A positive electrode sheet, its preparation method and application
By constructing a three-level nested particle structure of ultra-large-large-small and optimizing porosity and peak intensity ratio, the problem of insufficient energy density and fast charging performance of lithium-ion batteries was solved, and a synergistic improvement in high energy density and fast charging performance was achieved.
Patent Information
- Application Number
- CN202611240127.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing lithium-ion batteries have limited effectiveness in improving energy density and fast charging performance, and also suffer from excessively tortuous lithium-ion transport paths.
By employing a three-level nested particle structure consisting of ultra-large particles, large particles, and small particles, and by controlling the porosity and peak intensity ratio of the positive electrode, the lithium-ion transport path is optimized, thereby achieving high real density and fast charging performance of the positive electrode.
It significantly improves the energy density and fast-charging performance of lithium-ion batteries, ensuring high efficiency in lithium-ion transmission and battery stability.
Smart Images

Figure CN123073028A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium-ion battery technology, and in particular to a positive electrode sheet, its preparation method, and its application. Background Technology
[0002] Lithium-ion batteries are widely used in new energy vehicles, energy storage systems, and consumer electronics due to their high energy density, long cycle life, and environmental friendliness. With the rapid development of downstream industries such as new energy vehicles, users' demand for longer driving ranges is constantly increasing, which places more stringent requirements on the energy density of lithium-ion batteries. Developing lithium-ion batteries with higher energy density has become a core direction for the industry's development.
[0003] Most existing technologies employ a design strategy of combining positive electrode active materials of varying particle sizes. By optimizing particle size distribution, they improve the stacking efficiency of the positive electrode active materials, thereby increasing the compaction density of the positive electrode sheet and ultimately enhancing battery energy density. However, this method has not achieved the expected results in practical applications. On one hand, its improvement in energy density is limited; on the other hand, it also causes a significant degradation in the battery's fast-charging performance.
[0004] Therefore, there is an urgent need to develop a more precise electrode design to synergistically improve the energy density and fast charging performance of lithium-ion batteries. Summary of the Invention
[0005] This application provides a positive electrode sheet that achieves the technical effect of synergistically improving the energy density and fast charging performance of lithium-ion batteries.
[0006] This application also provides a lithium-ion battery, which includes the above-mentioned positive electrode and has excellent energy density and fast charging performance.
[0007] This application also provides an electrical device that includes the aforementioned lithium-ion battery, which has the advantages of high energy density and good fast charging performance.
[0008] The first aspect of this application provides a positive electrode sheet, the positive electrode sheet including a positive electrode active material layer, the positive electrode active material layer including a positive electrode active material, the positive electrode active material including lithium iron phosphate, the lithium iron phosphate including ultra-large particles, large particles and small particles;
[0009] The volumetric particle size distribution curve of the positive electrode active material includes a D peak corresponding to the ultra-large particles, a C peak corresponding to the large particles, and a B peak corresponding to the small particles. The particle size corresponding to the vertex of the D peak is I. D 4μm D ≤35μm; the particle size corresponding to the C peak apex is I C ,1μm≤I C ≤4μm; the particle size corresponding to the apex of peak B is IB 120nm≤I B ≤800nm;
[0010] The positive electrode plate satisfies 0.5 ≤ a / b ≤ 2.
[0011] Wherein, 'a' represents the porosity of the positive electrode; and 'b' = F D / F C F D F is the peak intensity corresponding to the peak of peak D. C This represents the peak intensity corresponding to the apex of peak C.
[0012] A second aspect of this application provides a lithium-ion battery, including the positive electrode sheet of the first aspect.
[0013] A third aspect of this application provides an electrical device, including the lithium-ion battery of the second aspect.
[0014] The cathode sheet of this application constructs a three-level nested particle structure of "ultra-large-large-small". Ultra-large particles form the main supporting framework as the macroscopic skeleton, large particles fill the pores between the ultra-large particles to form a secondary dense packing, and small particles further fill the micropores to achieve tertiary densification. Simultaneously, by establishing a relationship between the porosity 'a' of the cathode sheet and the ratio 'b' of the peak intensity corresponding to the D peak of the ultra-large particles and the peak intensity corresponding to the C peak of the large particles, and limiting its value within a target range, the compaction density of the cathode sheet is increased while the lithium-ion transport rate is improved, synergistically enhancing the energy density and fast-charging performance of the battery. Attached Figure Description
[0015] Figure 1 This is a schematic diagram of the volume particle size distribution curve of the positive electrode active material of this application. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0017] Lithium-ion batteries are widely used in new energy vehicles, energy storage systems, and consumer electronics due to their high energy density, long cycle life, and lack of memory effect. With the rapid development of downstream industries such as new energy vehicles, the market demand for extended driving range continues to increase, placing higher requirements on the energy density of lithium-ion batteries. Developing lithium-ion batteries with higher energy density has become a core trend in the industry. Most existing technologies employ a design strategy of combining large and small particles of the positive electrode active material. By optimizing the particle size distribution, the stacking efficiency of the positive electrode active material is improved, thereby increasing the compaction density of the positive electrode sheet and thus increasing the battery's energy density. However, this method has limited effectiveness in improving energy density in practical applications and also reduces the battery's fast-charging performance.
[0018] The inventors conducted research on this and believe that the limited increase in energy density is due to the fact that a large number of micro-nano-level pores still exist after the combination of large and small particles, the space for improving the stacking efficiency of the positive electrode active material is limited, and the increase in the compaction density of the positive electrode sheet is limited; the decline in battery fast charging performance is due to the excessive tortuosity of the lithium ion transport path after the combination of large and small particles, which increases the transport resistance.
[0019] Therefore, the inventors believe that it is necessary to find a balance between the maximum compaction density and the minimum tortuosity in order to improve energy density by utilizing gradation while maintaining good fast charging performance.
[0020] Based on this, the first aspect of this application provides a positive electrode sheet, the positive electrode sheet including a positive electrode active material layer, the positive electrode active material layer including a positive electrode active material, the positive electrode active material including lithium iron phosphate, and the lithium iron phosphate including ultra-large particles, large particles and small particles;
[0021] The volumetric particle size distribution curve of the positive electrode active material includes a D peak corresponding to ultra-large particles, a C peak corresponding to large particles, and a B peak corresponding to small particles. The particle size corresponding to the apex of the D peak is I. D 4μm D ≤35μm; the particle size corresponding to the C peak apex is I C ,1μm≤I C ≤4μm; the particle size corresponding to the peak of B is I B 120nm≤I B ≤800nm;
[0022] The positive electrode plate satisfies 0.5 ≤ a / b ≤ 2.
[0023] Where a is the porosity of the positive electrode; b = F D / F C F D F is the peak intensity corresponding to the peak of peak D. C This represents the peak intensity corresponding to the apex of peak C.
[0024] Lithium iron phosphate is a complex phosphate mainly composed of Li, Fe, P and O, which has advantages such as stable structure, long cycle life, low cost and environmental friendliness; lithium iron phosphate includes ultra-large particles, large particles and small particles.
[0025] In this application, lithium iron phosphate particles are distinguished as ultra-large, large, and small based on the particle size on the horizontal axis of the volumetric particle size distribution curve. The particle size relationship among the three is: ultra-large particle size > large particle size > small particle size.
[0026] like Figure 1 As shown, the volumetric particle size distribution curve of the positive electrode active material has particle size on the x-axis and peak intensity on the y-axis. This volumetric particle size distribution curve includes peaks D, C, and B. Peak D is the characteristic peak corresponding to ultra-large particles, peak C is the characteristic peak corresponding to large particles, and peak B is the characteristic peak corresponding to small particles; the particle size corresponding to the apex of peak D is I. D The characteristic particle size of ultra-large particles is 4μm. D ≤35μm, which is the most probable particle size of ultra-large particles; the particle size I corresponding to the C peak apex. C The characteristic particle size of large particles is 1μm≤I C ≤4μm, which is the most probable particle size for large particles; the particle size I corresponding to the peak of peak B. B The characteristic particle size of small particles is 120nm ≤ I. B ≤800nm, which is the most probable particle size of small particles.
[0027] Among them, the ultra-large particles form the main supporting framework as the macroscopic skeleton, the large particles fill the pores between the ultra-large particles to form a secondary dense packing, and the small particles further fill the micropores to achieve tertiary densification. The ultra-large particles, large particles and small particles form a "ultra-large-large-small" three-level nested particle structure, which significantly improves the compaction density of the positive electrode sheet, thereby greatly improving the energy density of the lithium-ion battery.
[0028] In lithium-ion batteries, lithium-ion transport and the compaction density of the cathode are key factors limiting performance improvement. By synergistically controlling two parameters—the porosity of the cathode and the ratio of the peak intensity corresponding to the D peak of ultra-large particles to the peak intensity corresponding to the C peak of large particles—an optimized match can be achieved at the physical level, ensuring efficient lithium-ion transport while maintaining compaction density.
[0029] Specifically, the porosity of the positive electrode reflects the number and connectivity of pores within the positive electrode, determining the electrolyte's ability to wet the positive electrode and thus affecting the lithium-ion transport rate, which is crucial for the battery's fast-charging performance. The ratio of the peak intensity corresponding to the D peak of ultra-large particles to the peak intensity corresponding to the C peak of large particles reflects the relative content and proportion of ultra-large and large particles in the positive electrode active material, determining the packing efficiency of the positive electrode active material and thus affecting the compaction density of the positive electrode, which is crucial for the battery's energy density.
[0030] By ensuring that 0.5 ≤ a / b ≤ 2, a synergistic optimization of energy density and fast-charging performance can be achieved. The inventors believe that if the formula is too low, it means that the porosity of the cathode sheet is too small or that the proportion of ultra-large particles in the cathode active material is too high, which increases the resistance to lithium-ion transport and lengthens the transport path, thus threatening the battery's fast-charging performance. If the formula is too high, it means that the porosity of the cathode sheet is too large or that the proportion of ultra-large particles in the cathode active material is too small, which reduces the compaction density of the cathode sheet, prevents ultra-large particles from providing enough pores for large particles to fill, results in poor particle gradation, and reduces the battery's energy density.
[0031] It should be noted that a) can be controlled by adjusting the mass ratio of the positive electrode active material during the preparation of the positive electrode sheet, or by adjusting the rolling pressure during the preparation of the positive electrode sheet; b) can be controlled by adjusting the mass ratio of ultra-large particles, large particles and small particles during the preparation of the positive electrode active material.
[0032] Therefore, this application constructs a three-level nested particle structure of "ultra-large-large-small" with a stepped decreasing particle size distribution curve, achieving three-level densification through ultra-large particles, large particles, and small particles. At the same time, by controlling the synergistic relationship between the porosity 'a' of the positive electrode sheet and the ratio 'b' of the peak intensity corresponding to the D peak corresponding to ultra-large particles and the peak intensity corresponding to the C peak corresponding to large particles, the compaction density of the positive electrode sheet is increased while promoting lithium-ion transport, thus synergistically improving the energy density and fast-charging performance of the lithium-ion battery.
[0033] In the specific preparation of the positive electrode active material, ultra-large particles, large particles, and small particles are mechanically mixed to obtain the positive electrode active material. In one specific embodiment, the positive electrode active material comprises, by mass percentage, 5% to 25% ultra-large particles, 25% to 65% large particles, and 30% to 50% small particles.
[0034] In one specific embodiment, the ultra-large particles are prepared by a method comprising the following steps:
[0035] Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, titanium dioxide, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:6:4:0.75:0.35:0.3:204 to obtain an ultra-large particle slurry. The ultra-large particle slurry was then subjected to sand milling to obtain an ultra-large particle slurry (Dv). 50 (100~400nm); ultra-large particle slurry is spray-treated to obtain ultra-large particle raw meal (Dv). 50 (4~40μm); ultra-large raw material is subjected to high-temperature sintering under nitrogen atmosphere to obtain ultra-large sintered material; ultra-large sintered material is subjected to vibration sieving to obtain ultra-large particles.
[0036] The inlet air temperature for spray treatment is 180~220℃, and the feed rate is 25~70m / s. 3 / h, the outlet air temperature is 80~100℃; the high-temperature sintering treatment temperature is 700~820℃, and the time is 6~12h.
[0037] In one specific embodiment, the large particles are prepared by a method comprising the following steps:
[0038] Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:3.5:4.5:0.35:0.8:204 to obtain a large-particle mixed slurry. The large-particle mixed slurry was then subjected to sand milling to obtain a large-particle slurry (Dv). 50 (1100nm); large particle slurry is spray-treated to obtain large particle raw meal (Dv). 50 (40μm); large-particle raw materials are subjected to high-temperature sintering under a nitrogen atmosphere to obtain large-particle sintered material; large particles are then crushed and deagglomerated to obtain large particles.
[0039] The inlet air temperature for spray treatment is 180~220℃, and the feed rate is 25~70m / s. 3 / h, the outlet air temperature is 80~100℃; the high temperature sintering treatment temperature is 700~820℃, the time is 6~12h; the pulverizing air pressure of the pulverizing and deagglomerating treatment is 460MPa, and the grading frequency is 60Hz.
[0040] In one specific embodiment, the small particles are prepared by a method comprising the following steps:
[0041] Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:3.5:4.5:0.35:0.8:204 to obtain a small-particle mixed slurry. The small-particle mixed slurry was then subjected to sand milling to obtain a small-particle slurry (Dv).50 (380nm); small particle slurry is spray-treated to obtain small particle raw meal (Dv) 50 (40μm); small-particle raw materials are subjected to high-temperature sintering under a nitrogen atmosphere to obtain small-particle sintered material; the small-particle sintered material is then crushed and deagglomerated to obtain small particles.
[0042] The inlet air temperature for spray treatment is 180~220℃, and the feed rate is 25~70m / s. 3 / h, the outlet air temperature is 80~100℃; the high temperature sintering treatment temperature is 700~820℃, the time is 6~12h; the pulverizing air pressure of the pulverizing and deagglomerating treatment is 460MPa, and the grading frequency is 60Hz.
[0043] In one specific implementation, 10% ≤ a ≤ 40%, 0.05 ≤ b ≤ 1. Optionally, a can be 10%, 20%, 30%, 40%, or any two of the above values, and b can be 0.05, 0.2, 0.4, 0.6, 0.8, 1, or any two of the above values.
[0044] By controlling 'a' within the aforementioned range, two advantages are achieved: firstly, sufficient and interconnected pores within the positive electrode sheet are ensured, facilitating electrolyte wetting, reducing lithium-ion transport resistance, and improving the battery's fast-charging performance; secondly, excessive porosity prevents loose accumulation of active materials, further increasing the positive electrode sheet's compaction density and guaranteeing the battery's energy density. Conversely, controlling 'b' within the aforementioned range allows for the dense stacking of ultra-large and large particles, effectively improving the stacking efficiency of the positive electrode active material, thereby increasing the positive electrode sheet's compaction density and significantly enhancing the lithium-ion battery's energy density. Simultaneously, ultra-large particles, acting as a macroscopic framework, provide continuous and interconnected macroscopic ion channels, while moderate filling with large particles shortens the transport distance, reducing lithium-ion transport resistance and optimizing fast-charging performance.
[0045] Furthermore, 20% ≤ a ≤ 30%, 0.15 ≤ b ≤ 0.40. Optionally, a can be 20%, 22%, 24%, 26%, 28%, 30%, or any two of the above values, and b can be 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, or any two of the above values.
[0046] By limiting 'a', we can ensure that the positive electrode sheet has both an appropriate number of pores and good pore connectivity, allowing the electrolyte to fully and quickly wet the positive electrode sheet, significantly shortening the lithium-ion transport path and further improving the battery's fast-charging performance. At the same time, we can also guarantee the compaction density of the positive electrode sheet, resulting in a higher energy density for the battery. By limiting 'b', we can achieve a better match between the relative content of ultra-large particles and large particles, achieving better dense packing, significantly increasing the compaction density of the positive electrode sheet, and further improving the battery's energy density. Simultaneously, the macroscopic framework constructed by ultra-large particles and the filling effect of large particles are better matched, further promoting lithium-ion transport and optimizing the battery's fast-charging performance.
[0047] It should be added that 0.5% ≤ F D ≤10%, 10%≤F C ≤40%. Optional, F D F can be 0.5%, 2%, 4%, 6%, 8%, 10%, or any range between two of the above values. C It can be 0.5%, 2%, 4%, 6%, 8%, 10%, or a range between any two of the above values. F D The content of ultra-large lithium iron phosphate particles in the positive electrode active material can be controlled to regulate the efficiency of the process. C The content of large-particle lithium iron phosphate in the positive electrode active material can be controlled.
[0048] F D Within the aforementioned range, the appropriate content of ultra-large particles in the positive electrode active material provides skeletal support for the three-level nested particle structure, which is conducive to forming a stable particle packing structure, increasing the compaction density of the positive electrode sheet, and thus improving the energy density of the battery. (The last sentence appears to be incomplete and possibly refers to a different topic.) C Within the aforementioned range, the content of large particles in the positive electrode active material is moderate, effectively filling the pores between ultra-large particles, further improving the stacking efficiency of the positive electrode active material, thereby increasing the compaction density of the positive electrode sheet, which is beneficial to improving the energy density of the battery.
[0049] In one specific implementation, I D -I C >2μm. I D -I C The particle size can be controlled by adjusting the spray particle size, sintering temperature and time, and vibratory sieve mesh size during the preparation of ultra-large and large particles. This can be achieved by controlling I... D -I C Within the above range, there is a significant difference in particle size between ultra-large particles and large particles, which is conducive to the construction of a stable skeleton structure by ultra-large particles, and the large particles effectively fill the pores of ultra-large particles to form a secondary dense packing, further improving the compaction density of the positive electrode sheet, thereby increasing the energy density of the battery.
[0050] In one specific implementation, I C -I B >0.5μm. I C -I B The particle size can be controlled by adjusting the spray particle size, sintering temperature and time, and vibratory sieve mesh size during the preparation of large and small particles. This can be achieved by controlling I... C -I B Controlling the density within the above range is beneficial for small particles to further fill micropores and achieve three-level densification, thereby increasing the compaction density of the positive electrode and thus improving the energy density of the battery. It can also form uniform and interconnected pore channels inside the positive electrode, promoting the wetting of the positive electrode by the electrolyte and improving the fast charging performance of the battery.
[0051] In addition, the peak intensity corresponding to the peak of B is F. B 10%≤F B ≤40%, F B <F C F B >F D F B <F C This indicates that the content of small particles in the positive electrode active material is lower than that of large particles. This hierarchical filling structure, with large particles as the backbone and small particles as a supplement, is conducive to forming more efficient dense stacking, increasing the compaction density of the positive electrode sheet, and thus improving the energy density of the battery. B >F D This indicates that the content of small particles in the positive electrode active material is higher than that of ultra-large particles. This limitation can avoid the increase in lithium-ion transport resistance caused by excessive ultra-large particle content, thus ensuring the fast charging performance of the battery.
[0052] It should be noted that 0.5% <F C -F B <3%. F C -F B The mass percentage of large-particle and small-particle lithium iron phosphate in the positive electrode active material can be controlled. This can be achieved by adjusting the F... C -F B By limiting the content of large particles to a significantly higher level than small particles, it is beneficial to achieve efficient densification, further improve the compaction density of the positive electrode sheet, and ensure the energy density of the battery.
[0053] In addition, F C -F D >10%. F C -F D The content of large-particle and ultra-large-particle lithium iron phosphate in the positive electrode active material can be controlled. This can be achieved by adjusting the F... C-F D By limiting the content of large particles to a significantly higher level than that of ultra-large particles, the porosity of the ultra-large particle skeleton can be optimized, the filling of large particles can be promoted, and the lithium-ion transport resistance can be reduced, thus balancing the energy density and fast charging performance of the battery.
[0054] In addition, F B -F D >10%. F B -F D The mass percentage of small-particle and ultra-large-particle lithium iron phosphate in the positive electrode active material can be controlled. This can be achieved by adjusting the F... B -F D By limiting the content of small particles to a higher percentage than that of ultra-large particles, it is beneficial for the small particles to fully fill the micropores of the ultra-large particles, effectively optimizing the pore distribution and pore connectivity. This not only increases the compaction density but also promotes the transport of lithium ions, achieving synergistic optimization of energy density and fast charging performance.
[0055] In one specific embodiment, lithium iron phosphate further includes ultra-small particles, and the volumetric particle size distribution curve of the positive electrode active material also includes an A peak corresponding to the ultra-small particles. The ultra-small particles further fill micro- and nano-pores to achieve four-level densification. Ultra-large particles, large particles, small particles, and ultra-small particles form a "ultra-large-large-small-ultra-small" four-level nested particle structure, further improving the stacking efficiency of the positive electrode active material and the compaction density of the positive electrode sheet, thereby increasing the energy density of the battery. Simultaneously, the ultra-small particles can optimize the distribution of pores within the positive electrode sheet, promoting electrolyte wetting of the positive electrode sheet, enabling the battery to further improve fast-charging performance on top of its high energy density.
[0056] It should be added that the peak intensity corresponding to the highest point of peak A is F. A F A <F B F A <F D F A <F B This indicates that the content of ultra-small particles in the positive electrode active material is lower than that of small particles, which ensures moderate slurry viscosity and uniform dispersion, helps maintain the internal pore structure of the positive electrode sheet, and improves the fast-charging performance of the battery. A <F D This indicates that the content of ultra-small particles in the positive electrode active material is lower than that of ultra-large particles. The ultra-small particles only serve as a pore-filling phase to finely fill the micro- and nano-pores. This can not only improve the stacking efficiency of the positive electrode active material and the compaction density of the positive electrode sheet, but also further reduce the interfacial impedance, thereby achieving synergistic optimization of energy density and fast charging performance.
[0057] Furthermore, F B -F A >2%. F B -FA The content of small-particle lithium iron phosphate and ultra-small-particle lithium iron phosphate in the positive electrode active material can be controlled. (The last part, "F," appears to be an unrelated fragment and is omitted from the translation.) B -F A Within the above range, the content of small particles is significantly higher than that of ultra-small particles. In the four-level nested particle structure, small particles are the main filling phase and ultra-small particles are the auxiliary filling phase. This can not only fully fill the micro-nano pores to improve the compaction density of the positive electrode sheet, but also avoid pore blockage, thus balancing the energy density and fast charging performance of the battery.
[0058] In one specific implementation, the particle size corresponding to the apex of peak A is I. A ,20nm≤I A ≤100nm. Optional, I A It can be 20nm, 40nm, 60nm, 80nm, 100nm, or a range between any two of the above values. By using I... A By controlling the energy density within the above range, on the one hand, the micro- and nano-pores between ultra-large particles, large particles, and small particles can be efficiently filled, further improving the packing density of the positive electrode active material and the compaction density of the positive electrode sheet, which is beneficial to improving the energy density of the battery; on the other hand, the electrode-electrolyte interface contact area can be increased, the lithium-ion diffusion path can be shortened, the interface impedance can be reduced, the lithium-ion transport efficiency can be improved, and the fast-charging performance of the battery can be improved.
[0059] Furthermore, I B -I A >50nm. I B -I A The particle size can be controlled by adjusting the spray particle size, sintering temperature and time, and vibration sieve mesh size during the preparation of small and ultra-small particles. This can be achieved by controlling I... B -I A Within the aforementioned range, a significant particle size gradient is formed between small and ultra-small particles. This facilitates the more complete and precise filling of the micro-nano pores between the small particles by the ultra-small particles, further enhancing the compaction and packing density of the positive electrode active material and increasing the compaction density of the positive electrode sheet. Simultaneously, continuous and unobstructed multi-level pore channels can be formed within the positive electrode sheet, promoting electrolyte wetting and lithium-ion transport, thus achieving further synergistic optimization of energy density and fast-charging performance.
[0060] In one specific embodiment, the ultrafine particles are prepared by a method comprising the following steps:
[0061] Lithium hydroxide monohydrate, ferrous sulfate heptahydrate, 85 wt% phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 0.167:1:0.433:2.4 to obtain a mixed slurry. The mixed slurry was transferred to a hydrothermal reactor for hydrothermal treatment to obtain lithium iron phosphate powder. The lithium iron phosphate powder, glucose, polyethylene glycol, vanadium pentoxide, and ultrapure water were mixed and dispersed in a mass ratio of 100:7:4.5:0.7:166 to obtain an ultrafine particle mixed slurry. The ultrafine particle mixed slurry was then subjected to sand milling to obtain ultrafine particle slurry (Dv). 50 (250nm) The ultra-small particle slurry is sprayed to obtain ultra-small particle raw material; the ultra-small particle raw material is sintered at high temperature under nitrogen atmosphere to obtain ultra-small particle sintered material; the ultra-small particle sintered material is crushed and deagglomerated to obtain ultra-small particles.
[0062] The hydrothermal treatment was carried out at a temperature of 200℃ for 3 hours; the spray treatment had an inlet air temperature of 180~220℃ and a feed rate of 25~70 m / s. 3 / h, the outlet air temperature is 80~100℃; the high temperature sintering treatment temperature is 700~820℃, the time is 6~12h; the pulverizing air pressure of the pulverizing and deagglomerating treatment is 460MPa, and the grading frequency is 60Hz.
[0063] In one specific embodiment, the ultra-large particle includes a lithium iron phosphate core and a coating layer covering at least a portion of the surface of the lithium iron phosphate core. The coating layer includes carbon and has a thickness of 0.5 to 120 nm. Optionally, the thickness of the coating layer can be 0.5 nm, 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, or any two of the above values.
[0064] It should be added that the ultra-small particles include a lithium iron phosphate core and a coating layer covering at least a portion of the surface of the lithium iron phosphate core. The coating layer includes carbon and has a thickness of 0.5~20 nm. Optionally, the thickness of the coating layer can be 0.5 nm, 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, or any two of the above values.
[0065] By applying a coating layer to the surface of ultra-large and ultra-small particles, the surface conductivity of lithium iron phosphate can be improved, the electrode interface impedance can be reduced, and the lithium-ion transport efficiency can be enhanced, which is beneficial to improving the fast-charging performance of the battery. Simultaneously, the coating layer can suppress side reactions between the core material and the electrolyte, reduce the formation of byproducts, and improve the structural stability of the battery. Controlling the thickness of the coating layer within the aforementioned range allows for the formation of a continuous, complete, and dense coating layer, effectively isolating the core material from the electrolyte and improving the battery's cycle stability. Furthermore, it provides a stable interfacial conductive network, reduces interfacial impedance, promotes lithium-ion transport, and optimizes the battery's fast-charging performance.
[0066] In one specific embodiment, the compaction density of the positive electrode sheet is 2~3 g / cm³. 3 Optionally, the compaction density of the positive electrode can be 2 g / cm³. 3 2.2g / cm 3 2.4g / cm 3 2.6g / cm 3 2.8g / cm 3 3g / cm 3 Or any two of the above values. By controlling the compaction density of the positive electrode within the above range, on the one hand, it can ensure that the positive electrode has a high degree of density and structural stability, increase the proportion of active material per unit volume, and significantly improve the volumetric energy density of the battery; on the other hand, it can avoid excessive compression of the internal pores of the positive electrode, difficulty in electrolyte wetting, and obstruction of lithium-ion transport channels caused by excessive compaction density, thus ensuring that the battery has good fast-charging performance.
[0067] Furthermore, the powder resistivity of the positive electrode active material is 2~20 Ω / cm. Optionally, the powder resistivity of the positive electrode active material can be 2 Ω / cm, 5 Ω / cm, 10 Ω / cm, 15 Ω / cm, 20 Ω / cm, or any two of the above values. Limiting the powder resistivity of the positive electrode active material ensures that it possesses suitable electronic conductivity, effectively reducing electron transport resistance between and within particles, improving electron conduction efficiency, and further enhancing the fast-charging performance of the battery.
[0068] It should be noted that the chemical composition of lithium iron phosphate is LiFe. x T yPO4, wherein 0.991≤x≤0.997, 0.003≤y≤0.007, and T is a dopant element, including at least one of Ti, V, Nb, Mg, Mn, Zn, Zr, Ni, and Al, and the mass percentage of the dopant element in the lithium iron phosphate is 3000~9000ppm. Optionally, the mass percentage of the dopant element in the lithium iron phosphate can be 3000ppm, 5000ppm, 7000ppm, 9000ppm, or any two of the above values.
[0069] Doping elements can stabilize the crystal structure, suppress volume effects and lattice distortions in the cathode active material during charge and discharge, and improve the structural stability of the cathode active material. They can also introduce crystal defects, optimize carrier concentration, improve the electronic conductivity and lithium-ion transport rate of the cathode active material, reduce battery polarization during fast charging, and significantly improve the battery's fast charging performance. Controlling the mass percentage of doping elements in lithium iron phosphate within the aforementioned range ensures that the doping elements fully function while avoiding the reduction in effective capacity of the active material due to excessive doping, thus synergistically improving the battery's cycle stability and fast charging performance.
[0070] In the specific preparation of the positive electrode sheet, the positive electrode active material, conductive agent, binder, and dispersant are dispersed in an appropriate amount of N-methylpyrrolidone (NMP) solvent and thoroughly stirred to form a uniform positive electrode slurry. The positive electrode slurry is then uniformly coated onto the positive electrode current collector, and after drying, rolling, and slitting, the positive electrode sheet is obtained. In one specific embodiment, the mass ratio of the positive electrode active material, conductive agent, binder, and dispersant is 90~99:0.5~5:0.5~5:0~2.
[0071] The conductive agent includes at least one of carbon black, acetylene black, graphene, Ketjen black, and carbon fiber; the binder includes at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinylpyrrolidone, and polyurethane; the dispersant includes polyvinylpyrrolidone; the positive electrode current collector material can be at least one of aluminum foil and nickel foil; the areal density of the positive electrode sheet is 150~500 g / cm³. 2 .
[0072] A second aspect of this application provides a lithium-ion battery, which includes the positive electrode of the first aspect.
[0073] In one specific embodiment, the lithium-ion battery further includes a negative electrode sheet with a compaction density of 1.6~1.7 g / cm³. 3 Optionally, the compaction density of the negative electrode can be 1.6 g / cm³. 31.62g / cm 3 1.64 g / cm 3 1.66 g / cm 3 1.68g / cm 3 1.7g / cm 3 Or any two of the above values. By controlling the compaction density of the negative electrode sheet within the above range, it is possible to ensure that the negative electrode sheet has both high packing density and reasonable pore structure. While ensuring the active material loading per unit volume and improving the volumetric energy density of the battery, it retains suitable pore channels, which is conducive to the electrolyte fully wetting the negative electrode sheet, ensuring rapid lithium ion insertion / extraction and transport, and maintaining excellent fast charging performance.
[0074] It should be added that the negative electrode sheet includes a negative electrode active material layer, which in turn includes a negative electrode active material, and the negative electrode active material has a Dv... 50 The diameter is 5~20 μm. Optionally, the Dv of the negative electrode active material... 50 It can be 5 μm, 10 μm, 15 μm, 20 μm, or any range between two of the above values. This applies to the Dv of the negative electrode active material. 50 Limiting the density and active material loading can, on the one hand, ensure the compaction density and the amount of active material loaded, thereby increasing the energy density of the battery; on the other hand, it can shorten the lithium-ion transport distance, reduce side reactions with the electrolyte, reduce the risk of interfacial gas generation, and improve the fast charging performance and safety performance of the battery.
[0075] In the specific preparation of the negative electrode sheet, the negative electrode active material, conductive agent, binder, and dispersant are dispersed in an appropriate amount of deionized water and thoroughly stirred to form a uniform negative electrode slurry. The negative electrode slurry is then uniformly coated onto the negative electrode current collector, and after drying, rolling, and slitting, the negative electrode sheet is obtained. In one specific embodiment, the mass ratio of the negative electrode active material, conductive agent, binder, and dispersant is 90~98:0~5:1.5~5:0.3~1.5.
[0076] The negative electrode active material includes at least one of graphite, hard carbon, soft carbon, mesophase carbon microspheres, silicon-based negative electrode materials (mainly including silicon suboxide and silicon-carbon negative electrodes), and tin-based negative electrode materials (mainly including tin and tin alloys); the conductive agent includes at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, and graphene; the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyvinyl alcohol, and sodium polyacrylate; the dispersant includes polyvinylpyrrolidone; the negative electrode current collector material can be at least one of copper foil, nickel foam, and copper foam; the areal density of the negative electrode sheet is 110~200 g / cm³. 2 .
[0077] In one specific embodiment, the lithium-ion battery further includes an electrolyte with a viscosity of 2-5 cP at 25°C. Optionally, the viscosity of the electrolyte at 25°C can be 2 cP, 3 cP, 4 cP, 5 cP, or any two of the above values. Limiting the viscosity of the electrolyte at 25°C ensures that the electrolyte has good fluidity and wettability, enabling it to quickly and fully wet the micropores inside the positive electrode, negative electrode, and separator, ensuring efficient lithium-ion transport between the electrode interface and the electrolyte, and improving the battery's fast-charging performance.
[0078] Further, the electrolyte includes additives, which include at least one of vinylene carbonate, fluoroethylene carbonate, ethylene sulfate, tris(trimethylsilyl) phosphite, and lithium difluorosulfonylimide, wherein the mass percentage of the additives in the electrolyte is 0.05% to 2.5%. Optionally, the mass percentage of the additives in the electrolyte may be 0.05%, 1%, 1.5%, 2%, 2.5%, or any two of the above values.
[0079] Vinylene carbonate (VC) and fluoroethylene carbonate (FEC) preferentially form films on the negative electrode surface, inhibiting the continuous decomposition of the electrolyte and reducing side reaction gas production; vinyl sulfate (DTD) can optimize the interfacial film density, reduce interfacial impedance, inhibit capacity decay during high-temperature cycling, and improve the high-temperature reliability of the battery; trimethylsilyl phosphite (TMSP) has the functions of removing acid and anti-oxidation, and can remove trace amounts of hydrofluoric acid and other impurities in the electrolyte, protecting the crystal structure of the positive electrode active material; lithium bis(fluorosulfonyl)imide (LiFSI) has both film-forming and ion-conducting auxiliary functions, which can improve the ionic conductivity of the electrolyte and reduce battery fast-charging polarization.
[0080] By controlling the mass ratio of additives in the electrolyte within the above-mentioned range, on the one hand, a continuous and complete interfacial protective film can be formed, giving full play to the functions of film formation, impurity removal, and structural stabilization, effectively improving the fast charging performance and cycle life of the battery; on the other hand, it can avoid the excessively thick interfacial film and high lithium-ion transport resistance caused by excessively high additive mass ratio, taking into account the battery's ion transport efficiency, wettability, and energy density, and achieving synergistic optimization of fast charging performance and energy density.
[0081] In the specific preparation of the electrolyte, lithium salt and additives are dissolved in a solvent to obtain the electrolyte.
[0082] The electrolyte concentration is 1 mol / L; the lithium salt includes LiPF6; the solvent includes at least one of ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl formate (MF), ethyl acetate (EA), methyl acetate (MA), methyl propionate (MP), and fluoroethylene carbonate (FEC), and further, the solvent includes EC, EMC, DEC, and FEC, and the volume ratio of EC, EMC, DEC, and FEC is 0.32:0.32:0.32:0.04.
[0083] In one specific embodiment, the lithium-ion battery further includes a separator with a permeability of 100~400 s / 100 mL. Optionally, the permeability of the separator can be 100 s / 100 mL, 200 s / 100 mL, 300 s / 100 mL, or 400 s / 100 mL. Limiting the permeability of the separator ensures that it possesses suitable porosity and pore connectivity, allowing the electrolyte to fully wet the separator pores, forming continuous and stable ion conduction channels. This significantly reduces the transport resistance of lithium ions penetrating the separator, alleviates battery polarization under fast charging conditions, ensures smooth high-current charging and discharging, and improves the battery's fast-charging performance.
[0084] This application does not strictly limit the choice of separator material. It can be at least one of the separator materials commonly used in lithium-ion batteries, including polypropylene separator (PP), polyethylene separator (PE), polypropylene / polyethylene bilayer composite membrane (PP / PE), polyimide electrospun separator (PI), polypropylene / polyethylene / polypropylene trilayer composite membrane (PP / PE / PP), cellulose nonwoven separator, and separator with ceramic coating.
[0085] In the specific fabrication of lithium-ion batteries, the positive electrode, separator, and negative electrode are wound or stacked to obtain a bare cell, which is then packaged into a pre-stamped aluminum-plastic film bag. After the packaged battery is dried at 85°C, the electrolyte is injected into the dried battery. The battery undergoes resting, formation, and secondary sealing to complete the fabrication of the lithium-ion battery.
[0086] A third aspect of this application provides an electrical device that includes the lithium-ion battery of the second aspect.
[0087] Thanks to the excellent energy density and fast-charging performance of this lithium-ion battery, the device can achieve efficient and long-lasting operation by relying on its stable energy supply and efficient charge and discharge characteristics, effectively improving the device's battery life and user experience, and has a wide range of application scenarios. The device in this application may include, but is not limited to, electric vehicles (such as pure electric vehicles, hybrid electric vehicles, and electric bicycles), consumer electronic devices (such as smartphones, laptops, and wearable devices), energy storage devices (such as home energy storage cabinets, industrial energy storage systems, and photovoltaic energy storage power stations), and power tools (such as electric drills, electric wrenches, and electric saws).
[0088] The present application will be further described below through specific embodiments.
[0089] Example 1
[0090] This embodiment provides a method for preparing a positive electrode sheet, including the following steps:
[0091] 1) Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, titanium dioxide, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:6:4:0.75:0.35:0.3:204 to obtain an ultra-large particle mixed slurry; the ultra-large particle mixed slurry was then subjected to sand milling to obtain an ultra-large particle slurry (Dv). 50 (250nm); spray treatment of ultra-large particle slurry (inlet air temperature 200℃, feed rate 50m). 3 / h, outlet air temperature 100℃), to obtain ultra-large particle raw meal (Dv) 50 (10μm); the ultra-large raw material was subjected to high-temperature sintering treatment under nitrogen atmosphere (temperature 790℃, time 8h) to obtain ultra-large sintered material; the ultra-large sintered material was subjected to vibration sieving to obtain ultra-large particles;
[0092] 2) Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:3.5:4.5:0.35:0.8:204 to obtain a large-particle mixed slurry; the large-particle mixed slurry was then subjected to sand milling to obtain a large-particle slurry (Dv). 50 (1100nm); large particle slurry is spray-treated (inlet air temperature 200℃, feed rate 50m). 3 / h, outlet air temperature 100℃), to obtain large-particle raw meal (Dv) 50 Large-particle raw materials were subjected to high-temperature sintering treatment under nitrogen atmosphere (temperature 810℃, time 8h) to obtain large-particle sintered material; the large particles were then subjected to crushing and deagglomeration treatment (crushing pressure 460MPa, classification frequency 60Hz) to obtain large particles.
[0093] 3) Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:3.5:4.5:0.35:0.8:204 to obtain a small-particle mixed slurry; the small-particle mixed slurry was then subjected to sand milling to obtain a small-particle slurry (Dv). 50 (380nm); spray treatment of small particle slurry (inlet air temperature 200℃, feed rate 50m). 3 / h, outlet air temperature 100℃), to obtain small-particle raw meal (Dv) 50 The small-particle raw material was subjected to high-temperature sintering treatment under nitrogen atmosphere (temperature 810℃, time 8h) to obtain small-particle sintered material; the small-particle sintered material was then subjected to crushing and deagglomeration treatment (crushing pressure 460MPa, classification frequency 60Hz) to obtain small particles.
[0094] 4) The ultra-large particles, large particles, and small particles are mechanically mixed in a mass ratio of 12.4:50.3:37.3 to obtain the positive electrode active material;
[0095] The mass percentage of doping elements (Ti, V) in the positive electrode active material is 4000 ppm, and the ratio of Ti to V is 1:2.
[0096] 5) Mix the positive electrode active material (96.7% by mass), SP, PVDF and polyvinylpyrrolidone and disperse them in NMP. Stir and mix thoroughly to form a uniform positive electrode slurry. Coat the positive electrode slurry uniformly on the aluminum foil current collector. After drying, rolling (rolling pressure of 32 tons) and slitting, the positive electrode sheet is obtained.
[0097] Example 2
[0098] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 46 tons, the mass ratio of positive electrode active material in step 5) is 97.3%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 7.9:59.1:33.
[0099] Example 3
[0100] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 32 tons, the mass ratio of positive electrode active material in step 5) is 96.7%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 10.1:54.9:35.
[0101] Example 4
[0102] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 22 tons, the mass ratio of positive electrode active material in step 5) is 96.1%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 7.7:59.5:32.8.
[0103] Example 5
[0104] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 43 tons, the mass ratio of positive electrode active material in step 5) is 97.2%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 7.1:60.8:32.1.
[0105] Example 6
[0106] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 27 tons, the mass ratio of positive electrode active material in step 5) is 96.5%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 8.6:57.8:33.6.
[0107] Example 7
[0108] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 43 tons, the mass ratio of positive electrode active material in step 5) is 97.2%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 12.2:50.7:37.1.
[0109] Example 8
[0110] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 23 tons, the mass ratio of positive electrode active material in step 5) is 96.3%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 7.3:60.4:32.3.
[0111] Example 9
[0112] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 54 tons, the mass ratio of positive electrode active material in step 5) is 97.6%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 6.5:62.1:31.4.
[0113] Example 10
[0114] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 17 tons, the mass ratio of positive electrode active material in step 5) is 95.8%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 14.7:45.6:39.7.
[0115] Example 11
[0116] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 100 tons, the mass ratio of positive electrode active material in step 5) is 98.5%, the mass ratio of ultra-large particles, large particles and small particles in step 4) is 19.9:35.1:45, and the mass ratio of dopant element (Ti) in positive electrode active material in step 4) is 4000ppm.
[0117] Example 12
[0118] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 74 tons, the mass ratio of positive electrode active material in step 5) is 98%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 15.3:44.4:40.3.
[0119] Example 13
[0120] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 50 tons, the mass ratio of positive electrode active material in step 5) is 97.4%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 12.6:49.8:37.6.
[0121] Example 14
[0122] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 10 tons, the mass ratio of positive electrode active material in step 5) is 95%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 25:25:50.
[0123] Example 15
[0124] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 12 tons, the mass ratio of positive electrode active material in step 5) is 95.2%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 6.7:61.6:31.7.
[0125] Example 16
[0126] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 16 tons, the mass ratio of positive electrode active material in step 5) is 95.7%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 5.4:64.2:30.4.
[0127] Example 17
[0128] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 18 tons, the mass ratio of positive electrode active material in step 5) is 95.9%, the mass ratio of ultra-large particles, large particles and small particles in step 4) is 5:65:30, and the mass ratio of dopant element (V) in positive electrode active material in step 4) is 4000ppm.
[0129] Example 18
[0130] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 74 tons, the mass ratio of positive electrode active material in step 5) is 98%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 14.9:45.2:39.9.
[0131] Example 19
[0132] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 75 tons, the mass ratio of positive electrode active material in step 5) is 98.1%, and the mass ratio of ultra-large particles, large particles, small particles and ultra-small particles in step 4) is 15.1:45.3:34.6:5.
[0133] The preparation method of ultrafine particles is as follows: Lithium hydroxide monohydrate, ferrous sulfate heptahydrate, 85wt% phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 0.167:1:0.433:2.4 to obtain a mixed slurry; the mixed slurry is transferred to a hydrothermal reactor for hydrothermal treatment (temperature 200℃, time 3h) to obtain lithium iron phosphate powder; lithium iron phosphate powder, glucose, polyethylene glycol, vanadium pentoxide, and ultrapure water are mixed and dispersed in a mass ratio of 100:7:4.5:0.7:166 to obtain an ultrafine particle mixed slurry; the ultrafine particle mixed slurry is then subjected to sand milling to obtain ultrafine particle slurry (Dv). 50 (250nm); spray treatment of ultrafine particle slurry (inlet air temperature 200℃, feed rate 50 m / s). 3 / h, outlet air temperature 100℃), to obtain ultra-small granular raw material; the ultra-small granular raw material is subjected to high-temperature sintering treatment under nitrogen atmosphere (temperature 730℃, time 8h) to obtain ultra-small granular sintered material; the ultra-small granular sintered material is subjected to crushing and deagglomeration treatment (crushing air pressure 460MPa, classification frequency 60Hz) to obtain ultra-small particles.
[0134] Example 20
[0135] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 79 tons, the mass ratio of positive electrode active material in step 5) is 98.2%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 14.3:46.5:39.2.
[0136] Example 21
[0137] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 17 tons, the mass ratio of positive electrode active material in step 5) is 95.8%, the mass ratio of ultra-large particles, large particles and small particles in step 4) is 5.4:64.2:30.4, and the mass ratio of dopant element (Ti) in positive electrode active material in step 4) is 9000ppm.
[0138] Example 22
[0139] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 13 tons, the mass ratio of positive electrode active material in step 5) is 95.4%, the mass ratio of ultra-large particles, large particles and small particles in step 4) is 5.6:63.7:30.7, and the mass ratio of dopant element (Ti) in positive electrode active material in step 4) is 3000ppm.
[0140] Example 23
[0141] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 108 tons, the mass ratio of positive electrode active material in step 5) is 98.6%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 17.8:39.3:42.9.
[0142] Example 24
[0143] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 20 tons, the mass ratio of positive electrode active material in step 5) is 96%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 4.8:65.4:29.8.
[0144] Comparative Example 1
[0145] The preparation method of this comparative example is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 13 tons, the mass ratio of positive electrode active material in step 5) is 95.4%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 5:65:30.
[0146] Comparative Example 2
[0147] The preparation method of this comparative example is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 93 tons, the mass ratio of positive electrode active material in step 5) is 98.4%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 24.2:26.7:49.1.
[0148] Comparative Example 3
[0149] The preparation method of this comparative example is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 6 tons, the mass ratio of positive electrode active material in step 5) is 94.3%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 5.2:64.6:30.2.
[0150] Comparative Example 4
[0151] The preparation method of this comparative example is basically the same as that of Example 1. The difference is that the rolling pressure in step 5) is 108 tons, the mass ratio of positive electrode active material in step 5) is 98.6%, and the mass ratio of ultra-large particles, large particles and small particles in step 4) is 27.1:22.8:50.1.
[0152] Experimental Example 1
[0153] The particle size distribution of the positive electrode active materials in all examples and comparative examples was tested (ultra-large particles, large particles, small particles, and ultra-small particles), and the results are shown in Table 1.
[0154] 1) Pretreatment: Use a ceramic knife to scrape off the active material powder from the surface of the positive electrode.
[0155] 2) SEM Testing: A layer of conductive adhesive is first applied to the sample holder, and the sample powder is then adhered to the sample holder. CP argon ion polishing is performed, followed by the deposition of a conductive film. The tools and sample stage are wiped with anhydrous ethanol. A certain amount of the sample to be tested is placed on the sample stage; observation is then performed under a scanning electron microscope (SEM); the magnification is adjusted using the SEM for testing and imaging. Ultra-small particles and small particles are imaged at 20kx, while large and ultra-large particles are imaged at 4kx.
[0156] 3) The dimensions of SEM images of ultra-small, small, large, and ultra-large particles were measured using graphic statistical software. The particle size was collected using the diagonal line method, and five different non-overlapping regions were selected (to avoid local area deviation). One clear SEM image was taken for each region. Edges and agglomerated areas were avoided to ensure that the particles in the image are independently dispersed and without obvious overlap.
[0157] ;
[0158] .
[0159] Among them, f i The average particle size of a single non-overlapping region, i ranges from 1 to 5, corresponding to 5 SEM images; f is the average particle size; x is the particle number within a single SEM image, ranging from 30 to 100; N ix N represents the particle size value of a single non-overlapping region. 总x The number of particles collected in a single non-overlapping region.
[0160] The statistically analyzed particle size and quantity percentages are converted into a particle size-volume percentage distribution map. The conversion formula is:
[0161] ,
[0162] .
[0163] Where Ni is the proportion of particles with diameter f, Vi' is the volume weight of particles with diameter f, and Vi is the volume percentage of particles with diameter f.
[0164] Table 1
[0165]
[0166] Experimental Example 2
[0167] The positive and negative electrode sheets, electrolytes, and separators of all the embodiments and comparative examples were assembled into lithium-ion batteries according to the following method:
[0168] 1) Graphite, carbon black, sodium carboxymethyl cellulose and polyvinylpyrrolidone are mixed in a mass ratio of 96.4:2:0.6:1 and dispersed in deionized water. The mixture is stirred thoroughly to form a uniform negative electrode slurry. The negative electrode slurry is uniformly coated on a copper foil current collector, and after drying, rolling and cutting, a negative electrode sheet is obtained.
[0169] The compaction density of the negative electrode is 1.65 g / cm³. 3 ;
[0170] 2) Mix EC, EMC, DEC, and FEC in a volume ratio of 0.32:0.32:0.32:0.04, then add LiPF6 and LiFSI to obtain the electrolyte;
[0171] The concentration of the electrolyte is 1 mol / L;
[0172] 3) Assemble the positive electrode, negative electrode and separator into a battery and inject electrolyte; after the battery is placed, formed and resealed, a lithium-ion battery is obtained.
[0173] The porosity of the positive electrode was tested, and the results are shown in Table 2.
[0174] Porosity a of the positive electrode:
[0175] The battery was discharged to 2.5V at 0.33C. The empty battery was removed, the electrodes were disassembled, and the electrodes were soaked in dimethyl carbonate (DMC) solution for 4 hours and then dried.
[0176] The electrode was then cut into 12mm diameter discs using an electrode punching machine. Simultaneously, the thicknesses of the electrode and the current collector were measured using a thickness gauge, denoted as h1 and h2 respectively. The mass of the cut electrode was measured using a balance with an accuracy of 0.00001g and recorded as m1. The volume v of the cut electrode was calculated using the formula v = πr²(h1 - h2). The electrode was then immersed in a sealed container containing a certain volume of hexadecane for 1 hour (the volume of hexadecane in the sealed solution is not critical, but the required amount must ensure complete immersion of the electrode). After 1 hour, the electrode was removed with tweezers and blotted dry on filter paper until a constant weight was achieved. Its mass was then measured using a balance and recorded as m2. The porosity a was calculated using the formula X / v, where X = (m2 - m1) / ρ, and ρ is the density of hexadecane, 0.7734 g / cm³. 3 .
[0177] Table 2
[0178]
[0179] Experimental Example 3
[0180] All the positive and negative electrode sheets, electrolytes and separators of the embodiments and comparative examples were assembled into lithium-ion batteries according to the method shown in Experimental Example 2. The energy density and fast charging performance of the lithium-ion batteries were tested, and the results are shown in Table 3.
[0181] 1. Energy density
[0182] Weigh the battery and record the weight as m; place the battery in a fixture, apply a force of 3000N, charge it with a constant current of 0.33C to the upper limit voltage of 3.65V, let it rest for 30min, discharge it with a constant current of 0.33C to the lower limit voltage of 2.5V, let it rest for 30min, and repeat the cycle 3 times; obtain the discharge capacity (in Ah) and energy E (average of three cycles), energy density = E / m (in Wh / kg).
[0183] 2. Fast charging performance
[0184] 1) Place the battery in a 25°C incubator until thermal equilibrium is reached;
[0185] 2) Charge the battery at a constant current rate of 1 / 3C to the upper limit voltage of 3.65V, charge it at a constant voltage rate until the current is less than 0.05C, and then discharge it at 0.33C to the lower limit voltage of 2.5V. Repeat this process more than 3 times to obtain the discharge capacity of the battery and record the battery capacity C1.
[0186] 3) Let it stand for 5 minutes;
[0187] 4) Adjust the battery charge to 50% SOC at a 1 / 3C discharge rate;
[0188] 5) Discharge at a 1C rate current for 18 seconds, record the battery voltage U2, current I before discharge stops, and battery voltage U1 after the battery voltage stabilizes. Calculate the DC internal resistance DCR using the formula DCR=(U2-U1) / I, in mΩ.
[0189] Table 3
[0190]
[0191] As shown in Table 3, this application constructs a three-level nested particle structure of "ultra-large-large-small" and regulates the synergistic relationship between a and b, thereby improving the compaction density of the positive electrode sheet and promoting lithium-ion transport, thus synergistically enhancing the energy density and fast-charging performance of the battery.
[0192] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
Claims
1. A positive electrode plate, characterized in that, The positive electrode sheet includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, the positive electrode active material includes lithium iron phosphate, and the lithium iron phosphate includes ultra-large particles, large particles and small particles; The volumetric particle size distribution curve of the positive electrode active material includes a D peak corresponding to the ultra-large particles, a C peak corresponding to the large particles, and a B peak corresponding to the small particles. The particle size corresponding to the vertex of the D peak is I. D 4μm D ≤35μm; the particle size corresponding to the C peak apex is I C ,1μm≤I C ≤4μm; the particle size corresponding to the apex of peak B is I B 120nm≤I B ≤800nm; The positive electrode plate satisfies 0.5 ≤ a / b ≤ 2. Wherein, 'a' represents the porosity of the positive electrode; and 'b' = F D / F C F D F is the peak intensity corresponding to the peak of peak D. C This represents the peak intensity corresponding to the apex of peak C.
2. The positive electrode sheet according to claim 1, characterized in that, 10%≤a≤40%, 0.05≤b≤1.
3. The positive electrode sheet according to claim 2, characterized in that, 20%≤a≤30%, 0.15≤b≤0.
40.
4. The positive electrode sheet according to any one of claims 1-3, characterized in that, 0.5%≤F D ≤10%,10%≤F C ≤40%。 5. The positive electrode sheet according to any one of claims 1-3, characterized in that, I D -I C >2μm; and / or, I C -I B >0.5μm。 6. The positive electrode sheet according to any one of claims 1-3, characterized in that, The peak intensity corresponding to the apex of peak B is F. B 10%≤F B ≤40%, F B <F C F B >F D .
7. The positive electrode sheet according to claim 6, characterized in that, 0.5% <F C -F B <3%; and / or, F C -F D >10%; and / or, F B -F D >10%。 8. The positive electrode sheet according to any one of claims 1-3, characterized in that, The lithium iron phosphate also includes ultra-small particles, and the volume particle size distribution curve of the positive electrode active material also includes the A peak corresponding to the ultra-small particles.
9. The positive electrode sheet according to claim 8, characterized in that, The peak intensity corresponding to the apex of peak A is F. A F A <F B F A <F D .
10. The positive electrode sheet according to claim 9, characterized in that, F B -F A >2%。 11. The positive electrode sheet according to claim 8, characterized in that, The particle size corresponding to the apex of peak A is I. A ,20nm≤I A ≤100nm.
12. The positive electrode sheet according to claim 11, characterized in that, I B -I A >50nm。 13. The positive electrode sheet according to any one of claims 1-3, characterized in that, The ultra-large particles include a lithium iron phosphate core and a coating layer covering at least a portion of the surface of the lithium iron phosphate core. The coating layer includes carbon and has a thickness of 0.5~120 nm.
14. The positive electrode sheet according to claim 8, characterized in that, The ultra-small particles comprise a lithium iron phosphate core and a coating layer covering at least a portion of the surface of the lithium iron phosphate core, the coating layer comprising carbon, and the coating layer having a thickness of 0.5~20 nm.
15. The positive electrode sheet according to any one of claims 1-3, characterized in that, The compaction density of the positive electrode sheet is 2~3 g / cm³. 3 ; and / or, The resistivity of the positive electrode active material is 2~20Ω / cm; and / or, The chemical composition of the lithium iron phosphate is LiFe x T y PO4, wherein 0.991≤x≤0.997, 0.003≤y≤0.007, and T is a doping element, including at least one of Ti, V, Nb, Mg, Mn, Zn, Zr, Ni, and Al, and the mass percentage of the doping element in the lithium iron phosphate is 3000~9000ppm.
16. A lithium-ion battery, characterized in that, The positive electrode includes any one of claims 1-15.
17. The lithium-ion battery according to claim 16, characterized in that, The lithium-ion battery also includes a negative electrode sheet, the negative electrode sheet having a compaction density of 1.6~1.7 g / cm³. 3 .
18. The lithium-ion battery according to claim 17, characterized in that, The negative electrode sheet includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material has a Dv 50 The value is 5~20μm.
19. The lithium-ion battery according to claim 16, characterized in that, The lithium-ion battery also includes an electrolyte, the viscosity of which is 2~5 cP at 25°C.
20. The lithium-ion battery according to claim 19, characterized in that, The electrolyte includes additives, which include at least one of vinylene carbonate, fluoroethylene carbonate, ethylene sulfate, tris(trimethylsilyl) phosphite, and lithium difluorosulfonylimide, and the additives account for 0.05% to 2.5% of the mass of the electrolyte.
21. The lithium-ion battery according to claim 16, characterized in that, The lithium-ion battery also includes a separator, the separator having an air permeability of 100~400s / 100mL.