 1.35, indicating a significant skin effect of the conventional circular compacted conductor. Although Comparative Example 2 retained the irregular interlocking structure and interface system, the matrix did not contain rare earth-graphene hybrid particles, and its DC resistance was 18.2 μΩ / m, still significantly higher than the embodiments. After removing the serrated interlocking structure, the AC / DC ratio in Comparative Example 3 increased to 1.28, indicating that the irregular interlocking structure plays a key role in suppressing the skin effect. The above comparisons show that rare earth-graphene hybrid modification can effectively reduce the DC resistance of the matrix, and combined with the serrated interlocking structure, it can significantly improve the current distribution inside the conductor and suppress the skin effect. The synergy of the two leads to a significant decrease in the AC / DC resistance ratio.
[0068] (II) Contact Stability Analysis The contact resistance change rate after 100 thermal cycles in each embodiment ranged from 3.0% to 4.8%. Comparative Example 2, without rare-earth-graphene hybridization, showed a contact resistance change rate as high as 18%; Comparative Example 4, without the TiC film, showed a change rate of 12%; Comparative Example 6, lacking both the TiC film and the coupling agent layer, showed a change rate of 15%, while Example 1 showed only 3.2%. These comparisons demonstrate that rare-earth-graphene hybridization imparts creep resistance to the matrix, providing a material basis for maintaining stable contact on the serrated interlocking surfaces under thermal cycling conditions; the TiC film provides a low-resistance conductive channel at the exposed interlocking surfaces and slows down oxidation and degradation of the contact surface; the combination of these two elements ensures stable contact resistance during thermal cycling, which is beneficial for reducing line losses during long-term operation.
[0069] (III) Insulation Interface Performance Analysis Except for Example 6, which verifies the thickness of the coupling agent layer, the interfacial peel strength of the other examples is 8.2–9.2 N / cm, the partial discharge initiation voltage is 41–46 kV, and the partial discharge at 1.5U0 is 1–3 pC. In Comparative Example 5, omitting the coupling agent layer causes a sharp drop in interfacial peel strength to 3.5 N / cm, a partial discharge initiation voltage to 30 kV, and a partial discharge at 1.5U0 to 12 pC. In Comparative Example 6, simultaneously lacking both the TiC film and the coupling agent layer, the interfacial peel strength further decreases to 3.0 N / cm, the partial discharge initiation voltage to 28 kV, and the partial discharge at 1.5U0 to 14 pC. This indicates that the coupling agent transition layer significantly reduces the microscopic interfacial gap between the conductor and the insulating layer through chemical bonding, enhances the interfacial bonding strength, and constructs a stable and dense interfacial transition layer between the conductor and the insulating layer, thereby effectively suppressing partial discharge.
[0070] (iv) Analysis of the rationality of parameter range Examples 2-11 verified the implementation effects under the extreme values of each numerical range. When the mass fraction of rare earth-graphene was 0.05% (Example 2) and 0.30% (Example 3), the conductivity and contact stability were better than those of the comparative examples. When the TiC film thickness was 50 nm (Example 4) and 200 nm (Example 5), the contact resistance change rate was 4.2% and 3.5%, respectively, both significantly better than that of the comparative example 4 (12%) without the TiC film. When the coupling agent layer thickness was 5 nm (Example 6), the interfacial peel strength was 6.5 N / cm and the partial discharge initiation voltage was 36 kV, which was slightly lower than that of Example 1, but still significantly better than that of the comparative example 5 (3.5 N / cm and 30 kV) without the coupling agent layer. The comprehensive performance of the equivalent cross-sectional area reduction ratios of 5% (Example 8) and 15% (Example 9) and the extreme values of the nodule diameter ratio (Examples 10 and 11) were all within acceptable ranges, providing experimental evidence for the rationality of the above numerical ranges.
[0071] (V) Synergistic Effect Analysis As shown in Table 1, there is a synergistic relationship between the TiC film and the coupling agent layer. When the TiC film is missing alone (Comparative Example 4), the contact resistance change rate is 12%, and the interface performance is acceptable (peel strength 8.5 N / cm, partial discharge 42 kV). When the coupling agent layer is missing alone (Comparative Example 5), the interface performance is severely degraded (peel strength 3.5 N / cm, partial discharge 30 kV), but the contact resistance change rate is still 3.8%. When both the TiC film and the coupling agent layer are missing simultaneously (Comparative Example 6), the contact resistance change rate increases to 15%, the peel strength decreases to 3.0 N / cm, and the partial discharge initiation voltage decreases to 28 kV. This indicates that the TiC film and the coupling agent layer work synergistically—the TiC film provides a low-resistance, oxidation-resistant conductive channel in the interlocking contact area, while the coupling agent layer establishes a chemical bonding interface between the conductor's outer arc surface and the insulation layer. The combination of these two elements gives the conductor-insulator interface system both excellent conductive contact and insulating interface bonding performance, achieving an overall effect that cannot be achieved by a single interface treatment method.
[0072] (vi) Overall effect In summary, Examples 1-11 outperform the comparative examples in terms of conductivity, contact stability, and insulation interface performance. Except for Example 6, which verifies the coupling agent layer thickness, the other examples reduce the DC resistance to 17.0-17.5 μΩ / m and the AC / DC ratio to 1.10-1.14, while controlling the contact resistance change rate after thermal cycling to 3.0%-4.8%, and achieving an interface peel strength of 8.2-9.2 N / cm. This indicates that this application, through the synergistic combination of rare-earth-graphene hybrid matrix material, serrated interlocking structure, TiC conductive conversion film, and titanate coupling agent transition layer, achieves stable operation with low AC resistance throughout the entire life cycle of large-section cables from three levels: material modification, structural design, and interface strengthening. This reduces line operating losses and achieves energy-saving goals.
[0073] The above description of the disclosed embodiments enables those skilled in the art to make or use this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An energy-saving power cable with an irregularly shaped conductor, characterized in that, It includes a central conductor layer and a cross-linked polyethylene insulation layer covering the outside of the central conductor layer; The central conductor layer is composed of multiple strands of irregularly shaped metal monofilaments twisted together in multiple layers; The metal shaped monofilament is prepared using rare earth modified oxygen-free copper or rare earth modified heat-resistant aluminum alloy, and rare earth-graphene hybrid nanoparticles are uniformly dispersed inside the matrix. The cross-section of the metal shaped monofilament is an asymmetric trapezoidal or arc-shaped variable cross-section structure, and adjacent layers of metal shaped monofilaments are interlocked and bonded to each other through serrated interlocking surfaces; The surface of the metal shaped monofilament is in situ coated with a titanium carbide conductive conversion film. A titanate coupling agent transition layer is provided between the titanium carbide conductive conversion film and the cross-linked polyethylene insulating layer. The titanate coupling agent transition layer is chemically bonded to the surface of the titanium carbide conductive conversion film and the cross-linked polyethylene insulating layer, respectively.
2. The energy-saving irregular-shaped conductor power cable according to claim 1, characterized in that, The outermost monofilament of the central conductor layer has a slightly convex arc surface, and the radius of curvature of the arc surface is adapted to the radius of curvature of the inner wall of the cross-linked polyethylene insulation layer.
3. The energy-saving irregular-shaped conductor power cable according to claim 1, characterized in that, The mass fraction of the rare earth-graphene hybrid nanoparticles in the metal matrix is 0.05% to 0.3%.
4. The energy-saving irregular-shaped conductor power cable according to claim 1, characterized in that, The thickness of the titanium carbide conductive conversion film is 50 nm to 200 nm, and the thickness of the titanate coupling agent transition layer is 5 nm to 50 nm.
5. The energy-saving irregular-shaped conductor power cable according to claim 1, characterized in that, Along the radial direction of the central conductor layer from the inside out, the equivalent cross-sectional area of the metal shaped monofilaments in each layer decreases in a gradient, with the decrease ratio of the equivalent cross-sectional area between adjacent layers being 5% to 15%.
6. A method for preparing an energy-saving power cable with an irregularly shaped conductor, used to prepare the energy-saving power cable with an irregularly shaped conductor as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1, high-purity copper liquid or aluminum liquid is melted under a protective atmosphere, rare earth-graphene intermediate alloy wire is added to it, and modified metal rod is prepared by continuous casting and rolling. S2, the modified metal rod is drawn through a continuous wire drawing machine in multiple passes, gradually drawn through a multi-pass transitional shaped wire drawing die, and then drawn into a shaped monofilament with a trapezoidal or arc-shaped cross section through an asymmetric shaped sizing die. S3, the irregular monofilament is continuously passed through the in-situ reaction chamber with built-in tetrabutyl titanate precursor, and a titanium carbide conductive conversion film is formed in-situ on the surface of the irregular monofilament. S4, the surface of the irregular monofilament with the titanium carbide conductive conversion film is coated with a tetrabutyl titanate coupling agent solution, and after drying and curing, a titanate coupling agent transition layer is formed. S5, multiple irregularly shaped monofilaments with titanium carbide conductive conversion film and titanate coupling agent transition layer are twisted in multiple layers, and radial compressive stress is applied at the converging mold, so that the irregularly shaped monofilaments in each layer are interlocked and pressed together by the sawtooth interlocking surface, thus obtaining the conductor. S6, the conductor is sequentially covered with a conductor shielding layer, a cross-linked polyethylene insulation layer, and an insulation shielding layer. After cross-linking treatment, the energy-saving irregular structure conductor power cable is obtained.
7. The preparation method according to claim 6, characterized in that, In step S1, the mass fraction of rare earth-graphene hybrid nanoparticles in the rare earth-graphene intermediate alloy wire is 1% to 5%, with the remainder being copper or aluminum.
8. The preparation method according to claim 6, characterized in that, In step S3, the temperature of the in-situ reaction chamber is 500℃~700℃, and the reaction time is 30s~120s.
9. The preparation method according to claim 6, characterized in that, In step S4, the concentration of the tetrabutyl titanate coupling agent solution is 0.5wt% to 5.0wt%.
10. The preparation method according to claim 6, characterized in that, In step S5, the twisting diameter ratio of each layer is: inner layer 18-25, middle layer 15-22, and outer layer 10-16.