A method for preparing large-size flow channel graphite composite bipolar plates
By combining high-temperature molding and water bath cooling, the problems of warping and low production efficiency of large-size graphite composite bipolar plates were solved, achieving efficient and flat bipolar plate preparation, improving electrical conductivity and mechanical properties, and meeting the needs of large-scale production.
Patent Information
- Application Number
- CN202611239064.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-16
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies for preparing large-size graphite composite bipolar plates suffer from problems such as warping deformation and low production efficiency, especially the inhomogeneity caused by stress concentration during molding and the difficulty in solving warping deformation.
The method of high-temperature molding combined with water bath cooling is adopted. By molding at 190-200℃ and cooling in a constant temperature water bath at 60-90℃, the holding time is shortened. The high thermal conductivity of water is used to uniformly release residual thermal stress, and moisture is removed by low-temperature drying, thus achieving a rapid and efficient preparation process.
The efficient preparation of large-size flow channel graphite composite bipolar plates has been achieved, with a flatness of 0.19-0.22 mm, significantly improved electrical conductivity and mechanical properties, and a single molding cycle shortened by more than 60%, meeting the needs of large-scale industrial production.
Smart Images

Figure CN123073091A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flow battery technology, specifically to a method for preparing a large-size flow channel graphite composite bipolar plate. Background Technology
[0002] In the existing technology, the preparation method of graphite composite bipolar plates includes molding. Molding has the advantages of one-time molding and high production efficiency, but it faces severe technical challenges when preparing large-size bipolar plates.
[0003] Large-size bipolar plates have a long, narrow, and deep flow channel groove structure. During molding, local peak stresses much higher than the nominal stress are generated at the intersection of the flow channel and the plane, forming typical geometric stress concentration areas. The fabrication of large-size bipolar plates further amplifies the non-uniformity during the pressing process, making stress concentration in certain areas more significant. If these stresses cannot be uniformly released during the demolding and cooling processes after heat preservation and pressure holding, it will directly lead to warping deformation of the bipolar plate.
[0004] To ensure molding quality, traditional techniques typically set the molding temperature at a low level, with holding time generally exceeding 40 minutes. This severely restricts the efficiency of large-size bipolar plates in mass production. Theoretically, increasing the holding temperature can reduce the holding time, but there is a temperature difference between the edge and center of a large mold. The resin curing speed and shrinkage vary in different areas, and the temperature difference with the ambient temperature is even greater. Excessive cooling will exacerbate warping problems.
[0005] To mitigate the problems caused by rapid cooling, the sheet can be placed in the mold after molding for slow cooling until it reaches room temperature. This cooling method can greatly alleviate the stress concentration problem caused by the sheet rapidly contacting the cooling medium. However, this will result in the mold being occupied for a long time, further slowing down the production cycle. Moreover, the mold will age faster during the heating and cooling cycle, which is not conducive to the long-term use of the mold. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing large-size flow channel graphite composite bipolar plates, so as to solve the technical problem that the preparation efficiency and plate quality cannot be coordinated in the prior art.
[0007] To solve the above-mentioned technical problems, the present invention specifically provides the following technical solution: A method for preparing a large-size flow channel graphite composite bipolar plate includes the following steps: S100. Preheat the mold. Preheat the upper and lower molds to 190-200℃ and maintain the temperature and pressure until the temperature inside the mold stabilizes. S200, Powder spreading and hot pressing: The composite graphite powder is evenly spread in the mold cavity and then hot-pressed into shape. S300, Open the mold and remove the plate. After opening the mold, remove the formed graphite plate from the mold to form the bipolar plate. S400, Water bath cooling: The entire molded bipolar plate is immersed in a water bath to cool down to the water bath temperature. The water bath temperature is a constant temperature value and is higher than the temperature of natural cooling, specifically set to 60-90℃. S500, drying treatment: After the formed bipolar plate is cooled in a water bath, it is placed in an oven to dry and remove moisture, thus obtaining the finished bipolar plate.
[0008] Furthermore, the composite graphite powder is obtained by mixing flake graphite, expanded graphite, and phenolic resin.
[0009] Furthermore, in the composite graphite powder, by mass percentage, flake graphite and expanded graphite together account for 80%-85%, and phenolic resin accounts for 15%-20%.
[0010] Furthermore, the flake graphite is 50-100 mesh, and the expanded graphite is 300-600 mesh.
[0011] Furthermore, the flake graphite and the expanded graphite are configured in a 1:1 mass ratio.
[0012] Furthermore, the method for opening the mold and removing the plate includes: using a suction cup robot to adhere to the top wall of the molded bipolar plate to grasp it and remove it from the mold cavity.
[0013] Furthermore, the method for cooling the molded bipolar plate in a water bath includes: placing the molded bipolar plate into a water bath device, the water bath device including a water bath tank and a support plate inside it, laying the molded bipolar plate on the support plate, and then covering the molded bipolar plate with a cover plate, so that both sides of the molded bipolar plate are stably clamped and bear clamping force, so as to suppress the deformation of the molded bipolar plate during the cooling process.
[0014] Furthermore, the method of applying clamping force includes applying pressure to the cover plate after the cover plate covers the shaped bipolar plate.
[0015] Compared with the prior art, the present invention has the following advantages: This invention raises the molding temperature to 190-200℃, shortens the heat preservation and pressure holding time from more than 40 minutes in the traditional process to 8-15 minutes, and reduces the single molding cycle by more than 60%. The water bath treatment and low temperature drying stages both have the ability to process multiple plates in parallel. The entire process can achieve continuous batch production, and still achieve a flatness of 0.19~0.22mm. This invention realizes the efficient and high flatness preparation of large-size flow channel graphite composite bipolar plates.
[0016] This invention utilizes the high thermal conductivity of water to achieve a relatively stable cooling of the plate from its high-temperature molding state to a water bath temperature. This solves the problem of residual thermal stress accumulated inside the plate during high-temperature curing and molding, reducing microcracks and interface defects caused by stress concentration. The electrical conductivity reaches 121.3 S / cm, and the contact resistance reaches 10.5 mΩ·cm. 2 The bending strength reaches 43.3 MPa and the compressive strength reaches 91.1 MPa. Under rapid preparation conditions, the above excellent properties can still be obtained, realizing the synergistic improvement of preparation efficiency and plate quality. Attached Figure Description
[0017] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.
[0018] Figure 1 This is a perspective view of an embodiment of the present invention; Figure 2 This is a perspective view of the water bath device and loading device according to an embodiment of the present invention; Figure 3 This is a top view of the water bath device according to an embodiment of the present invention; Figure 4 for Figure 3 A cross-sectional view along the AA direction, showing the first working condition; Figure 5 for Figure 4 A schematic diagram for the second operating condition; Figure 6 This is a top view of a partial structure of the cover plate according to an embodiment of the present invention; Figure 7 for Figure 6 A cross-sectional view along the BB direction.
[0019] The reference numerals in the figure are as follows: 1-Bipolar plate; 11-Upper mold; 12-Lower mold; 2-Water bath device; 21-Water bath tank; 22-Support plate; 221-Base; 222-Lower hollow plate; 3-Loading device; 31-Cover plate; 311-Upper hollow plate; 312-Pin; 313-Nut; 32-First moving mechanism; 33-Third moving mechanism; 34-Lower support block; 35-Upper pressure block; 36-Structural plate; 361-External threaded sleeve; 362-Quick connector; 37-Elastic element; 4-Transfer device; 41-Suction cup robot; 42-Second moving mechanism. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0021] This invention provides a method for preparing large-size flow channel graphite composite bipolar plates, comprising the following steps: S100. Preheat the mold. Preheat the upper and lower molds to 190-200℃ and maintain the temperature and pressure until the temperature inside the mold stabilizes. S200, Powder spreading and hot pressing: The composite graphite powder is evenly spread in the mold cavity and then hot-pressed into shape. S300, Mold opening and plate removal: After mold opening, the formed graphite plate is removed from the mold to form the bipolar plate. The uniform suction force supports the transfer of the formed graphite plate and suppresses the deformation of the formed graphite plate caused by contact with air after the mold cavity is opened. S400, Water bath cooling: The entire formed bipolar plate is immersed in a water bath to cool down to the water bath temperature. The water bath temperature is a constant temperature value and is higher than the temperature of natural cooling, specifically set to 60-90℃.
[0022] S500 Drying treatment: After the formed bipolar plate is cooled in a water bath, it is placed in an oven to dry and remove moisture, causing the residual moisture in the plate to diffuse and evaporate outward, so that the formed graphite plate changes from a wet state to a dry and stable state, and the finished bipolar plate is obtained.
[0023] During the synchronous cooling process, the water bath temperature reduces the temperature gradient between the inside and outside of the molded graphite plate compared to the auto-ignition temperature. The residual thermal stress accumulated inside the plate during high-temperature curing and molding can be released relatively evenly (or the release difference is small) under the efficient heat exchange of the water medium, thus producing a small impact.
[0024] The core feature of the preparation method provided by this invention is that: the curing time is greatly shortened by high temperature molding (190-200℃), and the plate is cooled synchronously and the internal stress is released uniformly by constant temperature water bath (60-90℃) which is higher than the natural cooling temperature. Finally, the moisture is removed by drying.
[0025] In this preparation process, water bath cooling does not occupy the mold, and the mold can immediately enter the next molding cycle, thus balancing the quality of the plate and the preparation efficiency.
[0026] Furthermore, large-size graphite composite bipolar plates with flow channel structures are directly molded using high-temperature rapid molding. When subjected to a water bath, the thermal conductivity of water is far superior to air cooling, resulting in more uniform cooling of all parts of the bipolar plate. This allows for the even release of internal thermal stress, preventing warping caused by uneven cooling and resulting in a smoother plate. Finally, low-temperature drying removes residual moisture, ensuring high production efficiency while yielding large-size bipolar plate products with excellent flatness.
[0027] Furthermore, during the heating process, water has a much higher heat transfer efficiency than air, and the homogeneity of water temperature is also higher than that of air. This results in almost uniform cooling rates across different parts of the board, with volume shrinkage occurring almost simultaneously. This reduces the impact of significant differences between the surface shrinkage and the core expansion at high temperatures, effectively eliminating internal stress caused by shrinkage due to significant non-uniformity.
[0028] In a preferred embodiment, the composite graphite powder is obtained by mixing flake graphite, expanded graphite, and phenolic resin. The phenolic resin can cure rapidly within the high-temperature molding temperature range (190-200℃), providing a material basis for short holding times. Simultaneously, the composite structure of flake graphite and expanded graphite imparts a certain degree of thermal conductivity to the plate, facilitating efficient heat transfer from the plate's interior to the water medium during the water bath cooling step, and reducing the temperature gradient between the inside and outside of the molded graphite plate.
[0029] The total content of graphite powder is 80%-85%, and phenolic resin is 15%-20%. As a resin system, if the content of phenolic resin is less than 15%, the bonding effect will be insufficient, and the plate will be difficult to obtain sufficient strength in a short time to support the mold opening and plate removal under high temperature molding. If it is more than 20%, the excessive amount of resin may lead to concentrated heat release during curing and increased shrinkage, which will affect the uniform release of stress during the water bath cooling step.
[0030] Furthermore, the preferred flake graphite is 50-100 mesh, and the preferred expanded graphite is 300-600 mesh. The particle size of the flake graphite and expanded graphite is closely related to the powder spreading and hot pressing step. The 50-100 mesh flake graphite, as the skeleton particles, can form a stable conductive network under a molding pressure of 800-1000 tons. The 300-600 mesh expanded graphite, as fine particles, fills the gaps between the flake graphite, improving the bulk density and spreading uniformity of the powder.
[0031] The ratio of the two particle sizes allows the particles to interlock, which facilitates a reduction in the porosity and a denser structure inside the plate after hot pressing. It also prevents the subsequent water bath from penetrating the plate, thus achieving water bath cooling.
[0032] In this invention, flake graphite and expanded graphite are configured in a 1:1 mass ratio. This 1:1 ratio is limited by the total amount of graphite, and this ratio ensures that the plate has a suitable thermal conductivity after hot pressing. If the thermal conductivity of the plate is too high, the surface of the plate will cool too quickly during water bath cooling, which is not conducive to synchronous cooling. If the thermal conductivity is too low, it will be difficult to dissipate heat from the core, prolonging the water bath time and reducing efficiency.
[0033] This ratio balances the thermal conductivity contributions of the two types of graphite, enabling the water bath cooling process to achieve uniform cooling within 20-40 minutes.
[0034] The conditions for hot pressing are: forming pressure of 800-1000 tons and holding time of 8-15 minutes.
[0035] The pressure of 800-1000 tons ensures the full flow and densification of powder within the large-sized mold cavity at high temperatures. Heat preservation and pressure holding are essential processes and cannot be omitted. However, compared to the traditional process where the pressure holding time often exceeds 40 minutes, this invention significantly shortens the curing time by increasing the molding temperature (traditionally 150℃). Furthermore, because subsequent water bath cooling is required, the single molding cycle can be compressed to less than 15 minutes, greatly improving production efficiency.
[0036] In a preferred embodiment of the present invention, the water bath time is 20-40 minutes.
[0037] Under normal production conditions, the pressure holding time will not exceed 40 minutes. For single boards, the maximum pressure holding and cooling time for the single boards of this invention is 55 minutes. The reason for the longer water bath time is that if the time is too short (<20 minutes), the board will not be able to fully cool down to the water bath temperature, and the residual internal stress will not be fully released. However, if the time is too long (>40 minutes), it will lead to a significant decrease in production efficiency, and the board may absorb more water due to prolonged immersion, increasing the burden on subsequent drying.
[0038] Although the production time is longer for single boards, the water bath can be used for multiple boards at the same time, so the molding time is still reduced from the existing 40 minutes to 15 minutes.
[0039] After water bath treatment, low-temperature drying is carried out, preferably at a temperature of 80-120℃, to gently remove residual moisture from the board and reduce the possibility of secondary defects caused by the violent evaporation of moisture due to high-temperature drying.
[0040] After water bath treatment, moisture remains on the surface and in the micropores of the graphite plates. If this moisture is directly introduced into subsequent battery assembly processes, it may cause a series of problems: the dimensions of the plates in a wet state differ from those in a dry working state; if wet plates are directly stacked, unpredictable shrinkage and deformation may occur after the stack heats up and evaporates the moisture; if the residual moisture vaporizes upon heating in a closed flow channel, its rapid expansion may generate localized high pressure, leading to plate damage. Therefore, residual moisture must be completely removed under controlled conditions.
[0041] The drying temperature is 80-120℃, far below the heat distortion temperature of phenolic resin. At this temperature, moisture evaporates slowly and gently, without impacting the board structure due to violent vaporization. The drying time is determined based on the board thickness and load, aiming to completely remove residual moisture. Unlike existing technologies that require flattening the monopolar plates, the water bath treatment of this invention fundamentally solves the warping problem. The drying process is only used to remove moisture, eliminating the need for additional flattening operations and simplifying the process.
[0042] The method for removing the molded bipolar plate includes: using a suction cup robot to pick up the top wall of the molded bipolar plate and remove it from the mold cavity.
[0043] The method for cooling a molded bipolar plate in a water bath includes: placing the molded bipolar plate into a water bath device, the water bath device including a water bath tank and a support plate inside it, laying the molded bipolar plate on the support plate, and then covering the molded bipolar plate with a cover plate, so that both sides of the molded bipolar plate are stably clamped and bear clamping force to suppress the deformation of the molded bipolar plate during the cooling process.
[0044] Furthermore, the method of applying clamping force includes applying pressure to the cover plate after the cover plate covers the shaped bipolar plate.
[0045] Example 1
[0046] This embodiment describes the preparation of a large-size flow channel graphite-based composite bipolar plate using a high-temperature rapid molding curing method and a hydrothermal stress release method. The prepared bipolar plate has dimensions of 650×550×5 (length×width×thickness).
[0047] The specific steps are as follows: S1: Select 50-mesh flake graphite and 300-mesh expanded graphite, mix them into graphite powder in a 1:1 mass ratio, and then add phenolic resin and mix thoroughly. After mixing, a dry, lumpy, uniformly composed, and well-dispersed composite graphite powder is obtained.
[0048] The mass ratio of each component is as follows: graphite powder accounts for 80% and phenolic resin accounts for 20%.
[0049] S2: Preheat the mold, set the mold temperature range between the upper and lower molds to 190℃, the molding pressure to 1000 tons, and the heat and pressure holding time to 10 minutes.
[0050] S3: After the mold temperature stabilizes, weigh 3.3 kg of the mixed graphite powder prepared in S1, spread it evenly in the mold cavity, use a scraper to flatten it and scrape off the excess powder, and then perform the hot pressing molding process.
[0051] S4: After the heat preservation and pressure preservation process is completed, the formed graphite plate is removed.
[0052] S5: Transfer the graphite plate that has just been taken out to a constant temperature water bath device and perform water bath heat treatment at a constant temperature of 80℃ for 30 minutes.
[0053] S6: After heat treatment, remove the electrode plate and place it in an oven to completely remove residual moisture, thus obtaining a large-size flow channel graphite bipolar plate.
[0054] Example 2
[0055] This embodiment describes the preparation of a large-size flow channel graphite-based composite bipolar plate using a high-temperature rapid molding curing method and a hydrothermal stress release method. The prepared bipolar plate has dimensions of 650×550×8mm (length×width×thickness).
[0056] The specific steps are similar to those in Example 1, except that the formulation and thickness of this plate are different from those in Example 1, as follows: S1: Select 50-mesh flake graphite and 325-mesh expanded graphite, mix them into graphite powder in a 1:1 mass ratio, and then add phenolic resin and mix thoroughly. After mixing, a dry, lumpy, uniformly composed, and well-dispersed composite graphite powder is obtained.
[0057] The mass ratio of each component is as follows: graphite powder accounts for 82% and phenolic resin accounts for 18%.
[0058] S2: Preheat the mold, set the mold temperature range between the upper and lower molds to 190℃, the molding pressure to 1000 tons, and the heat and pressure holding time to 10 minutes.
[0059] S3: After the mold temperature stabilizes, weigh 5.0 kg of the mixed graphite powder prepared in S1, spread it evenly in the mold cavity, use a scraper to flatten it and scrape off the excess powder before performing the hot pressing molding process.
[0060] S4: After the heat preservation and pressure preservation process is completed, the formed graphite plate is removed.
[0061] S5: Transfer the graphite plate that has just been taken out to a constant temperature water bath device and perform water bath heat treatment at a constant temperature of 80℃ for 30 minutes.
[0062] S6: After heat treatment, remove the electrode plate and place it in an oven to completely remove residual moisture, thus obtaining a large-size flow channel graphite bipolar plate.
[0063] Comparative Example 1: The material selection and preparation steps are the same as in Example 1. The difference is that Comparative Example 1 did not use water bath cooling, but natural air cooling.
[0064] Comparative Example 2: The material selection and preparation steps are the same as in Example 2, except that Comparative Example 2 did not use water bath cooling, but natural air cooling.
[0065] The composite bipolar plates prepared in Examples 1 and 2 and Comparative Examples 1 and 2 were tested for conductivity, contact resistance, airtightness, density, and hardness. Simultaneously, to address the warping issue, a flatness test was performed on the bipolar plates. The test method involved measuring the distance from different positions of the bipolar plate to the marble surface; the difference between the maximum and minimum values reflected the flatness of the bipolar plate. The smaller the difference, the flatter the bipolar plate. The test results are shown in Table 1.
[0066] Table 1
[0067] Data Analysis: (1) Flatness analysis: The thickness of Example 1 and Comparative Example 1 is 5 mm. The flatness of Example 1 is 0.19 mm, while that of Comparative Example 1 is 1.69 mm, representing an improvement of approximately 89%.
[0068] The thickness of Example 2 and Comparative Example 2 is 8 mm. The flatness of Example 2 is 0.22 mm, while that of Comparative Example 2 is 2.26 mm, representing an improvement of approximately 90%.
[0069] It is evident that the thicker the sheet, the more severe the warping (2.26 mm) in the comparison. This is because thicker sheets experience a greater temperature gradient between the core and surface during air cooling, resulting in more severe uneven shrinkage. The embodiment, through simultaneous cooling in a water bath, reduces the temperature gradient between the inside and outside of the molded graphite sheet, thereby controlling the flatness to around 0.2 mm and fundamentally suppressing the warping problem.
[0070] Meanwhile, the thicker the board, the more severe the warping problem of traditional processes. However, the flatness of Example 1 and Example 2 is 0.19mm and 0.22mm respectively, which is much smaller than the difference between Comparative Example 1 and Comparative Example 2. This shows that the water bath treatment method of the present invention has good adaptability to boards of different thicknesses.
[0071] (2) Conductivity analysis Example 1 has a conductivity of 121.3 S / cm, which is about 24% higher than Comparative Example 1 (97.8 S / cm); Example 2 has a conductivity of 119.4 S / cm, which is about 13% higher than Comparative Example 2 (105.8 S / cm); In terms of contact resistance, the examples are all lower than the comparative examples, with a reduction of about 9%-15%.
[0072] The essence of warping is the presence of uneven residual stress within the plate. This stress leads to poor bonding at the microscopic interfaces between graphite layers, increasing the interfacial barrier for electron transport. After the stress is uniformly released in a water bath, the internal microstructure of the plate becomes more uniform, and the contact between the graphite layers becomes tighter, thus improving the conductivity.
[0073] (3) Mechanical property analysis The flexural strengths of Examples 1 and 2 were 43.3 MPa and 42.6 MPa, respectively, both higher than those of the comparative examples (41.5 MPa and 39.9 MPa). The compressive strength of Example 1 was 82.2 MPa, which was about 12% higher than that of Comparative Example 1 (73.2 MPa). The compressive strength of Example 2 was 91.1 MPa, which was about 24% higher than that of Comparative Example 2 (73.5 MPa).
[0074] It is evident that the release of residual stress reduces microcracks and stress concentration points inside the plate, making it less likely for cracks to initiate from these defects when the plate is subjected to external loads, thereby improving its bending and compressive strength.
[0075] As can be seen from the above embodiments, the present invention solves the warping problem of large-size bipolar plates. The warping problem of large-size bipolar plates originates from the rapid and uneven cooling of the high-temperature plate material in the air environment after molding—the surface cools and shrinks rapidly, hardening while the core remains hot and expands, thus generating enormous internal stress. Existing technologies mostly employ physical correction methods such as flattening and leveling, which can only improve warping to a limited extent and increase process complexity. The present invention addresses the root cause of stress generation by using a water bath treatment to simultaneously and uniformly cool the entire plate material, fundamentally eliminating the conditions for uneven shrinkage and allowing the internal stress to be fully released.
[0076] The data from the examples show that the flatness of the large-size bipolar plate of 650×550mm prepared by the method of the present invention can reach 0.19-0.22mm, which is more than an order of magnitude better than that of the traditional method (1.69-2.26mm).
[0077] Meanwhile, traditional molding processes typically set the molding temperature at around 150℃ and require a holding time of over 40 minutes to ensure the molding quality of large-size sheets. This invention, however, raises the molding temperature to 190-200℃, significantly accelerating resin curing and shortening the holding time to 8-15 minutes, reducing the single molding cycle by over 60%. Furthermore, both the water bath heat treatment and drying stages support parallel processing of multiple sheets, allowing for simultaneous molding, transfer, and water bath treatment, meeting the needs of large-scale industrial production.
[0078] In summary, this invention constructs a complete and efficient preparation method for large-size flow channel graphite composite bipolar plates by combining high-temperature rapid molding, vacuum suction for conformal transfer, water bath uniform cooling for stress release, and low-temperature drying. This effectively overcomes the technical contradiction between warpage control and production efficiency in the preparation of large-size bipolar plates, and realizes rapid and high-performance preparation of large-size flow channel graphite-based composite bipolar plates.
[0079] Regarding the preparation method of large-size flow channel graphite composite bipolar plates described in Examples 1 and 2, this application further provides an automatic water bath drying system for large-size flow channel graphite bipolar plates to perform the above methods, as detailed below.
[0080] refer to Figure 1 and Figure 2 The large-size flow channel graphite bipolar plate automatic water bath drying system includes: water bath device 2, loading device 3, drying device and material transfer device 4.
[0081] The water bath device 2 is located on the side of the molding die, and includes a water bath tank 21 and a support plate 22 disposed in the water bath tank 21. The support plate 22 is used to place the bipolar plate 1 taken out from the molding die and to immerse the bipolar plate 1 in the water bath tank 21 for heat treatment. The loading device 3 is located on the side of the water bath 21 and has a cover plate 31 and a first moving mechanism 32 for driving the cover plate 31 to move. The cover plate 31 is used to cover the bipolar plate 1 on the support plate 22 to suppress the edge of the bipolar plate 1 from lifting. The drying device is located beside the water bath 21 and is used to receive and dry the heat-treated bipolar plates 1. The material transfer device 4 includes a suction cup manipulator 41 and a second moving mechanism 42 for driving the suction cup manipulator 41 to move. The suction cup manipulator 41 is used to adsorb the top wall of the bipolar plate 1 to grasp it, and the second moving mechanism 42 is used to drive the grasped bipolar plate 1 to move it between the molding mold, the water bath 21 and the drying device.
[0082] In the above system, the drying device is not shown in the figure. The first moving mechanism 32 and the second moving mechanism 42 can be multi-axis industrial robots. The cover plate 31 has a certain weight so that it can flatten the bipolar plate 1.
[0083] The specific operating steps of the large-size flow channel graphite bipolar plate automatic water bath drying system are as follows.
[0084] Step 1: The press drives the upper mold 11 and lower mold 12 of the forming mold to open, exposing the top of the bipolar plate 1.
[0085] Step 2: The second moving mechanism 42 drives the suction cup robot 41 to adsorb the top wall of the bipolar plate 1, and moves the bipolar plate 1 onto the support plate 22 through the second moving mechanism 42, and releases the vacuum adsorption so that the bipolar plate 1 is placed flat on the top surface of the support plate 22.
[0086] Step 3: The first moving mechanism 32 drives the cover plate 31 to cover the top wall of the bipolar plate 1 so that the bipolar plate 1 is flattened.
[0087] Step 4: Pour warm water into the water bath 21 until the bipolar plate 1 is submerged, then continue to flatten the bipolar plate 1 and maintain its temperature until the stress inside the bipolar plate 1 is uniformly released.
[0088] Step 5: Drain the warm water from the water bath 21 until the bipolar plate 1 is above the water surface. Then, the first moving mechanism 32 drives the cover plate 31 to leave the bipolar plate 1, and the second moving mechanism 42 drives the suction cup robot 41 to adhere to the top wall of the bipolar plate 1, moving the bipolar plate 1 from the water bath 21 into the interior of the drying device.
[0089] Step 6: The drying device dries the residual moisture on the surface of the bipolar plate 1 to obtain the finished bipolar plate 1.
[0090] In the above steps, the water bath 21 needs to be repeatedly filled and drained with warm water, which affects production efficiency. At the same time, when the bipolar plate 1 is placed on the top wall of the support plate 22, it may warp due to sudden cooling. In order to reduce the adverse effects of temperature changes in the support plate 22 and improve production efficiency,
[0091] refer to Figure 3 , Figure 4 and Figure 5 In a preferred embodiment, the loading device 3 further includes a third moving mechanism 33, the execution part of which is connected to the support plate 22 to lift the support plate 22 and the bipolar plate 1 it supports to above the water surface or below the water surface.
[0092] In this preferred embodiment, after the third moving mechanism 33 pushes the support plate 22 out of the water surface, the bipolar plate 1 can be placed on or removed from the support plate 22 without repeatedly injecting and draining warm water into the water bath 21, thereby improving production efficiency. Subsequently, the support plate 22 can be lowered below the water surface. The whole process takes a short time, and the temperature change of the support plate 22 is not significant, thereby reducing the warping caused by the sudden cooling of the bipolar plate 1.
[0093] Flattening the gypsum board requires a significant amount of weight, so the cover plate 31 is designed to be relatively thick and heavy, which will affect the heat conduction performance of the cover plate 31 and thus affect the efficiency of the temperature conduction of warm water to the bipolar plate 1.
[0094] Therefore, in this embodiment, the cover plate 31 is designed to be thinner, so that it has excellent heat conduction performance. At the same time, in order not to reduce the performance of the cover plate 31 in flattening the bipolar plate 1, an upper pressure block 35 is added to the execution part of the third moving mechanism 33, so that it has the function of pressing down the cover plate 31.
[0095] Specific design scheme reference Figure 5 and Figure 6 The actuator of the third moving mechanism 33 is connected to the lower support block 34 and the upper pressure block 35. The bottom of the support plate 22 is provided with a foot 221, which does not contact the lower support block 34. When the cover plate 31 covers the support plate 22, the lower support block 34 is located below the support plate 22, the upper pressure block 35 is located above the cover plate 31, and the distance between the lower support block 34 and the upper pressure block 35 is greater than the distance between the top wall of the cover plate 31 and the bottom wall of the support plate 22. In the first working condition, the lower support block 34 and the upper pressure block 35 descend to the first position, the bottom foot 221 contacts the bottom wall of the water bath tank 21, the lower support block 34 separates from the bottom wall of the support plate 22, and the upper pressure block 35 contacts the cover plate 31 and applies pressure to it. In the second working condition, the lower support block 34 and the upper pressure block 35 rise to the second position. The lower support block 34 contacts the bottom wall of the support plate 22 and lifts it out of the water surface. The upper pressure block 35 separates from the cover plate 31, and the gap height between the upper pressure block 35 and the cover plate 31 satisfies the following condition: the first moving mechanism 32 can move the cover plate 31 out from between the bipolar plate 1 and the upper pressure block 35.
[0096] First operating condition reference Figure 4 Second working condition reference Figure 5 The third moving mechanism 33 adopts a hydraulic cylinder. The piston rod of the hydraulic cylinder extends through the bottom plate of the water bath 21 to the inside of the water bath 21. The piston rod is connected to the water bath 21 by a guide sleeve and sealed by a sealing ring. The lower support block 34 and the upper pressure block 35 are both installed on the piston rod.
[0097] In the above design, only one set of hydraulic cylinders is needed to complete the synchronous lifting, moving closer and further away from each other of the support plate 22 and the cover plate 31. This can both push the bipolar plate 1 out of the water or submerge it below the water surface, and provide pressure to the cover plate 31 to flatten the bipolar plate 1.
[0098] Furthermore, in order to improve the heat conduction effect of the support plate 22 and the cover plate 31, both are designed to be relatively thin, for example, 3~5mm. This makes the support plate 22 and the cover plate 31 easy to bend when under pressure, which in turn causes the bipolar plate 1, which should have been flattened, to bend in an unexpected direction.
[0099] Therefore, it is necessary to improve the structural strength of the support plate 22 and the cover plate 31 without reducing their thermal conductivity. Based on the above objectives, the improvement schemes for the support plate 22 and the cover plate 31 are as follows: a lower perforated plate 222 is fixedly connected to the bottom of the support plate 22, which is used to suppress the bending of the support plate 22, and a foot 221 is fixedly installed at the bottom of the lower perforated plate 222; an upper perforated plate 311 is fixedly connected to the top of the cover plate 31, which is used to suppress the bending of the cover plate 31.
[0100] In the above design, the lower support block 34 no longer directly contacts the support plate 22, but lifts the support plate 22 by lifting the lower hollow plate 222.
[0101] The perforated plate can increase the bending resistance of the support plate 22 and the cover plate 31 on the one hand, and ensure that the warm water can directly contact the back of the support plate 22 and the cover plate 31 on the other hand, ensuring that the temperature of both is always close to the set temperature of the warm water.
[0102] However, the upper perforated plate 311 is different from the lower perforated plate 222. The lower perforated plate 222 is usually submerged below the water surface. Even if the support plate 22 pushes the bipolar plate 1 out of the water, the lower perforated plate 222 does not need to be removed from the water surface. Therefore, the temperature change of the lower perforated plate 222 is less than that of the upper perforated plate 311. The upper perforated plate 311 is more likely to deform due to its own thermal expansion and contraction.
[0103] Furthermore, the bottom feet 221 are fully distributed on the bottom of the lower perforated plate 222 so that the back of the lower perforated plate 222 is evenly supported and the lower perforated plate 222 deforms less when pressed. However, in order to facilitate the first moving mechanism 32 to move out and into the cover plate 31 between the bipolar plate 1 and the upper pressure block 35, the upper pressure block 35 only presses the edge of the upper perforated plate 311. Therefore, the upper perforated plate 311 deforms more when pressed, resulting in uneven force on the bipolar plate 1 and affecting the flattening effect of the bipolar plate 1.
[0104] For the reasons mentioned above, the upper perforated plate 311 requires additional stress compensation design to ensure that all parts of it output the same pressure to the bipolar plate 1, as shown in the reference. Figure 7 Figure 8: A structural plate 36 is installed on the top of the upper hollow plate 311. The upper hollow plate 311 can be suspended below the structural plate 36 by several pins 312. Each pin 312 is fitted with an elastic element 37, and the elastic element 37 connects the upper hollow plate 311 and the structural plate 36.
[0105] The staff can adjust the elastic force provided by each elastic element 37 as needed, for example, by changing the stiffness, pre-compression amount, and number of elastic elements 37, thereby compensating for the stress on the upper hollow plate 311.
[0106] Furthermore, in order to ensure that the lower pressure block can be accurately lifted to its original position after separating from the lower hollow plate 222, a guide structure is designed between the lower pressure block and the lower hollow plate 222; correspondingly, a guide structure is also designed between the structural plate 36 and the lower hollow plate 222; the guide structure can be a guide post, guide sleeve or conical positioning component or other structural component.
[0107] Based on the above embodiments, the force on the edge of the structural plate 36 is greater than the force on its center. In order to ensure that the structural plate 36 outputs a uniform force to the upper hollow plate 311, each elastic element 37 is configured such that, in the same compression stroke, the elastic force provided by each elastic element 37 near the edge of the upper hollow plate 311 is less than the elastic force provided by each elastic element 37 near the center of the upper hollow plate 311.
[0108] This allows the structural plate 36 to transmit the same pressure to the center and edge of the upper perforated plate 311 when the edge of the structural plate 36 is subjected to pressure from the upper pressure block 35, thereby keeping the cover plate 31 flat and simultaneously outputting the same pressure to all parts of the bipolar plate 1.
[0109] The specific stiffness, pre-compression amount, quantity, and other parameters of the elastic element 37 can be obtained through experiments. For example, several pressure sensors arranged in a rectangular array are placed on a flat plate, and then the cover plate 31 is driven to squeeze these pressure sensors. The rebound force of the elastic element 37 is adjusted according to the pressure data collected by the pressure sensors so that the pressure data collected by each pressure sensor is basically the same.
[0110] refer to Figure 7 The specific connection method between the upper perforated plate 311 and the structural plate 36 is as follows: one end of the pin 312 is fixedly connected to the upper perforated plate 311, the other end of the pin 312 passes through the structural plate 36 and is threaded, and a nut 313 is installed on the thread of each pin 312, and the nut 313 abuts against the top of the structural plate 36.
[0111] This design allows workers to rotate the nut 313 to change its height on the pin 312, thereby changing the distance between the upper perforated plate 311 and the structural plate 36.
[0112] Furthermore, in order to facilitate the staff to change the pre-compression amount of each elastic element 37, the following technical means are also designed in this embodiment: an external threaded sleeve 361 is fixedly installed on the structural plate 36, the external threaded sleeve 361 is threadedly connected to the structural plate 36, and the external threaded sleeve 361 is slidably connected to the pin 312, and the elastic element 37 is installed between the external threaded sleeve 361 and the upper hollow plate 311.
[0113] Simultaneously rotating the nut 313 and the external threaded sleeve 361 can change the height of the external threaded sleeve 361, but not the height of the upper hollow plate 311. This allows the relative distance between each external threaded sleeve 361 and the upper hollow plate 311 to be adjusted independently, thereby allowing the operator to change the pre-compression of each elastic element 37 based on this design, thus changing the elastic force provided by each elastic element 37.
[0114] In addition, the structural plate 36 includes a quick connector 362 for connecting the first moving mechanism 32, so that the first moving mechanism 32 can grasp or release the cover plate 31.
[0115] The water bath device 2 also includes a warm water circulation system, which is connected to the inlet and outlet of the water bath tank 21 to supply circulating warm water to the water bath tank 21.
[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. All such modifications or substitutions should be covered within the protection scope of this application, and should not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application. Therefore, the protection scope of this application should be determined by the protection scope of the claims.
Claims
1. A method for preparing a large-size flow channel graphite composite bipolar plate, characterized in that, Includes the following steps: S100. Preheat the mold. Preheat the upper and lower molds to 190-200℃ and maintain the temperature and pressure until the temperature inside the mold stabilizes. S200, Powder spreading and hot pressing: The composite graphite powder is evenly spread in the mold cavity and then hot-pressed into shape. S300, Open the mold and remove the plate. After opening the mold, remove the formed graphite plate from the mold to form the bipolar plate. S400, Water bath cooling: The entire molded bipolar plate is immersed in a water bath to cool down to the water bath temperature. The water bath temperature is a constant temperature value and is higher than the temperature of natural cooling, specifically set to 60-90℃. S500, drying treatment: After the formed bipolar plate is cooled in a water bath, it is placed in an oven to dry and remove moisture, thus obtaining the finished bipolar plate.
2. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 1, characterized in that, The composite graphite powder is obtained by mixing flake graphite, expanded graphite and phenolic resin.
3. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 2, characterized in that, In the composite graphite powder, by mass percentage, flake graphite and expanded graphite together account for 80%-85%, and phenolic resin accounts for 15%-20%.
4. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 3, characterized in that, The flake graphite is 50-100 mesh, and the expanded graphite is 300-600 mesh.
5. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 4, characterized in that, The flake graphite and the expanded graphite are configured in a 1:1 mass ratio.
6. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 1, characterized in that, The hot pressing pressure is 800-1000 tons, and the heat preservation and pressure holding time is 8-15 minutes.
7. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 1, characterized in that, The water bath heat treatment time is 20-40 minutes.
8. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 1, characterized in that, The method for opening the mold and removing the plate includes: using a suction cup robot to pick up the top wall of the molded bipolar plate and remove it from the mold cavity.
9. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 1, characterized in that, The method for cooling the molded bipolar plate in a water bath includes: placing the molded bipolar plate into a water bath device, the water bath device including a water bath tank and a support plate inside it, laying the molded bipolar plate on the support plate, and then covering the molded bipolar plate with a cover plate, so that both sides of the molded bipolar plate are stably clamped and bear clamping force, so as to suppress the deformation of the molded bipolar plate during the cooling process.
10. The method for preparing a large-size flow channel graphite composite bipolar plate according to claim 9, characterized in that, The method of applying clamping force includes applying pressure to the cover plate after the cover plate covers the shaped bipolar plate.