A positive electrode sheet, a preparation method, a sodium secondary battery, and an electrical device.
By using a sodium-supplemented composite material in the positive electrode of a sodium secondary battery, the problem of poor high-temperature cycle performance of sodium secondary batteries is solved, thereby improving the energy density and cycle performance of the battery and making it suitable for different application scenarios.
Patent Information
- Application Number
- CN202611510441.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2026-11-10
AI Technical Summary
Existing sodium-ion batteries have poor high-temperature cycle performance and exhibit high-temperature gas generation, which limits their further application.
Sodium-supplemented composites are used as components of the positive electrode. The sodium-supplemented composites include a core and a coating layer. The core is composed of sodium nitride, sodium phosphide, sodium peroxide, sodium oxide, etc., and the coating layer is composed of aluminum oxide, magnesium oxide, zirconium oxide, etc. A stable structure is formed by sintering, which improves the stability of the sodium-supplementing agent and the energy density and cycle performance of the battery.
It improves the battery's initial efficiency and cycle performance, reduces the residual alkali content of the sodium replenisher during the sintering process, and enhances the chemical stability of the sodium replenisher, making it suitable for different application scenarios.
Smart Images

Figure CN123073022A_ABST
Abstract
Description
[0001] This application is based on the divisional application of the application with the application number 202311425744.3, the application date of October 31, 2023, the applicant of Ningde era new energy technology Co., Ltd., and the invention name of "a positive electrode sheet, a preparation method, a sodium secondary battery and an electric device". TECHNICAL FIELD
[0002] The present application relates to the technical field of secondary batteries, in particular to a positive electrode sheet, a preparation method, a sodium secondary battery and an electric device. BACKGROUND
[0003] With the development of battery technology, lithium secondary batteries dominate the portable electronic market and gradually expand to large-scale electric energy storage application fields. However, due to the existing lithium resources cannot meet the urgent needs of establishing large-scale and high-energy density energy storage systems. Therefore, sodium secondary batteries with abundant sodium reserves, low cost and similar electrochemical characteristics to lithium secondary batteries have emerged. However, the current widely studied sodium secondary batteries have poor high-temperature cycle performance and are accompanied by serious high-temperature gas production, which greatly limits the further application of sodium secondary batteries. SUMMARY
[0004] The present application is carried out in view of the above-mentioned problems, and the purpose is to provide a positive electrode sheet and a preparation method thereof, the sodium supplementing compound included in the positive electrode sheet has good stability, and the energy density and cycle performance of the battery can be significantly improved after adding the sodium supplementing compound.
[0005] In order to achieve the above-mentioned purpose, the first aspect of the present application provides a positive electrode sheet, the positive electrode sheet includes a positive electrode film layer, the positive electrode film layer includes a sodium supplementing compound, the sodium supplementing compound includes a core and at least one coating layer coated on the core; the core includes a sodium supplementing agent, the sodium supplementing agent includes at least one of sodium nitride, sodium phosphide, sodium peroxide, sodium oxide and sodium carbonate; the coating layer includes an oxide, the oxide includes at least one of aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, silicon oxide, boron oxide, lanthanum oxide, cerium oxide and bismuth oxide.
[0006] In any embodiment, the oxide includes at least one of lanthanum oxide, cerium oxide and bismuth oxide.
[0007] In any embodiment, the sodium supplementing agent includes sodium nitride.
[0008] The sodium supplement compound provided in the application can effectively protect the sodium supplement agent in the inner core part, the mixed new product has a stable structure, improves the stability of the sodium supplement agent in the air, and reduces the residual alkali content of the sodium supplement agent in the sintering process, thereby effectively improving the initial efficiency and cycle performance of the battery. In addition, the sodium supplement compound provided in the application can be combined and matched with various different oxides and sodium supplement agents, and thus can be applied to different application scenarios.
[0009] In any embodiment, the mass ratio of the sodium supplement agent to the oxide is (40-99):(1-50).
[0010] In any embodiment, the mass ratio of the sodium supplement agent to the oxide is (40-90):(5-10).
[0011] Due to different application scenarios, a certain mass ratio needs to be adopted when the oxide is combined and matched with the sodium supplement agent. When the above ratio is adopted, the stability of the sodium supplement agent can be effectively improved, and good sodium supplement effect is also achieved.
[0012] In any embodiment, the Dv50 of the sodium supplement agent is 2-5 μm, and the Dv50 of the oxide is 15-50 nm.
[0013] In the sodium supplement compound, the sodium supplement agent and the oxide with the above Dv50 range are beneficial to reduce polarization, improve capacity, and improve the adaptability to the particle size of the positive electrode material.
[0014] In any embodiment, the oxide includes at least one of aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide; or the oxide includes at least one of silicon oxide, boron oxide; or the oxide includes at least one of lanthanum oxide, cerium oxide, bismuth oxide.
[0015] The type of the oxide can be selected according to different application scenarios. When a metal oxide such as aluminum oxide, magnesium oxide, zirconium oxide, or titanium oxide is adopted, good electrical conductivity is achieved; when a non-metal oxide such as silicon oxide or boron oxide is adopted, good structural stability is achieved; and when a rare earth metal oxide such as lanthanum oxide, cerium oxide, or bismuth oxide is adopted, the rare earth metal elements in the oxide form a heterostructure interface, which can effectively reduce the resistance of electron migration and increase the electron mobility.
[0016] In any embodiment, the sodium supplement compound includes the inner core, a first coating layer coated on the inner core, and a second coating layer coated on the first coating layer; the first coating layer includes at least one of aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, lanthanum oxide, cerium oxide, and bismuth oxide; and the second coating layer includes at least one of silicon oxide and boron oxide.
[0017] In any embodiment, the first coating layer comprises at least one of lanthanum oxide, cerium oxide, bismuth oxide.
[0018] When the sodium supplementing compound has multiple coating layers, the sodium supplementing effect is better, and the energy density of the battery can be further improved. Meanwhile, different coating layers have different technical effects, for example, the first coating layer is a metal oxide, which can provide better electrical conductivity; the second coating layer is a non-metal oxide, which can provide better structural stability; when the sodium supplementing agent with the above two coating layers is used in the positive electrode sheet, the chemical stability and ion transmission capacity can be improved, thereby effectively improving the initial efficiency and cycle performance of the battery.
[0019] In any embodiment, the mass content of the sodium supplementing compound is 0.3% to 2% based on the total mass of the positive electrode film layer.
[0020] In any embodiment, the mass content of the sodium supplementing compound is 1.0% to 1.6% based on the total mass of the positive electrode film layer.
[0021] A certain mass ratio of the sodium supplementing compound needs to be used in the positive electrode sheet. When the sodium supplementing compound with the above ratio is used, not only the sodium supplementing effect is good, but also the battery has good cycle performance.
[0022] In any embodiment, the positive electrode film layer further comprises a positive electrode active material, and the positive electrode active material comprises at least one of a layered transition metal oxide, a polyanion compound, and a Prussian blue compound.
[0023] In any embodiment, the positive electrode film layer further comprises a conductive agent, and the conductive agent comprises at least one of Ketjen black, Super P, acetylene black, carbon black, carbon nanotube, natural graphite, artificial graphite, and carbon nanofiber.
[0024] In any embodiment, the mass ratio of the sodium supplementing compound to the conductive agent is (23-150):(10-50).
[0025] When the mass ratio of the sodium supplementing compound to the conductive agent is within a certain range, the electrical conductivity can be further improved.
[0026] The second aspect of the present application further provides a method for preparing the positive electrode sheet of the first aspect of the present application, the method comprising: uniformly mixing raw materials comprising a sodium supplementing agent and an oxide to obtain a precursor; sintering the precursor in a nitrogen atmosphere to obtain a sodium supplementing compound; and using the sodium supplementing compound to prepare the positive electrode sheet.
[0027] In any embodiment, the method comprises: preparing a first precursor by uniformly mixing raw materials comprising a sodium supplement agent and a first oxide; preparing a second precursor by uniformly mixing raw materials comprising the first precursor and a second oxide; sintering the second precursor under a nitrogen atmosphere to obtain a sodium supplement compound; and preparing the positive electrode tab using the sodium supplement compound.
[0028] A third aspect of the present application provides a sodium secondary battery comprising the positive electrode tab of the first aspect of the present application.
[0029] A fourth aspect of the present application provides an electric device comprising the sodium secondary battery of the third aspect of the present application.
[0030] The sodium supplement compound provided by the present application has the functions of supplementing sodium, improving chemical stability and ion transport capacity. Therefore, the positive electrode tab prepared using the sodium supplement compound provided by the present application can effectively improve the energy density and cycle performance of the battery. Accordingly, the electric device provided by the present application also has good performance. BRIEF DESCRIPTION OF DRAWINGS
[0031] Figure 1 is a SEM electron microscope scanning image of the sodium supplement compound prepared in Example 1 of the present application; Figure 2 is a schematic diagram of a secondary battery according to an embodiment of the present application; Figure 3 is an exploded view of the secondary battery according to an embodiment of the present application; Figure 1 Figure 4 is a schematic diagram of an electric device using the secondary battery according to an embodiment of the present application as a power supply.
[0032] REFERENCE NUMERALS: 5 secondary battery; 51 housing; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0033] Hereinafter, embodiments of the present application are specifically disclosed with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of matters well known in the art, repeated descriptions of substantially the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter recited in the claims.
[0034] The ranges disclosed herein are intended to be "open" ranges, i.e., the upper and lower limits of the range are not included. The ranges are also intended to include any and all sub-ranges of the range, i.e., all combinations of any two of the range limits, unless otherwise indicated. For example, a range of "1 to 10" is intended to include any number from 1 to 10, including the numbers 1 and 10. Unless otherwise indicated, the use of "or" in the disclosed aspects herein is the inclusive, and not the exclusive use. Only the context, and not the number of times an item is used, can determine that it is the exclusive use. For example, the phrase "A or B" is intended to mean "A or B or both A and B." As used herein, the term "about" means that the recited numerical property or range is approximated, and that slight variations are expected to be within the scope of the disclosure. For example, the term "about" can mean that the recited numerical property or range is approximated to within 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 99% of the recited numerical property or range. For example, the term "about" can mean that the recited numerical property or range is approximated to within 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 99% of the recited numerical property or range. For example, the term "about" can mean that the recited numerical property or range is approximated to within 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 99% of the recited numerical property or range. For example, the term "about" can mean that the recited numerical property or range is approximated to within 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 99% of the recited numerical property or range. For example, the term "about" can mean that the recited numerical property or range is approximated to within 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 99% of the recited numerical property or range. For example, the term "about" can mean that the recited numerical property or range is approximated to within 1%, 2%,
[0035] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions.
[0036] Unless otherwise specified, all technical features and optional technical features of the present application can be combined with each other to form new technical solutions.
[0037] Unless otherwise specified, all steps of the present application can be performed in sequence or randomly, and preferably in sequence. For example, the method comprises steps (a) and (b), which means that the method can comprise steps (a) and (b) in sequence, or steps (b) and (a) in sequence. For example, the method also comprises step (c), which means that step (c) can be added to the method in any order, for example, the method can comprise steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), etc.
[0038] Unless otherwise specified, the "includes" and "contains" mentioned in the present application are open-ended, and can also be closed. For example, the "includes" and "contains" can mean that other components not listed can also be included or contained, or only the listed components can be included or contained.
[0039] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0040] Sodium-ion batteries have emerged as a novel type of rechargeable battery due to their abundant resources. The negative electrode often uses hard carbon without a sodium source, but this forms an SEI film and undergoes side reactions during charging and discharging, limiting its application. The use of sodium replenishment agents can effectively improve this problem. Common methods for negative electrode sodium replenishment include electrochemical sodium replenishment, chemical solution methods, and sodium powder methods. While these methods can effectively reduce irreversible sodium capacity loss by pre-forming an SEI or pre-intercalating sodium ions, they are complex to operate, have high requirements for the working environment, and the pre-sodium-treated negative electrode exhibits high activity, posing significant safety hazards and hindering industrial-scale production.
[0041] Currently, adding sodium-replenishing agents to the positive electrode is a relatively good solution to the above problems. Available sodium-replenishing agents include sodium nitride, sodium phosphide, sodium peroxide, sodium oxide, and sodium carbonate, but they suffer from poor stability and are prone to reaction in air. To solve these technical problems, this application develops a sodium-replenishing composite material that can be used in the positive electrode sheet. This sodium-replenishing composite material has good chemical stability and can effectively improve the energy density and cycle performance of the battery.
[0042] [Positive electrode plate] This application provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode film layer, the positive electrode film layer comprising a sodium-supplementing composite, the sodium-supplementing composite comprising a core and at least one coating layer covering the core; the core comprising a sodium-supplementing agent, the sodium-supplementing agent comprising at least one of sodium nitride, sodium phosphide, sodium peroxide, sodium oxide, and sodium carbonate; the coating layer comprising an oxide, the oxide comprising at least one of aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, silicon oxide, boron oxide, lanthanum oxide, cerium oxide, and bismuth oxide.
[0043] In some embodiments, the sodium supplement includes sodium nitride.
[0044] In some embodiments, the oxide includes at least one of lanthanum oxide, cerium oxide, and bismuth oxide.
[0045] In the sodium replenishment compound, the oxide coating on the surface of the sodium replenishing agent makes it less likely for the active material in the sodium replenishing agent to react with water, carbon dioxide, or other substances in the air to form alkaline substances. This reduces the residual alkali content of the sodium replenishing agent during the sintering process, thereby improving its chemical stability. Therefore, in the sodium replenishment compound provided in this application, the outer oxide coating effectively protects the sodium replenishing agent in the core, and the resulting coating structure improves the stability of the sodium replenishing agent in air, thus effectively improving the battery's initial efficiency and cycle performance. Furthermore, the sodium replenishment compound provided in this application can be combined with various different oxides and sodium replenishing agents, making it suitable for different application scenarios.
[0046] In some embodiments, the oxide includes at least one of aluminum oxide, magnesium oxide, zirconium oxide, and titanium oxide; or the oxide includes at least one of silicon oxide and boron oxide; or the oxide includes at least one of lanthanum oxide, cerium oxide, and bismuth oxide.
[0047] The type of oxide can be selected according to different application scenarios: When metal oxides such as aluminum oxide, magnesium oxide, zirconium oxide, and titanium oxide are used, they have good electrical conductivity. Among them, Al, Ti, and Mg undergo redox reactions during battery charging, changing from high valence states to low valence states, which helps sodium ion dissolution and sodium replenishment. Moreover, this coating structure can ensure the stability of the sodium replenishment agent in subsequent cycles of sodium-ion batteries.
[0048] When non-metallic oxides such as silicon oxide and boron oxide are used, the resulting sodium-supplementing complex exhibits good structural stability.
[0049] When using oxides such as lanthanum oxide, cerium oxide, and bismuth oxide, the rare earth metal elements will form a heterostructure interface, that is, an interface region formed between two materials with different conductivity. Using rare earth metal oxides to construct heterostructure interfaces can effectively reduce the resistance to electron migration and increase electron mobility.
[0050] In some embodiments, the sodium-supplementing complex includes the core, a first coating layer covering the core, and a second coating layer covering the first coating layer; the first coating layer includes at least one of aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, lanthanum oxide, cerium oxide, and bismuth oxide; and the second coating layer includes at least one of silicon oxide and boron oxide.
[0051] In some embodiments, the first coating layer includes at least one of lanthanum oxide, cerium oxide, and bismuth oxide.
[0052] When the sodium-replenishing compound has multiple coating layers, the sodium replenishment effect is better, and the energy density of the battery can be further improved. Meanwhile, different coating layers have different technical effects. For example, the first coating layer is a metal oxide, which provides better conductivity; the second coating layer is a non-metal oxide, which provides better structural stability. When a sodium-replenishing agent with these two coating layers is used in the positive electrode, it can simultaneously improve chemical stability and ion transport capacity, thereby effectively improving the battery's initial efficiency and cycle performance.
[0053] In some embodiments, the mass ratio of the sodium supplement to the oxide is (40~99):(1~50).
[0054] In some embodiments, the mass ratio of the sodium supplement to the oxide is (40~90):(5~10).
[0055] Due to different application scenarios, a specific mass ratio is required when combining oxides and sodium supplements. Using the ratio described above can effectively improve the stability of the sodium supplement while also achieving a good sodium supplementation effect.
[0056] In some embodiments, the Dv50 of the sodium supplement is 2-5 μm; the Dv50 of the oxide is 15-50 nm.
[0057] In sodium-supplemented composites, the use of sodium-supplementing agents and oxides within the aforementioned Dv50 range is beneficial for reducing polarization, increasing capacity, and improving compatibility with cathode material particle size.
[0058] In this article, "Dv50" refers to the particle size at which the cumulative volumetric percentage reaches 50% in the particle size distribution, measured from the smallest particle size side. The Dv50 is determined according to GB / T19077-2016 Particle Size Distribution Laser Diffraction Method, using a laser particle size analyzer such as the Mastersizer 2000E from Malvern Instruments Ltd., UK.
[0059] In some embodiments, the mass content of the sodium-supplementing complex is 0.3% to 2% based on the total mass of the positive electrode film.
[0060] In some embodiments, the mass content of the sodium supplementation complex is 1.0% to 1.6% based on the total mass of the positive electrode film.
[0061] The positive electrode needs to use a certain mass ratio of sodium-replenishing compound. When the above-mentioned proportion of sodium-replenishing compound is used, it not only has a good sodium-replenishing effect, but also enables the battery to have good cycle performance.
[0062] In some embodiments, the positive electrode film layer further includes a positive electrode active material, which includes at least one of layered transition metal oxides, polyanionic compounds, and Prussian blue compounds.
[0063] The transition metal in the layered transition metal oxide can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. Optionally, the layered transition metal oxide is, for example, NaxMO2, where M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr, and Cu, and 0 < x ≤ 1.
[0064] Polyanionic compounds can be those containing metal ions, transition metal ions, or tetrahedral (YO4) ions. n A class of compounds with anionic units. The metal ion may be one of sodium, lithium, potassium, or zinc; the transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y may be at least one of P, S, and Si; n represents (YO4). n The price state.
[0065] Prussian blue compounds can be compounds containing sodium ions, transition metal ions, and cyanide ions (CN). A class of compounds. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. Prussian blue compounds include, for example, Na. a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0 < a ≤ 2, 0 < b < 1, 0 < c < 1.
[0066] In some embodiments, the positive electrode film layer further includes a conductive agent, which includes at least one selected from Ketjen Black, SuperP, acetylene black, carbon black, carbon nanotubes, natural graphite, artificial graphite, and carbon nanofibers.
[0067] In some embodiments, the mass ratio of the sodium-supplementing complex to the conductive agent is (23~150):(10~50).
[0068] Using a certain mass ratio between the sodium-supplemented complex and the conductive agent can help to further improve the conductivity.
[0069] The positive electrode film layer may also include a binder to firmly bond the positive electrode active material and, optionally, a conductive agent, to the positive electrode current collector. The binder may be selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), ethylene... At least one of vinyl acetate copolymer (EVA), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), sodium alginate (SA), polymethacrylic acid (PMA), and carboxymethyl chitosan (CMCS).
[0070] The positive electrode current collector can be made of conductive carbon sheet, metal foil, carbon-coated metal foil, porous metal plate, or composite current collector. The conductive carbon material of the conductive carbon sheet can be selected from one or more of Super P, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers. The metal material of the metal foil, carbon-coated metal foil, and porous metal plate can be independently selected from at least one of copper, aluminum, nickel, and stainless steel. The composite current collector can be a composite current collector formed by combining metal foil with a polymer base film.
[0071] This application also provides a method for preparing the positive electrode sheet provided in this application, the method comprising: uniformly mixing raw materials including a sodium supplement agent and an oxide to prepare a precursor; sintering the precursor under a nitrogen atmosphere to obtain a sodium supplement compound; and using the sodium supplement compound to prepare the positive electrode sheet.
[0072] In some embodiments, the method includes: uniformly mixing raw materials including a sodium supplement agent and a first oxide to prepare a first precursor; uniformly mixing raw materials including the first precursor and a second oxide to prepare a second precursor; sintering the second precursor under a nitrogen atmosphere to obtain a sodium supplement compound; and using the sodium supplement compound to prepare the positive electrode sheet.
[0073] In some embodiments, the first oxide includes at least one selected from aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, lanthanum oxide, cerium oxide, and bismuth oxide, and the second oxide includes at least one selected from silicon oxide and boron oxide. In some preferred embodiments, the first oxide includes at least one selected from lanthanum oxide, cerium oxide, and bismuth oxide.
[0074] When the first oxide is a metal oxide (e.g., aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, lanthanum oxide, cerium oxide, bismuth oxide), it can provide good conductivity; when the second oxide is a non-metal oxide (e.g., silicon oxide, boron oxide), it can provide good structural stability. The sodium-supplemented composite with two coating layers prepared using the above two oxides can achieve both improved chemical stability and ion transport capacity when used in the positive electrode sheet, thereby effectively improving the battery's initial efficiency and cycle performance.
[0075] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as sodium-supplemented complex, positive electrode active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0076] Sodium secondary battery This application also provides a sodium secondary battery, which includes the positive electrode provided in this application.
[0077] In this article, the term "sodium secondary battery" refers to a secondary battery that uses sodium ions as charge carriers. The negative electrode active materials of sodium secondary batteries include carbon-based materials, titanium-based materials, alloy materials, layered transition metal oxides, layered transition metal selenides, organic materials, or metallic sodium. Among them, sodium secondary batteries that use metallic sodium as the negative electrode active material are called sodium metal batteries.
[0078] In some embodiments, the sodium secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0079] In some embodiments, the material of the separator can be selected from at least one of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester, and natural fibers. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0080] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0081] In some embodiments, the sodium secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.
[0082] In some embodiments, the outer packaging of a sodium secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of a sodium secondary battery can also be a soft pack, such as a pouch. The soft pack can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0083] This application does not impose any particular limitation on the shape of the sodium secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 2This is an example of a square-structured sodium secondary battery.
[0084] In some implementations, refer to Figure 3 The outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. A positive electrode, a negative electrode, and a separator can be formed into an electrode assembly 52 using a winding or stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. An electrolyte is immersed in the electrode assembly 52. The sodium secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0085] [Electrical appliances] In addition, this application also provides an electrical device, which includes the sodium secondary battery provided in this application. The sodium secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0086] As the electrical device, a sodium secondary battery can be selected according to its usage requirements.
[0087] Figure 4 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the sodium secondary battery in this device, a battery pack or battery module can be used.
[0088] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use sodium-ion batteries as their power source.
[0089] Examples The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0090] I. Preparation Method Example 1 1) Preparation of sodium supplementation complex Sodium source material was added to an ether-containing solution and mixed evenly. A measured amount of hydrochloric acid was added during stirring, denoted as solution A, to give the surface of A a negative charge. Aluminum nitrate was added to sodium source and aluminum source at a mass ratio of 60:10, and ammonia water was added to it, denoted as solvent B. B was added to A, and the mixture was reacted in a water bath at 25~60℃ for 10~60 min to obtain a precursor with aluminum salt coated on the surface of sodium source. The precursor mixture was then sintered at high temperature in an annealing furnace filled with nitrogen after filtering, washing, and drying the solid. The nitrogen flow rate was 1000 mL / min, the sintering temperature was 200℃, the holding time was 3 h, and the heating rate was 5℃ / min to obtain a uniformly mixed alumina-coated sodium nitride shell-core structure.
[0091] 2) Preparation of positive electrode sheet The prepared sodium-supplementing complex 1 and the positive electrode active material Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent Ketjen black, and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 1:8:1:1. N-methylpyrrolidone (NMP) solvent was added, and the mixture was stirred under vacuum until homogeneous, yielding a positive electrode slurry with a solid content of 50 wt%. The positive electrode slurry was coated onto a current collector aluminum foil and dried at 85°C, then cold-pressed. After edge trimming, cutting, and slitting, it was further dried under vacuum at 85°C for 4 hours to produce the positive electrode sheet.
[0092] 3) Preparation of negative electrode sheet The negative electrode active material hard carbon, conductive agent acetylene black, binder styrene-acrylic emulsion, and thickener sodium carboxymethyl cellulose (CMC-Na) are thoroughly mixed in an appropriate amount of deionized water at a weight ratio of 94:1:4:1 to form a uniform negative electrode slurry. The negative electrode slurry is coated on both surfaces of a negative electrode current collector copper foil with a thickness of 8μm. After drying at 100℃, the negative electrode sheet is obtained by pressing.
[0093] 4) Separating membrane Polyethylene film is used as the separator (celgard).
[0094] 5) Electrolyte Equal volumes of ethylene carbonate (EC) and propylene carbonate (PC) were mixed evenly to obtain an organic solvent. Then, NaPF6 was uniformly dissolved in the organic solvent to obtain an electrolyte, wherein the concentration of NaPF6 was 1 mol / L.
[0095] 6) Battery manufacturing The positive electrode, separator, and negative electrode are stacked in sequence, the electrolyte is added, and the container is sealed to obtain a sodium-ion battery.
[0096] Examples 2-3 The battery preparation methods in Examples 2 and 3 are basically similar to those in Example 1, but the type of sodium supplementer in the sodium supplementation complex is changed. The specific parameters are shown in Tables 1-3.
[0097] Examples 4-5 The battery preparation methods in Examples 4 and 5 are basically similar to those in Example 1, but the types of oxides in the sodium-supplemented composite are changed. The specific parameters are shown in Tables 1-3.
[0098] Examples 6-9 The battery preparation methods in Examples 6-9 are basically similar to those in Example 1, but the mass ratio of sodium supplement to oxide in the sodium supplementation complex is changed. The specific parameters are shown in Tables 1-3.
[0099] Examples 10-11 The battery preparation methods in Examples 10 and 11 are basically similar to those in Example 1, but the mass content of the sodium-supplemented composite in the positive electrode film is changed. The specific parameters are shown in Tables 1-3.
[0100] Example 12 The battery preparation method in Example 12 is basically similar to that in Example 1, but the type of positive electrode active material is changed. The specific parameters are shown in Tables 1-3.
[0101] Example 13 The battery preparation method in Example 13 is basically similar to that in Example 1, but the type of conductive agent is changed. The specific parameters are shown in Tables 1-3.
[0102] Examples 14-15 The battery preparation methods in Examples 14 and 15 are basically similar to those in Example 1, but the mass ratio of sodium-supplemented composite to conductive agent is changed. The specific parameters are shown in Tables 1-3.
[0103] Example 16 The battery preparation method in Example 16 is basically similar to that in Example 1, except that it involves adding an acidification step for the layered oxide and an ammonia treatment step for the outermost oxide to adjust the deposition environment, followed by high-temperature treatment in a nitrogen atmosphere. Specific parameters are shown in Tables 1-3.
[0104] Examples 17-19 The battery preparation methods in Examples 17-19 are basically similar to those in Example 16, but the types of materials for the inner and outer layers of the sodium-supplemented composite are changed. The specific parameters are shown in Tables 1-3.
[0105] II. Performance Testing Methods 1. Characterization of the sodium supplementation complex 1) SEM image of the sodium supplementation complex SEM scanning electron microscopy testing method: Sodium-added composite material powder is coated onto a glass slide and placed in a scanning electron microscope. The morphology of the composite is observed at different magnifications.
[0106] 2) Test method for Dv50 of sodium supplements and oxides Dv50 testing method: Take a quantitative amount of sodium supplement or oxide powder and put it into a laser particle size analyzer to test the particle size distribution. The post-processing yields the relationship between particle size distribution and proportion.
[0107] 2. Battery performance testing methods 1) First Coulomb Efficiency Test of Battery The initial coulombic efficiency test procedure is as follows: At 25°C, the prepared sodium-ion battery was charged to 4V at a rate of 0.1C, and then discharged to 1V at a rate of 0.1C. A full charge-discharge cycle test was performed, and the first charge capacity C0 and the first discharge capacity D0 were recorded. The initial coulombic efficiency was recorded as D0 / C0. 100%.
[0108] 2) Battery cycle performance test The cycle performance test process is as follows: At 25℃, the prepared sodium-ion battery is charged to 4V at a constant current of 0.1C, then charged at a constant voltage of 4V with a cutoff current of 1C, and then discharged at a constant current of 1C to 1.5V. This cycle is repeated until the battery capacity reaches 80%, and the number of cycles is recorded.
[0109] III. Analysis of Test Results for Each Embodiment and Comparative Example Secondary batteries for each embodiment and comparative example were prepared according to the above method, and various parameters were measured. The results are shown in Tables 1-3 below.
[0110] Table 1 Preparation parameters for single-layer coating
[0111] Table 2 Preparation parameters for double-layer coating
[0112] Table 3 Preparation parameters and performance test results
[0113] Based on the above results, it can be seen that the sodium-supplementing composites using a single-layer coating structure in Examples 1-15 and the sodium-supplementing composites using a double-layer coating structure in Examples 16-19 all produced batteries with good initial efficiency and cycle performance. Meanwhile, Figure 1The image shown is a SEM image of the sodium supplementation complex prepared in Example 1, which shows that the sodium supplementation complex prepared in this application has good morphological characteristics and its size meets the actual requirements.
[0114] In Examples 1-5 and 16-19, the sodium-supplementing agents in the sodium-supplementing composites were sodium nitride, sodium phosphide, and sodium peroxide, while the oxides were lanthanum oxide, aluminum oxide, magnesium oxide, and silicon oxide. In Examples 1-19, the Dv50 of the sodium-supplementing agents in the sodium-supplementing composites ranged from 3 to 5 μm, and the Dv50 of the oxides ranged from 15 to 50 nm. The batteries prepared in the above examples all exhibited good initial efficiency and cycle performance.
[0115] In Examples 1-19, the mass ratio of sodium supplement to oxide in the sodium supplementation complex ranged from (40-99):(1-50), and the batteries prepared under these conditions all exhibited good initial efficiency and cycle performance. Furthermore, when the mass ratio of sodium supplement to oxide was in the range of (40-90):(5-10), it further improved the initial efficiency and cycle performance of the battery.
[0116] In Examples 1-19, the mass content of the sodium-supplemented composite in the positive electrode film layer was 0.3% to 2%, and the batteries prepared using these methods all exhibited good initial efficiency and cycle performance. Furthermore, when the mass content of the sodium-supplemented composite in the positive electrode film layer was 1.0% to 1.6%, it further improved the initial efficiency and cycle performance of the battery.
[0117] In Example 12, the positive electrode active material used was Na 0.66 Zn 0.05 Ni 0.18 Cu 0.1 Mn 0.66 O2, Super P was used as the conductive agent in Example 13, and the batteries prepared by it all have good first-efficiency and cycle performance.
[0118] In Examples 14-15, the mass ratio of sodium-supplemented composite to conductive agent was (23-150): (10-50), and the batteries prepared by these methods all exhibited good initial efficiency and cycle performance.
[0119] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A sodium secondary battery, characterized in that, The sodium secondary battery includes a positive electrode sheet, the positive electrode sheet includes a positive electrode film layer, the positive electrode film layer includes a sodium-supplementing composite, and the sodium-supplementing composite includes a core and at least one coating layer covering the core; The core includes a sodium supplement, which includes at least one of sodium nitride and sodium phosphide; The coating layer comprises an oxide, which includes at least one of aluminum oxide, magnesium oxide, silicon oxide, and bismuth oxide.
2. The sodium secondary battery according to claim 1, characterized in that, The sodium supplement includes sodium nitride.
3. The sodium secondary battery according to claim 1, characterized in that, The oxide includes at least one of aluminum oxide, magnesium oxide, and silicon oxide.
4. The sodium secondary battery according to claim 3, characterized in that, The oxide includes aluminum oxide.
5. The sodium secondary battery according to claim 3, characterized in that, The oxide includes magnesium oxide.
6. The sodium secondary battery according to claim 3, characterized in that, The oxide includes silicon oxide.
7. The sodium secondary battery according to claim 1, characterized in that, The mass ratio of the sodium supplement to the oxide is (40~99):(1~50).
8. The sodium secondary battery according to claim 7, characterized in that, The mass ratio of the sodium supplement to the oxide is (40~90):(5~10).
9. The sodium secondary battery according to claim 1, characterized in that, The sodium supplement has a Dv50 of 2μm to 5μm; the oxide has a Dv50 of 15nm to 50nm.
10. The sodium secondary battery according to claim 9, characterized in that, The sodium supplement has a Dv50 of 3μm to 5μm.
11. The sodium secondary battery according to claim 1, characterized in that, The sodium supplementation complex includes the core, a first coating layer covering the core, and a second coating layer covering the first coating layer; The first coating layer includes at least one of aluminum oxide, magnesium oxide, and bismuth oxide; The second coating layer comprises silicon oxide.
12. The sodium secondary battery according to claim 11, characterized in that, The first coating layer comprises aluminum oxide.
13. The sodium secondary battery according to claim 11, characterized in that, The first coating layer comprises magnesium oxide.
14. The sodium secondary battery according to claim 11, characterized in that, The first coating layer comprises bismuth oxide.
15. The sodium secondary battery according to claim 1, characterized in that, Based on the total mass of the positive electrode film, the mass content of the sodium supplementation complex is 0.3% to 2%, and can be selected as 1.0% to 1.6%.
16. The sodium secondary battery according to claim 1, characterized in that, The positive electrode film layer further includes a positive electrode active material, which includes at least one of layered transition metal oxides, polyanionic compounds, and Prussian blue compounds.
17. The sodium secondary battery according to claim 1, characterized in that, The positive electrode film layer also includes a conductive agent, which includes at least one of Ketjen black, Super P, acetylene black, carbon black, carbon nanotubes, natural graphite, artificial graphite, and carbon nanofibers.
18. The sodium secondary battery according to claim 17, characterized in that, The mass ratio of the sodium-supplementing complex to the conductive agent is (23~150):(10~50).
19. A method for preparing a sodium secondary battery according to any one of claims 1-18, characterized in that, The method includes: The precursor is prepared by uniformly mixing raw materials including sodium supplement and oxide; The precursor was sintered under a nitrogen atmosphere to obtain a sodium-supplemented complex. The positive electrode sheet was prepared using the sodium-supplemented complex; The sodium secondary battery is prepared using the positive electrode sheet.
20. The method according to claim 19, characterized in that, The preparation of the precursor specifically includes: subjecting the raw material to a water bath reaction to prepare the precursor.
21. The method according to claim 20, characterized in that, The reaction temperature of the water bath reaction is 25℃~60℃.
22. The method according to claim 20, characterized in that, The reaction time for the water bath reaction is 10 min to 60 min.
23. The method according to claim 19, characterized in that, The method includes: The first precursor is prepared by uniformly mixing raw materials including sodium supplement and first oxide; The second precursor is prepared by uniformly mixing raw materials including the first precursor and the second oxide. The second precursor was sintered under a nitrogen atmosphere to obtain a sodium-supplemented complex. The positive electrode sheet was prepared using the sodium-supplementing complex; The sodium secondary battery is prepared using the positive electrode sheet.
24. An electrical appliance, characterized in that, Includes the sodium secondary battery according to any one of claims 1-18, or the sodium secondary battery prepared by the method according to any one of claims 19-23.