A gradient high-rate activation method for tellurium-based liquid metal batteries

By optimizing the interface structure of tellurium-based liquid metal batteries through a gradient high-rate activation method, the problems of low coulombic efficiency and poor cycle stability caused by existing low-rate activation processes are solved, achieving high-efficiency battery performance improvement and long-life application.

CN123073233APending Publication Date: 2026-11-10WUHAN JIZHAO ENERGY STORAGE TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611259825.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing low-rate activation processes for tellurium-based liquid metal batteries cannot fully activate the active reaction sites of the liquid tellurium cathode, resulting in low coulombic efficiency and poor cycle stability, which limits their large-scale application.

Method used

A gradient high-rate activation method is adopted, which involves a multi-stage discharge and charge process, including initial, intermediate and final activation stages, combined with appropriate discharge and charge rates and voltage conditions, to optimize the interface structure of tellurium-based liquid metal batteries and improve reaction reversibility and cycle stability.

Benefits of technology

It significantly improves the coulombic efficiency of tellurium-based liquid metal batteries to over 97% and extends cycle life to over 4500 cycles, solving the problems of low battery efficiency and poor stability under traditional activation processes, and is suitable for large-scale long-term energy storage needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073233A_ABST
    Figure CN123073233A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of liquid metal battery energy storage technology, specifically relating to a gradient high-rate activation method for tellurium-based liquid metal batteries. The gradient high-rate activation method includes the following steps: S1, heating the tellurium-based liquid metal battery to its rated operating temperature, and collecting the open-circuit voltage of the tellurium-based liquid metal battery during heating and holding; S2, initiating the initial activation stage; S3, entering the final activation stage; S4, after the final activation stage is completed, discharging the tellurium-based liquid metal battery obtained from the final activation stage; S5, charging the tellurium-based liquid metal battery, testing the coulombic efficiency of the tellurium-based liquid metal battery, and if the target value is reached, the gradient high-rate activation is complete. The gradient high-rate activation method of this invention can effectively suppress the shuttle effect caused by the dissolution of tellurium and its intermediate discharge product, lithium polytelluride, in the electrolyte under high-temperature conditions, improve the reversibility of the redox reaction, and thus improve the battery's coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of liquid metal battery energy storage technology, specifically relating to a method for optimizing the interfacial reaction characteristics of tellurium (Te)-based liquid metal batteries through a gradient rate activation process, thereby improving the battery's coulombic efficiency and long-cycle stability. Background Technology

[0002] Liquid metal batteries are novel electrochemical energy storage devices constructed from liquid electrodes and molten salt electrolytes. With their outstanding advantages such as fast liquid-liquid interface reaction kinetics, strong interface self-healing, simple structure, low cost, long lifespan, and high safety, they have become one of the technical solutions for large-scale, long-term energy storage. They can effectively adapt to the intermittent and fluctuating absorption needs of renewable energy sources such as wind power and photovoltaics, making them a preferred technical route for grid peak shaving and distributed energy storage. Among them, tellurium-based liquid metal batteries, compared with traditional antimony-based and bismuth-based liquid metal batteries, possess unique advantages in high operating voltage and energy density, and have irreplaceable application potential in high-power, long-term, and high-density energy storage scenarios.

[0003] Tellurium-based liquid metal batteries employ liquid alkali / alkaline earth metals as the negative electrode, tellurium-based alloys as the positive electrode, and molten inorganic salts as the electrolyte. Their all-liquid structure endows the battery with excellent interface self-healing capabilities and fast-charging performance. However, the application of this battery system is currently limited by core performance shortcomings stemming from modification strategies and activation processes. Currently, the activation of tellurium-based liquid metal batteries all employ traditional low-rate constant-current activation methods, a process that cannot match the characteristics of the Te-based high-temperature liquid-liquid reaction system.

[0004] The shortcomings of the existing technology are specifically reflected in the following aspects: First, under low-rate activation conditions, the active reaction sites of the liquid tellurium cathode melt are not fully activated. Under high-temperature conditions, the dissolution of tellurium and its intermediate discharge product lithium polytelluride in the electrolyte triggers a shuttle effect, and the reversible redox reaction is incomplete, resulting in a significant reduction in battery coulombic efficiency (~60%). Second, low-rate activation cannot regulate the interface structure between the electrode and the molten salt electrolyte. The liquid-liquid interface constructed by traditional activation processes is prone to instability. During long-term cycling, the interface is repeatedly reconstructed, leading to continuous and rapid capacity decay and short cycle life, which restricts the large-scale application of tellurium-based liquid metal batteries.

[0005] Current research on improving the performance of tellurium-based liquid metal batteries mainly focuses on cathode alloy modification, molten salt electrolyte composition optimization, and operating temperature control. These approaches suffer from complex processes, high manufacturing costs, and poor high-temperature compatibility, while neglecting the crucial role of initial activation in the interface evolution, reaction reversibility, and long-cycle stability of liquid metal batteries. Unlike traditional solid-state lithium batteries, the initial state of the liquid-liquid interface in liquid metal batteries often directly determines their electrochemical performance throughout their entire lifecycle. Conventional low-rate activation is unsuitable for the reaction characteristics of Te-based high-temperature liquid systems. To date, there are no activation techniques specifically for tellurium-based liquid metal battery systems, and no research on simultaneously optimizing the positive and negative electrode melt interfaces and improving coulombic efficiency and cycle stability through electrochemical activation processes. Therefore, developing a high-rate activation method suitable for high-temperature tellurium-based liquid metal battery systems is key to overcoming performance bottlenecks and promoting their industrialization. Summary of the Invention

[0006] The purpose of this invention is to provide a high-rate activation method that is suitable for high-temperature tellurium-based liquid metal battery systems, has a simple process, requires no additional modification costs, and can be scaled up, so as to solve the performance bottleneck of tellurium-based liquid metal batteries and promote their industrialization.

[0007] This invention provides a gradient high-rate activation method for tellurium-based liquid metal batteries, comprising the following steps: S1. Heat the tellurium-based liquid metal battery to its rated operating temperature; S2. Collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it stand for 1 to 2 hours. S3. Start the initial activation stage, set the initial discharge rate condition to 0.5-1 C and the discharge cutoff voltage condition to 0.5 V-0.4 V, and perform initial activation on the tellurium-based liquid metal battery to achieve a discharge depth of 100% DOD. Then, let the tellurium-based liquid metal battery rest for 5-10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.5-1 C, with a charging cut-off voltage of 2.2V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and repeat step S3 for 2-10 cycles. S5. Enter the intermediate activation stage, set the discharge rate condition to 1.1-4.9 C and the discharge cutoff voltage condition to 0.4-V-0.1V to activate the tellurium-based liquid metal battery, and then let the tellurium-based liquid metal battery rest for 5-10 minutes. S6. Charge the tellurium-based liquid metal battery at a rate of 1.1-4.9 C, with a charging cut-off voltage of 2.2V-2.8V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and repeat step S5 for 2-10 cycles. S7. Enter the final activation stage, set the discharge rate condition to 5-6 C, the discharge cutoff voltage condition to 0.1 V, and then let the tellurium-based liquid metal battery rest for 5-10 minutes. S8. Charge the tellurium-based liquid metal battery at a rate of 5-6 C, with a charging cut-off voltage of 2.8V-2.9V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and proceed to step S7 for 2-10 cycles. S9. Discharge the tellurium-based liquid metal battery at a rate of 0.35 ~ 1.4C, with a discharge cutoff voltage of 0.6 V-0.4V, and then let the battery rest for 5 ~ 10 minutes. S10. Charge the tellurium-based liquid metal battery at a rate of 0.35~1.4 C, with a charging cutoff voltage of 2.2 V-2.4 V. Then let the battery rest for 5~10 minutes. After repeating the cycle 2~3 times in step S9, test the coulombic efficiency of the tellurium-based liquid metal battery. If the coulombic efficiency of the tellurium-based liquid metal battery reaches the target value, the gradient high-rate activation of the tellurium-based liquid metal battery is complete.

[0008] Furthermore, in step S1, the rated operating temperature is 400~500℃, and the heating rate is 3~5℃ / min.

[0009] Furthermore, the intermediate activation stage is performed 2-5 times.

[0010] Furthermore, the intermediate activation stage is performed twice.

[0011] Furthermore, in step S10, the target value for coulomb efficiency is 95%.

[0012] The beneficial effects of this invention are as follows: (1) The gradient high-rate activation method of the present invention can effectively suppress the shuttle effect caused by the dissolution of tellurium and its intermediate discharge product lithium polytelluride in the electrolyte under high temperature environment, improve the reversibility of redox reaction, and thus improve the battery coulombic efficiency; secondly, the method can also construct a stable tellurium ion concentration interface structure, avoid the battery short circuit problem caused by the diffusion of discharge products to the negative electrode side, improve the battery long cycle performance, and after gradient high-rate activation, the average coulombic efficiency of Te-based liquid metal battery is stably increased to more than 97%, and the battery can maintain high coulombic efficiency for more than 4500 cycles with a capacity decay rate as low as less than 0.03%, solving the fundamental problems of low battery coulombic efficiency (~60%), fast cycle decay, and poor battery cycle stability under traditional activation process; (2) The gradient high-rate activation method of the present invention is adapted to the high-voltage tellurium-based liquid metal battery operating system. It does not require modification of positive and negative electrodes, optimization of molten salt electrolyte, or addition of auxiliary equipment. It only optimizes the battery activation process, with zero additional materials and production costs. It can be directly introduced into the battery mass production line. It has strong process adaptability and no additional costs. (3) The gradient high-rate activation method of the present invention effectively regulates the high-temperature liquid-liquid reaction interface, inhibits the dissolution and shuttle of intermediate products, solves the problems of high battery self-discharge current and easy short circuit of battery, greatly improves the high-temperature operation stability and service life of Te-based liquid metal battery, adapts to the working conditions of large-scale long-term energy storage, and improves the stability of battery throughout the entire life cycle. Attached Figure Description

[0013] Figure 1 This is a flowchart of the gradient high-rate activation method for the tellurium-based liquid metal battery of the present invention; Figure 2 This is a flowchart of the gradient high-rate activation method for the tellurium-based liquid metal battery according to Embodiment 1 of the present invention; Figure 3 The image shows the electrochemical performance of the tellurium-based liquid metal battery of Comparative Example 1 of this invention. Figure 4 The image shows the electrochemical performance of the tellurium-based liquid metal battery of Example 1 of this invention. Figure 5 The electrochemical performance diagram of the tellurium-based liquid metal battery in Example 2 of the present invention is shown. Figure 6 This is a graph showing the electrochemical performance of the tellurium-based liquid metal battery in Example 3 of the present invention. Detailed Implementation

[0014] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.

[0015] It should be noted that the tellurium-based liquid metal battery of the present invention is a liquid metal battery prepared by the method described in the invention patent with patent number CN121484047A and patent name entitled "A High Voltage Cathode Material for Liquid Metal Batteries and Its Preparation Method".

[0016] This invention protects a gradient high-rate activation method for tellurium-based liquid metal batteries, comprising the following steps: S1. Place the tellurium-based liquid metal battery in the test furnace and connect it to the test instrument, and heat it to the rated operating temperature; in this invention, the rated operating temperature is 400 ~ 500℃, and the heating rate is 3 ~ 5℃ / min; S2. Open the test program and collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it rest for 1 to 2 hours. S3. Start the initial activation stage, set the initial discharge rate condition to 0.5-1 C and the discharge cutoff voltage condition to 0.4V-0.5 V, and perform initial activation on the tellurium-based liquid metal battery to make the depth of discharge of the tellurium-based liquid metal battery 100% DOD. Then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.5-1 C, with a charging cut-off voltage of 2.3V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and repeat step S3 for 2-10 cycles. S5. Enter the intermediate activation stage, set the discharge rate condition to 1.1-4.9 C and the discharge cutoff voltage condition to 0.1V-0.4V to activate the tellurium-based liquid metal battery, and then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S6. Charge the tellurium-based liquid metal battery at a rate of 1.1-4.9 C, with a charging cut-off voltage of 2.3 V-2.8 V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and repeat step S5 for 2-10 cycles. It should be noted that, in this invention, in order to ensure the consistency of the electrochemical performance of the tellurium-based liquid metal battery during activation, and to prevent the increased risk of battery short circuits that may be caused by the high-rate step-by-step leap of the tellurium-based liquid metal battery, the intermediate activation stage is performed 2-5 times; preferably, the intermediate activation stage of this invention is performed 2 times.

[0017] S7. Enter the final activation stage, set the discharge rate condition to 5-6 C, the discharge cutoff voltage condition to 0.1 V, and then let the tellurium-based liquid metal battery rest for 5-10 minutes. S8. Charge the tellurium-based liquid metal battery at a rate of 5-6 C, with a charging cut-off voltage of 2.8-2.9 V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and proceed to step S7 for 2-10 cycles.

[0018] In this invention, the activation stage of the tellurium-based liquid metal battery is completed after the final activation stage. To verify whether the electrical performance of the activated tellurium-based liquid metal battery meets the requirements, the following steps are also included: S9. Discharge the tellurium-based liquid metal battery at a rate of 0.35 ~ 1.4C, with a discharge cutoff voltage of 0.4V-0.6V, and then let the battery rest for 5 ~ 10 minutes. S10. Charge the tellurium-based liquid metal battery at a rate of 0.35 ~ 1.4C, with a charging cutoff voltage of 2.2-2.4V. Then let the battery rest for 5 ~ 10 minutes, and proceed to step S9 for 2 ~ 5 cycles. Test the coulombic efficiency of the tellurium-based liquid metal battery. If the coulombic efficiency of the tellurium-based liquid metal battery is ≥95%, the gradient high-rate activation of the tellurium-based liquid metal battery is complete.

[0019] If the efficiency is less than 95%, then jump back to S9 for activation, and repeat steps S7 to S10 2 to 3 times until the coulombic efficiency of the tellurium-based liquid metal battery is ≥95%.

[0020] In this invention, the gradient high-rate activation method optimizes factors such as step-by-step discharge rate, operating cutoff voltage, number of cycles, and formation temperature to improve the efficiency and cycle stability of the formed battery. The charge / discharge voltage window should be strictly matched to the electrochemical range of the tellurium-based liquid metal battery, set to 0.1 V ~ 3.0 V, to avoid melt decomposition and interface damage caused by high-temperature overcharging and over-discharging.

[0021] This invention also includes a quality inspection method for activated batteries, the steps of which are as follows: (1) Discharge the activated tellurium-based liquid metal battery at a constant current rate of 0.1~0.7C to a cutoff voltage of 0.7~0.6V, so that the depth of discharge of the tellurium-based liquid metal battery is 100% DOD, and let the liquid metal battery rest for 5~10 minutes; (2) Charge the liquid metal battery at a rate of 0.1~0.7C to the cutoff voltage of 2.2-2.3V, and let it rest for 5~10 minutes; (3) Proceed to step (2) and repeat the cycle for the target number of cycles, and record the coulombic efficiency of the tellurium-based liquid metal battery per cycle.

[0022] Testing revealed that the activated battery achieved a coulombic efficiency of over 98% and maintained stable voltage and capacity per cycle, indicating that the gradient high-rate activation method of this invention is a high-quality activation method that can solve problems such as low battery coulombic efficiency, rapid cycle decay, and poor battery cycle stability under traditional activation processes.

[0023] <Example 1> This embodiment uses a tellurium-based liquid metal battery with a capacity of 1.68 Ah. The gradient high-rate activation method for the tellurium-based liquid metal battery includes the following steps: S1. Place the tellurium-based liquid metal battery in the test furnace and connect it to the test instrument, and heat it to 400-500℃ at a heating rate of 3-5℃ / min; S2. Open the test program and collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it rest for 1 to 2 hours. S3. Initially activate the tellurium-based liquid metal battery with an initial discharge rate of 0.7 C and a discharge cutoff voltage of 0.5 V to achieve a depth of discharge (DOD) of 100%. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.7 C, with a charging cut-off voltage of 2.3V. Then let the tellurium-based liquid metal battery rest for 5 to 10 minutes, and then proceed to step S3 for 10 cycles. S5. Discharge the tellurium-based liquid metal battery at a rate of 1.4 C, with a discharge cutoff voltage of 0.4 V, and then let the tellurium-based liquid metal battery rest for 10 minutes. S6. Charge the tellurium-based liquid metal battery at a rate of 1.4 C, with a charging cut-off voltage of 2.4 V. Then, let the tellurium-based liquid metal battery rest for 10 minutes and proceed to step S5 for 10 cycles. S7. Continue to increase the constant current discharge of the tellurium-based liquid metal battery, with a discharge rate of 2.8 C and a discharge cutoff voltage of 0.2 V. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S8. Charge the tellurium-based liquid metal battery at a constant current rate of 2.8C, with a charging cutoff voltage of 2.6V. Then let the tellurium-based liquid metal battery rest for 10 minutes and proceed to step S7 for 10 cycles. S9. Increment the activation rate of the tellurium-based liquid metal battery, discharge at a 5C rate, with a discharge cutoff voltage of 0.1V, and then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S10. Charge the tellurium-based liquid metal battery at a rate of 5 C, with a charging cut-off voltage of 2.8 V. Then let the battery rest for 5 to 10 minutes and proceed to step S9 for 10 cycles. S11. Discharge the tellurium-based liquid metal battery at a rate of 0.7 C with a discharge cutoff voltage of 0.5 V to achieve a depth of discharge (DOD) of 100% for the tellurium-based liquid metal battery. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S12. Charge the tellurium-based liquid metal battery at a rate of 0.7 C, with a charging cutoff voltage of 2.3 V. Then let the battery rest for 5 to 10 minutes, and then proceed to step S11 for 5 cycles to obtain the activated tellurium-based liquid metal battery.

[0024] <Example 2> This embodiment uses a tellurium-based liquid metal battery with a capacity of 1.68 Ah. The gradient high-rate activation method for the tellurium-based liquid metal battery includes the following steps: S1. Place the tellurium-based liquid metal battery in the test furnace and connect it to the test instrument, and heat it to 400-500℃ at a heating rate of 3-5℃ / min; S2. Open the test program and collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it rest for 1 to 2 hours. S3. Initially activate the tellurium-based liquid metal battery with an initial discharge rate of 0.7 C and a discharge cutoff voltage of 0.5 V to achieve a depth of discharge (DOD) of 100%. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.7 C, with a charging cut-off voltage of 2.3V. Then let the tellurium-based liquid metal battery rest for 5 to 10 minutes, and then proceed to step S3 for 10 cycles. S5. Discharge the tellurium-based liquid metal battery at a rate of 1.4 C, with a discharge cutoff voltage of 0.4 V, and then let the tellurium-based liquid metal battery rest for 10 minutes. S6. Charge the tellurium-based liquid metal battery at a rate of 1.4 C, with a charging cut-off voltage of 2.4 V. Then, let the tellurium-based liquid metal battery rest for 10 minutes and proceed to step S5 for 10 cycles. S7. Continue to increase the constant current discharge of the tellurium-based liquid metal battery to a discharge rate of 2.8 C, and then let the tellurium-based liquid metal battery rest for 10 minutes. S8. Charge the tellurium-based liquid metal battery at a constant current rate of 2.8C, with a charging cutoff voltage of 2.6V. Then let the tellurium-based liquid metal battery rest for 10 minutes and proceed to step S7 for 10 cycles. S9. Increment the activation rate of the tellurium-based liquid metal battery, discharge at a 5C rate, with a discharge cutoff voltage of 0.1V, and then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S10. Charge the tellurium-based liquid metal battery at a rate of 5 C, with a charging cut-off voltage of 2.8 V. Then let the battery rest for 5 to 10 minutes and proceed to step S9 for 10 cycles. S11. Discharge the tellurium-based liquid metal battery at a rate of 1.05C with a discharge cutoff voltage of 0.4V to achieve a depth of discharge (DOD) of 100% for the tellurium-based liquid metal battery. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S12. Charge the tellurium-based liquid metal battery at a rate of 1.05 C, with a charging cutoff voltage of 2.4 V. Then let the battery rest for 5 to 10 minutes, and then proceed to step S11 for 5 cycles to obtain the activated tellurium-based liquid metal battery.

[0025] <Example 3> This embodiment uses a tellurium-based liquid metal battery with a capacity of 1.68 Ah. The gradient high-rate activation method for the tellurium-based liquid metal battery includes the following steps: S1. Place the tellurium-based liquid metal battery in the test furnace and connect it to the test instrument, and heat it to 400-500℃ at a heating rate of 3-5℃ / min; S2. Open the test program and collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it rest for 1 to 2 hours. S3. Initially activate the tellurium-based liquid metal battery with an initial discharge rate of 0.7 C and a discharge cutoff voltage of 0.5 V to achieve a depth of discharge (DOD) of 100%. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.7 C, with a charging cut-off voltage of 2.3V. Then let the tellurium-based liquid metal battery rest for 5 to 10 minutes, and then proceed to step S3 for 10 cycles. S5. Discharge the tellurium-based liquid metal battery at a rate of 1.4 C, with a discharge cutoff voltage of 0.4 V, and then let the tellurium-based liquid metal battery rest for 10 minutes. S6. Charge the tellurium-based liquid metal battery at a rate of 1.4 C, with a charging cut-off voltage of 2.4 V. Then, let the tellurium-based liquid metal battery rest for 10 minutes and proceed to step S5 for 10 cycles. S7. Continue to increase the constant current discharge of the tellurium-based liquid metal battery to a discharge rate of 2.8 C, and then let the tellurium-based liquid metal battery rest for 10 minutes. S8. Charge the tellurium-based liquid metal battery at a constant current rate of 1.4 C, with a charging cutoff voltage of 2.6V. Then let the tellurium-based liquid metal battery rest for 10 minutes and proceed to step S7 for 10 cycles. S9. Increment the activation rate of the tellurium-based liquid metal battery, discharge at a 5C rate, with a discharge cutoff voltage of 0.1V, and then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S10. Charge the tellurium-based liquid metal battery at a rate of 5 C, with a charging cut-off voltage of 2.8 V. Then let the battery rest for 5 to 10 minutes and proceed to step S9 for 10 cycles. S11. Discharge the tellurium-based liquid metal battery at a rate of 1.4C with a discharge cutoff voltage of 0.4 V to achieve a depth of discharge (DOD) of 100% for the tellurium-based liquid metal battery. Then, let the tellurium-based liquid metal battery rest for 10 minutes. S12. Charge the tellurium-based liquid metal battery at a rate of 1.4C, with a charging cutoff voltage of 2.4V. Then let the battery rest for 5 to 10 minutes, and then proceed to step S11 for 5 cycles to obtain the activated tellurium-based liquid metal battery.

[0026] <Comparative Example 1> This comparative example uses a tellurium-based liquid metal battery with a capacity of 1.68 Ah. The activation method of the tellurium-based liquid metal battery includes the following steps: S1. Place the tellurium-based liquid metal battery in the test furnace and connect it to the test instrument, and heat it to the rated operating temperature; in this invention, the rated operating temperature is 400 ~ 500℃, and the heating rate is 3 ~ 5℃ / min; S2. Open the test program and collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it rest for 1 to 2 hours. S3. Start the initial activation stage, set the initial discharge rate condition to 0.35 C and the discharge cutoff voltage condition to 0.6 V, and perform initial activation on the tellurium-based liquid metal battery to make the depth of discharge of the tellurium-based liquid metal battery 100% DOD. Then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.35 C, with a charging cutoff voltage of 2.2V. Then, let the tellurium-based liquid metal battery rest for 5 to 10 minutes, and then repeat the cycle in step S3 for 20 cycles to obtain the activated tellurium-based liquid metal battery.

[0027] The tellurium-based liquid metal batteries activated in Examples 1-3 and Comparative Example 1 were tested using the above-described quality inspection methods. The parameters and test results for each example and comparative example are shown in Table 1. Figure 3-6 As shown, where, Figure 3 The electrochemical performance graph is shown as a comparative example under the condition that the discharge / charge rate is 0.7.

[0028] Table 1

[0029] As can be seen from the above test results, after adopting the gradient high-rate activation process, the coulombic efficiency of the tellurium-based liquid metal battery increased from about 60% to 97%~99%, an increase of 62%~65%; the cycle life was significantly extended from less than 100 cycles to more than 4500 cycles, and the cycle stability of the tellurium-based liquid metal was significantly improved.

[0030] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A gradient high-rate activation method for tellurium-based liquid metal batteries, characterized in that, Includes the following steps: S1. Heat the tellurium-based liquid metal battery to its rated operating temperature; S2. Collect the open-circuit voltage of the tellurium-based liquid metal battery during heating and heat preservation. After the battery open-circuit voltage is normal and stable, let it stand for a period of time. S3. Start the initial activation stage, set the initial discharge rate condition to 0.5-1 C and the discharge cutoff voltage condition to 0.4V-0.5 V, and perform initial activation on the tellurium-based liquid metal battery to make the depth of discharge of the tellurium-based liquid metal battery 100% DOD. Then let the tellurium-based liquid metal battery rest for 5 to 10 minutes. S4. Charge the tellurium-based liquid metal battery at a rate of 0.5-1 C, with a charging cut-off voltage of 2.3V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and repeat step S3 for 2-10 cycles. S5. Enter the intermediate activation stage, set the discharge rate condition to 1.1-4.9 C and the discharge cutoff voltage condition to 0.1V-0.4V to activate the tellurium-based liquid metal battery, and then let the tellurium-based liquid metal battery rest for 5-10 minutes. S6. Charge the tellurium-based liquid metal battery at a rate of 1.1-4.9 C, with a charging cut-off voltage of 2.3 V-2.8 V. Then let the tellurium-based liquid metal battery rest for 5-10 minutes and repeat step S5 for 2-10 cycles. S7. Enter the final activation stage, set the discharge rate condition to 5-6 C, the discharge cutoff voltage condition to 0.1 V, and then let the tellurium-based liquid metal battery rest for 5-10 minutes. S8. Charge the tellurium-based liquid metal battery at a rate of 5-6 C, with a charging cut-off voltage of 2.8-2.9 V. Then, let the tellurium-based liquid metal battery rest for 5-10 minutes, and then proceed to step S7 for 2-10 cycles. The final activation stage is now complete.

2. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 1, characterized in that, The gradient high-rate activation method further includes the following steps: S9. Discharge the tellurium-based liquid metal battery obtained in step S8 at a rate of 0.35 to 1.4C, and then let the battery rest for 5 to 10 minutes. S10. Charge the tellurium-based liquid metal battery at a rate of 0.35 ~ 1.4C, then let the battery rest for 5 ~ 10 minutes. After repeating the cycle 2 ~ 3 times in step S9, test the coulombic efficiency of the tellurium-based liquid metal battery. If the coulombic efficiency of the tellurium-based liquid metal battery reaches the target value, the gradient high-rate activation of the tellurium-based liquid metal battery is complete.

3. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 1, characterized in that, In step S1, the rated operating temperature is 400~500℃, and the heating rate is 3~5℃ / min.

4. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 1, characterized in that, In step S2, the resting time is 1 to 2 hours.

5. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 1, characterized in that, The intermediate activation stage is repeated 2-5 times.

6. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 3, characterized in that, The intermediate activation stage is performed twice.

7. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 2, characterized in that, In step S10, the target value for coulomb efficiency is 95%.

8. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 2, characterized in that, In step S9, the discharge cutoff voltage is 0.6 V-0.4 V.

9. The gradient high-rate activation method for a tellurium-based liquid metal battery according to claim 2, characterized in that, In step S10, the charging cutoff voltage is 2.2-2.4 V.

Citation Information

Patent Citations

  • High-voltage positive electrode material for liquid metal battery and preparation method of high-voltage positive electrode material

    CN121484047A