Application of a green blend solvent in the fabrication of perovskite photovoltaic devices

By using a blended solvent system of MDMO and EL, the process window challenge of green solvent systems in perovskite photovoltaic devices was solved, enabling the preparation of dense and uniform thin films, improving photoelectric conversion efficiency, and making it suitable for the preparation of perovskite photovoltaic devices.

CN123076159APending Publication Date: 2026-11-10SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611448910.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing green solvent systems have several drawbacks when preparing perovskite photovoltaic devices, including difficulty in transferring the process window, poor PbI2 solubility, difficulty in preparing dense and uniform thin films, and inability to achieve the nucleation rate control effect of traditional DMF/DMSO solvents.

Method used

A perovskite precursor solution was prepared by using a blend of methyl 5-(dimethylamino)-2-methyl-5-oxovalerate (MDMO) and ethyl lactate (EL) as solvents. By adjusting the solvent composition and spin-coating process, combined with ethyl acetate liquid displacement, pre-drying, vacuum solvent removal and heat treatment, a dense and uniform perovskite absorber layer was formed.

Benefits of technology

The fabrication of dense and uniform perovskite thin films was achieved, which improved the photoelectric performance. The photoelectric conversion efficiency of the perovskite photovoltaic module reached 25.54%, and the problem of poor edge crystallization during large-area fabrication was solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076159A_ABST
    Figure CN123076159A_ABST
Patent Text Reader

Abstract

This invention provides an application of a green blended solvent in the fabrication of perovskite photovoltaic devices. It utilizes MDMO and EL to form a binary precursor solvent, which is a low-toxicity solvent system with minimal environmental impact. MDMO provides a polar aprotic solvation environment for precursor components such as PbI2, PbBr2, FAI, MAI, CsI, and RbCl, while EL is used to adjust the viscosity, surface tension, wettability, and desolvation process of the mixed solvent. This fully green solvent system not only produces dense perovskite films with uniform surface morphology, resulting in more uniform film crystallization and solving the problem of poor edge crystallization in large-area fabrication, but also exhibits superior photoelectric performance compared to films prepared using traditional DMSO / DMF. The perovskite photovoltaic module achieves a maximum photoelectric conversion efficiency of 25.54%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of perovskite device technology, specifically relating to the application of a green blend solvent in the preparation of perovskite photovoltaic devices. Background Technology

[0002] Metal halide perovskites possess characteristics such as high absorption coefficients, tunable band gaps, long carrier diffusion lengths, high defect tolerance, and suitability for low-temperature solution processing. Compared to high-temperature vacuum deposition or high-temperature diffusion processes, solution processing can prepare absorber layers at lower temperatures, requires less equipment investment, has higher precursor material utilization, and can be integrated with processes such as spin coating, blade coating, slot coating, spraying, and printing. However, the environmental burden of perovskite solution processing cannot be judged solely by device efficiency. Currently, commonly used precursor solutions include N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), N,N-dimethylacetamide, N-methylpyrrolidone, or combinations thereof. DMF, N,N-dimethylacetamide, and N-methylpyrrolidone are of high concern regarding occupational exposure, reproductive toxicity, and regulatory management. Although DMSO, as a pure solvent, has a different hazard classification than DMF, it has a strong skin penetration promoting effect, increasing the requirements for personnel protection, waste collection, and closed-loop management of production lines in lead salt dissolution processes. During precursor coating, a large amount of solvent eventually needs to be removed from the wet film in the form of vapor. Therefore, solvent evaporation, condensation, reuse, and residual solvent treatment all affect the overall environmental performance in laboratory fume hoods, continuous coating equipment, and solvent recovery systems.

[0003] In recent years, research on green solvents has gradually shifted from screening single alternatives to solvent system engineering. Gamma-valerol, γ-butyrolactone alternatives, ethyl acetate, n-butyl acetate, ethanol, isopropanol, ethyl lactate, triethyl phosphate, cyclic carbonates, cyrene, and 5-(dimethylamino)-2-methyl-5-oxovalerate, which have bio-based origins or lower hazard characteristics, have been used for precursor dissolution, antisolvent treatment, or interfacial coating. Some studies have demonstrated that green solvents can achieve film quality and device efficiency comparable to traditional systems by stabilizing lead halide complexes, regulating the organic cation environment, guiding mesophase formation, or altering the nucleation rate. Other studies have combined green solvents with spin coating, slot coating, and small component fabrication, indicating that green processing is not limited to small-area spin coating. However, the development of green solvent systems has also exposed new technical problems, the main problems being as follows: (1) Existing green solvent research often discusses precursor solvents, antisolvents, additives, and annealing atmospheres separately, making it difficult to transfer the process window; (2) PbI2 has poor solubility in common alcohols, DMC, and esters, making it difficult to prepare high-concentration precursor solutions and thick and uniform films; (3) DMF / DMSO are strong coordination solvents and can react with PbI2. 2+By forming an intermediate phase solvent-lead complex and controlling the nucleation rate, dense, large-grained perovskite can be obtained. Current green solvents still cannot achieve this effect. Summary of the Invention

[0004] To overcome at least one of the problems existing in the prior art, one objective of this invention is to provide an application of a green blended solvent in the preparation of perovskite photovoltaic devices. A second objective of this invention is to provide a perovskite precursor solution. A third objective of this invention is to provide a method for preparing a perovskite absorber layer. A fourth objective of this invention is to provide a perovskite absorber layer obtained by the above preparation method. A fifth objective of this invention is to provide a perovskite solar cell. A sixth objective of this invention is to provide a perovskite battery module.

[0005] Methyl 5-(dimethylamino)-2-methyl-5-oxovalerate (MDMO, CAS No. 1174627-68-9) is a polar aprotic solvent with strong dipole response and solvation ability for ionic precursors, making it suitable as the main solvent for multi-component lead halide precursors. Its high boiling point is beneficial for increasing wet film leveling time, but it also increases the difficulty of solvent removal. Ethyl lactate has ester and hydroxyl groups, which can affect crystallization by altering the hydrogen bond network, surface tension, and volatilization process. For wide-bandgap mixed-halogen systems containing PbI2, PbBr2, rubidium salts, cesium salts, and organic ammonium salts, the solvent must also consider the dissolution of multiple salts, uniform distribution of iodine and bromine components, and rapid crystallization. This invention innovatively blends MDMO with ethyl lactate (EL), allowing the dissolution and coordination effects of MDMO and the rheological, wetting, and volatilization regulating effects of EL to be applied to 1.55 eV iodine-based systems and 1.82 eV wide-bandgap mixed-halogen systems.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first aspect of the present invention provides the application of a green blended solvent in the preparation of perovskite photovoltaic devices, wherein the green blended solvent comprises methyl 5-(dimethylamino)-2-methyl-5-oxovalerate and ethyl lactate.

[0007] Preferably, the volume ratio of methyl 5-(dimethylamino)-2-methyl-5-oxovalerate to ethyl lactate is (0.4-20):1.

[0008] More preferably, the volume ratio of methyl 5-(dimethylamino)-2-methyl-5-oxovalerate to ethyl lactate is (0.4-5):1.

[0009] More preferably, the volume ratio of methyl 5-(dimethylamino)-2-methyl-5-oxovalerate to ethyl lactate is any value or a range formed by any two of the following: 0.4:1, 0.6:1, 0.8:1, 1.0:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1, 2.0:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3.0:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4.0:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1, and 5.0:1.

[0010] A second aspect of the present invention provides a perovskite precursor solution comprising a perovskite precursor raw material and a green blend solution used in the first aspect.

[0011] Preferably, the perovskite precursor raw material is selected from one of the following two groups of precursor components: the first group includes PbI2, FAI, MAI and CsI; the second group includes CsI, FAI, MAI, RbCl, PbI2, PbBr2 and PbCl2.

[0012] More preferably, when the perovskite precursor raw material is selected from the first group, the total lead concentration in the perovskite precursor solution is 0.6 to 1.6 mol / L, preferably 0.8 to 1.3 mol / L.

[0013] More preferably, the second group also includes 4-guanidinobenzoate salt.

[0014] Preferably, the solvent of the perovskite precursor solution contains less than 1 wt% N,N-dimethylformamide and dimethyl sulfoxide. More preferably, it contains less than 0.1 wt%.

[0015] A third aspect of this invention provides a method for preparing a perovskite absorber layer, comprising the following steps: The perovskite precursor solution described in the second aspect is coated onto a base film, and a perovskite absorber layer is formed by antisolvent liquid displacement, pre-drying, desolvation under reduced pressure, and heat treatment.

[0016] Preferably, the basement membrane is a hole transport layer or an electron transport layer.

[0017] Preferably, the coating process includes: a first spin coating at a speed of 500-1500 rpm, and a second spin coating at a speed of 4000-6000 rpm.

[0018] More preferably, antisolvent liquid displacement is performed in the second spin coating.

[0019] Preferably, the antisolvent used in the antisolvent liquid displacement is ethyl acetate.

[0020] Preferably, the pre-drying includes pre-drying at 60–85°C for 1–5 min.

[0021] Preferably, the descaling process includes: depressurization treatment at 2–30 kPa for 0.5–10 min. Preferably, the temperature of the heat treatment is 80-150℃.

[0022] The fourth aspect of the present invention provides a perovskite absorber layer prepared by the preparation method described in the third aspect.

[0023] Preferably, the perovskite material of the perovskite absorber layer is ABX3; wherein A is at least one of MA, MDA, FA, PEA, Cs, Rb and K; MA is CH3NH3; MDA is NH3CH2NH3; FA is NH2CHNH2; PEA is C8H9NH3; B is at least one of Pb, Sn and Ge; and X is at least one of F, Cl, Br and I.

[0024] More preferably, the perovskite material of the perovskite absorber layer is Cs. 0.05 FA 0.85 MA 0.10 PbI3 or Rb 0.05 Cs 0.05 FA 0.75 MA 0.15 Pb(I 0.5 Br 0.5 3.

[0025] The fifth aspect of the present invention provides a perovskite solar cell, comprising the perovskite absorber layer described in the fourth aspect.

[0026] Preferably, the perovskite solar cell is a positive nip-type perovskite solar cell or an inverted pin-type perovskite solar cell.

[0027] More preferably, the upright nip-type perovskite solar cell includes a conductive substrate layer, an electron transport layer, a perovskite absorber layer, a hole transport layer, and a metal electrode arranged sequentially.

[0028] More preferably, the inverted pin-type perovskite solar cell includes a conductive substrate layer, a hole transport layer, a perovskite absorber layer, an electron transport layer, and a metal electrode arranged sequentially.

[0029] More preferably, the inverted pin-type perovskite solar cell includes a conductive substrate layer, a hole transport layer, a perovskite absorber layer, an interface passivation layer, an electron transport layer, a cathode interface modification layer, and a metal electrode arranged sequentially.

[0030] More preferably, the material of the conductive substrate layer includes, but is not limited to, transparent conductive glass (ITO).

[0031] More preferably, the material of the hole transport layer includes PEDOT:PSS, PTAA, 2PACz, and NiO. x At least one of 4PADCB.

[0032] More preferably, the material of the electron transport layer includes at least one of fullerene (C60) and its derivatives, PCBM, SnO2, TiO2, and ZnO.

[0033] More preferably, the thickness of the electron transport layer is 20-100 nm.

[0034] More preferably, the material of the interface passivation layer includes piperazine iodide.

[0035] More preferably, the material of the cathode interface modification layer includes bath copper alloy (BCP).

[0036] The sixth aspect of the present invention provides a perovskite battery module, comprising a plurality of perovskite solar cells as described in the fifth aspect.

[0037] The beneficial effects of this invention are: This invention provides an application of a green blended solvent in the fabrication of perovskite photovoltaic devices. It utilizes MDMO and EL to form a binary precursor solvent, which is a low-toxicity solvent system with minimal environmental impact. MDMO provides a polar aprotic solvation environment for precursor components such as PbI2, PbBr2, FAI, MAI, CsI, and RbCl, while EL is used to adjust the viscosity, surface tension, wettability, and desolvation process of the mixed solvent. This fully green solvent system not only produces dense perovskite films with uniform surface morphology, resulting in more uniform film crystallization and solving the problem of poor edge crystallization in large-area fabrication, but also exhibits superior photoelectric performance compared to films prepared using traditional DMSO / DMF. The perovskite photovoltaic module achieves a maximum photoelectric conversion efficiency of 25.54%. Attached Figure Description

[0038] Figure 1 This is a structural diagram of the perovskite solar cell device in Example 1.

[0039] Figure 2 The JV curves are representative of the 1.55 eV perovskite photovoltaic devices obtained in Examples 1-2 and Comparative Examples 1-3.

[0040] Figure 3The figures show representative JV curves of the 1.82 eV wide-bandgap perovskite photovoltaic devices obtained in Examples 3-4 and Comparative Examples 4-6; the wide-bandgap reference curve originally labeled "Comparative Example 1" in the figures corresponds to Comparative Example 2 in this specification.

[0041] Figure 4 The external quantum efficiency curves and integral short-circuit current densities of the devices obtained in Example 2 and Comparative Examples 1-3 are shown.

[0042] Figure 5 The images are scanning electron microscope images of the perovskite films obtained in Example 2 and Comparative Examples 1-3.

[0043] Figure 6 The image shows the atomic force microscopy height map and root mean square roughness of the perovskite films obtained in Example 2 and Comparative Examples 1-3.

[0044] Figure 7 The images show the X-ray diffraction patterns of the perovskite films obtained in Example 2 and Comparative Examples 1-2. Detailed Implementation

[0045] The present invention will be further described in detail below through specific embodiments. Unless otherwise specified, the raw materials used in the following embodiments can be obtained from conventional commercial channels or prepared and isolated through simple synthesis; unless otherwise specified, the processes employed are conventional processes in the art.

[0046] Example 1 This embodiment provides an inverted perovskite photovoltaic device, the structure of which is as follows: Figure 1 As shown, the inverted structure of FTO / 4PADCB / perovskite / piperazine iodide / C60 / bath copper spirit / Cu is used, and the specific preparation method is as follows: S1. FTO Substrate Treatment. FTO conductive glass sheets approximately 1.5 cm × 1.5 cm in size were sequentially ultrasonically cleaned in a cleaning agent aqueous solution, deionized water, anhydrous ethanol, and isopropanol, each step lasting approximately 15 minutes. After cleaning, the sheets were dried with nitrogen gas and subjected to UV ozone treatment for approximately 20 minutes. The treated substrate was used for hole transport layer fabrication within a short period to avoid re-adsorption of organic contaminants on the surface.

[0047] Preparation of the S2 and 4PADCB hole transport layers: 4PADCB was dissolved in anhydrous ethanol to prepare a solution of approximately 0.9 mg / mL. Approximately 60 μL of this solution was dropped onto the FTO surface and spin-coated at approximately 4000 rpm for 30 s, followed by annealing at 100℃ for 10 min to form a hole transport layer covering the FTO. All samples used the same 4PADCB solution concentration, coating volume, spin speed, and annealing program.

[0048] Preparation of conventional bandgap perovskite wet films at S3 and 1.55 eV: Preparation of conventional bandgap perovskite precursors: PbI2, FAI, MAI, and CsI are vacuum dried before use; MDMO and EL use dried solvents, and the entry of moisture from the air is minimized during solution preparation, filtration, and coating. Taking a total lead concentration of approximately 1.00 mol / L as an example, according to Cs... 0.05 FA 0.85 MA 0.10 The precursor salt was weighed according to the nominal stoichiometry of PbI3. First, PbI2 and FAI were added to MDMO and stirred at about 60°C until the system was homogeneous. Then, MAI and CsI were added, and finally EL was added and the volume ratio of MDMO:EL was adjusted to 70:30 to obtain a conventional bandgap perovskite precursor solution.

[0049] Approximately 50 μL of precursor solution was dropped onto the surface of the 4PADCB layer. The layer was then spin-coated at 1000 rpm for 10 s, followed by spin-coating at 5000 rpm for 30 s. Approximately 250 μL of ethyl acetate antisolvent was added approximately 12 s after the start of the second spin-coating stage.

[0050] S4. Segmented solvent removal and annealing. After spin coating, the 1.55 eV wet film is pre-dried at approximately 70°C for 3 min, then subjected to reduced pressure at approximately 10 kPa for 2 min, and finally annealed at 100°C for 20 min. The segmented treatment is used to stabilize the intermediate state formed by liquid displacement, promote the removal of high-boiling-point components such as MDMO, and complete the perovskite crystallization.

[0051] S5. Preparation of piperazine-onium iodide passivation layer. Dissolve piperazine-onium iodide in isopropanol to prepare a solution of approximately 0.5 mg / mL; take approximately 60 μL, spin-coat at 5000 rpm for 30 s, and treat at 100℃ for approximately 5 min.

[0052] S6. Electron transport layer, cathode interface modification layer, and electrode preparation. The sample was transferred to a vacuum evaporation apparatus, at an altitude not exceeding 5 × 10⁻⁶. -4 Under vacuum conditions of Pa, approximately 40 nm of C60 was deposited at a rate of approximately 0.05–0.15 nm / s; subsequently, approximately 8 nm of copper bath electrode and approximately 100 nm of Cu electrode were deposited sequentially to finally fabricate an inverted perovskite photovoltaic device with an effective area of ​​approximately 0.0736 cm². 2 .

[0053] Example 2 This embodiment provides an inverted perovskite photovoltaic device. The device structure and fabrication method are the same as in Embodiment 1, except that in step S3, the volume ratio of MDMO:EL is 30:70.

[0054] Example 3 This embodiment provides an inverted perovskite photovoltaic device, the structure of which is as follows: Figure 1 As shown, the inverted structure of FTO / 4PADCB / perovskite / piperazine iodide / C60 / bath copper spirit / Cu is used, and the specific preparation method is as follows: The steps of S1 and S2 are described in Example 1.

[0055] Preparation of S3, 1.82 eV wide-bandgap perovskite wet films: Preparation of wide-bandgap perovskite precursor: The nominal composition of wide-bandgap perovskite is Rb 0.05 Cs 0.05 FA 0.75 MA 0.15 Pb(I 0.5 Br 0.5 3. Taking the preparation of 1 mL of precursor as an example, weigh out 16.238 mg of CsI, 161.222 mg of FAI, 29.81 mg of MAI, 7.575 mg of RbCl, 161.35 mg of PbI2, 330.03 mg of PbBr2, and 10 mg of PbCl2; among which PbCl2 is used as a crystallization regulating additive. Use a mixed solvent with a volume ratio of MDMO:EL = 70:30, i.e., 700 μL of MDMO and 300 μL of EL, and then add 20-30 μL of pre-prepared 4-guanidinobenzoic acid salt (GBAC) additive solution. Stir thoroughly until clear, and filter through a 0.22 μm polytetrafluoroethylene filter membrane before use to obtain a wide-bandgap perovskite precursor solution.

[0056] Approximately 50 μL of precursor solution was dropped onto the surface of the 4PADCB layer. The layer was then spin-coated at 1000 rpm for 10 s, followed by spin-coating at 5000 rpm for 30 s. Approximately 250 μL of ethyl acetate antisolvent was added approximately 12 s after the start of the second spin-coating stage.

[0057] The steps S4-S6 are the same as in Example 1, and an inverted perovskite photovoltaic device is obtained.

[0058] Example 4 This embodiment provides an inverted perovskite photovoltaic device. The device structure and fabrication method are the same as those in Embodiment 3, except that in step S3, the volume ratio of MDMO:EL is 30:70.

[0059] Comparative Example 1 This comparative example provides an inverted perovskite photovoltaic device, the structure and preparation method of which are the same as in Example 1. The difference is that in step S3, the precursor solvent is the same 100 vol% MDMO, and the amount of precursor salt and solvent is kept constant.

[0060] Comparative Example 2 This comparative example provides an inverted perovskite photovoltaic device, whose device structure and preparation method are the same as in Example 1. The difference is that in step S3, the precursor solvent is 100 vol% EL, and the amounts of precursor salt and solvent are kept constant.

[0061] Comparative Example 3 This comparative example provides an inverted perovskite photovoltaic device. The device structure and preparation method are the same as in Example 1. The difference is that in step S3, the precursor solvent is a DMF:DMSO mixed solvent with a volume ratio of 4:1, while keeping the amount of precursor salt and solvent constant.

[0062] Comparative Example 4 This comparative example provides an inverted perovskite photovoltaic device, the structure and preparation method of which are the same as in Example 3. The difference is that in step S3, the precursor solvent is the same 100 vol% MDMO, and the amount of precursor salt and solvent is kept constant.

[0063] Comparative Example 5 This comparative example provides an inverted perovskite photovoltaic device, the structure and preparation method of which are the same as in Example 3. The difference is that in step S3, the precursor solvent is 100 vol% EL, and the amount of precursor salt and solvent remains unchanged.

[0064] Comparative Example 6 This comparative example provides an inverted perovskite photovoltaic device. The device structure and preparation method are the same as in Example 3. The difference is that in step S3, the precursor solvent is a DMF:DMSO mixed solvent with a volume ratio of 4:1, and the amount of precursor salt and solvent is kept constant.

[0065] Performance testing 1. Current-voltage characteristic curve detection Current-voltage characteristic curve ( J - V ( ) is an important indicator reflecting the performance of photovoltaic cell devices. Through J - V The open-circuit voltage of a perovskite solar cell can be obtained through testing. V OC ) and short-circuit current ( J SC The fill factor (FF) of the device is calculated by combining the maximum power point (MPP), and the power conversion efficiency (PCE) of the perovskite solar cell is further obtained to measure its ability to utilize sunlight.

[0066] The photovoltaic performance of the device was tested using the Guangyan SS-F5-3A solar simulator at a light intensity of 100 mW / cm², calibrated using a standard monocrystalline silicon solar cell (SRC-00019). The JV curve was measured using a Keithley 2400, and the effective area of ​​the device was 0.0736 cm². The PCE was calculated from the measured VOC, JSC, and FF. Representative parameters for the 1.55 eV and 1.82 eV devices are listed in Tables 1 and 2, respectively.

[0067] Figure 2 Table 1 shows that the 1.55 eV group all exhibit typical photovoltaic responses. The PCE of the pure MDMO system in Comparative Example 1 is 24.68%, indicating that MDMO can support the dissolution and film formation of multi-cationic iodide-based perovskites. The PCE of the pure EL system in Comparative Example 2 is 22.60%, indicating that EL alone still has limitations in solvation or crystallization when used as the main solvent. Examples 1 and 2 used an MDMO:EL blend solvent, achieving PCEs of 25.30% and 25.54%, respectively. The FF of Example 2 was 85.38%, indicating that the blend solvent can achieve a good balance between precursor dissolution, wet film spreading, and solvent removal crystallization.

[0068] From the perspective of marginal optimization difficulty for high-efficiency devices, PCE is not a single parameter, but rather the result of the combined effects of VOC, JSC, and FF. When the baseline efficiency has reached 24.68%, achieving an absolute improvement of more than 0.5 percentage points usually requires simultaneously suppressing recombination loss, improving charge transport, and maintaining film uniformity, significantly increasing the optimization difficulty compared to the lower efficiency range. In this group, Examples 1 and 2 improved by 0.62 and 0.86 percentage points, respectively, and Example 2 also saw a simultaneous improvement of 4.51 percentage points in FF. Combined with the results of continuous SEM coverage and reduced AFM roughness, this improvement can be attributed to the synergistic regulation of the wet film and crystallization process by the blended solvent, indicating significant technical effectiveness.

[0069] Table 11.55 Representative photovoltaic parameters of various eV perovskite examples and comparative examples

[0070] Table 21.82 Representative photovoltaic parameters of various eV wide-bandgap perovskite examples and comparative examples

[0071] Figure 3Table 2 further demonstrates that the green blend solvent is also suitable for 1.82 eV wide-bandgap perovskite devices. In Comparative Examples 4 and 5, using pure MDMO and pure EL, the PCE was 17.59% and 17.52%, respectively. In Example 3, using MDMO:EL = 70:30, VOC, JSC, and PCE increased to 1.356 V, 17.39 mA / cm², and 19.05%, respectively, with the PCE higher than Comparative Example 6's 18.71%. In Example 4, using MDMO:EL = 30:70, the PCE was 17.69%. The performance improvement in Example 3 mainly came from the higher VOC and JSC. Although its FF was slightly lower than Comparative Example 6, the overall output was still the highest among the wide-bandgap group, indicating that the 70:30 blend ratio is more beneficial for the film formation and carrier collection of the mixed-halogen wide-bandgap perovskite in this formulation.

[0072] 2. Photogenerated carrier generation and collection energy EQE testing is used to verify the ability of a device to generate and collect photogenerated carriers at different wavelengths. Figure 4 The actual comparison involved four groups of devices: Comparative Examples 1-3 and Example 2. The short-circuit current densities obtained by integrating the EQE curves are shown in the figure, labeled as 25.16, 25.08, 24.47, and 25.65 mA / cm², respectively. All four curves cover the main visible light response region of the perovskite absorption layer, indicating that all four groups of devices have a complete spectral response. Comparative Examples 3 and Example 2 maintain a high and relatively smooth response plateau in the main spectral region, indicating that the blend system can form an absorption layer with good optical absorption and charge collection continuity. The curves of Comparative Examples 1 and 2 show relative decreases or fluctuations in some wavelength bands, indicating that the single solvent endpoint has a more significant impact on film thickness uniformity, grain boundary recombination, or interface collection.

[0073] Structural and morphological characterization 1. Characterization using scanning electron microscopy and atomic force microscopy Figure 5The images show SEM images of the four perovskite films. Comparative Example 3 shows a surface composed of interconnected polygonal grains with clear grain boundaries, and locally visible smaller grains and bright / dark undulations; this reflects the characteristics of a polycrystalline film formed under traditional liquid displacement conditions in the DMF:DMSO system. Comparative Example 1 shows a change in grain size and morphology distribution on the pure MDMO film surface, with relatively gentle grain boundaries in some areas, but some bright areas or local undulations are still observable, indicating that high-boiling-point MDMO affects crystallization and surface shrinkage behavior. Comparative Example 2 shows a more obvious grain size inhomogeneity and grain boundary undulations on the pure EL film surface, with some grain connections being less smooth than in the blended system. This is consistent with the weaker high-voltage end collection characteristic in its JV curve, suggesting that the pure EL system may have inconsistent local nucleation rates, insufficient salt solvation, or differences in film surface shrinkage. The MDMO:EL blend film in Example 2 has clear grain boundaries, continuous connections between larger grains, and no large-area through-holes. Compared to the two pure solvent endpoints, the surface morphology is more uniform, indicating that the blend solvent has a balancing effect on wet film spreading and crystallization rate.

[0074] Figure 6 The AFM height map and corresponding root mean square roughness Rq are shown. Comparative Example 1 has an Rq of 22.4 nm, Comparative Example 2 has an Rq of 23.2 nm, Comparative Example 3 has an Rq of 20.1 nm, and Example 2 has an Rq of 19.8 nm. The scanning areas and micrometer-scale scales of the four samples are consistent, allowing for direct relative comparison. Example 2 has the lowest Rq, indicating that the surface height fluctuation of the MDMO:EL blend system is less than that of the three comparative samples. Comparative Examples 1 and 2 have higher Rqs than Comparative Example 3, indicating that pure MDMO and pure EL exhibit more pronounced local surface fluctuations at the endpoints under the experimental conditions.

[0075] AFM and SEM results are complementary: SEM mainly shows grain boundaries, grain connections, and microscopic defects, while AFM shows nanoscale height variations formed by grain tops and grain boundaries. Example 2 shows relatively continuous grain coverage in SEM and a low Rq of 19.8 nm in AFM, indicating that its morphological advantages are reflected not only in the planar direction but also in the surface height direction.

[0076] 2. X-ray diffraction characterization Figure 7The accompanying figures show the X-ray diffraction results of films formed by the three precursor solvents EL, MDMO, and MDMO:EL, as indicated in the actual figures. All three curves show the main diffraction peaks of the perovskite film within the same 2θ range, and the peak positions are generally consistent, indicating that EL, MDMO, and the MDMO:EL blend solvents can all induce the formation of the same type of perovskite main crystalline phase. The blend curves differ from the two pure solvent curves in peak intensity, peak shape, and background fluctuations, indicating that the blend solvents alter the crystal orientation distribution, grain size distribution, or intermediate phase transformation process, but do not show a fundamental change in the main crystalline phase.

[0077] In summary, the core of this invention lies in using a binary blend of MDMO and ethyl lactate as a precursor solvent, and matching the solvent composition with the salt formulation, spin-coating procedure, ethyl acetate liquid displacement, pre-drying, vacuum solvent removal, and annealing conditions for perovskites with different band gaps. Examples 1-2 and Comparative Examples 1-3 constitute a 1.55 eV group, and Examples 3-4 and Comparative Examples 4-6 constitute a 1.82 eV wide band gap group; within each band gap group, the perovskite composition, device structure, and testing conditions are kept consistent, thereby comparing the influence of the precursor solvent composition. The technical effects supported by the current figures and tables include: MDMO, EL, and their blends can be used to form the perovskite host phase; the MDMO:EL blend system achieves 25.54% PCE and 85.38% FF in a 1.55 eV device, and exhibits a relatively uniform surface morphology in surface SEM and AFM; in a 1.82 eV wide-bandgap device, MDMO:EL=70:30 achieves 19.05% PCE, higher than the 18.71% of Comparative Example 6, demonstrating that the green blending solvent is suitable for mixed-halogen wide-bandgap perovskite precursors. The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. The application of a green blend solvent in the preparation of perovskite photovoltaic devices, characterized in that, The green blend solvent includes methyl 5-(dimethylamino)-2-methyl-5-oxovalerate and ethyl lactate.

2. The application according to claim 1, characterized in that, The volume ratio of methyl 5-(dimethylamino)-2-methyl-5-oxovalerate to ethyl lactate is (0.4-20):

1.

3. A perovskite precursor solution, characterized in that, Includes perovskite precursor raw materials and green blend solutions in the applications described in claim 1 or 2.

4. A method for preparing a perovskite absorber layer, characterized in that, Includes the following steps: The perovskite precursor solution described in claim 3 is coated onto a base film, and a perovskite absorber layer is formed by antisolvent liquid displacement, pre-drying, desolvation under reduced pressure, and heat treatment.

5. The method for preparing the perovskite absorber layer according to claim 4, characterized in that, The antisolvent used in the liquid displacement process is ethyl acetate.

6. The method for preparing the perovskite absorber layer according to claim 4, characterized in that, The heat treatment temperature is 80-150℃.

7. The perovskite absorber layer prepared by the preparation method according to any one of claims 4-6.

8. The perovskite absorber layer according to claim 7, characterized in that, The perovskite material of the perovskite absorber layer is ABX3; wherein A is at least one of MA, MDA, FA, PEA, Cs, Rb and K; MA is CH3NH3; MDA is NH3CH2NH3; FA is NH2CHNH2; PEA is C8H9NH3; B is at least one of Pb, Sn and Ge; and X is at least one of F, Cl, Br and I.

9. A perovskite solar cell, characterized in that, Includes the perovskite absorber layer as described in claim 7.