A process for nickel Schottky annealing

By controlling the reaction between nickel and silicon in the nickel Schottky annealing process and using a nitrogen-oxygen mixed atmosphere and aqua regia treatment, the problem of increased leakage current in the nickel Schottky annealing process was solved, thereby improving device performance and yield.

CN123075931APending Publication Date: 2026-11-10XIAN MICROELECTRONICS TECH INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611213171.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing nickel Schottky annealing processes have difficulty effectively controlling the annealing temperature, leading to excessive silicide growth, interface erosion, or surface oxidation, which increases leakage current and consequently affects device performance.

Method used

In the nickel Schottky annealing process, a masking film is grown on the wafer surface and photolithography and etching are performed to form contact hole regions. Combined with electron beam evaporation and reactive tube annealing, a nitrogen and oxygen mixed atmosphere is used to control the reaction between nickel and silicon. Subsequent aqua regia treatment is performed to remove residual nickel metal and ensure the integrity of the nickel silicide interface.

Benefits of technology

The reverse leakage current was reduced from 2896 μA to 1015 μA, which improved product yield, improved the quality of the Schottky contact interface, suppressed the generation of interface leakage channels, and prevented device failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075931A_ABST
    Figure CN123075931A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of chip manufacturing technology and discloses a nickel Schottky annealing process, including the following steps: growing a masking film on the wafer surface; performing photolithography and etching on the masking film according to a preset circuit diagram to form contact hole regions on the wafer; performing a first cleaning on the etched wafer; placing the wafer after the first cleaning in an electron beam evaporation stage to deposit nickel metal on the wafer surface and contact hole regions; performing a second cleaning on the wafer after nickel metal deposition; placing the wafer after the second cleaning in a reaction tube, introducing a preset atmosphere within a preset annealing time, and performing nickel Schottky annealing, where the nickel metal in the contact hole regions reacts with silicon to form nickel silicide; treating the nickel silicide with aqua regia to remove unreacted residual nickel metal from the wafer surface; the preset atmosphere includes nitrogen and oxygen, reducing the number of surface defects by 20% and the reverse leakage current from 2896 μA to 1015 μA, thereby improving product yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chip manufacturing technology and relates to a nickel Schottky annealing process. Background Technology

[0002] Schottky diodes are semiconductor devices that operate on the majority carrier basis. With their advantages of fast switching speed and low forward voltage drop, they are used in high-speed circuits, power conversion, and radio frequency applications.

[0003] In the metallization process of Schottky contacts, electron beam evaporation has become the mainstream method for preparing nickel and its alloy thin films due to its advantages such as high film purity, good step coverage and strong film-substrate adhesion.

[0004] The deposited pure nickel film needs to undergo high-temperature annealing to undergo a solid-state reaction with the silicon substrate, generating low-resistivity nickel silicide (NiSi) in situ as the final electrode layer. However, the control of the annealing process window is quite stringent: if the process parameters are mismatched, defects such as excessive silicide growth, interface erosion, or surface oxidation can easily be induced, leading to a surge in leakage current and consequently causing device performance degradation or even failure. Secondly, when the annealing temperature is too high, NiSi will transform into high-resistivity disilicide (NiSi2), which not only increases contact resistance but also damages device performance. Summary of the Invention

[0005] In view of the shortcomings of the existing technology, the purpose of this invention is to provide a process for nickel Schottky annealing.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a nickel Schottky annealing process, comprising: growing a masking film on a wafer surface; performing photolithography and etching on the masking film according to a preset circuit diagram to form contact hole regions on the wafer; performing a first cleaning on the etched wafer; placing the first-cleaned wafer in an electron beam evaporation stage to deposit nickel metal on the wafer surface and contact hole regions; performing a second cleaning on the wafer after nickel metal deposition; placing the second-cleaned wafer in a reaction tube, introducing a preset atmosphere within a preset annealing time, and performing nickel Schottky annealing, wherein the nickel metal in the contact hole regions reacts with silicon to form nickel silicides; and treating the nickel silicides with aqua regia to remove unreacted residual nickel metal from the wafer surface.

[0007] Furthermore, the masking membrane is 700. 800nm ​​SiO2 masking film.

[0008] Furthermore, the etched wafer undergoes a first cleaning process, including: first, cleaning with a mixed solution of sulfuric acid and hydrogen peroxide at 110 °C. Wash at 130℃ for 10 minutes, rinse with water, and then rinse with a hydrofluoric acid solution at a volume ratio of 10:1 at 20℃. Wash at 25℃ for 1 minute, rinse and spin dry.

[0009] Furthermore, the thickness of the nickel metal deposition is 50±10 nm.

[0010] Furthermore, the wafer after the first cleaning is placed in an electron beam evaporation stage, and the evaporation vacuum pressure is... mbar, evaporation rate of 8 Å / s, evaporation temperature of Nickel metal deposition is performed on the wafer surface and contact hole area at ℃.

[0011] Furthermore, the volume ratio of sulfuric acid to hydrogen peroxide is 3:1.

[0012] Furthermore, the reaction tube is a quartz furnace tube; the temperature of the reaction tube is... The temperature was ℃, the pressure in the reaction tube was 226 Pa, and the heating rate was 7. 9 ℃ / min; the preset atmosphere includes nitrogen and oxygen, and the flow rate of nitrogen is... The oxygen flow rate is L / min. mL / min; the nickel Schottky annealing time is min.

[0013] Furthermore, the cooling rate of the reaction tube is... ℃ / min; the nickel Schottky annealed material is withdrawn from the reaction tube at a rate of 400 ℃ / min. mm / min.

[0014] Furthermore, the aqua regia comprises hydrochloric acid and nitric acid, wherein the volume of the hydrochloric acid is 13.5 L and the dosage deviation is ±10%.

[0015] Furthermore, the volume of the nitric acid is 4.5 L, with a dosage deviation of ±10%.

[0016] Compared with the prior art, the present invention has the following beneficial technical effects: This invention discloses a nickel Schottky annealing process. A masking film is grown on the wafer surface. The masking film is then photolithographically and etched according to a preset circuit diagram to form contact hole regions on the wafer. The etched wafer undergoes a first cleaning. After the first cleaning, the wafer is placed in an electron beam evaporation stage for nickel metal deposition. Following deposition, a second cleaning is performed. The wafer is then placed in a reaction tube for annealing. After cooling to room temperature, it undergoes aqua regia treatment to remove unreacted residual nickel metal from the wafer surface. This reduces the number of surface defects by 20% and the reverse leakage current from 28kJ / m³. 96 μA decreased to 10 15 μA improves product yield.

[0017] The preset atmosphere includes nitrogen and oxygen. Nitrogen can maintain the stability of the atmosphere inside the reaction tube, while the introduction of oxygen can regulate the nickel silicide interface formed by the reaction of nickel and silicon, improve the quality of the Schottky contact interface, suppress the generation of interface leakage channels, and reduce reverse leakage current.

[0018] Placing the wafer in an aqua regia bath for aqua regia treatment can selectively dissolve residual nickel metal on the wafer surface that has not undergone a solid-phase reaction with the silicon substrate, while retaining the nickel silicide (NiSi) formed in the contact holes. Aqua regia has strong oxidizing and complexing properties, which can remove excess free nickel metal distributed on the wafer surface, avoiding the increase in reverse leakage current and device failure caused by residual nickel metal. Aqua regia has a low corrosion rate on nickel silicide, which can ensure the structural integrity of the Schottky contact interface.

[0019] During the first cleaning of the etched wafer, a high-temperature cleaning is performed using a mixed solution of sulfuric acid and hydrogen peroxide to remove photoresist residue, organic contaminants, and various particulate impurities remaining from the photolithography etching process. Then, a short-time cleaning is performed using a hydrofluoric acid solution with a volume ratio of 10:1 to remove the natural oxide layer on the wafer surface. The high-temperature oxidation cleaning and hydrofluoric acid complement each other, removing contaminants while avoiding excessive etching of the silicon substrate. After cleaning, the wafer is rinsed and dried to prevent water residue and reduce the risk of device leakage. Attached Figure Description

[0020] Figure 1 This is a flowchart of a nickel Schottky annealing process according to the present invention; Figure 2 This is a graph showing the nickel Schottky annealing process in an embodiment of the present invention. Detailed Implementation

[0021] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0022] Example 1 This invention provides a process for nickel Schottky annealing, such as... Figure 1 As shown, the process includes the following steps: growing 700 on the wafer surface An 800nm ​​SiO2 masking film is photolithographically and etched according to a preset circuit diagram to form contact hole regions on a wafer. A mixed solution of sulfuric acid and hydrogen peroxide, with a volume ratio of sulfuric acid to hydrogen peroxide of 3:1, is used at 110 nm. Clean at 130°C for 10 minutes, preferably 120°C, then rinse with water and rinse with a hydrofluoric acid solution at a volume ratio of 10:1 at 20°C. Clean at 25°C for 1 minute, preferably 22°C, rinse with water and spin dry to perform the first cleaning of the etched wafer.

[0023] The wafer, after its first cleaning, is placed in an electron beam evaporation stage, where the evaporation vacuum pressure is... mbar, evaporation rate of 8 Å / s, evaporation temperature of At ℃, a nickel metal layer is deposited on the entire surface of the wafer and in the contact hole area. After the nickel metal deposition is completed, a second cleaning is performed to remove surface particles and contaminants generated during the deposition process.

[0024] The wafers, after the second cleaning, are fed into a quartz furnace tube for nickel Schottky annealing. The heating rate of the quartz furnace tube is 7... 9 ℃ / min, pressure 226 Pa, temperature rise to Constant temperature annealing after ℃ During the annealing process, a mixed atmosphere of nitrogen and oxygen is continuously introduced, with a nitrogen flow rate of [min]. L / min, oxygen flow rate is mL / min, the nickel metal in the contact hole undergoes a solid-state reaction with the silicon substrate to form nickel silicide (NiSi), and after annealing at 400 The wafer is removed from the quartz furnace tube at a rate of mm / min to avoid severe temperature shock and reduce film defects caused by thermal stress.

[0025] The wafer is then placed in an aqua regia bath for treatment to remove unreacted residual nickel metal from the wafer surface. The aqua regia consists of hydrochloric acid and nitric acid; the volume of hydrochloric acid is 13.5 L (with a dosage deviation of ±10%), and the volume of nitric acid is 4.5 L (with a dosage deviation of ±10%). This treatment selectively dissolves residual nickel metal on the wafer surface that has not undergone a solid-phase reaction with the silicon substrate, while retaining the nickel silicide (NiSi) formed within the contact holes. Aqua regia has strong oxidizing and complexing properties, effectively removing excess free nickel metal distributed on the wafer surface. This prevents residual nickel metal from increasing reverse leakage current and causing device failure. The low corrosion rate of aqua regia on nickel silicide ensures the structural integrity of the Schottky contact interface.

[0026] Example 2 by <111> Taking an N+N type epitaxial wafer with a specific crystal orientation as an example, firstly in <111> A 750nm thick SiO2 masking film is grown on an N+N type epitaxial wafer. Based on a pre-designed circuit, photolithography and etching processes are sequentially performed on the wafer to complete the patterning fabrication. The pre-designed circuit layout is transferred to a photoresist layer on the wafer surface using photolithography. Then, using the patterned photoresist as a mask, the SiO2 masking film is etched to remove the silicon oxide material corresponding to the implanted areas, exposing the underlying silicon substrate surface.

[0027] First, clean the area using a mixed solution of sulfuric acid and hydrogen peroxide, with a volume ratio of sulfuric acid to hydrogen peroxide of 3:1, at 110... Cleaning at 130℃ for 10 minutes, preferably 120℃, can remove residual photoresist, organic contaminants, and some metallic impurities from the wafer surface. After thoroughly removing residual acid with deionized water, a hydrofluoric acid solution with a volume ratio of 10:1 is used at 20℃. Clean at 25°C for 1 minute, with 22°C being the preferred temperature; hydrofluoric acid solution can remove the natural oxide layer and particulate impurities on the wafer surface, exposing the silicon surface. After cleaning, rinse the wafer with deionized water, and then spin dry to remove water stains from the wafer surface.

[0028] After the first cleaning, the wafer is stably mounted on a dedicated planetary carrier to ensure uniform heating during evaporation and improve the consistency of film thickness distribution across the entire surface. The planetary carrier is then inserted into the process chamber of the electron beam evaporation stage, and the vacuum system is activated to evacuate the chamber environment, setting the evaporation vacuum pressure to 1×10⁻⁶. - The 3mbar concentration reduces collision losses of gaseous particles, lowers the probability of impurity incorporation, and improves the density and purity of the metal film. An evaporation rate of 8 Å / s and an evaporation temperature of 140℃ are used to grow a 40nm thick Ni metal layer on the wafer surface.

[0029] After the nickel metal layer is grown, the wafer is vertically mounted on a dedicated quartz boat. This vertical mounting method reduces contact between the wafer's front-side metal layer and the carrier, preventing scratches and particle contamination. Once the quartz boat is placed in the isothermal zone of the quartz furnace tube, the annealing heating program is initiated. The temperature inside the furnace tube is uniformly increased to 490°C at a rate of 7°C / min. This gradual heating prevents wafer warping or film delamination due to thermal stress. Simultaneously, the furnace tube pressure is maintained at 226 Pa, and nitrogen gas at a flow rate of 7.5 L / min and oxygen at a flow rate of 75 mL / min are simultaneously introduced and maintained for 29 minutes to complete the nickel Schottky annealing process. During annealing, the nickel metal undergoes a solid-state reaction with the silicon substrate, forming a nickel silicide interface.

[0030] After nickel Schottky annealing, the wafer continues to cool inside a quartz furnace tube at a rate of 7°C / min to the unloading temperature. Figure 2As shown, slow cooling can gradually release the thermal stress inside the wafer, maintaining the stability of the film structure and wafer morphology. After the temperature drops to the unloading standard, the wafer is uniformly removed from the quartz tube along with the quartz boat at a speed of 400 mm / min, avoiding the impact of sudden temperature changes and airflow disturbances on the wafer surface condition.

[0031] This batch of processes produced a total of 50 wafers. After annealing, the surface morphology of the wafers was inspected and the electrical performance was tested. Two wafers were found to have surface defects, and the reverse leakage current of the device was 15μA.

[0032] Example 3 by <111> Taking an N+N type epitaxial wafer with a specific crystal orientation as an example, firstly in <111> A 750nm thick SiO2 masking film is grown on an N+N type epitaxial wafer. Based on a pre-designed circuit, photolithography and etching processes are sequentially performed on the wafer to complete the patterning fabrication. The pre-designed circuit layout is transferred to a photoresist layer on the wafer surface using photolithography. Then, using the patterned photoresist as a mask, the SiO2 masking film is etched to remove the silicon oxide material corresponding to the implanted areas, exposing the underlying silicon substrate surface.

[0033] First, clean the area using a mixed solution of sulfuric acid and hydrogen peroxide, with a volume ratio of sulfuric acid to hydrogen peroxide of 3:1, at 110... Cleaning at 130℃ for 10 minutes, preferably 120℃, can remove residual photoresist, organic contaminants, and some metallic impurities from the wafer surface. After thoroughly removing residual acid with deionized water, a hydrofluoric acid solution with a volume ratio of 10:1 is used at 20℃. Clean at 25°C for 1 minute, with 22°C being the preferred temperature; hydrofluoric acid solution can remove the natural oxide layer and particulate impurities on the wafer surface, exposing the silicon surface. After cleaning, rinse the wafer with deionized water, and then spin dry to remove water stains from the wafer surface.

[0034] After the first cleaning, the wafer is stably mounted on a dedicated planetary carrier to ensure uniform heating during evaporation and improve the consistency of film thickness distribution across the entire surface. The planetary carrier is then inserted into the process chamber of the electron beam evaporation stage, and the vacuum system is activated to evacuate the chamber environment, setting the evaporation vacuum pressure to 5 × 10⁻⁶. - ³mbar, evaporation rate 8 Å / s, evaporation temperature 140℃, and a Ni metal layer with a thickness of 50nm is grown on the wafer surface.

[0035] After the nickel metal layer is grown, the wafer is vertically mounted on a dedicated quartz boat. This vertical mounting method reduces contact between the wafer's front-side metal layer and the carrier, preventing scratches and particle contamination. Once the quartz boat is placed in the isothermal zone of the quartz furnace tube, the annealing heating program is initiated. The temperature inside the furnace tube is uniformly increased to 500°C at a rate of 8°C / min. This gradual heating prevents wafer warping or film peeling due to thermal stress. Simultaneously, the furnace tube pressure is maintained at 226 Pa, and nitrogen gas at a flow rate of 8.5 L / min and oxygen at a flow rate of 85 mL / min are simultaneously introduced and maintained for 30 minutes to complete the nickel Schottky annealing process. During annealing, the nickel metal undergoes a solid-state reaction with the silicon substrate, forming a nickel silicide interface.

[0036] After nickel Schottky annealing, the wafer continues to cool inside the quartz furnace tube. The quartz tube cools down to the unloading temperature at a rate of 8°C / min. This slow cooling gradually releases the internal thermal stress of the wafer, maintaining the stability of the film structure and wafer morphology. Once the temperature reaches the unloading standard, the wafer is uniformly removed from the quartz tube along with the quartz boat at a speed of 500 mm / min, avoiding the impact of sudden temperature changes and airflow disturbances on the wafer surface condition.

[0037] This batch of processes produced a total of 50 wafers. After annealing, the surface morphology of the wafers was inspected and the electrical performance was tested. The number of surface defects was 1 wafer, and the reverse leakage current of the device was 13.5μA.

[0038] Example 4 by <111> Taking an N+N type epitaxial wafer with a specific crystal orientation as an example, firstly in <111> A 750nm thick SiO2 masking film is grown on an N+N type epitaxial wafer. Based on a pre-designed circuit, photolithography and etching processes are sequentially performed on the wafer to complete the patterning fabrication. The pre-designed circuit layout is transferred to a photoresist layer on the wafer surface using photolithography. Then, using the patterned photoresist as a mask, the SiO2 masking film is etched to remove the silicon oxide material corresponding to the implanted areas, exposing the underlying silicon substrate surface.

[0039] First, clean the area using a mixed solution of sulfuric acid and hydrogen peroxide, with a volume ratio of sulfuric acid to hydrogen peroxide of 3:1, at 110... Cleaning at 130℃ for 10 minutes, preferably 120℃, can remove residual photoresist, organic contaminants, and some metallic impurities from the wafer surface. After thoroughly removing residual acid with deionized water, a hydrofluoric acid solution with a volume ratio of 10:1 is used at 20℃. Clean at 25°C for 1 minute, with 22°C being the preferred temperature; hydrofluoric acid solution can remove the natural oxide layer and particulate impurities on the wafer surface, exposing the silicon surface. After cleaning, rinse the wafer with deionized water, and then spin dry to remove water stains from the wafer surface.

[0040] After the first cleaning, the wafer is stably mounted on a dedicated planetary carrier to ensure uniform heating during evaporation and improve the consistency of film thickness distribution across the entire surface. The planetary carrier is then inserted into the process chamber of the electron beam evaporation stage, and the vacuum system is activated to evacuate the chamber environment, setting the evaporation vacuum pressure to 8 × 10⁻⁶. - ³ mbar, evaporation rate 8 Å / s, evaporation temperature 160℃, and a Ni metal layer with a thickness of 60 nm is grown on the wafer surface.

[0041] After the nickel metal layer is grown, the wafer is vertically mounted on a dedicated quartz boat. This vertical mounting method reduces contact between the wafer's front-side metal layer and the carrier, preventing scratches and particle contamination. Once the quartz boat is placed in the isothermal zone of the quartz furnace tube, the annealing heating program is initiated. The temperature inside the furnace tube is uniformly increased to 510°C at a rate of 9°C / min. This gradual heating prevents wafer warping or film delamination due to thermal stress. Simultaneously, the furnace tube pressure is maintained at 226 Pa, and nitrogen gas at a flow rate of 9.5 L / min and oxygen gas at a flow rate of 95 mL / min are simultaneously introduced and maintained for 31 minutes to complete the nickel Schottky annealing process. During annealing, the nickel metal undergoes a solid-state reaction with the silicon substrate, forming a nickel silicide interface.

[0042] After nickel Schottky annealing, the wafer continues to cool inside the quartz furnace tube. The quartz tube cools to the unloading temperature at a rate of 9 °C / min. Slow cooling gradually releases the internal thermal stress of the wafer, maintaining the stability of the film structure and wafer morphology. Once the temperature reaches the unloading standard, the wafer is uniformly removed from the quartz tube along with the quartz boat at a speed of 500 mm / min, avoiding the impact of sudden temperature changes and airflow disturbances on the wafer surface condition.

[0043] This batch of processes produced a total of 50 wafers. After annealing, the surface morphology of the wafers was inspected and the electrical performance was tested. The number of surface defects was 1 wafer, and the reverse leakage current of the device was 10μA.

[0044] In summary, depending on the annealing temperature, the number of surface defects on the annealed wafer is 0. 2 pieces, total of 50 pieces processed, reverse leakage current is 10. At 15μA, the nickel Schottky annealed wafers are used in the fabrication of Schottky chips, which are then fabricated on a semiconductor chip production line.

[0045] Two processes were used for wafer fabrication. In the first process, pure nitrogen was used during annealing. In the second process, 9.5 L of nitrogen and 95 mL of oxygen were introduced during annealing. The five-point method was used for testing, and one die was randomly selected from the top, middle, bottom, left, and right sides of the wafer for parameter testing. The test results are shown in Table 1.

[0046] Table 1 Test results of the two process methods

[0047] The reverse leakage currents at five points on the wafer corresponding to the first pure nitrogen annealing process were 28μA, 32μA, 26μA, 86μA, and 96μA, respectively. The measured values ​​at different locations on the wafer showed significant differences, with the leakage current in the left and right regions of the wafer being significantly higher. The reverse leakage currents at five points on the wafer corresponding to the second nitrogen-oxygen mixed atmosphere annealing process were 12.5μA, 13μA, 12.5μA, 12.5μA, and 12μA, respectively. The fluctuation range of the measured values ​​at each point was small. Compared with the pure nitrogen annealing scheme, it can reduce the reverse leakage current of the device and improve the uniformity of the electrical performance in the wafer plane. Introducing trace amounts of oxygen into the annealing atmosphere can optimize the state of the nickel silicide Schottky contact interface and suppress the formation of leakage channels.

[0048] The present invention and its embodiments have been described above illustratively. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention; the actual structure is not limited to this. Therefore, if a person skilled in the art, inspired by this description, designs a similar structure and embodiment without departing from the spirit of the invention, such design should fall within the scope of protection of this patent.

[0049] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

Claims

1. A process for nickel Schottky annealing, characterized in that, Includes the following steps: A masking film is grown on the surface of a wafer. The masking film is photolithographically etched and etched according to a preset circuit diagram to form a contact hole area on the wafer. The etched wafer is then cleaned for the first time. After the first cleaning, the wafer is placed in an electron beam evaporation stage to deposit nickel metal on the wafer surface and contact hole area. After the nickel metal is deposited, the wafer is cleaned a second time. After the second cleaning, the wafer is placed in a reaction tube and a preset atmosphere is introduced within a preset annealing time to perform nickel Schottky annealing. The nickel metal in the contact hole area reacts with silicon to form nickel silicide. The nickel silicide is then treated with aqua regia to remove unreacted residual nickel metal from the wafer surface.

2. The nickel Schottky annealing process according to claim 1, characterized in that: The masking membrane is 700. 800nm ​​SiO2 masking film.

3. The nickel Schottky annealing process according to claim 2, characterized in that: The first cleaning of the etched wafer includes: First, use a mixed solution of sulfuric acid and hydrogen peroxide at 110°C. Wash at 130℃ for 10 minutes, rinse with water, and then rinse with a hydrofluoric acid solution at a volume ratio of 10:1 at 20℃. Wash at 25℃ for 1 minute, rinse and spin dry.

4. The nickel Schottky annealing process according to claim 1, characterized in that: The thickness of the nickel metal deposition is 50±10 nm.

5. The nickel Schottky annealing process according to claim 1, characterized in that: The wafer, after the first cleaning, is placed in an electron beam evaporation stage, and evaporation is carried out under a vacuum pressure of [pressure value missing]. mbar, evaporation rate of 8 Å / s, evaporation temperature of Nickel metal deposition is performed on the wafer surface and contact hole area at ℃.

6. The nickel Schottky annealing process according to claim 5, characterized in that: The volume ratio of sulfuric acid to hydrogen peroxide is 3:

1.

7. The nickel Schottky annealing process according to claim 1, characterized in that: The reaction tube is a quartz furnace tube; The temperature of the reaction tube is The temperature was ℃, the pressure in the reaction tube was 226 Pa, and the heating rate was 7. 9 ℃ / min; The preset atmosphere includes nitrogen and oxygen, and the flow rate of the nitrogen is: The oxygen flow rate is L / min. mL / min; The nickel Schottky annealing time is min.

8. The nickel Schottky annealing process according to claim 7, characterized in that: The cooling rate of the reaction tube is ℃ / min; The nickel Schottky annealed material is withdrawn from the reaction tube at a rate of 400 km / h. mm / min.

9. The nickel Schottky annealing process according to claim 1, characterized in that: The aqua regia comprises hydrochloric acid and nitric acid, wherein the volume of hydrochloric acid is 13.5 L and the dosage deviation is ±10%.

10. The nickel Schottky annealing process according to claim 9, characterized in that: The volume of the nitric acid is 4.5 L, with a dosage deviation of ±10%.