A double-layer hole transport structure, a laminated solar cell and a preparation method thereof
By introducing a bilayer structure of a metal oxide hole transport layer and a self-assembled monolayer into a perovskite/crystalline silicon tandem solar cell, the problems of incomplete coverage of the self-assembled monolayer and limited energy level tuning range are solved, achieving high-efficiency energy level matching and stable transport, and improving photoelectric conversion efficiency and stability.
Patent Information
- Application Number
- CN202611001492.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-10
AI Technical Summary
In existing perovskite/crystalline silicon tandem solar cells, incomplete self-assembled monolayer coverage leads to lateral leakage, limited energy level control range, insufficient long-term stability, narrow process window and poor repeatability, making it difficult to achieve efficient energy level matching and stable transport.
A bilayer structure consisting of a metal oxide hole transport layer and a self-assembled monolayer is adopted. The metal oxide layer serves as a hole transport framework layer to cover defects on the crystalline silicon surface, while the self-assembled monolayer enables fine energy level control. The synergistic effect suppresses leakage current and optimizes energy level matching.
It significantly improves the photoelectric conversion efficiency and long-term stability of tandem solar cells, reduces leakage current, increases fill factor and open-circuit voltage, enhances hole selective transport capability, improves interfacial recombination loss, and improves the consistency and stability of the fabrication.
Smart Images

Figure CN123076104A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic device technology, specifically to a double-layer hole transport structure for tandem solar cells, tandem solar cells, and their fabrication methods. Background Technology
[0002] Perovskite / crystalline silicon tandem solar cells have broken through the theoretical efficiency limit of Shockley-Queisser (SQ) cells for single-crystal silicon cells, becoming an important direction for current high-efficiency photovoltaic technology. Tandem cell devices with perovskite as the top cell and crystalline silicon as the bottom cell have achieved certified efficiencies exceeding 35%, demonstrating enormous application potential. The hole transport interface between the crystalline silicon bottom cell and the perovskite top cell plays a decisive role in the device's performance, particularly in charge extraction and transport efficiency.
[0003] Currently, the hole transport interface structure mainly employs self-assembled monolayers (SAMs) or metal oxides as functional layers. Among these, self-assembled monolayers are widely used to adjust the interfacial work function and improve charge extraction due to their strong molecular-level energy level tuning capability and high interfacial dipole designability. However, self-assembled monolayers still have the following inherent problems: (1) Incomplete coverage of self-assembled monolayers leads to lateral leakage. Self-assembled monolayers are difficult to achieve complete conformal coverage on textured crystalline silicon or polycrystalline contact layers, and are prone to forming pinholes, gaps or desorption regions, which constitute lateral leakage channels, reduce parallel resistance (Rsh) and cause a decrease in fill factor (FF).
[0004] (2) Limited range of energy level regulation. The work function regulation range of a single self-assembled monolayer is limited, making it difficult to meet the differentiated energy level matching requirements between different crystalline silicon bottom cell systems (such as TOPCon, HJT, etc.) and perovskite layers.
[0005] (3) Insufficient long-term stability. Under heat, light and electric field conditions, the anchoring groups of the self-assembled monolayer are prone to desorption or degradation, leading to interfacial dipole failure and irreversible decay of hole transport capability.
[0006] (4) Narrow process window and poor repeatability. Self-assembled monolayer film formation is highly sensitive to substrate state, solution concentration, humidity, etc., and the repeatability of large-area preparation is insufficient.
[0007] To overcome these limitations, current research focuses on optimizing the molecular structure of self-assembled monolayers to improve coverage on rough substrates, improving deposition processes to enhance film quality, or replacing self-assembled monolayers with metal oxides to enhance stability. However, metal oxides have limited energy level modulation capabilities, making it difficult to achieve precise work function matching; optimizing the molecular structure of self-assembled monolayers alone cannot fundamentally solve the lateral leakage problem caused by incomplete coverage. Furthermore, existing methods typically use self-assembled monolayers and metal oxides as independent functional layers, lacking a synergistic mechanism, making it difficult to simultaneously achieve unified optimization of leakage suppression, energy level modulation, and stable transport.
[0008] Therefore, there is an urgent need to provide a novel hole transport interface structure that combines high conductivity and excellent leakage resistance, and whose energy level can be flexibly adjusted, so as to achieve a breakthrough in efficiency and stability in tandem battery systems. Summary of the Invention
[0009] The purpose of this invention is to provide a double-layer hole transport structure for tandem solar cells, which achieves lateral leakage suppression, enhanced hole selectivity, and optimized energy level matching through the synergistic effect of the metal oxide hole transport framework layer and the self-assembled monolayer, thereby improving conductivity and interface stability.
[0010] To achieve the above objectives, the present invention provides the following technical solution: a double-layer hole transport structure for tandem solar cells, comprising the following sequentially stacked components: A metal oxide hole transport layer is formed directly on the surface of a crystalline silicon bottom cell and constitutes a hole transport framework layer to cover the rough structure of the crystalline silicon bottom cell surface and suppress lateral leakage; the thickness of the metal oxide hole transport layer is any value from 0.3 nm to 30 nm. A self-assembled monolayer is formed on the surface of the metal oxide hole transport layer to adjust the interfacial dipole moment to achieve interfacial work function regulation, and works synergistically with the metal oxide hole transport layer to achieve selective hole transport and interfacial recombination suppression.
[0011] Furthermore, the material of the metal oxide hole transport layer is selected from one or more of vanadium oxide, tungsten oxide, or molybdenum oxide.
[0012] Furthermore, the self-assembled monolayer is an organic molecular layer containing hole transport groups and anchoring groups; the hole transport groups include carbazole groups, triphenylamine groups, fluorene groups or aromatic amine groups; the anchoring groups include phosphate or carboxylic acid anchoring groups.
[0013] This application also provides a tandem solar cell, comprising: a crystalline silicon bottom cell, a wide-bandgap perovskite top cell, and the aforementioned double-layer hole transport structure. The dual-layer hole transport structure is disposed between the crystalline silicon bottom cell and the perovskite top cell to achieve selective hole transport at the interface, suppression of lateral leakage current, and reduction of non-radiative recombination.
[0014] Furthermore, the crystalline silicon bottom cell is a tunneling silicon oxide passivated contact (TOPCon) cell, a heterojunction (HJT) cell, or a crystalline silicon cell with a passivated contact structure.
[0015] Furthermore, the tandem solar cell has a two-end tandem structure or a three-end tandem structure.
[0016] This application also provides a method for fabricating the above-mentioned stacked solar cell, comprising the following steps: S1. Fabrication of crystalline silicon bottom solar cells; S2. A metal oxide hole transport layer is deposited on the surface of the crystalline silicon substrate; S3. A self-assembled monolayer is deposited on the surface of the metal oxide hole transport layer; S4. Construct a perovskite top cell on the self-assembled monolayer to obtain the stacked solar cell.
[0017] Furthermore, in step S2, the metal oxide hole transport layer is deposited on the surface of the crystalline silicon bottom cell using vacuum evaporation, magnetron sputtering, or atomic layer deposition methods.
[0018] Furthermore, in step S3, the method for forming the self-assembled monolayer is a solution method or a vapor deposition method.
[0019] Furthermore, when the self-assembled monolayer is formed using a solution method, the metal oxide hole transport layer is immersed in a solution containing self-assembled monomolecules or the solution is coated onto its surface, followed by heat treatment.
[0020] Furthermore, when the self-assembled monolayer is formed using vapor deposition, it is formed by direct deposition on the surface of the metal oxide hole transport layer using vacuum evaporation or chemical vapor deposition.
[0021] The beneficial effects of this invention are as follows: The bilayer hole transport structure used in the tandem solar cell provided in this application, while retaining the fine energy level control capability of the self-assembled monolayer, introduces a metal oxide with high conductivity that can cover the defect sites on the silicon cell surface as a basic framework layer, constructing a bilayer interface structure of a metal oxide hole transport framework layer and a self-assembled monolayer dipole control layer. This achieves synergistic optimization of interface leakage suppression, wide-range energy level control, and selective hole transport, significantly improving the photoelectric conversion efficiency and long-term reliability of the corresponding perovskite / crystalline silicon tandem solar cell.
[0022] Metal oxide hole transport layers can form a uniform capping layer on textured silicon surfaces or multilayer heterostructures, effectively filling surface micro-defects and rough structures. This physically blocks lateral leakage channels caused by incomplete coverage of self-assembled monolayers, significantly improving device parallel resistance and reducing leakage current, thereby increasing fill factor and overall energy conversion efficiency. Simultaneously, metal oxides provide a stable high work function hole transport framework, facilitating basic energy level alignment and hole transport channel construction. The self-assembled monolayer, through the interface dipole effect, finely adjusts the local work function, forming a "coarse adjustment + fine adjustment" synergistic mechanism. This broadens the interface energy level adjustment window, enabling it to adapt to energy level differences between different crystalline silicon bottom cell systems such as TOPCon and HJT, and wide-bandgap perovskite layers, enhancing hole selective extraction and reducing interface recombination losses. Furthermore, the metal oxide itself possesses high electrical conductivity, effectively reducing resistive losses in the hole transport path. The self-assembled monolayer further optimizes the energy level barrier distribution at the interface, making carrier transport more selective and directional. The synergistic effect of these two elements significantly reduces the interfacial recombination rate and series resistance, improving the fill factor and open-circuit voltage. This metal oxide hole transport layer also maintains structural stability under external thermal, optical, and electric field conditions, thus providing physical support and chemical protection for the self-assembled monolayer. This effectively suppresses interfacial failure caused by the desorption or degradation of anchoring groups, significantly enhancing the long-term operational stability and environmental adaptability of the tandem solar cell.
[0023] The bilayer hole transport structure provided in this application has a wide fabrication process window and high repeatability. It can be well adapted to textured silicon surfaces and complex interface structures, which helps to reduce the dependence on the sensitivity of self-assembled monolayer film formation environment and improve the consistency and industrialization feasibility of large-area fabrication.
[0024] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of a double-layer hole transport structure according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the perovskite / textured TOPCon crystalline silicon tandem solar cell shown in Embodiment 1 of the present invention; Figure 3 This is a flowchart illustrating the fabrication process of the textured TOPCon crystalline silicon bottom cell and the perovskite top cell as shown in Embodiment 1 of the present invention. Figure 4 This is a JV characteristic curve of the perovskite / textured TOPCon crystalline silicon tandem solar cell shown in Example 1 of the present invention; Figure 5 This is a JV characteristic curve of the perovskite / textured TOPCon crystalline silicon tandem solar cell shown in Embodiment 2 of the present invention; Figure 6 This is a schematic diagram of the perovskite / HJT crystalline silicon tandem solar cell shown in Embodiment 3 of the present invention; Figure 7 This is a flowchart illustrating the fabrication process of the HJT crystalline silicon bottom cell as shown in Example 3 of the present invention; Figure 8 This is a JV characteristic curve of the perovskite / HJT crystalline silicon tandem solar cell shown in Example 3 of the present invention; Figure 9 This is a schematic diagram of the perovskite / HTBC crystalline silicon tandem solar cell shown in Embodiment 4 of the present invention. Figure 10 This is a flowchart illustrating the fabrication process of the HTBC crystalline silicon bottom cell shown in Example 4 of the present invention. Figure 11 This is a JV characteristic curve of the perovskite / HTBC crystalline silicon tandem solar cell shown in Example 4 of the present invention. Figure label: 1. Double-layer hole transport structure; 11. Metal oxide hole transport layer; 12, 210, 309, and 410 are all self-assembled monolayers; 2. Crystalline silicon bottom cell; 201, 301, and 401 are all n-type silicon substrates; 202 is a p+ type boron emitter layer; 203 and 402 are SiO2 substrates. x Layers; 204 and 403 are n + Type 105 is a polycrystalline silicon layer; 205 is an Al2O3 passivation layer; 206 is a SiN layer. x Antireflection layer; 207, 306, and 407 are silver electrodes; 208, 307, and 408 are indium zinc oxide composite layers; 209 and 308 are vanadium oxide hole transport layers; 211 is a perovskite light-absorbing layer; 212 is C 60 Electron transport layer; 213, SnO2 buffer layer; 214, transparent electrode layer; 215, magnesium fluoride antireflection layer; 216, silver grid line electrode; 302 and 404 are intrinsic hydrogenated amorphous silicon layers; 303 and 405 are boron-doped nanocrystalline silicon oxide layers; 304, phosphorus-doped nanocrystalline silicon oxide layer; 305 and 406 are indium tin oxide transparent electrode layers; 409, tungsten oxide hole transport layer. Detailed Implementation
[0026] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0028] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0029] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0030] A preferred embodiment of this application illustrates a double-layer hole transport structure 1 used in a stacked solar cell, such as... Figure 1 As shown, the bilayer hole transport structure 1 includes a metal oxide hole transport layer 11 and a self-assembled monolayer 12 stacked sequentially. The metal oxide hole transport layer 11 is directly formed on the surface of the crystalline silicon base cell 2 and constitutes a hole transport framework layer, used to cover the rough structure of the crystalline silicon base cell 2 surface and suppress lateral leakage. The thickness of the metal oxide hole transport layer 11 is preferably any value from 0.3 nm to 30 nm. The self-assembled monolayer 12 is formed on the surface of the metal oxide hole transport layer 11 and is used to adjust the interfacial dipole moment to achieve interfacial work function regulation. The self-assembled monolayer 12 can also synergistically work with the metal oxide hole transport layer 11 to achieve selective hole transport and interfacial recombination suppression. By combining the metal oxide hole transport layer 11 with the self-assembled monolayer 12 to construct a bilayer structure, the metal oxide layer effectively covers the textured or polycrystalline rough structure of the crystalline silicon surface in a framework form, thereby significantly suppressing the lateral leakage path caused by interface defects and pinholes. At the same time, the self-assembled monolayer 12 achieves fine adjustment of the work function through interface dipole modulation, optimizes interface energy level matching, thereby achieving selective extraction and transport of holes and reducing interface nonradiative recombination loss, thus synergistically improving the device fill factor and open-circuit voltage.
[0031] In one embodiment, the metal oxide hole transport layer 11 is made of vanadium oxide (VO₂O₃). x ), tungsten oxide (WO) x ) or molybdenum oxide (MoO) x Any one or more of ) . By selecting VO x WO x or MoO x High work function metal oxide materials enable the hole transport layer to possess better energy level matching capabilities and higher intrinsic conductivity, which is beneficial for energy level matching and hole transport. Simultaneously, different oxides can achieve interface energy level adaptation and adjustment through their varying oxygen vacancy concentrations and Fermi level positions, thereby improving hole extraction efficiency and enhancing the overall photoelectric conversion performance of the device.
[0032] In this embodiment or other embodiments, the self-assembled monolayer is an organic molecular layer formed by self-assembled monomolecules containing hole-transporting groups and anchoring groups. The hole-transporting groups include, but are not limited to, carbazole groups, triphenylamine groups, fluorene groups, or aromatic amine groups, while the anchoring groups include, but are not limited to, phosphate or carboxylic acid anchoring groups. For example, the self-assembled monolayer can be selected from 4-(7H-dibenzo(c,g)carbazole-7-yl)butylphosphonic acid (4PADCB), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), and [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid (MeO-4PACz), etc. These self-assembled monomolecules have a stronger π-conjugated structure and more stable anchoring ability, enabling the formation of stable and uniformly dense monolayers on metal oxide surfaces. This facilitates the construction of stable interfacial dipoles to regulate the interfacial work function, thereby enhancing hole-selective transport. Meanwhile, by utilizing the synergistic effect of the carbazole skeleton and phosphate or carboxylic acid anchoring groups, the risk of molecular desorption induced by heat, light and electric fields can be effectively reduced, thereby improving the long-term stability of the interface.
[0033] One embodiment provides a tandem solar cell. The tandem solar cell includes a crystalline silicon bottom cell 2, a wide-bandgap perovskite top cell, and the aforementioned double-layer hole transport structure 1. The double-layer hole transport structure 1 is disposed between the crystalline silicon bottom cell 2 and the perovskite top cell to achieve selective hole transport at the interface, suppression of lateral leakage, and reduction of non-radiative recombination. By disposing the double-layer hole transport structure 1 between the perovskite top cell and the crystalline silicon bottom cell 2, the double-layer hole transport structure 1 can effectively suppress interface recombination and lateral leakage while achieving efficient selective hole transport, thereby improving the open-circuit voltage, fill factor, and overall photoelectric conversion efficiency of the tandem solar cell, and improving the device's operational stability.
[0034] In one embodiment, the crystalline silicon base cell 2 is a TOPCon cell, an HJT cell, or a crystalline silicon cell with a passivated contact structure. The double-layer hole transport structure 1 provided in this application is compatible with different types of crystalline silicon base cell 2 systems, and can be adapted to TOPCon, HJT, or other passivated contact structure crystalline silicon base cells 2. It can also achieve stable interface energy level matching and charge transport performance under different structures, and has a wide range of applications.
[0035] In this embodiment or other embodiments, the tandem solar cell is a two-terminal or three-terminal tandem structure. By adopting a two-terminal or three-terminal tandem structure, the electrical connection method of the cell structure is adjustable, thereby enabling optimized selection of efficiency and power output modes in different application scenarios, improving system-level application flexibility and photoelectric conversion efficiency.
[0036] One embodiment also provides a method for fabricating the above-mentioned tandem solar cell, comprising the following steps: S1. Prepare crystalline silicon bottom solar cell 2; S2. A metal oxide hole transport layer 11 is deposited on the surface of the crystalline silicon bottom cell 2; S3. A self-assembled monolayer 12 is deposited on the surface of the metal oxide hole transport layer 11; S4. Construct a perovskite top cell on a self-assembled monolayer 12 to obtain a tandem solar cell.
[0037] The preparation method involves first depositing a metal oxide to form a framework layer, and then depositing a self-assembled monolayer 12 to construct an interface dipole layer. The metal oxide is used to eliminate defects and leakage channels on the rough surface of the crystalline silicon, and the self-assembled monolayer 12 is used to achieve fine control of the interface energy level. This allows for staged optimization of leakage suppression and energy level matching, thereby improving interface stability and repeatability.
[0038] In one embodiment, in step S2, a metal oxide hole transport layer 11 is deposited on the surface of the crystalline silicon bottom cell 2 using vacuum evaporation, magnetron sputtering, or atomic layer deposition. By using vacuum evaporation, magnetron sputtering, or atomic layer deposition to prepare the metal oxide hole transport layer 11, precise control over thickness uniformity and interface coverage can be achieved, thereby obtaining a low-defect, high-coverage hole transport framework layer, effectively reducing leakage probability and improving device consistency.
[0039] When a metal oxide hole transport layer 11 is deposited on the surface of a crystalline silicon substrate 2 using vacuum thermal evaporation, the specific steps include: cleaning the tungsten boat sequentially with acetone and ethanol to remove surface oil contamination; drying the tungsten boat and then fixing it in the corresponding position within the evaporation chamber; placing an appropriate amount of metal oxide powder on the tungsten boat after fixing it; fixing the substrate on the sample tray and placing it on the sample holder within the evaporation chamber, then closing the evaporation chamber door. The instrument is then started, and a vacuum of 5.0 × 10⁻⁶ is created. -4 After Pa, sample rotation is initiated to prepare for the coating process. The power connector is set, the power is turned on, and the power is gradually increased until the rate stabilizes at the appropriate level. The substrate baffle is then opened to deposit the metal oxide. Once the metal oxide has deposited to a certain thickness, the substrate baffle and power supply are turned off, and the vacuum thermal evaporation equipment is shut down and the sample is removed. During the deposition process, the quality and thickness of the interface layer can be controlled by changing the background vacuum level, deposition rate, and deposition time. Before depositing the metal oxide hole transport layer 11 on the substrate, the substrate can be pretreated, specifically including: polishing and etching the substrate with a 5%wt-15%wt NaOH aqueous solution to remove the silicon wafer damage layer; then preparing a pyramidal textured surface on the substrate surface using a 1%wt-3%wt NaOH solution; and finally cleaning the substrate with the pyramidal textured surface using the RCA method. This substrate is selected from an n-type monocrystalline silicon wafer or a crystalline silicon bottom cell 2.
[0040] When a metal oxide hole transport layer 11 is deposited on the surface of a crystalline silicon substrate 2 using magnetron sputtering, the specific steps include: fixing the metal oxide or metal target to the corresponding target position within the magnetron sputtering chamber. After fixing, the substrate is fixed on the sample tray, placed on the sample holder within the magnetron sputtering chamber, and the target-substrate distance is adjusted to the set value before closing the sputtering chamber door. Subsequently, the vacuum system is activated, and a vacuum is evacuated to a background vacuum level better than 5.0 × 10⁻⁶. -4 Pa. Then, high-purity argon and oxygen, and other reactive gases, are introduced into the magnetron sputtering chamber. After adjusting the working pressure to the set value, sample rotation is started to prepare for the coating process. The sputtering power is set, and the power supply is turned on. Pre-sputtering is performed for several minutes in an argon atmosphere to clean the target surface. After the glow discharge stabilizes, the substrate baffle is opened, and sputtering is carried out. After the metal oxide has been deposited to the set thickness, the substrate baffle and power supply are turned off, the argon gas supply is stopped, and the magnetron sputtering equipment is turned off and removed. During the deposition process, the quality and thickness of the interface layer can be controlled by changing the sputtering power, working pressure, argon gas flow rate, and deposition time. The target material used in this magnetron sputtering method is selected from pure metal targets or corresponding ceramic oxide targets, such as pure tungsten targets, pure molybdenum targets, pure vanadium targets, tungsten oxide targets, molybdenum oxide targets, and vanadium oxide targets. Before depositing the metal oxide hole transport layer 11 on the substrate, the substrate can also be pretreated.
[0041] When depositing a metal oxide hole transport layer 11 on the surface of a crystalline silicon substrate 2 using atomic layer deposition (ALD), the specific steps include: fixing the substrate on a sample tray and placing it on a pad in the ALD chamber. Then, the automatic vacuum system is activated to evacuate to a baseline vacuum level better than 0.005 torr, and the substrate is preheated to the set temperature. Next, the corresponding metal source bottle is opened, and the deposition process is started. After the metal oxide has deposited to the set thickness, high-purity nitrogen gas is introduced into the ALD chamber to 760 torr to stop the ALD process. Afterward, the ALD equipment is shut down and removed. During the deposition process, the quality and thickness of the interface layer can be controlled by changing the precursor pulse time, purge time, and deposition cycle number. The substrate can also be pretreated before depositing the metal oxide hole transport layer 11 on it.
[0042] In one embodiment, in step S3, the method for forming the self-assembled monolayer 12 is a solution method or a vapor deposition method.
[0043] When using a solution method, the concentration of the self-assembled monomolecules in the solution is preferably any value between 0.1 mg / mL and 5 mg / mL. The solution containing the self-assembled monomolecules is coated onto the surface of the metal oxide hole transport layer 11, and the coating method includes at least one of spin coating, immersion coating, or blade coating. After coating, heat treatment is performed, and the heat treatment temperature is preferably any value between 80℃ and 150℃. By controlling the concentration of the self-assembled molecule solution and the subsequent heat treatment temperature range, the self-assembled monomolecule layer 12 can form a stable and uniform molecular coating layer on the metal oxide surface, thereby improving the interfacial dipole uniformity, enhancing the energy level modulation effect, and improving the interfacial bonding strength and long-term operational stability. In some embodiments, the specific steps of spin-coating a solution containing self-assembled monomolecules onto the surface of the metal oxide hole transport layer 11 include: dropping a solution containing self-assembled monomolecules with a concentration of 0.1 mg / mL to 5 mg / mL onto the metal oxide hole transport layer 11; turning on the power supply and mechanical pump switch of the spin coater to perform spin coating, setting the corresponding rotation speed to 3000 rpm to 5000 rpm and the rotation time to 20 s to 40 s.
[0044] When using vapor deposition, a self-assembled monolayer 12 is formed directly on the surface of the metal oxide hole transport layer 11 by vacuum evaporation or chemical vapor deposition. When using vacuum evaporation, parameters such as the evaporation source temperature, deposition rate, and deposition time are controlled to enable the self-assembled monomolecules to complete self-assembly on the surface of the metal oxide hole transport layer 11.
[0045] In this embodiment or other embodiments, the self-assembled monomolecule is an organic molecule containing hole transport groups and anchoring groups. The hole transport groups include, but are not limited to, carbazole groups, triphenylamine groups, fluorene groups, or aromatic amine groups; the anchoring groups include, but are not limited to, phosphate or carboxylic acid anchoring groups. The self-assembled monolayer 12 formed from this type of molecule possesses high charge transport capability, excellent interface anchoring capability, and tunable dipole moment, thereby improving interface hole extraction efficiency while ensuring energy level matching flexibility and enhancing the stability of the device under illumination, thermal, and electric field conditions.
[0046] Example 1
[0047] like Figure 2 As shown, this embodiment provides a perovskite / textured TOPCon crystalline silicon tandem solar cell. The structure of this tandem solar cell includes a textured TOPCon crystalline silicon bottom cell, a double-layer hole transport structure 1 located thereon, and a perovskite top cell structure, enabling efficient light absorption and carrier separation. Specifically, the metal oxide hole transport layer 11 of the double-layer hole transport structure 1 is made of vanadium oxide, and the self-assembled monolayer 210 is made of [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid. Its preparation method specifically includes the following steps: S1. Fabrication of textured TOPCon crystalline silicon bottom solar cells. For example... Figure 3 As shown in (a), the fabrication method of this textured TOPCon crystalline silicon substrate specifically includes: selecting n-type monocrystalline silicon as the substrate, first using a 10wt% KOH aqueous solution to polish and etch it to remove the damaged layer on the substrate surface; then using a 2wt% KOH solution for anisotropic etching to form a regular pyramid textured structure, and combining this with a single-sided alkaline polishing process to flatten the non-light-receiving surface; next, using an RCA cleaning process to perform standard cleaning on the substrate to obtain a clean n-type silicon substrate 201. The n-type silicon substrate 201 is placed in a boron diffusion furnace, and diffusion treatment is performed using BBr3 as the boron source to form p-type silicon substrates on the front side of the silicon wafer. + Type 202 boron emitter layer, denoted as c-Si:B(p + A silicon layer, approximately 150 nm thick, was then used. Subsequently, an industrial HF / HNO3 mixed etching process was employed to remove the residual diffusion layer and related contaminant layers on the front side. A thin SiO2 layer was then grown on the front side using a thermal oxidation process. x Layer 203, approximately 1.5 nm thick, is used for interface passivation. Then, an intrinsic polycrystalline silicon layer is deposited on the front side of the silicon wafer via low-pressure chemical vapor deposition (LPCVD) at 550 °C, followed by phosphorus doping in a POCl3 diffusion furnace to form n... + Type 204 polycrystalline silicon layer, denoted as Poly-Si:(n +A 150 nm thick Al2O3 passivation layer was formed to create the passivation contact structure. A single-sided KOH selective etching process was used to remove the polysilicon layer surrounding the back side, and HF solution was used to remove the front borosilicate glass (BSG) and the back phosphorosilicate glass (PSG). RCA cleaning and deionized water rinsing were then performed to obtain a clean textured silicon surface. An Al2O3 passivation layer 205, 3 nm thick, was deposited on the textured silicon surface using atomic layer deposition (ALD) for surface defect passivation and interface recombination suppression. SiN was then deposited on the Al2O3 passivation layer 205 using plasma-enhanced chemical vapor deposition (PECVD). x An antireflection layer 206, with a thickness of 80 nm, is used to reduce surface reflection and improve light absorption efficiency. Subsequently, a silver electrode 207 is fabricated on the back side of the electrode using a screen printing process. This silver electrode 207 is then bonded to the p-side surface. + A boron emitter layer 202 forms an ohmic contact with a thickness of approximately 1 μm. A magnetron sputtering process is used to deposit the ohmic contact on the front side. + An indium zinc oxide composite layer 208 with a thickness of 15 nm is deposited on a polycrystalline silicon layer 204 to serve as a subsequent interface composite connection layer, thereby obtaining a textured TOPCon crystalline silicon bottom cell.
[0048] S2. A vanadium oxide hole transport layer 209 is deposited on the surface of the indium zinc oxide composite layer 208 of the textured TOPCon crystalline silicon bottom cell to cover the surface defect sites of the silicon bottom cell. Specifically, this involves: first, wiping and cleaning the tungsten boat sequentially with acetone and ethanol to remove surface oil contamination; then, drying the cleaned tungsten boat and fixing it in place at the evaporation source position of the vacuum evaporation system. After fixing, an appropriate amount of vanadium oxide powder is placed on the tungsten boat, and the textured TOPCon crystalline silicon bottom cell sample is fixed on the sample stage and placed in the sample holder position inside the evaporation chamber. The evaporation chamber door is then closed. Subsequently, a vacuum is drawn to achieve a base vacuum level of 5.0 × 10⁻⁶. -4 Below Pa, the sample rotation function is simultaneously activated to improve the uniformity of film deposition. Then, the evaporation power supply is started, and the heating power is gradually increased to allow the vanadium oxide powder to reach a stable evaporation state. Once the deposition rate stabilizes, the substrate baffle is opened, allowing vanadium oxide to begin depositing on the surface of the indium zinc oxide composite layer 208. When the thickness of the vanadium oxide hole transport layer 209 deposited on the surface of the indium zinc oxide composite layer 208 reaches 10 nm, the substrate baffle and power supply are turned off. After the system cools down, the vacuum state is released, the sample is removed, and the preparation of the vanadium oxide hole transport layer 209 is completed.
[0049] S3. A solution containing self-assembled monomolecules is dropped onto the vanadium oxide hole transport layer 209, wherein the self-assembled monomolecule is [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid. Then, the spin coater is turned on, the spin coater is set to 3000 rpm, and spin coating is performed. After 30 seconds of rotation, the mixture is heat-treated at 100°C. After 10 minutes of heat treatment, a self-assembled monomolecule layer 210 is formed on the surface of the vanadium oxide hole transport layer 209.
[0050] S4. Construct a perovskite top cell on a self-assembled monolayer 210. For example... Figure 3 As shown in (b), the process specifically includes: firstly, preparing a wide-bandgap perovskite light-absorbing layer 211 on the surface of the self-assembled monolayer 210 using a spin-coating method, the chemical composition of which is Cs. 0.05 MA 0.15 FA 0.8 PbI 2.25 Br 0.75 The bandgap is approximately 1.68 eV, which is used to achieve efficient absorption and carrier generation in the visible light range. Next, C is deposited on the perovskite light-absorbing layer 211 using a high-temperature thermal evaporation method. 60 An electron transport layer 212, approximately 10 nm thick, is used to achieve selective electron transport and suppress interfacial recombination. It is fabricated on C using atomic layer deposition (ALD). 60 A SnO2 buffer layer 213, with a deposition temperature of 100°C and a thickness of 15 nm, is deposited on the electron transport layer 212 to further optimize electron transport selectivity and improve interface stability. Subsequently, a zinc-doped indium oxide (IZO) transparent electrode layer 214, with a thickness of 45 nm, is deposited on the SnO2 buffer layer 213 using magnetron sputtering to achieve high transmittance and low resistance charge collection. Next, a silver grid electrode 216, with a thickness of approximately 500 nm, is fabricated on the transparent electrode layer 214 using a high-temperature thermal evaporation method to achieve external circuit charge collection and transport. Finally, a magnesium fluoride antireflection layer 215, with a thickness of 110 nm, is further deposited on the surface of the transparent electrode layer 214 to reduce incident light reflection loss and improve light utilization efficiency. This results in a perovskite / textured TOPCon crystalline silicon tandem solar cell.
[0051] The performance of this perovskite / textured TOPCon crystalline silicon tandem solar cell was tested, and its JV characteristic curve and key photovoltaic parameters are as follows: Figure 4 As shown.
[0052] Depend on Figure 4 It can be seen that, with an effective area of 1cm 2 Under the given device conditions, this tandem solar cell can achieve a photoelectric conversion efficiency (PCE) of 32.65%. Its open-circuit voltage (V0) OC The voltage is 1.940V, and the short-circuit current density (J) is...SC The value is 20.45 mA / cm. 2 The fill factor (FF) is 82.32%.
[0053] Example 2
[0054] The perovskite / textured TOPCon crystalline silicon tandem solar cell provided in this embodiment differs from that in Embodiment 1 in that the metal oxide hole transport layer 11 in the double-layer hole transport structure 1 is made of molybdenum oxide.
[0055] The method for fabricating the perovskite / textured TOPCon crystalline silicon tandem solar cell provided in this embodiment differs from that in Example 1 in that: In step S2, the molybdenum target is fixedly installed on the target position within the magnetron sputtering chamber. The textured TOPCon crystalline silicon bottom cell sample is then fixed on the sample tray and placed in the sample holder within the sputtering chamber. The target-substrate distance is adjusted to the preset distance, and the sputtering chamber door is sealed. The vacuum system is activated, and the sputtering chamber is evacuated to a background vacuum level better than 5.0 × 10⁻⁶. -4 Pa. Subsequently, high-purity argon and oxygen were introduced into the sputtering chamber as reactants, and the working pressure was adjusted to the set value. Simultaneously, the sample rotation system was activated to ensure deposition uniformity. The sputtering power was set and the power supply was turned on. The molybdenum target was pre-sputtered for several minutes in an argon atmosphere to remove surface contaminants and stabilize the plasma state. After the glow discharge stabilized, the substrate baffle was opened to initiate the deposition process. During sputtering, molybdenum oxide was gradually deposited on the surface of the indium zinc oxide composite layer, forming a metal oxide hole transport layer 11 that covers the defect sites on the silicon substrate cell surface. When the deposited layer thickness reached 10 nm, the substrate baffle was closed and the sputtering power was stopped. Simultaneously, the introduction of argon and oxygen was stopped, the magnetron sputtering system was shut down, and the sample was removed to complete the preparation of the metal oxide hole transport layer 11.
[0056] In step S3, ([4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid) is deposited on the molybdenum oxide hole transport layer by high-temperature vapor deposition, forming a self-assembled monolayer 12 on the surface of the molybdenum oxide hole transport layer. The self-assembled monolayer is an organic molecule containing triphenylamine and phosphate groups.
[0057] Finally, a perovskite / textured TOPCon crystalline silicon tandem solar cell was obtained, and its performance was tested. Its JV characteristic curve and key photovoltaic parameters are shown below. Figure 5 As shown.
[0058] Depend on Figure 5 It can be seen that, with an effective area of 1cm 2 Under the given device conditions, this tandem solar cell can achieve a photoelectric conversion efficiency of 31.50%. Its open-circuit voltage (V...OC The voltage is 1.938V, and the short-circuit current density (J) is... SC The value is 20.40 mA / cm. 2 The fill factor (FF) is 80.10%.
[0059] Example 3
[0060] The difference between this embodiment and Embodiment 1 is that: Figure 6 As shown, this embodiment provides a perovskite / HJT crystalline silicon tandem solar cell. The bottom cell of this tandem solar cell is an HJT crystalline silicon bottom cell; The method for fabricating the perovskite / HJT crystalline silicon tandem solar cell provided in this embodiment differs from that in Example 1 in that: In step S1, the HJT crystalline silicon bottom cell is fabricated. For example... Figure 7 As shown, the specific fabrication method of this HJT crystalline silicon bottom cell includes: selecting n-type monocrystalline silicon as the substrate, first using a 10wt% KOH aqueous solution to polish and etch it to remove the damaged layer on the substrate surface; then using a 2wt% KOH solution for anisotropic etching to form a regular pyramidal textured structure, and combining it with a single-sided alkaline polishing process to planarize the non-light-receiving surface; then using an RCA cleaning process to perform standard cleaning on the substrate to obtain a clean n-type silicon substrate 301. Next, at a deposition temperature of 400℃, using a plasma-enhanced chemical vapor deposition (PECVD) process, an intrinsic hydrogenated amorphous silicon layer 302, denoted as a-Si:H(i), with a thickness of approximately 5nm, is deposited on the front and back sides of the n-type silicon substrate 301 for interface passivation. Subsequently, at a deposition temperature of 170°C, a boron-doped nanocrystalline silicon oxide layer 303, denoted as nc-Si:H(p), with a thickness of 25 nm, was deposited on the back side of the intrinsic hydrogenated amorphous silicon layer 302 using a PECVD process, forming a hole-selective contact layer covering the entire back surface. At the same temperature, a phosphorus-doped nanocrystalline silicon oxide layer 304, denoted as nc-SiOx:H(n), with a thickness of approximately 20 nm, was deposited on the front side of the intrinsic hydrogenated amorphous silicon layer 302 using a PECVD process, forming an electron-selective contact layer on the front side. Then, an indium tin oxide transparent electrode layer 305, with a thickness of 110 nm, was deposited on the boron-doped nanocrystalline silicon oxide layer 303 using magnetron sputtering for charge collection and extraction. A silver electrode 306 was fabricated on the back side using a low-temperature silver paste screen printing process and then dried and cured in air at 400°C. Finally, an indium zinc oxide composite layer 307 with a thickness of 15 nm was deposited on the front phosphorus-doped nanocrystalline silicon oxide layer 304 by magnetron sputtering to optimize interface recombination and improve the interface matching performance of subsequent stacking; finally, the HJT crystalline silicon bottom cell was obtained.
[0061] In step S2, a vanadium oxide hole transport layer 308 is deposited on the surface of the indium zinc oxide composite layer 307 of the HJT crystalline silicon solar cell to cover the defect sites on the silicon solar cell surface. Specifically, this includes fixing the HJT crystalline silicon solar cell onto a sample tray and placing it in the sample support position within the atomic layer deposition reaction chamber. Then, the automatic vacuum system is activated to evacuate the reaction chamber to a background vacuum level better than 0.005 torr, and the system is preheated to the set reaction temperature to ensure stable deposition. After reaching the set process conditions, the metal precursor source gas and the reaction gas are sequentially introduced, and the atomic layer deposition process is initiated using a cyclic pulse method, allowing vanadium oxide to be deposited layer by layer on the surface of the indium zinc oxide composite layer 307 of the HJT crystalline silicon solar cell, forming the vanadium oxide hole transport layer 308 that covers the defect sites on the silicon solar cell surface. When the deposited layer reaches a preset thickness of 10 nm, the precursor pulse introduction is stopped, and high-purity nitrogen gas is introduced into the reaction chamber at 760 torr for displacement and passivation treatment, thereby terminating the deposition reaction. Finally, the atomic layer deposition equipment was shut down, and the sample was removed after the system returned to normal pressure, completing the preparation of the vanadium oxide hole transport layer 308.
[0062] In step S3, anhydrous ethanol containing 2 mg / mL of [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid was added dropwise onto the vanadium oxide hole transport layer 308. The spin coater was turned on, and the spin speed was set to 3000 rpm. After spin coating for 30 seconds, the layer was placed at 100°C for heat treatment. After heat treatment for 10 minutes, a self-assembled monolayer 309 was formed on the surface of the vanadium oxide hole transport layer 308.
[0063] Finally, a perovskite / HJT crystalline silicon tandem solar cell was obtained, and its performance was tested. Its JV characteristic curve and key photovoltaic parameters are shown below. Figure 8 As shown.
[0064] Depend on Figure 8 It can be seen that, with an effective area of 1cm 2 Under the given device conditions, this tandem solar cell achieves a photoelectric conversion efficiency of 33.46%. Its open-circuit voltage is 1.972V, and its short-circuit current density is 20.87mA / cm². 2 The fill factor is 81.30%.
[0065] Example 4
[0066] The difference between this embodiment and Embodiment 1 is that: Figure 9 As shown, this embodiment provides a perovskite / HTBC crystalline silicon tandem solar cell. The bottom cell of this tandem solar cell is an HTBC crystalline silicon bottom cell; and the metal oxide hole transport layer 11 in its double-layer hole transport structure 1 is made of tungsten oxide.
[0067] The method for fabricating the perovskite / HTBC crystalline silicon tandem solar cell provided in this embodiment differs from that in Example 1 in that: In step S1, an HTBC crystalline silicon bottom cell is fabricated. For example... Figure 10 As shown, in this embodiment, the fabrication method of the crystalline silicon substrate specifically includes: selecting n-type monocrystalline silicon, using a 10% (wt)-NaOH aqueous solution for polishing and etching to remove the damaged layer of the silicon wafer, then using a 2% (wt)-NaOH solution to prepare a pyramidal textured surface and a single-sided alkaline polishing process, and then cleaning the silicon wafer using the RCA method to obtain an n-type silicon substrate 401. A tunneling oxide layer (i.e., SiO2) is sequentially deposited on the silicon wafer using an LPCVD process. x Layer 402) and n + Type 403 polycrystalline silicon layer, SiO x The thickness of layer 402 is 1.0–2.0 nm, n + A 150nm thick polycrystalline silicon 403 layer is used to construct SiO2. x / n-poly-Si stacked structure. The n-poly-Si layered structure was processed using a POCl3 tube furnace thermal diffusion process. + The 403 polycrystalline silicon layer is heavily phosphorus-doped in the n-type polycrystalline silicon layer. + A 100nm thick PSG (phosphosilicate glass) layer is grown in situ on the surface of a 403 polycrystalline silicon layer, ultimately forming SiO2. x / n + A polycrystalline silicon / PSG three-layer stacked passivation structure is used. A SiNᵧ sacrificial protective layer with a thickness of 90 nm is deposited on the surface of the PSG layer using PECVD process at a deposition temperature of 350℃ to protect the underlying SiO₂. x / n + A polycrystalline silicon / PSG passivation stack is used as a hard mask for subsequent laser patterning and wet etching. Using ultraviolet laser technology at room temperature, the SiNᵧ protective layer and the underlying PSG layer in a predetermined area on the back of the silicon wafer are selectively etched away, while the SiNᵧ / PSG / n layer on the front of the wafer is completely preserved. + Type polycrystalline silicon / SiO x Passivation layering was performed, reserving a texturing area on the back of the silicon wafer. The silicon wafer was heat-treated using a tube furnace nitrogen atmosphere annealing process at 880℃ for 30 minutes to activate phosphorus-doped impurities within the n-poly-Si layer and simultaneously repair interface defects introduced during laser etching to remove the PSG layer. Anisotropic etching of the exposed back surface of the silicon wafer was then performed using NaOH alkaline etching at 75℃ to create a pyramid-shaped optical textured surface with a height of 5μm. Subsequent room-temperature acid-alkali cleaning removed residual texturing impurities. AlO₂ was deposited on the textured back surface of the silicon wafer using an ALD process. x A passivation layer, 25 nm thick, was deposited at a temperature of 150 °C. It was applied to AlO₂ using a PECVD process. x SiN deposited above the layerx The passivation and antireflection layer, with a thickness of 90 nm, was deposited at a temperature of 350 °C, and was combined with AlO₂. x This forms the back-side composite passivation antireflection film system. An HF-based mixed acid wet etching process is used at room temperature to etch the SiNᵧ and AlO₂ layers onto the front side of the silicon wafer. x The SiNᵧ and underlying PSG layers were all etched and peeled off layer by layer, exposing the n-type silicon dioxide. + The front side substrate of a polycrystalline silicon wafer is prepared. An intrinsic hydrogenated amorphous silicon layer 404 and a boron-doped nanocrystalline silicon oxide layer 405 are sequentially deposited on the front side of the wafer using PECVD. The intrinsic hydrogenated amorphous silicon layer 404 has a thickness of 8 nm, and the boron-doped nanocrystalline silicon oxide layer 405 has a thickness of 15 nm. The deposition temperature is 200℃, forming a hole-selective passivation transport stack. At room temperature, a UV laser is used to selectively etch away the hole-selective passivation transport stack in the electrode contact window area, achieving electrical isolation between the n-type and p-type contact areas on the front side of the battery. An indium tin oxide transparent electrode layer 406 with a thickness of 100 nm is deposited on the surface of the boron-doped amorphous silicon film using magnetron sputtering PVD at a deposition temperature of 120℃, enabling lateral transport of photogenerated carriers on the surface. A wet edge etching process is used at room temperature to remove a ring of indium tin oxide conductive film around the perimeter of the silicon wafer, preventing leakage and short circuits caused by overlapping of the conductive layers on the front and back sides of the battery. Silver electrode paste was printed on the surface of the indium tin oxide conductive layer using screen printing. The silver electrode 407 was then rapidly sintered at a peak temperature of 800℃, resulting in a thickness of 20 μm after sintering, thus completing the fabrication of the metallized current collection structure for the battery. An indium zinc oxide composite layer 408 with a thickness of 15 nm was deposited on the side of the HTBC crystalline silicon bottom cell used for connection with the perovskite top cell. This layer was used to optimize the interface matching performance of subsequent stacking layers, resulting in the HTBC crystalline silicon bottom cell.
[0068] In step S2, the tungsten target is fixedly installed on the target position within the magnetron sputtering chamber. The HTBC crystalline silicon bottom cell sample is then fixed on the sample tray and placed in the sample holder within the sputtering chamber. The target-substrate distance is adjusted to the preset distance, and the sputtering chamber door is sealed. The vacuum system is activated, and the sputtering chamber is evacuated to a background vacuum level better than 5.0 × 10⁻⁶. -4Pa. Subsequently, high-purity argon and oxygen were introduced into the sputtering chamber as reactants, and the working pressure was adjusted to the set value. Simultaneously, the sample rotation system was activated to ensure uniform deposition. The sputtering power was set and the power supply was turned on. The tungsten target was pre-sputtered for several minutes in an argon atmosphere to remove surface contaminants and stabilize the plasma state. After the glow discharge stabilized, the substrate baffle was opened to initiate the deposition process. During sputtering, tungsten oxide was gradually deposited on the surface of the indium zinc oxide composite layer 408, forming a tungsten oxide hole transport layer 409 covering surface defect sites. When the deposited layer thickness reached 10 nm, the substrate baffle was closed, the sputtering power was stopped, the introduction of argon and oxygen was stopped, the magnetron sputtering system was shut down, and the sample was removed, completing the preparation of the tungsten oxide hole transport layer 409.
[0069] In step S3, anhydrous ethanol containing 2 mg / mL of [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid was dropped onto the tungsten oxide hole transport layer 409. The spin coater was turned on, and the spin speed was set to 3000 rpm. After spin coating for 30 seconds, the layer was placed at 100°C for heat treatment. After heat treatment for 10 minutes, a self-assembled monolayer 410 was formed on the surface of the tungsten oxide hole transport layer 409.
[0070] Finally, a perovskite / HTBC crystalline silicon tandem solar cell was obtained, and its performance was tested. Its JV characteristic curve and key photovoltaic parameters are shown below. Figure 11 As shown.
[0071] Depend on Figure 11 It can be seen that, with an effective area of 1cm 2 Under the given device conditions, this tandem solar cell achieves a photoelectric conversion efficiency of 30.03% with output from the two-terminal tandem cells, an open-circuit voltage of 1.966V, and a short-circuit current density of 19.01mA / cm². 2 The fill factor is 80.34%. With a stacked structure, the HTBC bottom cell achieves a photoelectric conversion efficiency of 10.90%, an open-circuit voltage of 0.719V, and a short-circuit current density of 19.93mA / cm². 2 The fill factor is 76.10%.
[0072] Therefore, this application constructs a bilayer interface structure consisting of a metal oxide hole transport framework layer and a self-assembled monomolecular dipole control layer, achieving synergistic optimization between interface coverage and energy level control. This results in leakage current suppression, energy level matching adjustment, and enhanced hole selective transport. Specifically, the metal oxide layer effectively covers the rough silicon interface and suppresses lateral leakage channels caused by incomplete local coverage of the self-assembled monomolecular layer 12, while providing hole transport channels. The self-assembled monomolecular layer 12 adjusts the interface work function through interfacial dipole interaction, thereby improving the energy level matching relationship between the perovskite layer and the bottom cell. The synergistic effect of these two layers achieves a combined improvement in interface leakage current suppression and hole selective extraction. Compared to a single self-assembled monomolecular layer 12 structure or a single metal oxide hole transport layer 11 structure, the bilayer structure provided in this application exhibits a synergistic enhancement effect in interface integrity, carrier selectivity, and interface recombination suppression. This results in improved photoelectric conversion efficiency and fill factor at the device level, while simultaneously improving device operational stability.
[0073] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0074] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A double-layer hole transport structure used in a tandem solar cell, characterized in that, Including those set up in a stacked manner: A metal oxide hole transport layer is formed directly on the surface of a crystalline silicon bottom cell and constitutes a hole transport framework layer to cover the rough structure of the crystalline silicon bottom cell surface and suppress lateral leakage; the thickness of the metal oxide hole transport layer is any value from 0.3 nm to 30 nm. A self-assembled monolayer is formed on the surface of the metal oxide hole transport layer to adjust the interfacial dipole moment to achieve interfacial work function regulation, and works synergistically with the metal oxide hole transport layer to achieve selective hole transport and interfacial recombination suppression.
2. The double-layer hole transport structure as described in claim 1, characterized in that, The material of the metal oxide hole transport layer is selected from one or more of vanadium oxide, tungsten oxide, or molybdenum oxide.
3. The double-layer hole transport structure as described in claim 1, characterized in that, The self-assembled monolayer is an organic molecular layer containing hole transport groups and anchoring groups; the hole transport groups include carbazole groups, triphenylamine groups, fluorene groups or aromatic amine groups; the anchoring groups include phosphate or carboxylic acid anchoring groups.
4. A stacked solar cell, characterized in that, include: Crystalline silicon bottom cell, wide-bandgap perovskite top cell, and the double-layer hole transport structure according to any one of claims 1 to 3; The dual-layer hole transport structure is disposed between the crystalline silicon bottom cell and the perovskite top cell to achieve selective hole transport at the interface, suppression of lateral leakage current, and reduction of non-radiative recombination.
5. The tandem solar cell as described in claim 4, characterized in that, The crystalline silicon bottom cell is a tunneling silicon oxide passivated contact cell, a heterojunction cell, or a crystalline silicon cell with a passivated contact structure.
6. The tandem solar cell as described in claim 4, characterized in that, Stacked solar cells are either stacked at two ends or stacked at three ends.
7. The method for preparing a tandem solar cell according to any one of claims 4 to 6, characterized in that, Includes the following steps: S1. Fabrication of crystalline silicon bottom solar cells; S2. A metal oxide hole transport layer is deposited on the surface of the crystalline silicon substrate; S3. A self-assembled monolayer is deposited on the surface of the metal oxide hole transport layer; S4. Construct a perovskite top cell on the self-assembled monolayer to obtain the stacked solar cell.
8. The preparation method according to claim 7, characterized in that, In step S3, the method for forming the self-assembled monolayer is either a solution method or a vapor deposition method.
9. The preparation method according to claim 8, characterized in that, When the self-assembled monolayer is formed using a solution method, the metal oxide hole transport layer is immersed in a solution containing self-assembled monomolecules or the solution is coated onto its surface, followed by heat treatment.
10. The preparation method according to claim 8, characterized in that, When the self-assembled monolayer is formed using vapor deposition, it is formed by direct deposition on the surface of the metal oxide hole transport layer using vacuum evaporation or chemical vapor deposition.