Self-supporting electrode film and its manufacturing method
By using a dry process to prepare a self-supporting electrode film by coating carbon nanotubes on the surface of SiC active material particles, the problem of reduced electronic conductivity caused by the expansion and contraction of SiC active material particles was solved, thereby improving the capacity retention and electronic conductivity of the secondary battery.
Patent Information
- Application Number
- CN202610347696.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-03-20
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, the expansion and contraction of SiC active material particles during the fabrication of self-supporting electrode films leads to a decrease in electronic conductivity, which in turn affects the capacity retention rate of secondary batteries.
A self-supporting electrode film is prepared by coating the surface or vicinity of SiC active material particles with carbon nanotubes and using a dry process. This ensures the composite morphology of carbon nanotubes and SiC active material particles and suppresses the reduction in electronic conductivity caused by expansion and contraction.
It effectively suppressed the expansion and contraction of SiC active material particles, improved electronic conductivity, and enhanced the capacity retention and electronic conductivity of secondary batteries.
Smart Images

Figure CN123073010A_ABST
Abstract
Description
Technical Field
[0001] The technologies disclosed in this specification relate to self-supporting electrode films and their manufacturing methods. Background Technology
[0002] In recent years, self-supporting electrode films have begun to be manufactured using dry processes. For example, self-supporting electrode films containing polytetrafluoroethylene (PTFE) are known (US Patent Application Publication US2024 / 0105955). In US Patent Application Publication US2024 / 0105955, PTFE is used as the main binder, and a composite binder composed of polyvinylidene fluoride (PVDF) and polyethylene oxide (PEO) is used to improve adhesion performance. The method describes the preparation of a mixture of active material particles, conductive additives, and a composite binder, followed by applying shear force to fibrillate the PTFE, and then pressing to form a self-supporting electrode film.
[0003] For example, silicon-based active material particles such as SiC are sometimes used as negative electrode active material particles. Summary of the Invention
[0004] However, it was found that even when a self-supporting electrode film is fabricated using the method described in US Patent Application Publication US2024 / 0105955, there is a tendency for the electronic conductivity to decrease as the SiC active material particles expand and contract, resulting in a decrease in the capacity retention of the secondary battery with this self-supporting electrode film.
[0005] This specification provides a self-supporting electrode film that effectively suppresses the expansion and contraction of SiC active material particles, as well as the technique for manufacturing such a self-supporting electrode film.
[0006] The technology disclosed in this specification is embodied in a self-supporting electrode film.
[0007] The aforementioned self-supporting electrode film comprises carbon-based active material particles, SiC active material particles, carbon nanotubes that are predominantly present on or near the surface of the aforementioned SiC active material particles, and a first binder having a fibrillated morphology.
[0008] This self-supporting electrode film can contain SiC active material particles and carbon nanotubes in a form that is predominantly located on or near the surface of the SiC active material particles. Therefore, the carbon nanotubes effectively suppress the decrease in electronic conductivity that accompanies the expansion and contraction of the SiC active material particles. As a result, the capacity retention rate of the secondary battery equipped with this self-supporting electrode film can be suppressed.
[0009] The technology disclosed in this specification is also reflected in the manufacturing method of the self-supporting electrode film.
[0010] The above manufacturing method includes the following steps:
[0011] The solvent is removed from the mixture containing SiC active material particles, carbon nanotubes and solvent to prepare a first mixture containing composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes.
[0012] The first mixture, carbon-based active material particles, and fibrillable first binder are mixed by a dry process to prepare a second mixture;
[0013] The first binder in the second mixture is fibrillated to prepare a third mixture containing the first binder in a fibrillated form; and
[0014] The third mixture is pressurized and shaped to produce the self-supporting electrode membrane.
[0015] According to the manufacturing method of this self-supporting electrode film, at least a portion of the surface of SiC active material particles is coated with carbon nanotubes by solvent removal ("drying"), resulting in a first mixture containing composite SiC active material particles. This first mixture is prepared in advance, and then a second mixture is obtained by "drying," thereby maintaining the composite morphology of the composite SiC active material particles. Therefore, composite SiC active material particles are retained in the self-supporting electrode film. According to this manufacturing method, SiC active material particles and carbon nanotubes are contained in a morphology where at least a portion of the surface of the SiC active material particles is selectively coated with carbon nanotubes. As a result, a self-supporting electrode film containing carbon nanotubes in a morphology predominantly present on or near the surface of the SiC active material particles can be readily obtained. Attached Figure Description
[0016] The features, advantages, and technical and industrial significance of exemplary embodiments are described with reference to the accompanying drawings, wherein the same symbols denote the same elements.
[0017] Figure 1 This is a schematic diagram illustrating an example of a lithium-ion secondary battery cell.
[0018] Figure 2 This is a schematic diagram illustrating the structure of the self-supporting electrode film disclosed in this specification, and an enlarged view showing composite SiC active material particles.
[0019] Figure 3 This is a process diagram illustrating an example of a method for manufacturing a self-supporting electrode film.
[0020] Figure 4This is a graph showing the measurement results of the interface resistance between the self-supporting electrode film and the current collector in the embodiments and comparative examples.
[0021] Figure 5 This is a graph showing the measurement results of the DC resistance of the battery cells in the embodiments and comparative examples.
[0022] Figure 6 This is a graph showing the measurement results of the capacity retention rate of the battery cells of the embodiments and comparative examples. Detailed Implementation
[0023] The following description, with appropriate reference to the accompanying drawings, explains the vertical electrode film and its manufacturing method. It should be noted that this specification includes the following components.
[0024] [1] A self-supporting electrode film comprising: carbon-based active material particles; SiC active material particles; carbon nanotubes that are predominantly present on or near the surface of the SiC active material particles; and a first binder having a fibrillated morphology.
[0025] [2] According to the self-supporting electrode film of [1], it contains composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is covered by the carbon nanotubes.
[0026] [3] The self-supporting electrode film according to [1] or [2], wherein the first adhesive comprises polytetrafluoroethylene.
[0027] [4] A lithium-ion secondary battery comprising, as any one of [1] to [3], a self-supporting electrode film as a negative electrode film.
[0028] [5] A method for manufacturing a self-supporting electrode film, comprising the following steps:
[0029] The solvent is removed from the mixture containing SiC active material particles, carbon nanotubes and solvent to prepare a first mixture containing composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes.
[0030] The first mixture, carbon-based active material particles, and fibrillable first binder are mixed by a dry process to prepare a second mixture;
[0031] The first binder in the second mixture is fibrillated to prepare a third mixture containing the first binder in a fibrillated form; and
[0032] The third mixture is pressurized and shaped to produce the self-supporting electrode membrane.
[0033] [6] According to the manufacturing method described in [5], the step of preparing the first mixture includes: mixing the SiC active material particles with a paste formed by dispersing the carbon nanotubes in the solvent to obtain the mixture.
[0034] It should be noted that, in this specification, the self-supporting electrode film is, for example, a self-supporting electrode film constituting the negative electrode of a lithium-ion secondary battery. A self-supporting electrode film is an electrode film in which active material particles are entangled using a fibrillated binder, thereby enabling it to support itself.
[0035] Self-supporting electrode film
[0036] Figure 1 This is a schematic diagram illustrating an example of a battery cell 2 of a lithium-ion secondary battery (hereinafter referred to as a secondary battery) 100. Figure 1 As shown, the battery cell 2, which is the unit structure of the secondary battery 100, includes a positive electrode 4, a separator 10, and a negative electrode 12. The secondary battery 100 typically has a structure consisting of two or more battery cells 2 stacked together.
[0037] The positive electrode 4 may contain known positive electrode active materials, conductive additives, and binders in the positive electrode layer 6. The positive electrode layer 6 is not particularly limited; for example, it may be a self-supporting electrode film made using a fibrillable binder as at least part of the binder. The positive electrode layer 6 may, as appropriate, include a positive electrode current collector 8.
[0038] The membrane 10 can, for example, hold a liquid or gel-like electrolyte. The membrane 10 is made of known materials such as a polyolefin microporous membrane with fine pores. The membrane 10 is impregnated with a liquid electrolyte containing lithium salts such as lithium hexafluorophosphate, using organic solvents such as ethylene carbonate (EC), dimethyl carbonate (DMC), or diethyl carbonate (DEC) as a medium. It should be noted that a solid electrolyte layer can also be used instead.
[0039] The negative electrode 12 has a self-supporting electrode film 14, which includes carbon-based active material particles 20, SiC active material particles 22, and carbon nanotubes 24 (or composite SiC active material particles 26), as well as a first binder 28. The self-supporting electrode film (hereinafter also referred to as the electrode film) 14 may appropriately include a negative electrode current collector 16 as needed.
[0040] Carbon-based active material particles
[0041] As the carbon-based active material particle 20, known carbon-based active material particles can be used. Examples include natural graphite, artificial graphite, soft carbon, and hard carbon. The carbon-based active material particle 20 exhibits stable charge-discharge characteristics. The content of the carbon-based active material particles in the electrode film 14 is not particularly limited. For example, it is 20% by mass or more and 80% by mass or less relative to the total mass of all materials constituting the electrode film 14 (carbon-based active material particles 20, SiC active material particles 22, CNT 24, and the first binder 28, etc.). Alternatively, it can be 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, and 70% by mass or more. Furthermore, it can be 80% by mass or less, 70% by mass or less, 60% by mass or less, and 50% by mass or less. In addition to the above ranges, the content range of the carbon-based active material particles can also be set by appropriately combining the above upper and lower limits. The content range of carbon-based active material particles is, for example, 40% by mass or more and 80% by mass or less, 50% by mass or more and 80% by mass or less, 60% by mass or more and 80% by mass or less, 70% by mass or more and 80% by mass or less, etc. Furthermore, although not specifically limited, it can be set to an average particle size of 1 μm or more and 50 μm or less, or 5 μm or more and 20 μm or less, as determined by laser diffraction / scattering methods.
[0042] SiC active material particles and carbon nanotubes, CNTs
[0043] like Figure 2 As shown, the electrode film 14 contains SiC active material particles 22 and CNTs 24 in a form where CNTs 24 are predominantly present on or near the surface of the SiC active material particles 22. CNTs 24 can possess high electronic conductivity, high strength, and high surface area. Unlike conventional methods, CNTs 24 are not uniformly dispersed throughout the electrode film 14 in a manner that, for example, forms a network. This effectively suppresses the decrease in electronic conductivity that sometimes accompanies the expansion and contraction of the SiC active material particles 22.
[0044] The SiC active material particle 22 can be any SiC active material particle, such as β-SiC active material particles, or doped with nitrogen, phosphorus, or other atoms. Doped SiC active material particles sometimes exhibit excellent conductivity and lithium-ion conductivity. The shape of the SiC active material particle 22 is not particularly limited, and particles of known shapes can be used appropriately. Examples of SiC active material particles include amorphous particles and whiskers. The average particle size of the SiC active material particle 22 can be appropriately set considering factors such as mixability and recombination with CNT24 (described later). Although not particularly limited, it can be set to an average particle size of 1 μm or more and 50 μm or less, or 5 μm or more and 20 μm or less, as measured by laser diffraction / scattering. The SiC active material particle 22 is sometimes preferably amorphous. Recombination will be explained later.
[0045] Examples of CNT24 include single-walled carbon nanotubes (SW-CNTs) and multi-walled carbon nanotubes (MW-CNTs) that include double-walled carbon nanotubes (DW-CNTs). These CNTs can be used individually or in combination of two or more. The average particle size of the CNT24 can be appropriately set considering factors such as mixability and composite composition with SiC active material particles 22.
[0046] Composite SiC active material particles
[0047] In the electrode film 14, as a way to predominantly contain CNT 24 on or near the surface of the SiC active material particles 22, the electrode film 14 includes composite SiC active material particles 26, which have a composite morphology in which at least a portion of the surface of the SiC active material particles 22 is coated with CNT 24. The composite SiC active material particles 26 are then placed in... Figure 2 The image is enlarged in the middle.
[0048] In the electrode film 14 containing composite SiC active material particles 26, CNTs 24 are distributed alongside SiC active material particles 22, and are selectively distributed with a greater emphasis on the surface of the SiC active material particles 22. By incorporating composite SiC active material particles 26, the reduction in electronic conductivity that sometimes accompanies the expansion and contraction of the SiC active material particles 22 can be more effectively suppressed.
[0049] In the composite SiC active material particles 26, CNT24 only needs to coat a portion of the surface of the SiC active material particles 22, but it can also coat the entire surface. It should be noted that, in the case where CNT24 that is not composited with the SiC active material particles 22 is also included, this CNT24 is uniformly dispersed throughout the entire electrode film 14.
[0050] The content of SiC active material particles 22 in the electrode film 14 is not particularly limited. For example, it is 5% by mass or more and 60% by mass or less relative to the total mass of the materials constituting the electrode film 14. Other examples include 10% by mass or more, 15% by mass or more, 20% by mass or more, 30% by mass or more, and 40% by mass or more. Furthermore, it is 55% by mass or less, 50% by mass or less, 45% by mass or less, and 40% by mass or less. In addition to the above, the content range of composite SiC active material particles 26 can also be set to 15% by mass or more and 50% by mass or less, 15% by mass or more and 40% by mass or less, 15% by mass or more and 25% by mass or less, and 15% by mass or more and 20% by mass or less.
[0051] The content of CNT24 in the electrode film 14 is not particularly limited, and can be set to 0.05% by mass or more and 3.0% by mass or less, 0.05% by mass or more and 2.5% by mass or less, 0.05% by mass or more and 1.5% by mass or less, etc. It should be noted that the mass ratio of CNT24 to SiC active material particles 22 is not particularly limited. Regarding the mass ratio of CNT24 to SiC active material particles 22, for example, relative to 100 parts by mass of SiC active material particles 22, CNT24 can be 1 part by mass or more and 4 parts by mass or less, 1 part by mass or more and 3 parts by mass or less, or 1 part by mass or more and 2 parts by mass or less.
[0052] The content of the composite SiC active material particles 26 in the electrode film 14 is not particularly limited. For example, it is 5% by mass or more and 60% by mass or less relative to the total mass of the materials constituting the electrode film 14. Other examples include 10% by mass or more, 15% by mass or more, 20% by mass or more, 30% by mass or more, and 40% by mass or more. Furthermore, it is 55% by mass or less, 50% by mass or less, 45% by mass or less, and 40% by mass or less. In addition to the above, the content range of the composite SiC active material particles 26 can also be set to 15% by mass or more and 50% by mass or less, 15% by mass or more and 40% by mass or less, 15% by mass or more and 25% by mass or less, 15% by mass or more and 20% by mass or less, etc.
[0053] It should be noted that the mass ratio of CNT24 to SiC active material particles 22 in the composite SiC active material particles 26 is the same as previously stated. Even in the electrode film 14 containing composite SiC active material particles 26, there are cases where SiC active material particles 22 and CNT24 are not completely composited. The total mass of composite SiC active material particles 26, SiC active material particles 22, and CNT24 can be expressed as a mass ratio equal to the content of composite SiC active material particles 26.
[0054] It should be noted that the electrode film 14 may also contain active material particles other than carbon-based active material particles 20 and composite SiC active material particles 26. Although there are no particular limitations, particles such as Si, SiO, tin oxide, and lithium titanate can be listed as active material particles.
[0055] In addition, the electrode film 14 may also contain known conductive additives other than CNTs as conductive additives. Examples of conductive additives include graphene, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal cracking black.
[0056] First adhesive
[0057] The first binder 28 is a polymer having a fibrillated morphology (hereinafter also simply referred to as fibrillated morphology) in the electrode film 14. The first binder 28 is derived from a fibrillable polymer. When a specified shear force is applied to the fibrillable polymer, fibrillation occurs, that is, the initial polymer is refined and becomes fibrous. As a result, the polymer having a fibrillated morphology can form a network. Therefore, the polymer having a fibrillated morphology can entwine and constrain the active material particles in a fibrous manner, thereby imparting mechanical strength and contributing to the self-supporting property of the self-supporting electrode film. It should be noted that in Figure 2 In the diagram, the first adhesive 28 and the second adhesive 30, which will be described later, are shown in simplified form.
[0058] As the first binder 28, there are no particular limitations, and any known fibrillable polymer can be used. Examples of fibrillable polymers include polytetrafluoroethylene (PTFE), polyolefins, polyalkylene compounds, polyethers, styrene-butadiene, polysiloxanes and copolymers of polysiloxanes, branched polyethers, polyvinyl ethers, and copolymers thereof. Furthermore, cellulose containing carboxyl cellulose such as carboxymethyl cellulose (CMC) can also be used. One or more of these can be used as the fibrillating polymer. For example, PTFE is sometimes preferred as the fibrillating polymer because it exhibits excellent fibrillability and binder properties.
[0059] The content of the first binder 28 in the electrode film 14 is not particularly limited, as long as it can bind the constituent materials of the electrode film 14 and integrate them. The content of the first binder 28 is, for example, 1.0% by mass or more and 10% by mass or less relative to the total mass of the materials constituting the electrode film 14. Furthermore, it is, for example, 1.5% by mass or more, 2.0% by mass or more, 2.5% by mass or more, 3.0% by mass or more, and 4.0% by mass or more. And, it is 9.0% by mass or less, 8.0% by mass or less, 7.0% by mass or less, 6.0% by mass or less, 5.0% by mass or less, 4.5% by mass or less, and 3.5% by mass or less. The content range of the first binder 28 can be set by appropriately combining these lower and upper limits, in addition to the above ranges. For example, it is 1.5% by mass or more and 4.5% by mass or less, 2.0% by mass or more and 4.0% by mass or less, and 2.5% by mass or more and 3.5% by mass or less.
[0060] Second adhesive
[0061] The electrode film 14 may contain a second binder 30 as needed. The second binder 30 is added to the first binder 28 as needed and is included in the electrode film 14. The second binder 30 is a polymer that does not undergo fibrillation. The second binder 30 is used from the viewpoint of binder performance and lithium-ion conductivity. There are no particular limitations on the second binder 30, and examples include polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polypropylene oxide, polyacrylonitrile, polyvinyl chloride, polymethyl methacrylate, ethylene carbonate, polyethylene, polypropylene, polystyrene, ABS resin, polyacrylate, polymethyl methacrylate, polyvinyl alcohol, and polycarbonate. One or more of these can be used.
[0062] The content of the second binder 30 in the electrode film 14 is not particularly limited, and can be determined as needed from the viewpoint of binder performance and lithium-ion conductivity. For example, the content of the second binder 30 is 1.0% by mass or more and 10% by mass or less relative to the total mass of the material constituting the electrode film 14 containing the first binder 28 described above. Alternatively, it may be 1.5% by mass or more, 2.0% by mass or more, 2.5% by mass or more, 3.0% by mass or more, or 4.0% by mass or more. Furthermore, it may be 9.0% by mass or less, 8.0% by mass or less, 7.0% by mass or less, 6.0% by mass or less, 5.0% by mass or less, 4.5% by mass or less, or 3.5% by mass or less. The content range of the second binder 30 can be set by appropriately combining these lower and upper limits, in addition to the ranges described above. For example, it may be 1.5% by mass or more and 4.5% by mass or less, or 2.0% by mass or more and 4.0% by mass or less.
[0063] It should be noted that, sometimes, the total amount of the first binder 28 and the second binder 30 is preferably 10% by mass or less relative to the total mass of the materials constituting the electrode film 14. Alternatively, it can be 9% by mass or less, 8% by mass or less, 7% by mass or less, or 6% by mass or less.
[0064] It should be noted that, in addition to the above, the electrode film 14 may also contain a polymer that functions as a binder, as needed. For example, known polymers suitable for use in this electrode film, other than the first binder 28 and the second binder 30 described above, can be used. The electrode film 14 described above may, for example, have a thickness of several μm or more and approximately 2000 μm or less.
[0065] According to this electrode film 14, since it contains composite SiC active material particles 26, the expansion and contraction of the SiC active material particles 22 during charging and discharging can be effectively suppressed, and the decrease in the electronic conductivity of the SiC active material particles 22 can be suppressed. As a result, the decrease in the capacity retention rate of the secondary battery 100 equipped with this electrode film 14 can be suppressed. In addition, the SiC active material particles 22 can sometimes contribute to high capacity.
[0066] It should be noted that, as described below, the electrode film 14 is preferably manufactured by "drying" and a "dry process". Such an electrode film 14 is completely solvent-free or substantially solvent-free.
[0067] Additionally, according to this specification, a secondary battery 100 having the electrode film 14 can also be provided.
[0068] Method for manufacturing self-supporting electrode films
[0069] Next, refer to the appropriate Figure 3 A suitable method for manufacturing the electrode film 14 will be described. The manufacturing method includes a step S10 for preparing a first mixture, a step S20 for preparing a second mixture, a step S30 for preparing a third mixture, and a step S40 for manufacturing a self-supporting electrode film 14.
[0070] Step S10 for preparing the first mixture
[0071] Step S10 is a step of preparing a first mixture containing composite SiC active material particles 26 by removing the solvent from a mixture containing SiC active material particles 22, CNT 24, and a solvent. The composite SiC active material particles 26 have a composite morphology in which at least a portion of the surface of the SiC active material particles 22 is coated with CNT 24. In step S10, the solvent is removed from the mixture containing SiC active material particles 22, CNT 24, and a solvent by any method (“drying”). Therefore, a composite morphology in which the surface of the SiC active material particles 22 is coated with CNT 24 can be formed, thereby obtaining a first mixture containing composite SiC active material particles 26.
[0072] The mixture contains no or substantially no carbon-based active material particles 20, the first binder 28, and the second binder 30. Here, "substantially no" means completely free of the material or containing only an amount of the material insufficient to fulfill its technical significance. By omitting carbon-based active material particles 20, the first binder 28, etc., CNT24 can be composited in a manner that selectively coats the surface of SiC active material particles 22.
[0073] As the SiC active material particles 22 and CNT 24 used in process S10, various types of SiC active material particles 22 and CNT 24 as described with respect to electrode film 14 can be used. The sizes of SiC active material particles 22 and CNT 24 are chosen to allow CNT 24 to coat the surface of SiC active material particle 22. Furthermore, SiC active material particles 22 and CNT 24 can be used in the mass ratio described above.
[0074] There are no particular limitations on the solvent used, as long as it can disperse CNT24. For example, aprotic polar solvents such as N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), and dimethyl sulfoxide (DMSO) can be used appropriately. Additionally, polar solvents such as water and lower alcohols can also be used. Furthermore, suitable mixtures of these solvents can also be used.
[0075] The solvent is used in an amount sufficient to disperse CNT24 to the extent that it can coat the surface of the SiC active material particles 22. The solvent can also be used, for example, as a solvent for a CNT paste in which CNT24 has been pre-dispersed and held. In step S10, a mixture can be prepared by mixing the SiC active material particles 22 with the paste formed by dispersing CNT24 in the solvent. This allows for the supply of well-dispersed CNT24 to the SiC active material particles 22, resulting in the easy realization of a composite coating of CNT24 on the surface of the SiC active material particles 22.
[0076] In the preparation of such a mixture, a known mixer can be appropriately used. Drying is performed to remove the solvent from the mixture (“drying”) in a manner that maintains the composite morphology of the SiC active material particles 22 and CNT24. For example, as a drying method, from the viewpoint of maintaining the composite morphology, it is sometimes preferable to use conduction drying, radiation drying, and vacuum drying alone or in combination of two or more methods. The resulting first mixture is then appropriately crushed.
[0077] Step S20 for preparing the second mixture
[0078] Step S20 is a process of preparing a second mixture by mixing the aforementioned first mixture, carbon-based active material particles 20, and fibrillable first binder 28 using a "dry process." In this step, the carbon-based active material particles 20, SiC active material particles 22, CNT 24, and first binder 28 in the first mixture can be used in such a way that the aforementioned mass ratio is achieved relative to the materials constituting the electrode film 14. If a second binder 30 is used, it can be added in this step.
[0079] "Dry process" refers to a process that is carried out without or substantially without solvent. By employing a "dry process," it is possible to maintain the composite state in which CNT24 constituting the composite SiC active material particles 26 obtained in step S10 still coats the surface of the SiC active material particles 22. This is because, in a "wet process" using solvents, CNT24 would redisperse into the solvent, making it difficult to selectively coat the surface of the SiC active material particles 22.
[0080] In the preparation of the second mixture, a known mixer can be appropriately used. It should be noted that the second mixture can be mixed in a manner that maintains the composite SiC active material particles 26. Furthermore, in order to uniformly disperse the fibrillable first binder 28, mixing can be carried out under conditions where fibrillation of the first binder 28 does not occur. Such mixing conditions can be appropriately set by those skilled in the art.
[0081] Step S30 for preparing the third mixture
[0082] Step S30 is a step of preparing a third mixture by fibrillating the first binder 28 in the second mixture. The third mixture contains the first binder 28 in a fibrillated form. With the fibrillation of the first binder 28, the first binder 28 becomes a network with the ability to constrain carbon-based active material particles 20, composite SiC active material particles 26, etc. Therefore, the third mixture can form a self-supporting film by pressing and shaping. It should be noted that step S30 is a "dry process" that does not use or substantially does not use solvents.
[0083] The shear force and other conditions used for fibrillating the first adhesive 28 are known to those skilled in the art, and they can appropriately set the conditions for fibrillating the first adhesive 28. For example, fibrillating the first adhesive 28 can be achieved by mixing a third mixture using a known mixer such as a kneader.
[0084] Step S40 for fabricating the electrode film
[0085] Step S40 is a step of pressing and shaping the third mixture to produce the electrode film 14. By pressing and shaping, a self-supporting electrode film 14 can be obtained. Regarding pressing and shaping, for example, a compression calendering device such as a roller press can be used for film formation. It should be noted that the electrode film 14 can be cut, etc., as needed.
[0086] The resulting electrode film 14 contains composite SiC active material particles 26, and therefore exhibits a selectively greater presence (predominant presence) of CNTs 24 on or near the surface of the SiC active material particles 22. Consequently, the expansion and contraction of the SiC active material particles 22 during charging and discharging is suppressed by the CNTs 24, thereby preventing a decrease in the electronic conductivity of the SiC active material particles 22. Furthermore, due to the use of a "drying" and "dry process," the electrode film 14 contains no or is substantially free of solvents.
[0087] Using the self-supporting electrode film 14 obtained in this way, a secondary battery 100 is fabricated, which includes other components of a secondary battery 100, a negative current collector 16, a positive electrode 4, and a separator 10. The secondary battery 100 can be fabricated into various known forms of secondary batteries using known winding methods, stacking methods, etc.
[0088] According to this secondary battery 100, since the electrode film 14 contains composite SiC active material particles 26, the expansion and contraction of the SiC active material particles 22 during charging and discharging is suppressed by CNTs 24. As a result, the decrease in the electronic conductivity of the SiC active material particles 22 can be suppressed. Furthermore, the CNTs also ensure the conductive path. As a result, the decrease in the capacity retention rate of the secondary battery 100 during charging and discharging can be suppressed.
[0089] The above description mainly focuses on the electrode film 14, the secondary battery 100, and the manufacturing method of the electrode film 14. However, according to this specification, the composite SiC active material particles 26 used for the electrode film 14 can be provided as active material particles for self-supporting electrode films. Furthermore, the first mixture, the second mixture, and the third mixture containing the composite SiC active material particles 26 can each be provided as composite materials for self-supporting electrode films.
[0090] Furthermore, while the above description describes a method for manufacturing a self-supporting electrode film such as electrode film 14, a method for manufacturing composite SiC active material particles 26 can also be provided. According to step S10 of preparing the first mixture, a first mixture containing composite SiC active material particles 26 can be obtained.
[0091] Furthermore, according to this specification, a method for preparing a composite material for an electrode film as a second or third mixture can also be provided. Furthermore, based on each step in the method for manufacturing the self-supporting electrode film 14, a method for manufacturing a negative electrode 12 using the self-supporting electrode film 14 can also be provided. Furthermore, a method for manufacturing a secondary battery 100 including a manufacturing step for using this battery to manufacture a secondary battery 100 can also be provided.
[0092] According to this specification, in addition to the above-mentioned [1] to [6] configurations, the following configurations are also included.
[0093] [7] An active material particle for a self-supporting electrode film, comprising composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes.
[0094] [8] A composite material for a self-supporting electrode film, comprising composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes.
[0095] [9] The self-supporting electrode film composite material according to [8] further comprises carbon-based active material particles and a fibrillable first binder.
[0096]
[10] The self-supporting electrode film composite material according to [9] further comprises a second binder that does not undergo fibrillation.
[0097]
[11] The self-supporting electrode film composite material according to [9] or
[10] , wherein the first binder has a fibrillated morphology.
[0098] The following describes embodiments that embody the disclosure of this specification, but these embodiments are only for illustrating the disclosure of this specification and are not intended to limit it.
[0099] In this embodiment, a self-supporting electrode film for the negative electrode of a lithium-ion secondary battery was fabricated using the following method, and then an evaluation electrode and an evaluation battery cell were fabricated, and the electrode and battery cell were evaluated.
[0100] In the self-supported electrode film, graphite particles (average particle size 10 μm) and SiC active material particles (amorphous, average particle size 10 μm) are used as the active material particles of the negative electrode film. Furthermore, CNTs are used as a conductive additive, PTFE as a fibrillable binder, and PVDF as a non-fibrillable binder. The mass ratio of these components in the negative electrode film (graphite:SiC:CNT:PTFE:PVDF) is set to 75.4:18.8:3.0:2.5.
[0101] (1) Preparation of the first mixture
[0102] First, SiC active material particles and a CNT paste containing CNTs dispersed in NMP were mixed using a mixer (2000 rpm, 5 minutes) to achieve the aforementioned mass ratio of SiC active material particles to CNTs. Then, the mixture was dried on a hot plate at 120°C for 1 hour, followed by vacuum drying at 80°C for 8 hours. The resulting dried product is the first mixture described in this specification. Observation of the first mixture confirmed that the CNTs were coated around the surface of the SiC active material particles.
[0103] (2) Preparation of the second mixture
[0104] Graphite, PTFE, and PVDF were added to the first mixture in the manner described above in terms of mass ratio. The mixture was then mixed at 300 rpm for 180 seconds and then at 3000 rpm for 8 minutes to obtain the second mixture.
[0105] (3) Preparation of the third mixture
[0106] The second mixture was mixed at 10 rpm for 180 seconds at 100°C using an intermittent kneader to fibrillate the PTFE, resulting in the third mixture.
[0107] (4) Fabrication of self-supporting electrode film
[0108] The third mixture is calendered using a roller press to produce a self-supporting electrode film.
[0109] It should be noted that graphite, SiC active material particles, CNTs, PTFE, and PVDF were mixed together using a dry process without the use of solvents. Then, the PTFE was fibrillated, and otherwise, the self-supporting electrode film of the comparative example was fabricated in the same manner as described above.
[0110] For these self-supporting electrode films, at 0.2 t / cm 2 The copper foil (8 μm thick) was flattened under load to fabricate the electrodes (negative electrodes) for the examples and comparative examples. Then, evaluation battery cells were fabricated using conventional methods.
[0111] Electrode Evaluation
[0112] Electrode evaluation was performed using an electrode resistance measurement system (HIOKI RM2610) to measure the interfacial resistance between the electrode film and foil. The results are shown below. Figure 4 .
[0113] Battery cell evaluation
[0114] The impedance of the evaluation battery cells was measured at 50% SOC, and the DC resistance was calculated. The results are presented below. Figure 5 Furthermore, the charging and discharging capacities were measured using a 1 / 10C CCCV (constant current constant voltage) charge. The voltage range was set to 3.0V to 4.25V, and the number of cycles was set to 6. The ratio of the discharging capacity to the initial charging capacity (capacity retention rate) was calculated. The results are presented below. Figure 6 .
[0115] like Figure 4 As shown, compared to the electrode of the comparative example, the electrode film and foil of the embodiment exhibit reduced interfacial resistance. Furthermore, as... Figure 5 As shown, the DC resistance of the battery cell in the embodiment is also reduced compared to the battery cell in the comparative example. From these results, it can be said that the electronic conductivity introduced by the SiC active material particles contributes to the reduction in the resistance of the electrode film in the embodiment.
[0116] In the fabrication of the self-supporting electrode film in this embodiment, a dry process was employed using SiC active material particles with CNTs coated on their surface. In contrast, the self-supporting electrode film of the comparative example employed a dry process in which CNTs were simultaneously mixed with other electrode materials. Therefore, it can be said that the dispersion morphology of CNTs in these self-supporting electrode films differs. In the self-supporting electrode film of this embodiment, by using CNTs to composite SiC active material particles, CNTs can be selectively concentrated on or near the surface of the SiC active material particles. Therefore, the electronic conductivity of the SiC active material particles can be improved, resulting in a reduction in the resistance of the self-supporting electrode film.
[0117] In addition, such as Figure 6 As shown, the battery cell of the embodiment improves capacity retention compared to the battery cell of the comparative example. In the self-supporting electrode film of the embodiment, since CNTs are selectively distributed on or near the surface of SiC active material particles, the interruption of conduction pathways caused by the expansion and contraction of SiC during charging and discharging can be suppressed, thus improving capacity retention.
[0118] The technical elements described in this specification or drawings, whether individually or in various combinations, possess technical utility and are not limited to the combinations listed in the claims at the time of application. Furthermore, the technologies illustrated in this specification or drawings can achieve multiple objectives simultaneously, and achieving any one of these objectives is itself technically practical.
Claims
1. A self-supporting electrode film, comprising: Carbon-based active material particles; SiC active material particles; Carbon nanotubes, which are predominantly present on or near the surface of the SiC active material particles; and The first adhesive having a fibrillated morphology.
2. The self-supporting electrode film according to claim 1, comprising composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes.
3. The self-supporting electrode film according to claim 2, wherein, The first adhesive contains polytetrafluoroethylene.
4. A lithium-ion secondary battery comprising a self-supporting electrode film as described in any one of claims 1 to 3 as a negative electrode film.
5. A method for manufacturing a self-supporting electrode film, comprising the following steps: The solvent is removed from a mixture containing SiC active material particles, carbon nanotubes and a solvent to prepare a first mixture containing composite SiC active material particles, wherein the composite SiC active material particles have a composite morphology in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes. The first mixture, carbon-based active material particles, and a fibrillable first binder are mixed by a dry process to prepare a second mixture; The first adhesive in the second mixture is fibrillated to prepare a third mixture containing the first adhesive in a fibrillated form; and The third mixture is pressurized and shaped to produce the self-supporting electrode membrane.
6. The manufacturing method according to claim 5, wherein, The steps for preparing the first mixture include: The SiC active material particles are mixed with a paste formed by dispersing the carbon nanotubes in the solvent to obtain the mixture.
Citation Information
Patent Citations
Dry energy storage device electrode and methods of making the same
US20240105955A1