A Sb₂O₃ / C composite material, its preparation method, and its application in an aqueous zinc-iodine battery.

By preparing Sb2O3/C composite material as the positive electrode of zinc-iodine battery, the problems of slow iodine migration and reaction kinetics in zinc-iodine battery were solved, the charge-discharge performance and stability of battery were improved, and the effects of high capacity and low internal resistance were achieved.

CN123073069APending Publication Date: 2026-11-10LIAONING UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611283259.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Zinc-iodine batteries suffer from problems such as loss of active material and slow reaction kinetics due to the migration of soluble polyiodide intermediates generated from the iodine cathode during charging and discharging, which affect the utilization rate of active material, discharge capacity and cycle stability.

Method used

Sb2O3/C composite material is used as the positive electrode material. It is prepared by hydrothermal method and calcination method. Iodine is anchored on the material by gas phase thermal diffusion method to enhance conductivity and ion diffusion rate. The specific surface area is increased by particulate structure.

Benefits of technology

It significantly improves the conductivity and ion diffusion rate of the material, increases the specific surface area, improves the charge-discharge performance and stability, increases the capacity to 210 mAh/g, reduces the internal resistance, and has high energy density and power density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073069A_ABST
    Figure CN123073069A_ABST
Patent Text Reader

Abstract

This invention discloses an Sb₂O₃ / C composite material, its preparation method, and its application in aqueous zinc-iodine batteries, belonging to the field of electrode material technology. This invention prepares the Sb₂O₃ / C composite material through a simple hydrothermal and calcination method. The granular structure on its surface increases the specific surface area of ​​the material and effectively promotes ion diffusion and charge transfer, improving the conductivity of Sb₂O₃ / C, reducing its internal resistance, and maintaining the structural flexibility and stability of the material, thereby enhancing the overall performance of the aqueous zinc-iodine battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrode material technology, specifically relating to an Sb2O3 / C composite material, its preparation method, and its application in aqueous zinc-iodine batteries. Background Technology

[0002] With the continued growth of global energy consumption and the increasingly prominent resource shortages and environmental pollution caused by the large-scale use of traditional fossil fuels, the development of advanced energy storage technologies that combine economic efficiency and long-term cycle stability has become a crucial task in the energy sector. Among various electrochemical energy storage systems, lithium-ion batteries, with their high energy density and good cycle life, have been widely used for the storage, grid connection, and efficient utilization of intermittent renewable energy sources such as solar and wind power. However, due to the relatively limited reserves of lithium resources in the Earth's crust and their uneven geographical distribution, lithium-ion batteries still face challenges such as high raw material prices, insufficient resource supply stability, and strong dependence on the industrial chain. Meanwhile, the rapid development of rail transit electrification and next-generation portable electronic devices has placed higher demands on the safety, cost, and overall performance of energy storage devices. Therefore, developing alternative electrochemical energy storage systems that are rich in resources, have low manufacturing costs, and possess inherent safety is of great significance.

[0003] Rechargeable aqueous zinc-ion batteries (RAZBs) utilize safer aqueous electrolytes, while zinc metal anodes offer advantages such as abundant resources, low cost, suitable redox potential, and high theoretical specific capacity. Therefore, they are considered one of the most promising energy storage technologies in the post-lithium-ion battery era. Among numerous cathode material systems, halogen cathode materials based on conversion reaction mechanisms, such as chlorine, bromine, and iodine, have attracted widespread attention due to their high theoretical specific capacity and abundant raw material sources. Iodine, in particular, possesses relatively abundant sources, suitable reactivity, and a high theoretical specific capacity, providing a good resource foundation for the large-scale promotion and application of zinc-iodine batteries. Because zinc-iodine batteries achieve a good balance between electrochemical performance, operational safety, and economic cost, they are considered one of the most industrially promising aqueous battery systems.

[0004] However, zinc-iodine batteries still face several unresolved issues in practical applications. Firstly, during charging and discharging, iodine cathodes generate soluble polyiodide intermediates. These polyiodides readily migrate between the positive and negative electrodes, causing a shuttle effect. This not only leads to the continuous loss of active material from the positive electrode but may also diffuse to the zinc anode surface, triggering self-discharge and other side reactions. Secondly, the redox process between iodine species typically involves multiple consecutive conversion steps, resulting in relatively slow overall reaction kinetics. These problems interact, leading to insufficient utilization of active material, low actual discharge capacity, decreased coulombic efficiency, and poor cycle stability in zinc-iodine batteries, severely hindering their further commercialization and large-scale application. Summary of the Invention

[0005] To address the above problems, this invention provides an Sb2O3 / C composite material, its preparation method, and its application in an aqueous zinc-iodine battery.

[0006] The technical solution adopted in this invention is: a Sb2O3 / C composite material, with a molar ratio of C:Sb2O3 = (100 -400):1.

[0007] A method for preparing an Sb2O3 / C composite material includes: dissolving antimony salt and urea in a mixed solution of deionized water and ethylene glycol, adding biomass carbon, ultrasonicating and stirring at room temperature, transferring the resulting mixture to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene for hydrothermal reaction, cooling to room temperature, centrifuging and washing, vacuum drying, and calcining the resulting product under an argon atmosphere to obtain the Sb2O3 / C composite material.

[0008] Furthermore, the antimony salt is antimony trichloride.

[0009] Furthermore, in the mixed solution of deionized water and ethylene glycol, the volume ratio of deionized water to ethylene glycol is 1:(0.5 - 1.5).

[0010] Furthermore, the biomass carbon is biomass carbon produced by calcining coconut shells.

[0011] Furthermore, the hydrothermal reaction is carried out at a temperature of 155 ℃ - 165 ℃ for a reaction time of 12 h - 14 h.

[0012] Furthermore, the calcination is performed by heating to 350°C - 450°C at a heating rate of 5°C / min - 10°C / min and holding at that temperature for 2 h - 3 h.

[0013] The application of the Sb2O3 / C composite material provided by this invention as a positive electrode material in aqueous zinc-iodine batteries.

[0014] Further, the method includes the following steps: the active material iodine is anchored on the Sb2O3 / C composite material by gas-phase thermal diffusion of Sb2O3 / C composite material with elemental iodine; the obtained product is mixed evenly with binder and conductive material; a small amount of N-methylpyrrolidone (NMP) is added dropwise as a solvent; after mixing evenly, it is directly coated on a substrate and vacuum dried to obtain a positive electrode sheet coated with Sb2O3 / C-I2 composite material.

[0015] Furthermore, by mass ratio, the Sb2O3 / C composite material : iodine element = 1 : 1.

[0016] Furthermore, the adhesive is polyvinylidene fluoride (PVDF).

[0017] Furthermore, the conductive material is Super P.

[0018] The beneficial effects of this invention are:

[0019] 1. This invention prepares Sb2O3 / C composite materials through a simple hydrothermal and calcination method, which significantly improves the conductivity and ion diffusion rate of the material while reducing the internal resistance.

[0020] 2. The Sb2O3 / C composite material prepared by this invention has a granular structure on its surface that increases the specific surface area of ​​the material, thereby improving the specific capacity and rate performance of the material during charge and discharge.

[0021] 3. The Sb2O3 / C composite material prepared by this invention has the characteristics of low cost, simple preparation process, readily available raw materials and good electrochemical stability.

[0022] 4. The Sb2O3 / C composite material prepared by this invention has advantages such as high energy density and power density.

[0023] 5. The aqueous zinc-iodine battery provided by this invention has relatively simple material synthesis and battery assembly processes, and the reaction conditions are easy to control, thus having certain potential for large-scale preparation.

[0024] 6. The modified Sb2O3 / C composite material prepared according to the present invention, as an electrode material, improves the stability of the electrode and increases the capacity from 140 mAh / g to 210 mAh / g. Attached Figure Description

[0025] Figure 1 This is the XRD pattern of the Sb2O3 / C composite material prepared in Example 1.

[0026] Figure 2 This is the SEM image of the Sb2O3 / C composite material prepared in Example 1.

[0027] Figure 3 This is a cyclic voltammetry curve of the Sb2O3 / C composite material prepared in Example 1.

[0028] Figure 4 This is a cycle diagram of the Sb2O3 / C composite material prepared in Example 1. Detailed Implementation

[0029] The technical solution of the present invention will be further described below, but it is not limited thereto. Any modifications or equivalent substitutions to the technical solution of the present invention that do not depart from the spirit and scope of the technical solution of the present invention should be covered within the protection scope of the present invention.

[0030] Example 1: Sb2O3 / C composite material

[0031] I. Preparation Method

[0032] Antimony trichloride (35 mg, 0.153 mmol) and urea (80 mg, 1.33 mmol) were dissolved in a mixture of 17.5 mL deionized water and 17.5 mL ethylene glycol. Then, 200 mg (16.65 mmol) of biomass charcoal (AC) made from coconut shells was added. The mixture was then sonicated for 30 min and stirred for 1 h at room temperature to ensure thorough mixing. After thorough mixing, the mixture was transferred to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene (PTFE) and hydrothermally reacted at 160 °C for 12 h. Once the reactor had completely cooled to room temperature, the product was removed, washed three times by centrifugation with deionized water and anhydrous ethanol, respectively. After vacuum drying, the product was transferred to a tube furnace and heated to 400 °C at a rate of 5 °C / min under an argon atmosphere. The mixture was then calcined at this temperature for 2 h and allowed to cool naturally to room temperature, yielding an Sb₂O₃ / C composite material with a C to Sb₂O₃ molar ratio of 200:1.

[0033] II. Testing

[0034] Figure 1 This is the XRD pattern of the Sb₂O₃ / C prepared in this embodiment. Figure 1 As can be seen, the XRD pattern of the sample is basically consistent with the standard pattern of Sb₂O₃, with a carbon peak at 22°. This indicates that Sb₂O₃ / C was successfully synthesized.

[0035] Figure 2 This is the SEM image of the Sb₂O₃ / C prepared in this embodiment. Figure 2 It is evident that the Sb2O3 in the prepared Sb2O3 / C has a typical granular structure.

[0036] Example 2 Sb2O3 / C composite material

[0037] Preparation method

[0038] Antimony trichloride (17.75 mg, 0.076 mmol) and urea (40 g, 0.65 mmol) were dissolved in a mixture of 17.5 mL deionized water and 17.5 mL ethylene glycol. Then, 200 mg (16.65 mmol) of biomass charcoal (AC) made from coconut shells was added. The mixture was then sonicated for 30 min and stirred for 1 h at room temperature to ensure thorough mixing. After thorough mixing, the mixture was transferred to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene (PTFE) and hydrothermally reacted at 160 °C for 12 h. Once the reactor had completely cooled to room temperature, the product was removed and washed three times by centrifugation with deionized water and anhydrous ethanol, respectively. After vacuum drying, the product was transferred to a tube furnace and calcined at 400 °C at a heating rate of 5 °C / min under an argon atmosphere for 2 h. The mixture was then naturally cooled to room temperature to obtain an Sb₂O₃ / C composite material with a C to Sb₂O₃ molar ratio of 400:1.

[0039] Example 3 Sb2O3 / C composite material

[0040] Preparation method

[0041] Antimony trichloride (70 mg, 0.306 mmol) and urea (160 mg, 2.66 mmol) were dissolved in a mixture of 17.5 mL deionized water and 17.5 mL ethylene glycol. Then, 200 mg (16.65 mmol) of biomass charcoal (AC) made from coconut shells was added. The mixture was then sonicated for 30 min and stirred for 1 h at room temperature to ensure thorough mixing. After thorough mixing, the mixture was transferred to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene (PTFE) and hydrothermally reacted at 160 °C for 12 h. After the reactor had completely cooled to room temperature, the product was removed, washed three times by centrifugation with deionized water and anhydrous ethanol, respectively, and vacuum dried. The product was then transferred to a tube furnace and calcined at 400 °C at a heating rate of 5 °C / min under an argon atmosphere for 2 h. After natural cooling to room temperature, an Sb₂O₃ / C composite material with a C to Sb₂O₃ molar ratio of 100:1 was obtained.

[0042] Example 4: Application of Sb2O3 / C composite material as positive electrode material in aqueous zinc-iodine batteries

[0043] I. Aqueous Zinc-Iodine Batteries

[0044] 1. The preparation method is as follows:

[0045] 1) Preparation of positive electrode sheet:

[0046] The Sb2O3 / C composite material prepared in Example 1 was mixed with elemental iodine at a mass ratio of 1:1 using a gas-phase thermal diffusion method to anchor the active material iodine onto the Sb2O3 / C composite material. 80 mg of the obtained product was weighed and mixed evenly with 10 mg of PVDF and 10 mg of Super-p. A small amount of NMP was added as a solvent and mixed evenly. The mixture was then directly coated onto a carbon paper substrate and dried in a vacuum drying oven at 60 °C. The resulting positive electrode sheet coated with the Sb2O3 / C-I2 composite material was obtained.

[0047] 2) Negative electrode preparation:

[0048] Zinc sheets with a thickness of 0.1 mm and a purity of 99.99% are repeatedly sanded to remove the oxide layer on the surface. The sanded zinc sheets are then cut into circles with a diameter of 12 mm to make negative electrode sheets.

[0049] 3) Assembling aqueous zinc-iodine batteries:

[0050] Using the positive electrode sheet prepared in step 1) as the positive electrode and the negative electrode sheet prepared in step 2) as the negative electrode, and selecting 1M zinc sulfate and 0.1M potassium iodide as the electrolyte, an Sb2O3 / C aqueous zinc-iodine battery is obtained.

[0051] 2. Electrochemical performance testing

[0052] Comparative Experiments: 1) Biomass carbon (AC) made from coconut shells was mixed with elemental iodine at a mass ratio of 1:1 using a gas-phase thermal diffusion method to anchor the active material iodine onto the biomass carbon. 80 mg of the resulting product was weighed and mixed evenly with 10 mg of PVDF and 10 mg of SuperP. A small amount of NMP was added as a solvent, and the mixture was thoroughly mixed. This mixture was then directly coated onto a carbon substrate and dried in a vacuum drying oven at 60 ℃. The resulting positive electrode was coated with AC-I2. 2) A zinc sheet with a thickness of 0.1 mm and a purity of 99.99% was repeatedly sanded to remove the oxide layer. The sanded zinc sheet was then cut into circles with a diameter of 12 mm to form the negative electrode. 3) Using the prepared positive electrode as the positive electrode and the prepared negative electrode as the negative electrode, a zinc-iodine battery was obtained by selecting 1M zinc sulfate and 0.1M potassium iodide as the electrolyte.

[0053] Figure 3 This is the cyclic voltammogram of an Sb₂O₃ / C aqueous zinc-iodine battery. (From...) Figure 3 It is evident that the cyclic voltammetry curve area of ​​the Sb₂O₃ / C aqueous zinc-iodine battery is larger than that of the aqueous zinc-iodine battery made from pure biomass carbon (AC) produced from coconut shells. This indicates that the capacity of the Sb₂O₃ / C aqueous zinc-iodine battery is improved.

[0054] Figure 4 This is a cycle diagram of an Sb₂O₃ / C aqueous zinc-iodine battery. (From...) Figure 4It can be seen that the Sb₂O₃ / C aqueous zinc-iodine battery operates at a current density of 1 A·g⁻¹. -1 The material exhibits a high cycle life of 1000 cycles with excellent capacity retention. This is attributed to the more uniform and ordered deposition of Sb₂O₃ on carbon in the Sb₂O₃ / C composite material formed at a molar ratio of C:Sb₂O₃ = 200:1. This increases the specific surface area of ​​the material, providing more active sites and thus more interfacial sites for adsorption and anchoring of iodine and polyiodides. This helps to inhibit the diffusion and shuttle of soluble polyiodides and promotes the reversible redox transformation of iodine species, thereby improving its electrochemical performance. Figure 4 It is evident that the Sb2O3 / C aqueous zinc-iodine battery exhibits superior cycle stability compared to the AC aqueous zinc-iodine battery made from pure biomass carbon produced from coconut shells.

[0055] II. The Influence of Sb₂O₃ / C Composite Materials with Different Molar Ratios as Cathode Materials on the Electrochemical Performance of Assembled Aqueous Zinc-Iodine Batteries

[0056] 1. The preparation method is as follows:

[0057] 1) Preparation of positive electrode sheet:

[0058] The Sb2O3 / C composite materials prepared in Examples 1-3 were respectively mixed with elemental iodine at a mass ratio of 1:1 using a gas-phase thermal diffusion method to anchor the active material iodine onto the Sb2O3 / C composite material. 80 mg of the obtained product was weighed and mixed evenly with 10 mg of PVDF and 10 mg of Super P. A small amount of NMP was added as a solvent and mixed evenly. The mixture was then directly coated onto a carbon paper substrate and dried in a vacuum drying oven at 60 °C. The resulting positive electrode sheets were obtained with different molar ratios of C to Sb2O3, respectively.

[0059] 2) Negative electrode preparation:

[0060] Zinc sheets with a thickness of 0.1 mm and a purity of 99.99% are repeatedly sanded to remove the oxide layer on the surface. The sanded zinc sheets are then cut into circles with a diameter of 12 mm to make negative electrode sheets.

[0061] 3) Assembling aqueous zinc-iodine batteries:

[0062] Using the positive electrode sheet prepared in step 1) as the positive electrode and the negative electrode sheet prepared in step 2) as the negative electrode, and selecting 1M zinc sulfate and 0.1M potassium iodide as the electrolyte, different Sb2O3 / C aqueous zinc-iodine batteries were obtained.

[0063] 2. Electrochemical performance testing

[0064] The experimental method was the same as that used in the above-mentioned aqueous zinc-iodine battery test, and the test results are shown in Table 1.

[0065] Table 1. Effect of different molar ratios of Sb₂O₃ / C composite materials as cathode materials on the specific capacity of assembled aqueous zinc-iodine batteries.

[0066]

[0067] Based on the three different aqueous zinc-iodine batteries assembled according to the above embodiments, the results in Table 1 show that Example 1 exhibits the best electrochemical performance. This is because, at a molar ratio of C:Sb₂O₃ = 200:1, the Sb₂O₃ deposits more uniformly and orderly on the carbon in the resulting Sb₂O₃ / C composite material, increasing the specific surface area of ​​the material and providing more active sites. This provides more interfacial sites for adsorption and anchoring of iodine and polyiodides, which helps to inhibit the diffusion and shuttle of soluble polyiodides and promotes the reversible redox transformation of iodine species, thereby improving its electrochemical performance.

Claims

1. A Sb₂O₃ / C composite material, characterized in that, In the Sb2O3 / C composite material, the molar ratio is C : Sb2O3 = (100 - 400):

1.

2. The method for preparing the Sb₂O₃ / C composite material according to claim 1, characterized in that, The preparation method includes: dissolving antimony salt and urea in a mixed solution of deionized water and ethylene glycol, adding biomass carbon, sonicating and stirring at room temperature, transferring the resulting mixture to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene, carrying out a hydrothermal reaction, cooling to room temperature, centrifuging and washing, vacuum drying, and calcining the resulting product under an argon atmosphere to obtain the Sb2O3 / C composite material.

3. The method for preparing a Sb₂O₃ / C composite material according to claim 2, characterized in that, The antimony salt is antimony trichloride.

4. The method for preparing a Sb₂O₃ / C composite material according to claim 2, characterized in that, In the mixed solution of deionized water and ethylene glycol, the volume ratio of deionized water to ethylene glycol is 1:(0.5 - 1.5).

5. The method for preparing a Sb₂O₃ / C composite material according to claim 2, characterized in that, The biomass carbon is biomass carbon produced by calcining coconut shells.

6. The method for preparing a Sb₂O₃ / C composite material according to claim 2, characterized in that, The hydrothermal reaction is carried out at a temperature of 155 ℃ - 165 ℃ for a time of 12 h - 14 h.

7. The method for preparing a Sb₂O₃ / C composite material according to claim 2, characterized in that, The calcination is performed by heating to 350℃-450℃ at a heating rate of 5℃ / min-10℃ / min and holding at that temperature for 2-3 hours.

8. The application of the Sb2O3 / C composite material as a positive electrode material in an aqueous zinc-iodine battery according to claim 1.

9. The application according to claim 8, characterized in that, The method includes the following steps: Iodine is anchored onto the Sb2O3 / C composite material via gas-phase thermal diffusion of the Sb2O3 / C composite material with elemental iodine. The resulting product is then mixed uniformly with a binder and conductive material. A small amount of N-methylpyrrolidone is added as a solvent, and the mixture is further mixed uniformly. The mixture is then directly coated onto a substrate and vacuum dried to obtain a positive electrode coated with the Sb2O3 / C-I2 composite material.

10. The application according to claim 9, characterized in that, By mass ratio, the Sb2O3 / C composite material: iodine element = 1:1; the binder is polyvinylidene fluoride; the conductive material is Super P.