Methods for preparing solar cells and solar cells
By forming a mask layer with varying thickness on the back surface of the TBC battery and combining it with a high-temperature diffusion process, the problem of uneven morphology on the back surface of the TBC battery was solved, achieving uniform coverage of the passivation layer and improved optical reflectivity, which significantly improved the battery's conversion efficiency.
Patent Information
- Application Number
- CN202611114692.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-10
AI Technical Summary
Existing TBC batteries suffer from uneven surface morphology in the P-region, N-region, and isolation region of the backlight due to multiple laser film opening and alkaline etching processes during fabrication. This results in uneven passivation layer coverage, severe carrier recombination, and low optical reflectivity, which limits the improvement of conversion efficiency.
By forming a first mask layer with a thickness difference on the back surface of the substrate, combined with a high-temperature diffusion process, the doped region is precisely defined and the residual mask layer in the isolation region is removed, thus achieving a planar structure across the entire domain. This ensures atomic-level uniform coverage of the passivation layer and avoids sidewall exposure and film breakage.
This achievement realizes a flat, coplanar structure with consistent backlight surface height, reducing carrier recombination losses, improving open-circuit voltage, fill factor, and short-circuit current density, enhancing long-wave reflection effects, and synergistically improving the optical absorption and electrical passivation performance of the battery.
Smart Images

Figure CN123076041A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic cell technology, specifically relating to a method for preparing a solar cell and the solar cell itself. Background Technology
[0002] Back-contact (BC) cells are a key technological direction for high-efficiency crystalline silicon solar cells. Their core structural feature is that both the P-type and N-type doped regions are fabricated on the back surface of the cell, with the positive and negative electrodes correspondingly positioned on these doped regions. Because there are no metal grid lines obstructing the light-receiving surface, BC cells effectively eliminate electrode shading losses, significantly enhancing the optical absorption of incident light and thus achieving excellent short-circuit current density. Simultaneously, the elimination of the front-surface emitter effectively suppresses recombination losses on the front surface of the cell.
[0003] With technological advancements, carrier-selective passivation contact technology has been introduced into BC structures. Among them, the tunneling layer passivation contact (TOPCon) technology achieves excellent interface passivation and selective carrier transport by fabricating a stacked structure of an ultrathin tunneling layer and a doped polycrystalline silicon layer on the back surface of a silicon substrate. This ultrathin oxide layer can tunnel electrons and block holes, significantly reducing recombination current, while the doped polycrystalline silicon layer reduces series resistance due to its lateral transport characteristics. Together, they improve the open-circuit voltage and fill factor of the battery.
[0004] The TBC (Transient Carbon Cell) battery, which combines TOPCon passivation technology with the BC structure, theoretically possesses the advantages of both, making it a potential direction for further improving conversion efficiency. However, existing TBC batteries require multiple laser film-cutting and alkaline etching processes during fabrication, resulting in significant uneven surface morphology in the P-region, N-region, and isolation region (GAP region) of the finished battery's back surface. Existing passivation systems are mainly optimized for planar or textured substrates. For the side sections between the P-region and GAP region, and between the N-region and GAP region, the passivation layer coverage uniformity and interface quality are poor, leading to severe carrier recombination. Furthermore, the textured structure formed in the GAP region after etching not only increases recombination centers but also reduces the reflectivity of long-wavelength light, further weakening the battery's optical management effect. These problems ultimately limit further improvements in the conversion efficiency of TBC batteries.
[0005] The information disclosed in this background section is intended only to enhance the understanding of the overall background of the invention and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a solar cell and a solar cell that can improve the passivation effect of the cell, thereby improving the conversion efficiency of the cell.
[0007] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:
[0008] A method for preparing a solar cell, comprising:
[0009] A substrate is provided, the backlight surface of the substrate including a first region, a second region, and an isolation region located between the first region and the second region;
[0010] A first mask layer is formed in the second region and the isolation region. The first mask layer in the second region has a first thickness D1, and the first mask layer in the isolation region has a second thickness D2. The first thickness D1 is less than the second thickness D2.
[0011] A first doped structure is formed in the first region;
[0012] The first mask layer of the second region and the isolation region are simultaneously etched to completely remove the first mask layer of the second region. The remaining first mask layer in the isolation region has a third thickness D3, which is less than the second thickness D2.
[0013] A second doped structure is formed in the second region, the doping type of the second doped structure being opposite to that of the first doped structure;
[0014] Remove the remaining first mask layer from the isolation area.
[0015] In one or more embodiments of the present invention, the ratio R of the second thickness to the first thickness satisfies: 1.6 ≤ R ≤ 5; and / or,
[0016] The remaining first mask layer in the isolation zone is 30%-60% of the initial first mask layer thickness in the isolation zone; and / or,
[0017] The first thickness is 10nm-60nm, and the second thickness is 20nm-120nm.
[0018] In one or more embodiments of the present invention, the first mask layer of the second region and the first mask layer of the isolation region are made of the same mask material; and / or,
[0019] The first mask layer is an alkali-resistant mask layer; and / or,
[0020] The masking material of the first mask layer includes one or more of aluminum oxide, silicon oxide, silicon nitride, and silicon oxynitride.
[0021] In one or more embodiments of the present invention, a wet etching process is used to perform a synchronous etching step of the first mask layer, and a wet etching process is used to remove the residual first mask layer in the isolation region; wherein the etching solution includes an acid solution.
[0022] In one or more embodiments of the present invention, a first doped structure is formed in the first region, including:
[0023] A first tunneling layer is formed in a first region on the back surface of the substrate;
[0024] An intrinsic amorphous silicon layer is formed on the entire back surface of the substrate. The intrinsic amorphous silicon layer covers the surface of the first mask layer covering the second region and the isolation region, and the surface of the first tunneling layer covering the first region.
[0025] The intrinsic amorphous silicon layer is subjected to a first diffusion process to transform the intrinsic amorphous silicon layer into a first doped polycrystalline silicon layer, and a second mask layer is formed on the surface of the first doped polycrystalline silicon layer.
[0026] The second mask layer of the second region and the isolation region of the backlight surface is removed using a laser process;
[0027] The first doped polysilicon layer of the second region and the isolation region of the backlight surface is removed by an alkaline etching process.
[0028] In one or more embodiments of the present invention, a second doped structure is formed in the second region, including:
[0029] A second tunneling layer is formed in a second region on the back surface of the substrate;
[0030] An intrinsic amorphous silicon layer is formed on the entire back surface of the substrate. The intrinsic amorphous silicon layer covers the surface of a first mask layer covering the isolation region, the surface of a second mask layer covering the first region, and the surface of a second tunneling layer covering the second region.
[0031] A second diffusion process is performed on the intrinsic amorphous silicon layer to transform it into a second doped polycrystalline silicon layer, and a third mask layer is formed on the surface of the second doped polycrystalline silicon layer.
[0032] The third mask layer of the first region and the isolation region of the backlight surface is removed using a laser process;
[0033] The second doped polysilicon layer in the first region and the isolation region of the backlight surface is removed by an alkaline etching process.
[0034] In one or more embodiments of the present invention, prior to the step of removing the residual first mask layer in the isolation region, the method further includes:
[0035] A pyramidal velvet structure is formed on the light-receiving surface of the substrate using a velvet-making process.
[0036] In one or more embodiments of the present invention, after the step of removing the residual first mask layer in the isolation region, the method further includes:
[0037] A first passivation layer and / or a first antireflection layer are prepared on the light-receiving surface of the substrate; and / or,
[0038] A second passivation layer and / or a second antireflection layer are prepared on the back surface of the substrate; and / or,
[0039] Electrodes are fabricated on the back surface of the substrate, respectively in contact with the first doped layer and the second doped layer.
[0040] In one or more embodiments of the present invention, prior to the step of forming a first mask layer in the second region and the isolation region of the backlight surface of the substrate, the method further includes:
[0041] The light-receiving surface and the back-light-receiving surface of the substrate are subjected to a double-sided polishing process.
[0042] A solar cell, comprising:
[0043] The substrate includes a light-receiving surface and a backlighting surface, wherein the backlighting surface includes a first region, a second region, and an isolation region located between the first region and the second region;
[0044] The first doped structure is located in the first region of the backlight surface;
[0045] The second doped structure is located in the second region of the backlight surface, and the doping type of the second doped structure is opposite to that of the first doped structure.
[0046] The substrate backlight side of the first region and the second region are flush with each other within the process error range.
[0047] In one or more embodiments of the present invention, the backlight side of the substrate of the isolation zone is flush with the backlight side of the substrate of the first region and the second region within the range of process error.
[0048] In one or more embodiments of the present invention, the first doped structure includes a first tunneling layer and a first doped polysilicon layer, the thickness of the first tunneling layer is 1 nm-2 nm, the first doped polysilicon layer is a P-type doped polysilicon layer, the thickness of the first doped polysilicon layer is 50 nm-500 nm, and the doping concentration of the first doped polysilicon layer is 1E19-1E21 atoms / cm². 3 ; and / or,
[0049] The second doped structure includes a second tunneling layer and a second doped polysilicon layer. The thickness of the second tunneling layer is 1 nm-2 nm. The second doped polysilicon layer is an N-type doped polysilicon layer with a thickness of 50 nm-500 nm and a doping concentration of 8E19-9E20 atoms / cm². 3 ; and / or,
[0050] The light-receiving surface of the substrate has a pyramidal textured surface, and the reflectivity of the textured surface of the light-receiving surface of the substrate is 7%-10%; and / or,
[0051] The back surface of the substrate is a polished surface, and the reflectivity of the back surface of the substrate is 35%-40%.
[0052] In one or more embodiments of the present invention, a first passivation layer and / or a first antireflection layer are stacked on the light-receiving surface of the substrate; and / or,
[0053] A second passivation layer and / or a second antireflection layer are stacked on the back surface of the substrate; and / or,
[0054] Electrodes are respectively disposed on the first doped structure and the second doped structure.
[0055] In one or more embodiments of the present invention, the first passivation layer is an aluminum oxide passivation layer with a thickness of 3nm-10nm; and / or,
[0056] The first antireflection layer is a stacked film formed by any one or more of silicon nitride, silicon oxynitride, and silicon oxide layers, with a thickness of 70nm-90nm; and / or,
[0057] The second passivation layer is an aluminum oxide passivation layer with a thickness of 3nm-10nm; and / or,
[0058] The second antireflection layer is a stacked film formed by any one or more of silicon nitride, silicon oxynitride, and silicon oxide layers, with a thickness of 70nm-90nm.
[0059] Compared with existing technologies, the solar cell fabrication method and solar cell of the present invention achieve precise definition of different doped regions and isolation regions by utilizing the thickness difference of the first mask layer in the second region and the isolation region, combined with the blocking effect of the first mask layer of different thicknesses on the doping source during high-temperature diffusion. This eliminates the need for physical removal of the silicon substrate, resulting in a uniform surface height among the first region, second region, and isolation region of the cell's backlight surface, presenting a flat coplanar structure. This flat coplanar structure fundamentally avoids defects such as discontinuous passivation film coverage and exposed sidewalls caused by stepped terrain in traditional processes.
[0060] The solar cell fabrication method and solar cell of the present invention eliminate the uneven morphology of the back surface of the cell in the prior art, achieving a fully planar structure. This fully planar structure enables atomically uniform and dense conformal coverage of the passivation layer during subsequent deposition, eliminating the film breakage or thinning phenomena at the conventional cross-section. Consequently, the interface defect state density in each region, especially at the boundary between the first / isolation region and the second / isolation region, is significantly reduced, effectively suppressing carrier recombination in the edge regions, thereby significantly improving the open-circuit voltage (Voc) and fill factor (FF) of the cell.
[0061] The solar cell fabrication method and solar cell of the present invention have an isolation region that is not etched from beginning to end, and is ultimately retained as a smooth polished surface structure, which has a better passivation effect and long-wave reflection effect, significantly increases the short-circuit current density (Jsc) of the cell, and achieves a synergistic improvement in optical absorption and electrical passivation. Attached Figure Description
[0062] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0063] Figure 1 This is a process flow diagram of the method for preparing solar cells in this invention;
[0064] Figures 2a-2p This is a flowchart illustrating the process steps of the solar cell fabrication method in this invention. Detailed Implementation
[0065] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions in the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.
[0066] As the conversion efficiency of crystalline silicon solar cells continues to improve and gradually approaches its theoretical limit, the limiting effect of any residual optical and electrical losses on efficiency becomes increasingly significant. Reducing these two types of losses has become a key breakthrough for further efficiency improvement.
[0067] Back contact (BC) batteries, by transferring all electrodes to the back surface of the battery, completely eliminate the shading caused by the grid lines on the light-receiving side, significantly improving short-circuit current density and becoming one of the mainstream architectures for next-generation high-efficiency batteries. Meanwhile, the carrier selection mechanism based on tunneling layer passivated contacts (TOPCon) is widely recognized as the passivation technology with the most promising industrial applications due to its excellent interface passivation performance and low contact resistance.
[0068] Based on the aforementioned complementary advantages, the TBC cell, which integrates the TOPCon passivated contact structure with the BC back contact structure, can theoretically achieve dual gains of enhanced optical absorption and optimized electrical passivation, and is considered one of the important technical routes for the next generation of high-efficiency crystalline silicon cells.
[0069] However, at the engineering fabrication level, existing TBC battery processes generally employ a combination of multiple laser film-cutting and alkaline etching to achieve spatial definition and electrical isolation of the P-type doped region (P-region), N-type doped region (N-region), and isolation region (GAP region) on the back surface. This process inevitably leads to inconsistent surface heights among the P-region, GAP region, and N-region on the finished battery back surface, resulting in a significant stepped non-planar morphology. While the subsequently deposited back surface passivation layer performs well in the horizontal region, the side sections at the P / GAP and N / GAP region boundaries exhibit significantly increased interface defect state density and intensified carrier recombination due to insufficient passivation film uniformity and decreased film density. This directly deteriorates the open-circuit voltage and fill factor.
[0070] Meanwhile, the GAP region exhibits a rough, textured surface after alkaline etching. This structure increases the specific surface area, introducing additional recombination centers. However, it also causes diffuse reflection of long-wavelength light (especially infrared light with wavelengths greater than 800 nm), weakening the back reflector's effective recovery of long-wavelength light and leading to long-wavelength response loss. This, in turn, limits further improvement in short-circuit current density. These dual electrical and optical defects make it difficult for existing TBC cells to achieve the theoretically expected conversion efficiency.
[0071] To address the above problems, existing technologies have attempted to alleviate them by adjusting laser parameters (such as power and scanning rate) or optimizing the etching solution concentration, but none of them have fundamentally solved the passivation conformal preservation problem under non-planar topography and the optical design contradictions of the GAP area.
[0072] Therefore, how to accurately define and planarize the P-region, N-region and GAP-region of the backlight surface of TBC battery without alkaline etching, and simultaneously optimize the surface morphology of the GAP-region to improve passivation quality and long-wave reflection characteristics, has become a key technical challenge that urgently needs to be overcome in this field.
[0073] Based on this, such as Figure 1 As shown, the present invention provides a method for preparing a solar cell, specifically including the following steps:
[0074] S1 provides a substrate, the backlight surface of which includes a first region, a second region, and an isolation region located between the first region and the second region.
[0075] S2, a first mask layer is formed in the second region and the isolation region. The first mask layer in the second region has a first thickness D1, and the first mask layer in the isolation region has a second thickness D2. The first thickness D1 is less than the second thickness D2.
[0076] S3 forms the first doped structure in the first region.
[0077] S4, simultaneously etch the first mask layer of the second region and the isolation region to completely remove the first mask layer of the second region. The remaining first mask layer in the isolation region has a third thickness D3, which is less than the second thickness D2.
[0078] S5, a second doped structure is formed in the second region, and the doping type of the second doped structure is opposite to that of the first doped structure.
[0079] S6, remove the remaining first mask layer in the isolation area.
[0080] In step S2, the first mask layer is an alkali-resistant mask layer; the first mask layer in the second region and the first mask layer in the isolation region are made of the same mask material; the ratio R of the second thickness to the first thickness satisfies: 1.6≤R≤5; the remaining first mask layer in the isolation region is 30%-60% of the initial thickness of the first mask layer in the isolation region.
[0081] Before removing the remaining first mask layer in the isolation area in step S6, the process further includes forming a pyramidal textured surface structure on the light-receiving surface of the substrate using a texturing process.
[0082] Without adding extra high-cost photolithography processes, this invention achieves topographic planarization and low recombination transition interfaces between the first region, the second region, and the isolation region through process innovation and structural improvement, thereby reducing carrier recombination losses at the boundaries of each region and simultaneously improving the long-wavelength light reflection capability of the isolation region.
[0083] This invention utilizes the thickness difference of the first mask layer in the second region and the isolation region, combined with the blocking effect of the first mask layer of different thicknesses on the doping source during high-temperature diffusion, to achieve precise definition of different doped regions and isolation regions. This eliminates the need for physical removal of the silicon substrate, resulting in a uniform surface height among the first region, second region, and isolation region of the battery backlight surface, presenting a flat coplanar structure. This flat coplanar structure fundamentally avoids the defects in traditional processes, such as discontinuous passivation film coverage and exposed sidewalls caused by stepped terrain.
[0084] This invention eliminates the uneven morphology of the battery back surface in existing technologies, achieving a fully planar structure. This fully planar structure enables atomically uniform and dense conformal coverage of the passivation layer during subsequent deposition, eliminating film breakage or thinning at the traditional cross-section. Consequently, the interface defect state density in each region, especially at the boundaries of the first / isolation region and the second / isolation region, is significantly reduced, effectively suppressing carrier recombination in the edge regions and thus significantly improving the battery's open-circuit voltage (Voc) and fill factor (FF).
[0085] The isolation region of this invention is not etched from beginning to end, and is ultimately retained as a smooth polished surface structure, which has better passivation effect and long-wave reflection effect, significantly increases the short-circuit current density (Jsc) of the battery, and achieves a synergistic improvement in optical absorption and electrical passivation.
[0086] The present invention will be further described below with reference to the accompanying drawings. The solar cell in this invention is illustrated using a TBC cell as an example. The specific preparation method of the TBC cell in this invention includes the following steps:
[0087] like Figure 2a As shown, a silicon substrate 10 is provided.
[0088] The silicon substrate 10 of the present invention includes a first surface S1 and a second surface S2 disposed opposite to each other. The first surface S1 is a light-receiving surface, and the second surface S2 is a backlight surface. The backlight surface includes a first region S21, a second region S22, and an isolation region S23. The first region S21 and the second region S22 are distributed alternately, and the isolation region S23 is located between the first region S21 and the second region S22.
[0089] For example, the silicon substrate 10 in this invention is an N-type crystalline silicon substrate. First, the silicon substrate 10 is double-sided polished to form a polished surface (not shown). The reflectivity of the light-receiving surface of the silicon substrate 10 is 35%-40%, for example, it can be 35%, 38%, 40%, or any range of the above values. The reflectivity of the backlight surface of the silicon substrate 10 is 35%-40%, for example, it can be 35%, 38%, 40%, or any range of the above values.
[0090] Specifically, organic contaminants and particles on the silicon substrate surface are first removed in a mixed solution of potassium hydroxide (KOH) and hydrogen peroxide (H2O2). Then, alkaline polishing is performed in a solution of alkaline solution (such as potassium hydroxide KOH or sodium hydroxide NaOH) and polishing additives. The etching depth of the alkaline solution during alkaline polishing is 3μm-8μm, for example, 3μm, 5μm, 8μm, or any range of these values. After alkaline polishing, the substrate is rinsed again in a mixed solution of KOH and H2O2 to remove residues. Finally, acid washing is performed using a mixed solution of hydrofluoric acid (HF) and hydrochloric acid (HCl) to neutralize residual alkaline solution and remove metal ion contamination; the substrate is then rinsed with water and dried.
[0091] like Figure 2b As shown, a high-temperature diffusion-resistant first mask layer A is deposited in the second region S22 and the isolation region S23 of the backlight surface of the silicon substrate 10. The first mask layer A deposited above the second region S22 has a first thickness D1, and the first mask layer A deposited above the isolation region S23 has a second thickness D2, where the second thickness D2 > the first thickness D1. The first region S21 is not deposited with the first mask layer A, or the first mask layer A in this region is removed by a subsequent process. The first mask layer A is used to selectively block dopant atoms (boron atoms, phosphorus atoms) from entering the silicon substrate during subsequent high-temperature diffusion.
[0092] The first mask layer A is an alkali-resistant mask layer. The first mask layer A of the second region S22 and the first mask layer A of the isolation region S23 are made of the same mask material, which can be selected from alumina (Al2O3) or silicon dioxide (SiO2). X Silicon nitride (SiN) X ), silicon oxynitride (SiON) X One or more of the following materials are used. The above materials exhibit excellent chemical stability at high-temperature diffusion process temperatures, effectively blocking the penetration of boron atoms and / or phosphorus atoms, and have good adhesion and thermal compatibility with the silicon substrate 10. At the same time, the above materials have extremely low corrosion rates (corrosion rate < 1 nm / min) in alkaline environments (such as NaOH, KOH or TMAH solutions), and can maintain the integrity of the film structure and the stability of the thickness during alkaline etching and / or alkaline cleaning processes, without significant thinning or pinhole expansion.
[0093] In some embodiments of the present invention, the first thickness D1 of the second region S22 and the second thickness D2 of the isolation region S23 satisfy at least one of the following conditions:
[0094] First, the first thickness D1 ranges from 10nm to 60nm, for example, it can be 10nm, 15nm, 20nm, 40nm, 60nm, etc., or any range of the above values. The second thickness D2 ranges from 20nm to 120nm, for example, it can be 20nm, 40nm, 60nm, 80nm, 120nm, etc., or any range of the above values. The values of the first thickness D1 and the second thickness D2 must ensure that D2 > D1, and that there is a sufficient thickness difference between the two.
[0095] Second, the ratio R of the second thickness D2 to the first thickness D1 satisfies: 1.6 ≤ R ≤ 5, for example, it can be 1.6, 2.0, 4.6, 5, etc., or it can be any range of the above values. When the ratio R is too small (R < 1.6), the thickness difference between the first thickness D1 and the second thickness D2 is insufficient. In the subsequent etching and thinning process, it is difficult to ensure that the first mask layer A of the isolation region S23 retains sufficient residual thickness while completely removing the first mask layer A of the second region S22. This can easily lead to the residual first mask layer A of the isolation region S23 failing to effectively block dopant atoms from penetrating in the subsequent diffusion process, resulting in the silicon substrate 10 of the isolation region S23 being misdoped. When the ratio R is too large (R > 5), the second thickness D2 is too thick. On the one hand, this increases the mask deposition time and raw material consumption. On the other hand, the excessively thick first mask layer A of the isolation region S23 is difficult to completely remove in the final mask removal process, and the residue may affect the passivation quality and optical performance of the isolation region S23 surface. Therefore, by controlling the ratio R within the range of 1.6-5, both the selectivity of mask removal and the residual thickness requirement of the mask in the isolation zone S23 can be taken into account.
[0096] Third, after removing the first mask layer A from the second region S22, the thickness of the remaining first mask layer A in the isolation region S23 is 30% to 60% of the initial thickness of the first mask layer A in the isolation region S23. For example, it can be 30%, 40%, 50%, 60%, or any range of the above values. The thickness of the remaining first mask layer A in the isolation region S23 is sufficient (usually ≥20nm) to ensure that the first mask layer A in the isolation region S23 can effectively block the penetration of dopant atoms during subsequent diffusion. On the other hand, the residual thickness should not exceed 60% of the initial thickness to ensure that the residual layer can be completely removed in the final mask removal process, avoiding adverse effects of mask material residue on the passivation quality and long-wave reflection characteristics of the isolation region S23 surface.
[0097] like Figure 2cAs shown, a first tunneling layer 22 is formed in the first region S21 (the region not covered by the first mask layer A) on the backlight surface of the silicon substrate 10 using LPCVD (low-pressure chemical vapor deposition) technology, and a first intrinsic amorphous silicon layer 23' is deposited across the entire surface. The first intrinsic amorphous silicon layer 23' covers the surface of the first mask layer A in the second region S22 and the isolation region S23, as well as the surface of the first tunneling layer 22 in the first region S21. The first tunneling layer 22 can be a silicon oxide layer with a thickness of 1nm-2nm, for example, it can be 1nm, 1.5nm, 2nm, etc., or any range of the above values. The thickness of the first intrinsic amorphous silicon layer 23' is 50nm-500nm, for example, it can be 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, etc., or any range of the above values.
[0098] It should be noted that during the process of preparing the first tunneling layer 22 and depositing the first intrinsic amorphous silicon layer 23' on the back surface of the silicon substrate 10 using the LPCVD (low-pressure chemical vapor deposition) process, a wrap-around plating will be formed on the side of the silicon substrate, and the first tunneling layer 22 and the first intrinsic amorphous silicon layer 23' will also be formed on the light-receiving surface of the silicon substrate. However, the layer structures of the side wrap-around plating and the light-receiving surface will be removed together during the subsequent removal of the layer structures of the second region and the isolation region.
[0099] like Figure 2d As shown, the silicon substrate 10 is placed in a diffusion carrier, and a first diffusion process is performed on the first intrinsic amorphous silicon layer 23' to convert the first intrinsic amorphous silicon layer 23' into a first doped polycrystalline silicon layer 23, and a second mask layer 24 is formed on the surface of the first doped polycrystalline silicon layer 23.
[0100] The first doped polysilicon layer 23 is a p-type doped (boron-doped) polysilicon layer, and the doping concentration of the first doped polysilicon layer 23 is 1E19 atoms / cm². 3 -1E21 atoms / cm 3 For example, it could be 1E19 atoms / cm 3 2E19 atoms / cm 3 1E20 atoms / cm 3 1E21 atoms / cm 3 etc., or can be a range of any of the above values; the second mask layer 24 is a boron-doped glass layer (BSG layer).
[0101] For example, a silicon substrate is loaded into a quartz boat and fed into a boron diffusion furnace tube for high-temperature diffusion. Boron tribromide (BBr3) or boron trichloride (BCl3) is used as the boron source, nitrogen as the carrier gas, and oxygen as the oxidizing atmosphere. Under these conditions, boron atoms diffuse from the gas phase into the first intrinsic amorphous silicon layer 23', forming a p-type doped polycrystalline silicon layer.
[0102] After boron diffusion is completed, high-temperature oxidation is performed in situ inside the diffusion furnace tube. Under these high-temperature oxidation conditions, oxygen reacts with the boron-rich layer on the back surface of the silicon substrate 10, growing a BSG layer on its surface.
[0103] It should be noted that the first intrinsic amorphous silicon layer 23' on the light-receiving surface of the silicon substrate 10 is also converted into a first doped polycrystalline silicon layer 23 in the first diffusion process, and a second mask layer 24 (BSG) is generated on the surface.
[0104] like Figure 2e As shown, a laser process is used to remove the second mask layer 24 of the second region S22 and the isolation region S23, while retaining the second mask layer 24 of the first region S21. Specifically, a purple or green laser (typical wavelengths of 355nm and 532nm) is used to pattern the second mask layer 24 covering the first doped polysilicon layer 23. The laser etching process parameters are controlled so that the laser beam is precisely focused on the surface of the first doped polysilicon layer 23. Through photothermal effect, the material of the second mask layer 24 in the irradiated area is instantly vaporized or peeled off, thereby forming a patterned groove window. The etching endpoint is determined by precisely removing the second mask layer 24 and exposing the underlying first doped polysilicon layer 23.
[0105] like Figures 2f to 2h As shown, RCA cleaning removes the second mask layer 24, the first doped polysilicon layer 23, and the first tunneling layer 22 from the light-receiving surface of the silicon substrate 10, removes the first doped polysilicon layer 23 from the second region S22 and the isolation region S23 of the backlight surface of the silicon substrate 10, and removes all of the first mask layer A from the second region.
[0106] Specifically, such as Figure 2f As shown, a chain-type single-sided cleaning device is used to pass the silicon substrate 10 through a chain-type pickling tank. The pickling solution is diluted hydrofluoric acid. The cleaning is carried out at room temperature to remove the second mask layer 24 on the light-receiving surface of the silicon substrate 10.
[0107] like Figure 2g As shown, the first doped polysilicon layer 23 of the light-receiving surface and the second region S22 of the backlight surface and the isolation region S23 of the backlight surface are removed by alkaline etching.
[0108] Specifically, the solar cell is etched in an alkaline etching solution (preferably potassium hydroxide KOH or tetramethylammonium hydroxide TMAH) with a mass fraction of 5%-15%, for example, 5%, 9%, 11%, 15%, or any range thereof; the etching temperature is 70℃-80℃, for example, 70℃, 75℃, 80℃, or any range thereof; the etching time is 60-120 seconds, for example, 60s, 80s, 100s, 120s, or any range thereof. Under these conditions, the alkaline etching solution selectively etches the exposed first doped polycrystalline silicon layer 23.
[0109] like Figure 2h As shown, the first mask layer A of the second region S22 is removed by acid etching (hydrofluoric acid), and the first tunneling layer 22 of the photosensitive surface of the silicon substrate 10 is also removed. After the first mask layer A of the second region S22 is completely etched, a certain thickness of the first mask layer A is still retained on the isolation region S23; the residual first mask layer A in the isolation region S23 has a third thickness D3, D3 is less than D2, and D3 / D2 = 0.3-0.6.
[0110] like Figure 2i As shown, a second tunneling layer 32 and a second intrinsic amorphous silicon layer 33' are sequentially stacked on the back surface of the silicon substrate 10. The second intrinsic amorphous silicon layer 33' covers the surface of the first mask layer A of the isolation region S23, the surface of the second mask layer 24 of the first region S21, and the surface of the second tunneling layer 32 of the second region S22.
[0111] Specifically, a second tunneling layer 32 is grown in the second region S22 of the backlight surface of the silicon substrate 10 using LPCVD thermal oxidation, and a second intrinsic amorphous silicon layer 33' is deposited across the entire backlight surface of the silicon substrate 10. The second tunneling layer 32 can be a silicon oxide layer with a thickness of 1nm-2nm, such as 1nm, 1.5nm, 2nm, or any range of the above values; the thickness of the second intrinsic amorphous silicon layer 33' is 50nm-500nm, such as 50nm, 100nm, 200nm, 400nm, 500nm, or any range of the above values.
[0112] It should be noted that during the process of preparing the second tunneling layer 32 and depositing the second intrinsic amorphous silicon layer 33' on the backlight surface of the silicon substrate 10 using the LPCVD (low-pressure chemical vapor deposition) process, a wrap-around plating will be formed on the side of the silicon substrate, and the second tunneling layer 32 will also be formed and the second intrinsic amorphous silicon layer 33' will be deposited on the light-receiving surface of the silicon substrate. However, the layer structure of the side wrap-around plating and the light-receiving surface will be removed together during the subsequent removal of part of the layer structure of the first region and the isolation region.
[0113] like Figure 2j As shown, the silicon substrate 10 is placed in a diffusion carrier, and a second diffusion process is performed on the second intrinsic amorphous silicon layer 33' to form a second doped polycrystalline silicon layer 33, and a third mask layer 34 is formed on the surface of the second doped polycrystalline silicon layer 33.
[0114] The second doped polysilicon layer 33 is an N-type doped (phosphorus doped) polysilicon layer, and the doping concentration of the second doped polysilicon layer 33 is 8E19 atoms / cm². 3 -9E20 atoms / cm 3 For example, it could be 8E19 atoms / cm 3 9E19 atoms / cm 3 8E20 atoms / cm 3 9E20 atoms / cm 3 etc., or can be any range of the above values, the third mask layer 34 is a phosphorus-doped glass layer (PSG layer).
[0115] For example, a silicon substrate is transferred to a phosphorus diffusion furnace tube, and phosphorus oxychloride (POCl3) is used as the phosphorus source for high-temperature phosphorus diffusion. During the phosphorus diffusion process, phosphorus atoms diffuse from the gas phase into the second intrinsic amorphous silicon layer 33', forming an N-type doped polycrystalline silicon layer. During the phosphorus diffusion process, a third mask layer 34 is simultaneously formed on the surface of the second doped polycrystalline silicon layer 33. This third mask layer 34 serves as a sacrificial layer for laser film opening and a protective layer for the second doped polycrystalline silicon layer 33 in subsequent processes.
[0116] It should be noted that the second intrinsic amorphous silicon layer 33' on the light-receiving surface of the silicon substrate 10 is simultaneously transformed into a second doped polycrystalline silicon layer 33 and a third mask layer 34 is generated on the surface.
[0117] like Figure 2k As shown, the third mask layer 34 of the first region S21 and the isolation region S23 is removed by laser process, while the third mask layer 34 of the second region S22 is retained.
[0118] Specifically, a purple or green laser (typical wavelengths of 355nm and 532nm) is used to etch the third mask layer 34 on the first region S21 and the isolation region S23. The laser process parameters are controlled so that the third mask layer 34 on the first region S21 and the isolation region S23 is completely removed, exposing the underlying second doped polysilicon layer 33.
[0119] like Figure 2lAs shown, a chain-type single-sided cleaning device is used to remove the third mask layer 34 on the light-receiving surface of the silicon substrate 10. Exemplarily, the solar cell is placed on a chain conveyor belt with the light-receiving surface facing down and conveyed through an HF etching tank. The etching solution is a 10%-20% hydrofluoric acid solution by mass. The chain speed is controlled at 2m / min-3m / min, for example, 2m / min, 2.5m / min, 3m / min, or any range thereof. The process temperature is maintained at 20℃-25℃, for example, 20℃, 22℃, 24℃, 25℃, or any range thereof.
[0120] like Figure 2m As shown, the second doped polysilicon layer 33 of the first region S21 and the isolation region S23 is removed by alkaline etching, and a light-trapping structure is prepared on the light-receiving surface of the silicon substrate 10 by texturing.
[0121] Specifically, the solar cell is etched in an alkaline etching solution (preferably KOH or TMAH) with a mass fraction of 5%-15%, for example, 5%, 9%, 11%, 15%, or any range thereof; the etching temperature is 70℃-80℃, for example, 70℃, 75℃, 80℃, or any range thereof; the etching time is 60-120 seconds, for example, 60s, 80s, 100s, 120s, or any range thereof. Under these conditions, the alkaline etching solution selectively etches the exposed second doped polysilicon layer 33 (including the second doped polysilicon layer 33 exposed on the light-receiving surface and the second tunneling layer 32).
[0122] The cleaning process involves using a mixed solution of 1%-10% (by mass) alkaline solution (preferably KOH) and 1%-20% hydrogen peroxide (H2O2) at a temperature of 60℃-70℃ (e.g., 60℃, 65℃, 70℃, or any range thereof) for a time of 120-240 seconds (e.g., 120s, 170s, 190s, 210s, 240s, or any range thereof). Hydrogen peroxide acts as an oxidant, oxidizing and decomposing organic contaminants and metallic impurities on the surface, while the alkaline solution assists in removing residual particles, providing a clean surface for subsequent texturing.
[0123] Anisotropic texturing is performed using a mixture of 0.05%-10% (by mass) alkaline solution (preferably KOH or TMAH) and 0.05%-5% BC texturing additive. The etching temperature is 70℃-80℃, for example, 70℃, 75℃, 80℃, or any range thereof, and the etching time is 520-800 seconds, for example, 520s, 640s, 760s, 800s, or any range thereof. The texturing additive controls the alkaline etching rate, inhibits bubble adhesion, and promotes the uniform formation of the pyramidal textured surface. After texturing, the reflectivity of the light-receiving surface of the silicon substrate 10 is 7%-10%, for example, 7%, 9%, 10%, or any range thereof; the texture size is 1μm-2μm, for example, 1μm, 1.5μm, 2μm, or any range thereof. Since the first mask layer A with residual thickness still exists on the isolation area S23 after this step, the texturing process does not affect the back surface of the isolation area S23.
[0124] Post-cleaning is performed using the same alkali-H2O2 mixed solution (1%-10% alkali, 1%-20% H2O2) as the cleaning steps described above, at a temperature of 60℃-70℃ for 120-240 seconds, to remove residual organic additives and metallic contaminants from the texturing process.
[0125] like Figure 2n As shown, the residual thickness of the first mask layer A in the isolation region S23, the second mask layer 24 in the first region S21, and the third mask layer 34 in the second region S22 are removed by acid etching.
[0126] Specifically, a 5%-10% (w / w) hydrofluoric acid solution is used to remove residual first mask layer A, second mask layer 24, and third mask layer 34. For example, the concentration could be 5%, 7%, 9%, 10%, or any range of these values. The etching time is 120-360 seconds, for example, 120s, 180s, 260s, 360s, or any range of these values. Afterwards, a mixture of 50ppm ozone (O3) and 0.08% hydrochloric acid (HCl) is used for cleaning at 25℃-30℃ for 240-360 seconds. Ozone, as a strong oxidant, effectively removes trace organic contaminants from the surface; hydrochloric acid provides an acidic environment and complexes metal ions, preventing residual metal contamination.
[0127] Finally, a 1%-5% (by mass) dilute hydrofluoric acid solution is used to remove the natural oxide layer formed on the surface of the battery cell during the ozone cleaning process. For example, the concentration could be 1%, 3%, 5%, or any range of the above values. The reaction time is 180-360 seconds, for example, 180s, 240s, 360s, or any range of the above values. This process yields a fresh and clean battery cell surface, preparing it for subsequent passivation film deposition.
[0128] like Figure 2o As shown, an atomic layer deposition (ALD) or plasma-enhanced chemical vapor deposition (PECVD) process is used to prepare a first passivation layer 41 and / or a first antireflection layer 51 on the light-receiving surface of the silicon substrate 10, and a second passivation layer 42 and / or a second antireflection layer 52 on the backlight surface of the silicon substrate 10.
[0129] The first passivation layer 41 and the second passivation layer 42 are both aluminum oxide passivation layers with a thickness of 3nm-10nm, such as 3nm, 4nm, 5nm, 6nm, 8nm, 10nm, or any range of the above values. The first antireflection layer 51 and the second antireflection layer 52 can be a stacked film formed by any one or more of silicon nitride, silicon oxynitride, and silicon oxide layers, with a thickness of 70nm-90nm, such as 70nm, 80nm, 90nm, or any range of the above values.
[0130] like Figure 2p As shown, the first electrode 61 and the second electrode 62 are prepared on the backlight surface using processes such as screen printing or copper electroplating.
[0131] Specifically, the first electrode 61 and the second electrode 62 are distributed in an interdigitated manner. The first electrode 61 is located in the first region S21 of the backlight surface and is in contact with the first doped polysilicon layer 23. The second electrode 62 is located in the second region S22 of the backlight surface and is in contact with the second doped polysilicon layer 33.
[0132] The back contact battery of this invention can be obtained by following the above steps.
[0133] This invention also provides a solar cell, prepared by the above-described method for preparing a solar cell. The solar cell in this invention will also be described using a TBC cell as an example, such as... Figure 2p As shown, the TBC battery in this invention includes:
[0134] The silicon substrate 10 includes a first surface S1 and a second surface S2 disposed opposite to each other. The first surface S1 is a light-receiving surface, and the second surface S2 is a backlight surface. The backlight surface includes a first region S21, a second region S22, and an isolation region S23 that are spaced apart. The first region S21 and the second region S22 are spaced apart, and the isolation region S23 is located between the first region S21 and the second region S22.
[0135] The first doped structure is located in the first region S21 of the backlight surface. The first doped structure includes a first tunneling layer 22 and a first doped polysilicon layer 23 stacked sequentially. The first doped polysilicon layer 23 is stacked on the side of the first tunneling layer 22 away from the silicon substrate 10.
[0136] The second doped structure is located in the second region S22 of the backlight surface. The second doped structure includes a second tunneling layer 32 and a second doped polysilicon layer 33 stacked sequentially. The second doped polysilicon layer 33 is stacked on the side of the second tunneling layer 32 away from the silicon substrate 10, and the doping type of the first doped polysilicon layer 23 is opposite to that of the second doped polysilicon layer 33.
[0137] The first antireflection layer 41 and the second antireflection layer 42 are formed on the light-receiving surface of the silicon substrate 10, and the second antireflection layer 42 is formed on the side away from the light-receiving surface of the silicon substrate 10. The second antireflection layer 42 covers the surface of the silicon substrate 10 of the first doped polysilicon layer 23 in the first region S21, the second doped polysilicon layer 33 in the second region S22, and the isolation region S23.
[0138] The first passivation layer 51 and the second passivation layer 52 are formed on the light-receiving surface of the silicon substrate 10 and located on the surface of the first antireflection layer 41, and the second passivation layer 52 is formed on the side away from the light-receiving surface of the silicon substrate 10 and located on the surface of the second antireflection layer 42.
[0139] The first electrode 61 is located in the first region S21 and penetrates the second antireflection layer 42 and the second passivation layer 52, and is in electrical contact with the first doped polysilicon layer 23. The second electrode 62 is located in the second region S22 and penetrates the second antireflection layer 42 and the second passivation layer 52, and is in electrical contact with the second doped polysilicon layer 33.
[0140] The silicon substrate 10 in this invention can be an N-type silicon substrate or a P-type silicon substrate. In this embodiment, an N-type silicon substrate is used as an example for illustration.
[0141] In this invention, the light-receiving surface of the silicon substrate 10 has a light-trapping textured structure. For example, the light-receiving surface can be a pyramid textured structure prepared by an alkaline texturing process. The reflectivity of the textured surface of the silicon substrate 10 is 7%-10%, for example, it can be 7%, 9%, 10%, or any range of the above values. The texture size is 1μm-2μm, for example, it can be 1μm, 1.5μm, 2μm, or any range of the above values. The backlighting surface of the silicon substrate 10 is a polished surface. The reflectivity of the backlighting surface of the silicon substrate 10 is 35%-40%, for example, it can be 35%, 38%, 40%, or any range of the above values.
[0142] In this invention, the backlight side of the second region S22 and the first region S21 of the silicon substrate 10 are flush with each other within the process tolerance range. Furthermore, the backlight side of the isolation region S23 is flush with the backlight side of the first region S21 and the second region S22 within the process tolerance range.
[0143] In this invention, the first tunneling layer 22 and the second tunneling layer 32 can be silicon oxide layers with a thickness of 1nm-2nm, for example, 1nm, 1.5nm, 2nm, or any range of the above values. In other back-contact batteries, the first tunneling layer 22 and the second tunneling layer 32 can also be oxide layers with a thickness greater than this range.
[0144] In this invention, the first doped polysilicon layer 23 and the second doped polysilicon layer 33 have opposite doping types, namely P-type doping (such as boron doping) and N-type doping (such as phosphorus doping), respectively. Therefore, the first region S21 is the P-region of the battery backlight surface, the second region S22 is the N-region of the battery backlight surface, and the isolation region S23 is the isolation region (GAP).
[0145] In this invention, the first doped polysilicon layer 23 is a P-type doped polysilicon layer (P-Poly), preferably a boron doped polysilicon layer; the second doped polysilicon layer 33 is an N-type doped polysilicon layer (N-Poly), preferably a phosphorus doped polysilicon layer.
[0146] For example, the doping concentration of the first doped polysilicon layer 23 is 1E19 atoms / cm². 3 -1E21 atoms / cm 3 For example, it could be 1E19 atoms / cm 3 2E19 atoms / cm 3 1E20 atoms / cm 3 1E21 atoms / cm 3The thickness of the first doped polysilicon layer 23 is 50nm-500nm, for example, it can be 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, etc., or it can be any of the above values. The doping concentration of the second doped polysilicon layer 33 is 8E19 atoms / cm². 3 -9E20 atoms / cm 3 For example, it could be 8E19 atoms / cm 3 8E20 atoms / cm 3 9E19 atoms / cm 3 9E20 atoms / cm 3 The thickness of the second doped polycrystalline silicon layer 33 is 50nm-500nm, for example, it can be 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, etc., or it can be any of the above values.
[0147] In addition, dielectric layers are stacked on the light-receiving surface and the backlight surface of the silicon substrate in this invention. The dielectric layers can be passivation layers 41 / 42 and / or antireflection layers 51 / 52, which are at least one of aluminum oxide layer, silicon oxide layer, gallium oxide layer, silicon nitride layer, aluminum nitride layer, silicon oxynitride layer, etc.
[0148] For example, the dielectric layer can be a stacked film of an aluminum oxide layer and a silicon nitride layer. The aluminum oxide layer serves as a passivation layer, and its thickness is preferably 3nm-10nm, such as 3nm, 4nm, 5nm, 6nm, 8nm, 10nm, etc., or any range of the above values. The silicon nitride layer serves as an antireflection layer, and its thickness is preferably 70nm-90nm, such as 70nm, 80nm, 90nm, etc., or any range of the above values.
[0149] In addition, the first electrode 61 in this invention is located in the first region S21 of the backlight surface and is in electrical contact with the first doped polysilicon layer 23, but cannot penetrate the lower first tunneling layer 22 to contact the silicon substrate 10; the second electrode 62 is located in the second region S22 of the backlight surface and is in electrical contact with the second doped polysilicon layer 33, but cannot penetrate the lower second tunneling layer 32 to contact the silicon substrate 10.
[0150] Example 1:
[0151] This embodiment provides a method for preparing a TBC monocrystalline solar cell, specifically including the following steps:
[0152] (1) Silicon substrate preparation and double-sided polishing
[0153] N-type single-crystal silicon wafers were selected as the silicon substrate, with a resistivity of 0.5Ω·cm-30Ω·cm and a thickness of 130μm.
[0154] The light-receiving and back-light-receiving surfaces of the silicon substrate were polished using a tank-type texturing machine. First, the damaged layer on the silicon wafer surface was removed in a mixed solution of KOH and H₂O₂, followed by alkaline polishing in a sodium hydroxide or potassium hydroxide solution. After polishing, the silicon wafer surface was smooth, with a substrate size of 15 μm and a reflectivity of 40%.
[0155] (2) Deposition mask in N-zone and GAP-zone
[0156] Mask layers can be deposited on the N-region and GAP-region of the backlight surface of a silicon substrate using methods such as spraying, coating, printing, and transfer. The mask thickness in the N-region is 15 nm, and the mask thickness in the GAP-region is 30 nm. The mask layers are selected from one or more combinations of alumina, silicon oxide, silicon nitride, and silicon oxynitride.
[0157] (3) LPCVD preparation of tunneling layer and intrinsic amorphous silicon layer (first time)
[0158] A tunneling layer and an intrinsic amorphous silicon layer were fabricated on the back surface of a silicon wafer using LPCVD technology. The tunneling layer had a thickness of 1.4 nm, and the intrinsic amorphous silicon layer had a thickness of 280 nm.
[0159] (4) High-temperature boron diffusion
[0160] High-temperature boron diffusion was performed on the back surface of a silicon wafer using a tubular diffusion apparatus to achieve doping and crystallization of the amorphous silicon layer, transforming it into a boron-doped polycrystalline silicon layer. The high-temperature boron diffusion temperature was 950℃, and the doping concentration of the p-region polycrystalline silicon after diffusion was 6E10. 19 atoms / cm 3 .
[0161] (5) Laser film opening to remove BSG from N-region and GAP-region
[0162] Laser ablation was used to remove the borosilicate glass (BSG) layer from the N-region and GAP-region surfaces. A green-skinned laser with a power of 50W was used.
[0163] (6) RCA cleaning
[0164] Chain-type acid etching is used to remove the BSG from the light-receiving surface using HF (10% concentration). Then, a tank-type alkaline etching apparatus is used to remove the N-region and P-poly of the light-receiving and back-light-receiving surfaces of the silicon substrate, as well as for alkaline polishing of the N-region using sodium hydroxide or potassium hydroxide solution. Finally, the N-region mask and tunneling layer of the light-receiving surface are removed using an acid bath (HF, 10% concentration).
[0165] (7) LPCVD preparation of tunneling layer and intrinsic amorphous silicon layer (second time)
[0166] A tunneling layer and an intrinsic amorphous silicon layer were fabricated on the back surface of a silicon wafer using LPCVD technology. The tunneling layer had a thickness of 1.4 nm, and the intrinsic amorphous silicon layer had a thickness of 220 nm.
[0167] (8) High-temperature phosphorus diffusion
[0168] High-temperature phosphorus diffusion was performed on the back surface of a silicon wafer using a tubular diffusion apparatus to achieve doping and crystallization of the amorphous silicon layer, transforming it into a phosphorus-doped polycrystalline silicon layer. The high-temperature phosphorus diffusion temperature was 890℃, and the doping concentration of the polycrystalline silicon after diffusion was 5E10. 20 atoms / cm 2 .
[0169] (9) Laser film opening to remove PSG layers in P-region and GAP region
[0170] Laser ablation was used to remove the phosphorosilicate glass (PSG) layer from the P-region and GAP-region surfaces. A purple laser with a power of 30W was used.
[0171] (10) Wool making
[0172] The PSG on the light-receiving surface is removed using a chain pickling device. The N-poly layer on the light-receiving surface, the P-region on the backlight surface, and the GAP region is removed using a de-coating bath, along with the tunneling layer on the light-receiving surface. A texturing tank is used to create a textured surface on the silicon substrate's light-receiving surface, with a pyramid size of 2 μm and a reflectivity of 8%. Finally, the remaining mask in the GAP region is removed using an acid bath (HF, 10% concentration).
[0173] (11) Double-sided deposited alumina film
[0174] Alumina films with a thickness of 4 nm were deposited on the light-receiving and back-light-receiving surfaces of a silicon wafer using an ALD device.
[0175] (12) Double-sided deposition of silicon nitride film
[0176] Silicon nitride films with a thickness of 80 nm were deposited on the light-receiving and back-light-receiving sides of a silicon wafer using a PECVD device.
[0177] (13) Screen printing
[0178] TBC monocrystalline solar cells are fabricated by screen printing on the back surface of a silicon wafer to form interdigitated emitters.
[0179] Comparative Example 1:
[0180] Comparative Example 1 provides a method for preparing a TBC monocrystalline solar cell, specifically including the following steps:
[0181] (1) Silicon substrate preparation and double-sided polishing
[0182] N-type single-crystal silicon wafers were selected as the silicon substrate, with a resistivity of 0.5Ω·cm-30Ω·cm and a thickness of 130μm.
[0183] The light-receiving and back-light-receiving surfaces of the silicon substrate were polished using a tank-type texturing machine. First, the damaged layer on the silicon wafer surface was removed in a mixed solution of KOH and H₂O₂, followed by alkaline polishing in a sodium hydroxide or potassium hydroxide solution. After polishing, the silicon wafer surface was smooth, with a substrate size of 15 μm and a reflectivity of 40%.
[0184] (2) Preparation of tunneling oxide layer and intrinsic amorphous silicon layer by LPCVD (first time)
[0185] A tunneling layer and an intrinsic amorphous silicon layer were fabricated on the back surface of a silicon wafer using LPCVD technology. The tunneling layer had a thickness of 1.4 nm, and the intrinsic amorphous silicon layer had a thickness of 280 nm.
[0186] (3) High-temperature boron diffusion
[0187] High-temperature boron diffusion was performed on the back surface of a silicon wafer using a tubular diffusion apparatus to achieve doping and crystallization of the amorphous silicon layer, transforming it into a boron-doped polycrystalline silicon layer. The high-temperature boron diffusion temperature was 950℃, and the doping concentration of the polycrystalline silicon after diffusion was 6E10. 19 atoms / cm 3 .
[0188] (4) Laser film opening to remove BSG from N-region and GAP-region
[0189] Laser ablation was used to remove the borosilicate glass (BSG) layer from the N-region and GAP-region surfaces. A green-skinned laser with a power of 50W was used.
[0190] (5) RCA cleaning
[0191] Chain-type acid pickling was used to remove the BSG from the light-receiving surface, with HF as the acid solution and a concentration of 10%. Then, a tank-type alkaline etching device was used to remove the P-poly in the N-region and GAP region of the light-receiving and back-light-receiving surfaces of the silicon substrate, remove the tunneling layer on the light-receiving surface, and perform alkaline polishing on the N-region. The etching depth was 4 μm, and the alkaline solution was sodium hydroxide solution or potassium hydroxide solution.
[0192] (6) LPCVD preparation of tunneling oxide layer and intrinsic amorphous silicon layer (second time)
[0193] A tunneling layer and an intrinsic amorphous silicon layer were fabricated on the back surface of a silicon wafer using LPCVD technology. The tunneling layer had a thickness of 1.4 nm, and the intrinsic amorphous silicon layer had a thickness of 220 nm.
[0194] (7) High-temperature phosphorus diffusion
[0195] High-temperature phosphorus diffusion was performed on the back surface of a silicon wafer using a tubular diffusion apparatus to achieve doping and crystallization of the amorphous silicon layer, transforming it into a phosphorus-doped polycrystalline silicon layer. The high-temperature phosphorus diffusion temperature was 890℃, and the doping concentration of the polycrystalline silicon after diffusion was 5E10. 20 atoms / cm 2 .
[0196] (8) Laser film opening to remove PSG layers in P-region and GAP region
[0197] Laser ablation was used to remove the phosphorosilicate glass (PSG) layer from the P-region and GAP-region surfaces. A purple laser with a power of 30W was used.
[0198] (9) Wool making
[0199] The PSG on the light-receiving surface is removed using a chain-type acid etching system. The N-poly layer on the light-receiving and back-light-receiving P-regions and GAP regions, as well as the tunneling layer on the light-receiving surface, is removed using a chain-type alkaline etching system. A textured surface is formed on the light-receiving and back-light-receiving GAP regions of the silicon substrate using a tank-type texturing system. The pyramid size of the GAP regions on both the light-receiving and back-light-receiving surfaces is 2 μm, the reflectivity is 8%, and the etching depth of the GAP regions is 4 μm.
[0200] (10) Double-sided deposited alumina film
[0201] Alumina films with a thickness of 4 nm were deposited on the light-receiving and back-light-receiving surfaces of a silicon wafer using an ALD device.
[0202] (11) Double-sided deposition of silicon nitride film
[0203] Silicon nitride films with a thickness of 80 nm were deposited on the light-receiving and back-light-receiving sides of a silicon wafer using a PECVD device.
[0204] (12) Screen printing
[0205] TBC monocrystalline solar cells are fabricated by screen printing on the back surface of a silicon wafer to form interdigitated emitters.
[0206] The electrical performance of Comparative Example 1 and Example 1 was tested using the Weixin IV testing equipment, and the results are shown in Table 1.
[0207] Table 1: Comparison of Performance Parameters of Back Contact Batteries
[0208]
[0209] Note: VOC represents open-circuit voltage, Jsc represents current density, FF represents fill factor, and EFF represents conversion efficiency.
[0210] The experimental results show that, compared to the comparative example, in Example 1, after adopting the technical solution of the present invention, the N-region and GAP region on the back of the battery are transformed from a groove structure to a planar structure, thus improving the passivation effect. Simultaneously, the GAP region has a polished surface structure, further enhancing the passivation effect and increasing the utilization rate of long-wavelength light, thereby increasing the short-circuit current. Therefore, the solar cell prepared by the present invention has a higher conversion efficiency.
[0211] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0212] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for preparing a solar cell, characterized in that, include: A substrate is provided, the backlight surface of the substrate including a first region, a second region, and an isolation region located between the first region and the second region; A first mask layer is formed in the second region and the isolation region. The first mask layer in the second region has a first thickness D1, and the first mask layer in the isolation region has a second thickness D2. The first thickness D1 is less than the second thickness D2. A first doped structure is formed in the first region; The first mask layer of the second region and the isolation region are simultaneously etched to completely remove the first mask layer of the second region. The remaining first mask layer in the isolation region has a third thickness D3, which is less than the second thickness D2. A second doped structure is formed in the second region, the doping type of the second doped structure being opposite to that of the first doped structure; Remove the remaining first mask layer from the isolation area.
2. The method for preparing a solar cell according to claim 1, characterized in that, The ratio R of the second thickness to the first thickness satisfies: 1.6 ≤ R ≤ 5; and / or, The remaining first mask layer in the isolation zone is 30%-60% of the initial first mask layer thickness in the isolation zone; and / or, The first thickness is 10nm-60nm, and the second thickness is 20nm-120nm.
3. The method for preparing a solar cell according to claim 1, characterized in that, The first mask layer in the second region and the first mask layer in the isolation region are made of the same mask material; and / or, The first mask layer is an alkali-resistant mask layer; and / or, The masking material of the first mask layer includes one or more of aluminum oxide, silicon oxide, silicon nitride, and silicon oxynitride.
4. The method for preparing a solar cell according to claim 1, characterized in that, The first mask layer is simultaneously etched using a wet etching process, and the remaining first mask layer in the isolation area is removed using a wet etching process; wherein the etching solution includes an acid solution.
5. The method for preparing a solar cell according to claim 1, characterized in that, Forming a first doped structure in the first region includes: A first tunneling layer is formed in a first region on the back surface of the substrate; An intrinsic amorphous silicon layer is formed on the entire back surface of the substrate. The intrinsic amorphous silicon layer covers the surface of the first mask layer covering the second region and the isolation region, and the surface of the first tunneling layer covering the first region. The intrinsic amorphous silicon layer is subjected to a first diffusion process to transform the intrinsic amorphous silicon layer into a first doped polycrystalline silicon layer, and a second mask layer is formed on the surface of the first doped polycrystalline silicon layer. The second mask layer of the second region and the isolation region of the backlight surface is removed using a laser process; The first doped polysilicon layer of the second region and the isolation region of the backlight surface is removed by an alkaline etching process.
6. The method for preparing a solar cell according to claim 5, characterized in that, Forming a second doped structure in the second region includes: A second tunneling layer is formed in a second region on the back surface of the substrate; An intrinsic amorphous silicon layer is formed on the entire back surface of the substrate. The intrinsic amorphous silicon layer covers the surface of a first mask layer covering the isolation region, the surface of a second mask layer covering the first region, and the surface of a second tunneling layer covering the second region. A second diffusion process is performed on the intrinsic amorphous silicon layer to transform it into a second doped polycrystalline silicon layer, and a third mask layer is formed on the surface of the second doped polycrystalline silicon layer. The third mask layer of the first region and the isolation region of the backlight surface is removed using a laser process; The second doped polysilicon layer in the first region and the isolation region of the backlight surface is removed by an alkaline etching process.
7. The method for preparing a solar cell according to claim 1, characterized in that, Prior to the step of removing the remaining first mask layer in the isolation area, the method further includes: A pyramidal velvet structure is formed on the light-receiving surface of the substrate using a velvet-making process.
8. The method for preparing a solar cell according to claim 1, characterized in that, After the step of removing the remaining first mask layer in the isolation area, the method further includes: A first passivation layer and / or a first antireflection layer are prepared on the light-receiving surface of the substrate; and / or, A second passivation layer and / or a second antireflection layer are prepared on the back surface of the substrate; and / or, Electrodes are fabricated on the back surface of the substrate, respectively in contact with the first doped layer and the second doped layer.
9. The method for preparing a solar cell according to claim 1, characterized in that, Before the step of forming the first mask layer in the second region and the isolation region of the backlight surface of the substrate, the method further includes: The light-receiving surface and the back-light-receiving surface of the substrate are subjected to a double-sided polishing process.
10. A solar cell, characterized in that, include: The substrate includes a light-receiving surface and a backlighting surface, wherein the backlighting surface includes a first region, a second region, and an isolation region located between the first region and the second region; The first doped structure is located in the first region of the backlight surface; The second doped structure is located in the second region of the backlight surface, and the doping type of the second doped structure is opposite to that of the first doped structure. The substrate backlight side of the first region and the second region are flush with each other within the process error range.
11. The solar cell according to claim 10, characterized in that, The backlight side of the substrate of the isolation zone is flush with the backlight side of the substrate of the first region and the second region within the range of process error.
12. The solar cell according to claim 10, characterized in that, The first doped structure includes a first tunneling layer and a first doped polysilicon layer. The thickness of the first tunneling layer is 1 nm-2 nm, and the first doped polysilicon layer is a p-type doped polysilicon layer with a thickness of 50 nm-500 nm. The doping concentration of the first doped polysilicon layer is 1E19-1E21 atoms / cm². 3 ; and / or, The second doped structure includes a second tunneling layer and a second doped polysilicon layer. The thickness of the second tunneling layer is 1 nm-2 nm. The second doped polysilicon layer is an N-type doped polysilicon layer with a thickness of 50 nm-500 nm and a doping concentration of 8E19-9E20 atoms / cm². 3 ; and / or, The light-receiving surface of the substrate has a pyramidal textured surface, and the reflectivity of the textured surface of the light-receiving surface of the substrate is 7%-10%; and / or, The back surface of the substrate is a polished surface, and the reflectivity of the back surface of the substrate is 35%-40%.
13. The solar cell according to claim 10, characterized in that, A first passivation layer and / or a first antireflection layer are stacked on the light-receiving surface of the substrate; and / or, A second passivation layer and / or a second antireflection layer are stacked on the back surface of the substrate; and / or, Electrodes are respectively disposed on the first doped structure and the second doped structure.
14. The solar cell according to claim 13, characterized in that, The first passivation layer is an aluminum oxide passivation layer with a thickness of 3nm-10nm; and / or, The first antireflection layer is a stacked film formed by any one or more of silicon nitride, silicon oxynitride, and silicon oxide layers, with a thickness of 70nm-90nm; and / or, The second passivation layer is an aluminum oxide passivation layer with a thickness of 3nm-10nm; and / or, The second antireflection layer is a stacked film formed by any one or more of silicon nitride, silicon oxynitride, and silicon oxide layers, with a thickness of 70nm-90nm.